Plastic floor and method for manufacturing the same

By first applying a primer layer and sanding it onto the PVC substrate, and then applying a topcoat layer, the problem of inconsistent reflectivity in PVC flooring was solved, achieving uniform gloss and improving the customer experience.

CN112354826BActive Publication Date: 2026-11-24JIANGSU BBL HOME TECH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202011194945.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-10-30
Publication Date
2026-11-24
Estimated Expiration
2040-10-30

AI Technical Summary

Technical Problem

The reflective properties of vinyl flooring vary depending on the visual range and viewing angle, which affects the customer experience.

Method used

First, a primer layer is rolled onto the PVC substrate. When the primer layer is 60-70% cured, it is sanded. Then, a topcoat layer is rolled onto the substrate and cured again. By controlling parameters such as sanding rate and abrasive belt grit size, the surface roughness is made suitable and the gloss is consistent.

Benefits of technology

This results in minimal difference in the gloss of the PVC flooring surface from different viewing angles, significantly improving the customer experience.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0002753760820000101
    Figure BDA0002753760820000101
  • Figure BDA0002753760820000111
    Figure BDA0002753760820000111
Patent Text Reader

Abstract

The application discloses plastic floor and a preparation method thereof, and relates to the technical field of plastic floor. The preparation method of the plastic floor comprises the following steps: firstly, coating a primer layer on a PVC base material by rolling; when the primer layer is partially solidified by 60-70%, polishing the primer layer; and then, coating a topcoat layer by rolling and solidifying again. The surface of the primer layer is roughened by polishing the partially solidified primer layer, and the surface structure is not damaged, so that the light reflection angle is changed, the glossiness of the final plastic floor surface is controlled in a better range, and the difference in the glossiness observed from different visual angles is very small, and the customer experience is significantly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of plastic flooring technology, and particularly to plastic flooring and its preparation method. Background Technology

[0002] PVC flooring, also known as vinyl flooring, is primarily composed of polyvinyl chloride and is a popular lightweight flooring material worldwide. After surface treatment, PVC flooring exhibits varying gloss levels when viewed from different angles and directions, resulting in visual differences in the overall room décor and thus impacting the user experience.

[0003] Therefore, this application is submitted. Summary of the Invention

[0004] The purpose of this invention is to provide a method for preparing plastic flooring, which aims to ensure that the resulting plastic flooring maintains a consistent reflective effect across different visual ranges and viewing angles.

[0005] Another object of the present invention is to provide a plastic flooring that maintains a consistent reflective effect across different visual ranges and viewing angles.

[0006] The technical problem solved by this invention is achieved by the following technical solution.

[0007] This invention proposes a method for preparing plastic flooring, comprising: first, rolling a primer layer onto a PVC substrate; then, when the primer layer has cured 60-70%, sanding the primer layer; and finally, rolling a topcoat layer onto the primer layer and curing it again.

[0008] In a preferred embodiment of the present invention, grinding is performed using a sanding belt with a grit size of 60-120 mesh, and the grinding speed is controlled at 4-6 meters per minute.

[0009] In a preferred embodiment of the present invention, the abrasive belt has a grit size of 70-90 mesh, and the grinding speed is controlled at 4.5-5.5 meters per minute during grinding.

[0010] In a preferred embodiment of the present invention, during the roller coating process of the primer layer, the temperature of the coating is controlled at 30-40°C, and the temperature of the PVC substrate is 30-40°C during roller coating; preferably, the surface gloss of the PVC substrate is less than 10.

[0011] In a preferred embodiment of the present invention, the primer layer coating amount is 15-35 g / m². 2 Preferably, the roller coating speed is 12-14 mm / s, and the speed ratio of the steel roller to the rubber roller is 1:3-5.

[0012] In a preferred embodiment of the present invention, during the roller coating process of the topcoat layer, the temperature of the coating is controlled at 30-40°C, and the coating amount of the topcoat layer is 8-12 g / m². 2 Preferably, the roller coating speed is 12-14 mm / s, and the speed ratio of the steel roller to the rubber roller is 1:3-5.

[0013] In a preferred embodiment of the present invention, the materials coated on the primer layer and the topcoat layer are obtained by mixing paint and surface-modifying additives for increasing the surface tension of the paint; preferably, the mass ratio of paint to surface-modifying additives is 100:1-2.

[0014] In a preferred embodiment of the present invention, the surface modifying agent is a polyolefin mineral oil; preferably, the surface modifying agent is a C3-C5 short-chain polyolefin mineral oil; more preferably, the surface modifying agent is a C3-C5 short-chain polyolefin white oil.

[0015] In a preferred embodiment of the present invention, during the re-curing process, a curing device with an irradiation power of 60-80 watts is used to irradiate for 2-3 seconds, and then the topcoat layer is completely cured.

[0016] The present invention also proposes a plastic flooring, which is prepared by the above-described plastic flooring preparation method.

[0017] The beneficial effects of the plastic flooring and its preparation method provided by this invention are as follows: A primer layer is first roller-coated onto a PVC substrate. When the primer layer has cured 60-70%, it is sanded, and then a topcoat layer is roller-coated for further curing. Sanding the partially cured primer layer roughens the surface without damaging the surface structure, altering the light reflection angle and controlling the gloss of the final plastic flooring surface within a good range. Furthermore, the difference in gloss observed from different viewing angles is minimal, significantly improving the customer experience. Detailed Implementation

[0018] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.

[0019] The following is a detailed description of the plastic flooring and its preparation method provided in the embodiments of the present invention.

[0020] This invention provides a method for preparing plastic flooring, comprising: first, rolling a primer layer onto a PVC substrate; then, when the primer layer has cured 60-70%, sanding the primer layer; and finally, rolling a topcoat layer onto the primer layer for further curing.

[0021] The inventors creatively applied partial curing after the primer was applied, and then sanded the surface to make it rough without damaging the surface structure. This changed the angle of light reflection, allowing the gloss of the final PVC flooring surface to be controlled within a good range. Moreover, the difference in gloss observed from different angles was very small, significantly improving the customer experience.

[0022] S1, Primer layer formation

[0023] During the roller coating process of the primer layer, the temperature of the coating should be controlled at 30-40℃, and the temperature of the PVC substrate should also be 30-40℃. The surface gloss of the PVC substrate should be less than 10. Before roller coating, the PVC substrate should be preheated to the temperature of the coating, preferably slightly higher, with the temperature difference between the substrate and the coating controlled at 2-8℃. Preheating the substrate allows it to provide energy to the coating, enabling the coating to flow and wet sufficiently, which helps with batch-to-batch stability. It also ensures that the matte powder in the coating is fully dispersed, affecting light refraction after curing and drying. The surface gloss of the PVC substrate should ideally be less than 10; excessive gloss will lead to increased gloss error in the later flooring.

[0024] In a preferred embodiment of the present invention, the primer layer coating amount is 15-35 g / m². 2 The roller coating speed is 12-14 mm / s, and the speed ratio of the steel roller to the rubber roller is 1:3-5. By further controlling the parameters of the roller coating process, the visual smoothness of the coating surface can be improved. Roller coating speed that is too fast or too slow will produce overlapping marks, and the faster the speed, the denser the overlapping marks.

[0025] It should be noted that the curing degree of the primer layer is a general understanding and can be tested using the "hardness test". If it is fully cured, the hardness is too high, making it difficult to sand; if the curing degree is too low, the hardness is too low, which can easily damage the surface structure and is also not conducive to sanding.

[0026] Specifically, the PVC substrate can be commercially available PVC sheets, which will not be elaborated on here. Both the primer and topcoat are commercially available paints, such as polyurethane paint, which is commonly used for PVC flooring.

[0027] In a preferred embodiment of the present invention, the materials coated on the primer and topcoat layers are obtained by mixing paint and a surface-modifying agent for reducing the surface tension of the paint; the mass ratio of paint to surface-modifying agent is 100:1-2, and high-speed dispersion at a speed of 1200-1500 rpm is required during the preparation process. By using the surface-modifying agent to change the surface tension of the paint, the paint surface exhibits an orange peel-like effect, thereby achieving a deviation range of 5±2° for the test results at 60 degrees and 85 degrees.

[0028] Specifically, the surface-modifying agent is a polyolefin mineral oil; preferably, it is a C3-C5 short-chain polyolefin mineral oil; more preferably, it is a C3-C5 short-chain polyolefin white oil. Using a mineral oil with polyolefin as the main component can create a micro-uneven surface on the coating, similar to an orange peel effect, which is beneficial for controlling gloss differences.

[0029] S2, Polishing

[0030] Sanding is performed using a 60-120 mesh abrasive belt, with a sanding speed controlled at 4-6 meters per minute. Preferably, the abrasive belt has a grit size of 70-90 mesh, and the sanding speed is controlled at 4.5-5.5 meters per minute. By further controlling the grit size of the abrasive belt used in the primer layer sanding process and controlling the sanding speed, the inventors have ensured that the roughness of the final product is within a good range, and that the gloss is good, with minimal difference in gloss observed from different viewing angles. If the roughness exceeds the aforementioned range, it will affect the product's gloss. For example, excessively high roughness will affect the refractive index of the coating, resulting in greater light scattering on the floor surface and less change in gloss; conversely, excessively low roughness will result in too high a gloss level, making the floor too smooth, and causing greater differences in gloss from different viewing angles.

[0031] S3, Formation of the topcoat layer

[0032] In a preferred embodiment of the present invention, during the roller coating process of the topcoat layer, the temperature of the coating is controlled at 30-40°C, and the coating amount of the topcoat layer is 8-12 g / m². 2 The roller coating speed is 12-14 mm / s, and the speed ratio of the steel roller to the rubber roller is 1:3-5. If the topcoat layer is too thick, it will cover the sanding marks and obscure the advantage of small gloss differences brought about by roughness; if the topcoat layer is too thin, it will not cover the sanding marks.

[0033] In a preferred embodiment of the present invention, during the re-curing process, a curing device with an irradiation power of 60-80 watts is used to irradiate for 2-3 seconds, allowing the topcoat layer to fully cure. Using a high-energy curing device of 60-80 watts, the expected instantaneous surface temperature is 190-200°C. The high-energy light can penetrate the coating to reach the substrate, where the substrate surface is photoexcited and released as heat. This heat excites the flow of the semi-cured coating. The resin and powdered solids in the coating flow at different speeds, resulting in dark flow and achieving a rough surface effect after curing.

[0034] The present invention also proposes a type of plastic flooring, which is prepared by the above-mentioned plastic flooring preparation method. It can maintain a consistent reflective effect in different visual ranges and different viewing angles, resulting in a better customer experience.

[0035] The features and performance of the present invention will be further described in detail below with reference to embodiments.

[0036] Example 1

[0037] This embodiment provides a method for preparing plastic flooring, wherein the coating materials used for the primer layer and topcoat layer are obtained by mixing polyurethane paint and C4 short-chain polyolefin mineral oil in a ratio of 100:1.5, and specifically includes the following steps:

[0038] (1) Primer layer formation: Preheat the PVC substrate with a surface gloss of less than 10 to 35°C, then control the temperature of the primer coating at 30°C, the roller coating speed at 13 mm / s, the speed ratio of the steel roller to the rubber roller at 1:4, and the primer coating amount at 25 g / m. 2 .

[0039] (2) Grinding: After the primer layer has cured 65%, use an 80-grit sander to grind the surface of the primer layer, controlling the grinding speed to 5 meters / minute.

[0040] (3) Topcoat layer formation: The temperature of the topcoat is controlled at 30℃, the roller coating speed is 13mm / s, the speed ratio of the steel roller to the rubber roller is 1:4, and the topcoat layer coating amount is 10g / m. 2 Irradiate the surface with a 70-watt curing device for 2 seconds, then allow the topcoat layer to fully cure.

[0041] Example 2

[0042] This embodiment provides a method for preparing plastic flooring, wherein the coating materials used for the primer and topcoat layers are obtained by mixing polyurethane modified UV-curable paint and C3 short-chain polyolefin mineral oil in a 100:1 ratio, specifically including the following steps:

[0043] (1) Primer layer formation: Preheat the PVC substrate with a surface gloss of less than 10 to 40°C, then control the temperature of the primer coating at 40°C, the roller coating speed at 12 mm / s, the speed ratio of the steel roller to the rubber roller at 1:3, and the primer coating amount at 15 g / m. 2 .

[0044] (2) Grinding: After the primer layer has cured 65%, use a 60-mesh sander to grind the surface of the primer layer, controlling the grinding speed to 4 meters / minute.

[0045] (3) Topcoat layer formation: The temperature of the topcoat is controlled at 30℃, the roller coating speed is 12mm / s, the speed ratio of the steel roller to the rubber roller is 1:3, and the topcoat layer coating amount is 8g / m. 2 Irradiate the surface with a 60-watt curing device for 3 seconds, then allow the topcoat layer to fully cure.

[0046] Example 3

[0047] This embodiment provides a method for preparing plastic flooring, wherein the coating materials used for the primer and topcoat layers are obtained by mixing polyurethane modified UV-curable paint and C5 short-chain polyolefin mineral oil in a ratio of 100:2, specifically including the following steps:

[0048] (1) Primer layer formation: Preheat the PVC substrate with a surface gloss of less than 10 to 30°C, then control the temperature of the primer coating at 30°C, the roller coating speed at 14 mm / s, the speed ratio of the steel roller to the rubber roller at 1:5, and the primer coating amount at 35 g / m. 2 .

[0049] (2) Grinding: After the primer layer has cured 65%, use a 120-grit sander to grind the surface of the primer layer, controlling the grinding speed to 6 meters / minute.

[0050] (3) Topcoat layer formation: The temperature of the topcoat is controlled at 30℃, the roller coating speed is 14mm / s, the speed ratio of the steel roller to the rubber roller is 1:5, and the topcoat layer coating amount is 12g / m. 2 Irradiate the surface with an 80-watt curing device for 2 seconds, then allow the topcoat layer to fully cure.

[0051] Comparative Example 1

[0052] This comparative example provides a method for preparing plastic flooring, which differs from Example 1 only in that it does not involve sanding.

[0053] Comparative Example 2

[0054] This comparative example provides a method for preparing plastic flooring, which differs from Example 1 only in that sanding is performed when the primer layer is 50% cured.

[0055] Comparative Example 3

[0056] This comparative example provides a method for preparing plastic flooring, which differs from Example 1 only in that sanding is performed when the primer layer is 80% cured.

[0057] Comparative Example 4

[0058] This comparative example provides a method for preparing plastic flooring, which differs from Example 1 only in that the sanding rate is controlled at 3 meters per minute.

[0059] Comparative Example 5

[0060] This comparative example provides a method for preparing plastic flooring, which differs from Example 1 only in that the sanding rate is controlled at 8 meters per minute.

[0061] Comparative Example 6

[0062] This comparative example provides a method for preparing plastic flooring, which differs from Example 1 only in that mineral oil is not added to the coating material.

[0063] Comparative Example 7

[0064] This comparative example provides a method for preparing plastic flooring, which differs from Example 1 only in that: when the topcoat layer is cured, a 30-watt curing device is used to irradiate it for 2 seconds, and then the topcoat layer is completely cured.

[0065] Experimental Example 1

[0066] The surface gloss of the plastic flooring prepared in Examples 1-3 was tested using a gloss meter at angles of 60 degrees and 85 degrees.

[0067] Testing revealed that the gloss difference of the plastic flooring obtained in Examples 1-3 was 5±2° when tested at the same location on the flooring at 60° and 85° angles; the gloss difference was also 5±2° when tested at different locations on the flooring at 60° angles; and the gloss difference was also 5±2° when tested at different locations on the flooring at 85° angles.

[0068] Experimental Example 2

[0069] The surface gloss of the plastic flooring prepared in Comparative Examples 1-7 was tested using a gloss meter at angles of 60 degrees and 85 degrees.

[0070] Table 1. Test results of surface gloss of PVC flooring in the examples and comparative examples.

[0071]

[0072]

[0073] Testing revealed that the gloss of the plastic flooring prepared in the embodiments of the present invention showed little difference from various angles, with a deviation value significantly lower than that of the comparative example.

[0074] In summary, the PVC flooring and its preparation method provided by this invention involve first rolling a primer layer onto a PVC substrate, then sanding the primer layer when it is 60-70% cured, and finally rolling on a topcoat layer for further curing. By sanding the partially cured primer layer to create a rough surface without damaging the surface structure, the angle of light reflection can be altered, resulting in a better control of the gloss level of the final PVC flooring surface. Furthermore, the difference in gloss level observed from different viewing angles is minimal, significantly improving the customer experience.

[0075] The embodiments described above are some, but not all, embodiments of the present invention. The detailed description of the embodiments of the present invention is not intended to limit the scope of the claimed invention, but merely to illustrate selected embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort are within the scope of protection of the present invention.

Claims

1. A method for preparing plastic flooring, characterized in that, This includes: first, roller coating a primer layer onto a PVC substrate; then, when the primer layer has cured 60-70%, sanding the primer layer; and finally, roller coating a topcoat layer onto the primer layer and curing it again. Sanding is performed using a 70-90 mesh abrasive belt, with a sanding speed controlled at 4.5-5.5 meters per minute. The materials coated on the primer and topcoat layers are a mixture of paint and surface modifiers. The mass ratio of the paint to the surface modifier is 100:1-2. The surface modifier is C3-C5 short-chain polyolefin mineral oil. During the second curing process, the topcoat layer is irradiated for 2-3 seconds using a curing device with an irradiation power of 60-80 watts to ensure complete curing.

2. The method for preparing plastic flooring according to claim 1, characterized in that, During the roller coating process of the primer layer, the temperature of the coating is controlled at 30-40℃, and the temperature of the PVC substrate is 30-40℃ during roller coating.

3. The method for preparing PVC flooring according to claim 2, characterized in that, The surface gloss of the PVC substrate is less than 10.

4. The method for preparing plastic flooring according to claim 3, characterized in that, The coating amount of the primer layer is 15-35 g / m 2 .

5. The method for preparing plastic flooring according to claim 4, characterized in that, The roller coating speed of the primer layer is 12-14 mm / s, and the speed ratio of the steel roller to the rubber roller is 1:3-5.

6. The method for preparing plastic flooring according to claim 1, characterized in that, During the roll coating of the top coat layer, the temperature of the paint is controlled to be 30-40°C, and the coating amount of the top coat layer is 8-12 g / m 2 .

7. The method for preparing PVC flooring according to claim 6, characterized in that, The roller coating speed of the topcoat layer is 12-14 mm / s, and the speed ratio of the steel roller to the rubber roller is 1:3-5.

8. A type of plastic flooring, characterized in that, It is prepared by the method of any one of claims 1-7 for preparing plastic flooring.

Citation Information

Patent Citations

  • Manufacture method for anti-scraping and wear-resistant paint wood floor

    CN103225383A

  • Film coating process for cement fiber board production

    CN109647681A

  • Plastic floor surface treatment method

    CN110053383A

  • Ecological floor and preparation method thereof

    CN111250373A

  • Laminated board

    CN207241033U