Secondary battery and method for manufacturing the same

By covering the surface of the secondary battery positive electrode with a film of carbon-carbon unsaturated bonds and fluorine to form a compound, the problem of low lithium ion conductivity is solved, the internal resistance is reduced, the cycle characteristics are improved, and the battery life is extended.

CN112368871BActive Publication Date: 2024-10-11PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN201980044947.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-07-27
Filing Date
2019-02-21
Publication Date
2024-10-11
Estimated Expiration
2039-02-21

Smart Images

  • Figure CN112368871B_ABST
    Figure CN112368871B_ABST
Patent Text Reader

Abstract

The secondary battery comprises a positive electrode including a positive electrode active material, a negative electrode and an electrolyte. The electrolyte comprises a solvent, a lithium salt dissolved in the solvent and a film-forming compound. The film-forming compound has an unsaturated bond between carbon and carbon and fluorine. At least a portion of the surface of the positive electrode active material is covered by a film comprising lithium, oxygen, carbon and fluorine.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a secondary battery and a method for manufacturing the same. Background Art

[0002] On the surfaces of the positive and negative electrode active materials of secondary batteries represented by lithium-ion batteries, a portion of the electrolyte containing a non-aqueous solvent and a lithium salt may react irreversibly during charging and discharging.

[0003] Patent Document 1 discloses that by adding trifluoromethylmaleic anhydride to an electrolyte, an SEI (Solid Electrolyte Interphase) film is formed on the negative electrode surface to suppress an irreversible reaction on the negative electrode surface. Generally, the SEI film has lithium ion permeability.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2007-317647 Summary of the invention

[0007] Problem that the invention aims to solve

[0008] On the positive electrode side, during normal charge and discharge reactions, a coating can be formed on the positive electrode surface by oxidation reactions of additives contained in the electrolyte, etc. However, the coating formed by oxidation reactions has low lithium ion conductivity and tends to increase internal resistance.

[0009] Solutions for solving problems

[0010] One aspect of the present disclosure relates to a secondary battery comprising a positive electrode including a positive electrode active material, a negative electrode and an electrolyte, wherein the electrolyte comprises a solvent, a lithium salt dissolved in the above solvent and a film-forming compound, the above film-forming compound has an unsaturated carbon-carbon bond and fluorine, and at least a portion of the surface of the above positive electrode active material is covered by a film comprising lithium, oxygen, carbon and fluorine.

[0011] Another aspect of the present disclosure relates to a method for manufacturing a secondary battery, which includes the following steps: an assembly step of assembling a secondary battery having a positive electrode, a negative electrode and an electrolyte; and a coating formation step of immersing the above-mentioned positive electrode in a solution containing a coating-forming compound having an unsaturated carbon-carbon bond and fluorine and a lithium salt, and covering the surface of the above-mentioned positive electrode with a coating formed by reductive decomposition of the above-mentioned coating-forming compound.

[0012] Effects of the Invention

[0013] According to the above aspects of the present disclosure, a secondary battery having a coating film having excellent lithium ion conductivity and high oxidation resistance on the positive electrode surface can be obtained, thereby realizing a secondary battery having low internal resistance and high cycle characteristics.

[0014] Although the novel features of the present invention are described in the appended claims, the present invention relates to both structural and content aspects and will be better understood through the following detailed description taken in conjunction with other objects and features of the present invention and with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 This is a partially cutaway perspective view of a secondary battery according to an embodiment of the present disclosure.

[0016] Figure 2 This is a graph showing the capacity retention rate in each charge and discharge cycle for the secondary batteries of Examples and Comparative Examples. DETAILED DESCRIPTION

[0017] The secondary battery of the embodiment of the present disclosure has a positive electrode, a negative electrode and an electrolyte containing a positive electrode active material. The electrolyte contains a solvent, a lithium salt dissolved in the solvent and a film-forming compound. The film-forming compound has an unsaturated bond between carbon and carbon and fluorine (hereinafter also referred to as a CC unsaturated bond). At least a portion of the surface of the positive electrode active material is covered by a film containing lithium, oxygen, carbon and fluorine.

[0018] The coating containing lithium, oxygen, carbon and fluorine has excellent lithium ion conductivity and high oxidation resistance. We believe that by making the coating contain lithium, the lithium transfer resistance is reduced. It is also believed that by making the coating contain fluorine, the oxidation resistance of the coating is improved. By covering the surface of the positive electrode active material with the above-mentioned coating, the internal resistance of the secondary battery is low and has high cycle performance.

[0019] As the film-forming compound having fluorine and C—C unsaturated bonds, for example, cyclic anhydrides and / or cyclic carbonate compounds are used. As the cyclic anhydride, for example, derivatives obtained by replacing hydrogen in maleic anhydride with fluorine or a fluorine-containing alkyl group can be used. As the cyclic carbonate compound, for example, derivatives obtained by replacing hydrogen in vinylene carbonate or vinyl ethylene carbonate with fluorine or a fluorine-containing alkyl group can be used. In the film-forming compound, the C—C unsaturated bond can exist in the cyclic structure or in a substituent bonded to the cyclic structure. It is believed that the polymerization reaction of the film-forming compound is carried out starting from the C—C unsaturated bond, and the surface of the positive electrode active material can be covered with a dense polymer film.

[0020] In the film-forming compound, trifluoromethylmaleic anhydride is present in an amount based on Li (i.e., relative to Li +The redox equilibrium potential of / Li is about +2.5 V and has a reduction potential, and is easily decomposed by reduction. The proportion of trifluoromethylmaleic anhydride in the film-forming compound is preferably 80% by mass or more, and the film-forming compound may be entirely trifluoromethylmaleic anhydride.

[0021] It is generally believed that under normal battery usage conditions, the film-forming compound will hardly undergo a reduction reaction to form a film on the positive electrode side. However, by placing the battery in an overdischarge state, the potential of the positive electrode can be reduced to below the reduction potential of the film-forming compound. Through overdischarge treatment, the reduction reaction of the film-forming compound proceeds on the positive electrode, and a film with excellent lithium ion conductivity is formed on the surface of the positive electrode active material.

[0022] It should be noted that in the present disclosure, the fully discharged state of a secondary battery refers to a state in which the battery is discharged to a lower voltage limit within a specified voltage range in the field of equipment using the battery. The lower voltage limit may be, for example, 2.5 V. Overdischarge processing refers to a state in which the battery is discharged to a voltage lower than the lower voltage limit (overdischarge state).

[0023] From the viewpoint of suppressing structural changes of the positive electrode active material caused by overdischarge treatment, it is preferred to maintain the positive electrode potential at +2.0 V or higher based on Li during overdischarge treatment. In other words, the film-forming compound preferably has a reduction potential at a position of +2.0 V or higher based on Li.

[0024] On the other hand, overdischarge treatment sometimes causes oxidation reaction on the negative electrode, dissolving the copper foil used as the negative electrode current collector, or the negative electrode potential becomes higher than the positive electrode potential, causing polarity reversal. In order to prevent the above situation, the negative electrode may contain a lithium-containing material having a lithium ion release potential in the range of +2.0V to +3.5V based on Li. During overdischarge treatment, lithium ions are released from the lithium-containing material, thereby compensating for the charge consumed on the positive electrode side during overdischarge treatment.

[0025] As lithium-containing substances having a lithium ion release potential within the above range, for example, phosphates belonging to the space group Pnma and containing lithium and a transition metal element MA can be cited. As the transition metal element MA, Ni, Fe, Mn, Co, Cu, etc. can be cited. As specific examples of such phosphates, Li x FePO4 (0.5≤x≤1.1). Up to 30% of Fe may be replaced by transition metal elements other than Fe or Al.

[0026] As another example of a lithium-containing substance, a composite oxide belonging to the space group Immm and containing lithium and a transition metal element MB can be cited. As the transition metal element MB, Ni, Fe, Mn, Co, Cu, etc. can be cited. As a specific example of such a lithium-containing substance, Li 2+x NiO2 (-0.5≤x≤0.3). Up to 30% of Ni may be substituted with a transition metal element other than Ni or Al.

[0027] The positive electrode usually includes a positive electrode collector and a positive electrode active material layer, and the positive electrode active material layer is formed on the positive electrode collector in a manner opposite to the negative electrode with a separator sandwiched therebetween. In this case, the coating containing lithium, oxygen, carbon and fluorine can be formed in a manner covering the surface of the positive electrode active material particles contained in the positive electrode active material layer. The positive electrode active material layer has a porous structure, and when the coating is formed by overdischarge treatment, the coating forming compound can invade the voids in the positive electrode active material layer. Therefore, the coating containing lithium, oxygen, carbon and fluorine covers the positive electrode active material particles located on the surface of the positive electrode active material layer on the side opposite to the negative electrode with a separator sandwiched therebetween, and also covers the positive electrode active material particles located inside the positive electrode active material layer.

[0028] In the case where the positive electrode active material layer is a mixture (composite material) comprising a positive electrode active material, a binder (adhesive), etc., the coating comprising lithium, oxygen, carbon and fluorine may partially cover the surface of the binder. In the case where the positive electrode active material layer comprises a conductive agent, the coating may partially cover the surface of the conductive agent. Thus, the decomposition of the electrolyte components starting from the binder and the conductive agent can be suppressed.

[0029] Furthermore, the coating containing lithium, oxygen, carbon and fluorine can cover the surface of the positive electrode collector. From a microscopic point of view, the surface of the positive electrode collector has a small exposed surface and is not completely covered by the positive electrode active material and the binder. In addition, there are also cases where the cut end face and the lead mounting portion are exposed. The above-mentioned coating can also be formed on the exposed surface of the positive electrode collector. By making the above-mentioned coating cover the positive electrode collector, the decomposition of the electrolyte components starting from the surface of the positive electrode collector can also be suppressed.

[0030] The fact that the coating contains lithium, oxygen, carbon and fluorine can be confirmed by X-ray photoelectron spectroscopy (XPS) on the surface of the positive electrode taken out from the disassembled secondary battery. XPS is a method in which the sample surface is irradiated with X-rays, the kinetic energy of the photoelectrons released from the sample surface is measured, and the composition and chemical bonding state of the elements constituting the sample surface are analyzed. Energy correction can use the C1s spectrum (248.5 eV) of graphite. As a measuring device, for example, the following device can be used.

[0031] Measurement device: PHI5000VersaProbe manufactured by ULVAC-PHI, Inc.

[0032] X-ray source used: monochromatic Mg-Kα ray, 200nmΦ, 45W, 17kV

[0033] Analysis area: about 200μmΦ

[0034] The manufacturing method of the secondary battery of the embodiment of the present disclosure includes the following steps: an assembly step of assembling a secondary battery having a positive electrode, a negative electrode and an electrolyte; and a coating formation step of immersing the positive electrode in a solution containing a coating-forming compound having an unsaturated carbon-carbon bond and fluorine and a lithium salt, and covering the surface of the positive electrode with a coating formed by reductive decomposition of the coating-forming compound.

[0035] As a solution containing a film-forming compound and a lithium salt, an electrolyte can be used. For example, the film-forming process can be carried out as follows: the film-forming compound is included in the electrolyte, and after the process of assembling the secondary battery, the secondary battery is subjected to an overdischarge treatment so that the potential of the positive electrode reaches below the reduction potential of the film-forming compound, thereby carrying out. Alternatively, before the process of assembling the secondary battery or during the production of the secondary battery, the positive electrode can be immersed in a solution containing a film-forming compound, and a voltage is applied to the positive electrode to carry out a reduction reaction of the film-forming compound. When the voltage is applied, the electrode that forms a pair with the positive electrode can be either the negative electrode of the secondary battery, or other electrodes (such as lithium metal) can be used. In this case, the electrolyte of the manufactured battery may not contain a film-forming compound. By making the film-forming compound contain fluorine, a film with excellent oxidation resistance and low lithium transfer resistance can be formed on the surface of the positive electrode.

[0036] Figure 1 It is a perspective view schematically showing a square secondary battery according to one embodiment of the present disclosure. Figure 1 1 and 2 are partially cut away to illustrate the main structure of the secondary battery 1. A flat electrode group 10 and an electrolyte (not shown) are accommodated in a rectangular battery case 11.

[0037] The electrode group 10 is formed by winding a sheet-shaped positive electrode and a sheet-shaped negative electrode with a separator. However, the type and shape of the secondary battery are not particularly limited in the present disclosure. As an alternative to the wound electrode group, other electrode groups such as a stacked electrode group in which a positive electrode and a negative electrode are stacked with a separator may be used.

[0038] One end of a positive lead 14 is connected to the positive current collector of the positive electrode contained in the electrode group 10. The other end of the positive lead 14 is connected to a sealing plate 12 that functions as a positive terminal. One end of a negative lead 15 is connected to the negative current collector, and the other end of the negative lead 15 is connected to a negative terminal 13 disposed approximately in the center of the sealing plate 12. A gasket 16 is arranged between the sealing plate 12 and the negative terminal 13 to insulate the two. A frame 18 formed of an insulating material is arranged between the sealing plate 12 and the electrode group 10 to insulate the negative lead 15 from the sealing plate 12. The sealing plate 12 is joined to the open end of the square battery case 11 and seals the square battery case 11. The sealing plate 12 is formed with an injection hole 17a, and the electrolyte is injected into the square battery case 11 from the injection hole 17a. Thereafter, the injection hole 17a is blocked with a sealing plug 17.

[0039] (positive electrode)

[0040] The positive electrode includes a sheet-shaped positive electrode current collector and a positive electrode active material layer provided on the surface of the positive electrode current collector. The positive electrode active material layer may be formed on one surface or on both surfaces of the positive electrode current collector.

[0041] (Positive electrode collector)

[0042] Examples of the positive electrode current collector include metal foils, metal sheets, etc. Examples of the material of the positive electrode current collector include stainless steel, aluminum, aluminum alloys, titanium, etc. The thickness of the positive electrode current collector can be selected from a range of, for example, 3 to 50 μm.

[0043] (Positive Electrode Active Material Layer)

[0044] The case where the positive electrode active material layer is a mixture (composite material) containing positive electrode active material particles is described. The positive electrode active material layer may contain positive electrode active material particles and a binder as essential components and a conductive agent as an optional component. The amount of the binder contained in the positive electrode active material layer is preferably 0.1 to 20 parts by mass, more preferably 1 to 5 parts by mass, relative to 100 parts by mass of the positive electrode active material. The thickness of the positive electrode active material layer is, for example, 10 to 150 μm.

[0045] As the positive electrode active material, lithium-containing transition metal oxides are preferred. As transition metal elements, Sc, Y, Mn, Fe, Co, Ni, Cu, Cr, Zr, W, etc. can be listed. Among them, Ni, Co, Mn, Fe, Cu, Cr, etc. are preferred, and Mn, Co, Ni, etc. are more preferred. The lithium-containing transition metal oxide may contain one or more typical metal elements as required. As typical metal elements, Mg, Al, Ca, Zn, Ga, Ge, Sn, Sb, Pb, Bi, etc. can be listed.

[0046] Among lithium-containing transition metal oxides, lithium nickel composite oxides containing Li, Ni, and other metals are particularly preferred from the viewpoint of obtaining a high capacity. Examples of lithium nickel composite oxides include Li a Ni b M 1 1-b O2(M 1 At least one selected from the group consisting of Mn, Co and Al, 0.95≤a≤1.2, 0.3≤b≤1. ). From the viewpoint of high capacity, it is more preferable that the Ni ratio b satisfies 0.5≤b≤1. If the Ni ratio b is within the above range, it is easy to stably maintain the structure of the lithium nickel composite oxide even when overdischarged to a potential of +2.0 V based on Li. From the viewpoint of structural stability during overdischarge, the lithium nickel composite oxide further preferably contains Mn as Mn. 1 Li a Ni b Mn c Co 1-b-c O2 (0.5≤b<1, 0.1≤c≤0.4).

[0047] Specific examples of lithium nickel composite oxides include lithium-nickel-cobalt-manganese composite oxides (LiNi 0.5 Co 0.2 Mn 0.3 O2、LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2、LiNi 0.4 Co 0.2 Mn 0.4 O2, etc.), lithium-nickel-manganese composite oxide (LiNi 0.5 Mn 0.5 O2, etc.), lithium-nickel-cobalt composite oxide (LiNi 0.8 Co 0.2 O2, etc.), lithium-nickel-cobalt-aluminum composite oxide (LiNi 0.8 Co 0.15 Al 0.05 O2、LiNi 0.8 Co 0.18 Al 0.02 O2、LiNi 0.88 Co 0.09 Al 0.03 O2) etc.

[0048] The compressive strength of the lithium nickel composite oxide particles is preferably 250 MPa or more, more preferably 350 MPa or more. When the compressive strength of the lithium nickel composite oxide particles meets the above range, the particle breakage during overdischarge can be suppressed compared to when the above range is not met. It should be noted that the upper limit of the compressive strength of the lithium nickel composite oxide particles is not particularly limited, for example, from the viewpoint of material performance, it is preferably 1500 MPa or less. The compressive strength can be measured by the method specified in JIS-R1639-5.

[0049] That is, the particle compression test in the present disclosure is a test as follows: a positive electrode slurry containing the above-mentioned composite oxide particles, a conductive material, a binder, etc. is applied to a positive electrode current collector, and dried to form a positive electrode active material layer, and the obtained positive electrode active material layer is rolled to a composite material density of 3.4 g / cm 3 .

[0050] The surface of the positive electrode active material particles is covered with a film containing lithium, oxygen, carbon and fluorine and having high lithium ion conductivity and excellent oxidation resistance. The above-mentioned film is not easy to oxidize and decompose even when charged at a high voltage, and will not become an obstacle to lithium transfer during charging and discharging. Thus, even after repeated charging and discharging, the decomposition reaction of the electrolyte components on the surface of the positive electrode active material can be effectively suppressed. As a result, the capacity can be maintained at a high level after multiple charge and discharge cycles, and a long-life battery can be obtained. In addition, a battery with low internal resistance can be obtained.

[0051] The film thickness of the coating is, for example, 10 to 200 nm.

[0052] When a coating containing lithium, oxygen, carbon and fluorine is formed by overdischarge treatment of the battery, there may be regions where the coating is not formed at the contact interface between positive electrode active material particles and the bonding interface between positive electrode active material particles and the binder.

[0053] From the viewpoint of improving the filling property of the positive electrode active material in the positive electrode active material layer, it is desired that the average particle size (D50) of the positive electrode active material particles is sufficiently small relative to the thickness of the positive electrode active material layer. The average particle size (D50) of the positive electrode active material particles is, for example, preferably 5 to 30 μm, and more preferably 10 to 25 μm. It should be noted that the average particle size (D50) refers to the median particle size at which the cumulative volume reaches 50% in the volume-based particle size distribution. The average particle size can be measured, for example, using a laser diffraction / scattering particle size distribution measuring device.

[0054] Examples of the binder (adhesive) include fluororesins such as polyvinylidene fluoride (PVdF), polytetrafluoroethylene (PTFE), and tetrafluoroethylene-hexafluoropropylene copolymer (HFP); acrylic resins such as polymethyl acrylate and ethylene-methyl methacrylate copolymer; rubber-like materials such as styrene-butadiene rubber (SBR) and acrylic rubber; and water-soluble polymers such as carboxymethyl cellulose (CMC) and polyvinyl pyrrolidone.

[0055] As the conductive agent, carbon black such as acetylene black and Ketjen black is preferred.

[0056] The positive electrode active material layer can be formed as follows: positive electrode active material particles, binders, etc. are mixed with a dispersion medium to prepare a positive electrode slurry, the positive electrode slurry is applied to the surface of the positive electrode collector, dried, and then rolled, thereby forming. As a dispersion medium, water, alcohols such as ethanol, ethers such as tetrahydrofuran, N-methyl-2-pyrrolidone (NMP), etc. can be used. In the case of using water as a dispersion medium, it is preferred to use a rubber-like material and a water-soluble polymer in combination as a binder.

[0057] (negative electrode)

[0058] The negative electrode has a sheet-shaped negative electrode collector. The negative electrode may also have a negative electrode active material layer arranged on the surface of the negative electrode collector. The negative electrode active material layer contains a negative electrode active material capable of absorbing and releasing lithium. The negative electrode active material layer may be formed on one surface of the negative electrode collector or on both surfaces.

[0059] (Negative electrode current collector)

[0060] Examples of the negative electrode current collector include metal foil, metal sheet, mesh, punched sheet, expanded metal, etc. The negative electrode current collector may be made of stainless steel, nickel, copper, copper alloy, etc. The thickness of the negative electrode current collector may be selected from a range of 3 to 50 μm, for example.

[0061] (Negative Electrode Active Material Layer)

[0062] The negative electrode active material layer can be formed using a negative electrode slurry containing a negative electrode active material, a binder (adhesive) and a dispersion medium, using a method based on the manufacture of a positive electrode active material layer. The negative electrode active material layer may contain any component such as a conductive agent as needed. The amount of binder contained in the negative electrode active material layer is preferably 0.1 to 20 parts by mass, more preferably 1 to 5 parts by mass relative to 100 parts by mass of the negative electrode active material. The thickness of the negative electrode active material layer is, for example, 10 to 150 μm.

[0063] The negative electrode active material may be a non-carbon material, a carbon material, or a combination thereof. The carbon material used as the negative electrode active material is not particularly limited, and is preferably at least one selected from the group consisting of graphite and hard carbon. Among them, graphite has a high capacity and a small irreversible capacity, and is the most promising.

[0064] It should be noted that graphite is a general term for carbon materials with a graphite structure, including natural graphite, artificial graphite, expanded graphite, graphitized mesophase carbon particles, etc. Examples of natural graphite include flaky graphite and earthy graphite. Generally, the interplanar spacing d of the 002 plane of the graphite structure calculated from the X-ray diffraction spectrum is 002 Carbon materials with a 0.35-3.44 angstrom spacing are classified as graphite. On the other hand, hard carbon is a carbon material in which tiny graphite crystals are arranged in random directions and are basically not further graphitized. The interplanar spacing d of the 002 plane is 002 Greater than 3.44 angstroms.

[0065] The non-carbon material used as the negative electrode active material is preferably an alloy material. The alloy material preferably includes any one selected from silicon, tin, Ga, and In, among which silicon alone and silicon compounds are preferred. Silicon compounds include silicon oxides and silicon alloys. Metal lithium or lithium alloys can also be used as the negative electrode active material.

[0066] The negative electrode active material layer may contain a lithium-containing substance. The lithium-containing substance preferably has a lithium ion release potential in the range of +2.0V to +3.5V based on Li. For the lithium-containing substance, when a coating is formed on the positive electrode surface by overdischarge treatment, the lithium contained in the lithium-containing substance will dissolve in the electrolyte, thereby preventing deterioration caused by dissolution of the negative electrode collector (such as copper foil). As the lithium-containing substance, a material that can release lithium ions at a relatively low potential and is used as a positive electrode active material for a lithium secondary battery can be used. Examples include phosphates of lithium and transition metal elements belonging to the space group Pnma (Li x FePO4 (0.5≤x≤1.1), etc.) and composite oxides of lithium and transition metal elements belonging to the space group Immm (Li 2+x NiO2 (-0.5≤x≤0.3), etc.).

[0067] (Separator)

[0068] As the separator, a microporous film, nonwoven fabric, woven fabric, etc. made of resin is used. As the resin, polyolefins such as polyethylene (PE) and polypropylene (PP), polyamide, polyamide-imide, etc. are used.

[0069] (Electrolytes)

[0070] The electrolyte includes a solvent, a solute dissolved in the solvent, and a film-forming compound. The electrolyte may contain a known additive. The film-forming compound can be any compound having an unsaturated bond between carbon and carbon and fluorine. For example, trifluoromethyl maleic anhydride is preferably used.

[0071] Examples of the solvent include non-aqueous solvents such as cyclic carbonates, chain carbonates, cyclic carboxylates, chain carboxylates, and water. These solvents may be used alone or in combination of two or more.

[0072] As cyclic carbonate, ethylene carbonate (EC), fluoroethylene carbonate (FEC), propylene carbonate (PC), butylene carbonate, vinylene carbonate, vinyl ethylene carbonate and these derivatives etc. can be used.These can be used alone, and two or more combinations can also be used.From the viewpoint of the ionic conductivity of electrolyte, preferably use at least one in the group consisting of ethylene carbonate, fluoroethylene carbonate, propylene carbonate.

[0073] Examples of the chain carbonate include diethyl carbonate (DEC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC).

[0074] Examples of the cyclic carboxylic acid ester include γ-butyrolactone (GBL) and γ-valerolactone (GVL).

[0075] As the chain carboxylic acid ester, methyl acetate (MA), ethyl acetate (EA), propyl acetate, methyl propionate, ethyl propionate, propyl propionate and fluorides thereof can be used. As the fluoride of the chain carboxylic acid ester, methyl 3,3,3-trifluoropropionate (FMP) and 2,2,2-trifluoroethyl acetate (FEA) are preferably used from the viewpoint of viscosity and the like.

[0076] The above solvents are usually not reduced at a potential of 2.0 V or more based on Li. However, when the film-forming compound is reduced during overdischarge, its reduction decomposition product (anion radicals, etc.) may react with the above solvents. Therefore, the film formed on the positive electrode during overdischarge may contain the above solvent components.

[0077] From the viewpoint of including more fluorine in the film formed on the positive electrode, it is preferred to use a fluorinated solvent containing fluorine, oxygen and carbon as the solvent. The proportion of the fluorinated solvent containing fluorine, oxygen and carbon relative to the whole solvent is, for example, 30% by mass or more and 100% by mass or less. Thus, a film with high oxidation resistance can be formed on the positive electrode.

[0078] The fluorinated solvent containing fluorine, oxygen and carbon is preferably at least one selected from the group consisting of fluoroethylene carbonate (FEC), methyl 3,3,3-trifluoropropionate (FMP) and 2,2,2-trifluoroethyl acetate (FEA) from the viewpoint of ion conductivity of the electrolyte.

[0079] As the solute, various lithium salts are used. The concentration of the lithium salt in the electrolyte is, for example, 0.5 to 2 mol / L. Examples of lithium salts include LiPF6, LiBF4, LiClO4, LiAsF6, LiCF3SO3, LiN(SO2F)2, and LiN(SO2CF3)2. The lithium salts may be used alone or in combination of two or more.

[0080] [Example]

[0081] Hereinafter, the secondary battery of the present disclosure will be specifically described based on Examples and Comparative Examples; however, the present disclosure is not limited to the following Examples.

[0082] 《Example 1》

[0083] A secondary battery for positive electrode evaluation using metal Li as a counter electrode was prepared according to the following procedure.

[0084] (1) Preparation of positive electrode

[0085] The lithium-containing transition metal oxide (LiNi 0.60 Co 0.20 Mn 0.20 O2 (NCM)), acetylene black (AB) as a conductive material and polyvinylidene fluoride (PVdF) as a binder are mixed in a mass ratio of NCM: AB: PVdF = 100: 1: 0.9, and then an appropriate amount of N-methyl-2-pyrrolidone (NMP) is added and stirred to prepare the positive electrode slurry. After that, the obtained positive electrode slurry is applied on one side of the aluminum foil (positive electrode collector) and dried, and the coating of the positive electrode active material layer is rolled with a roller. The mass of the composite material per unit area on the produced plate was measured, and the result was 8.0 mg / cm 2 .

[0086] The obtained laminate of the positive electrode current collector and the positive electrode active material layer is cut into a predetermined electrode size to form a positive electrode having the positive electrode active material layer on one surface of the positive electrode current collector.

[0087] (2) Preparation of electrolyte

[0088] To 100 parts by mass of a mixed solution containing FEC and FMP at a mass ratio of 15:85, 1 part by mass of vinylene carbonate and 1 part by mass of trifluoromethylmaleic anhydride were added to obtain a non-aqueous solvent. LiPF6 was dissolved in the non-aqueous solvent at a concentration of 1.0 mol / L to prepare a non-aqueous electrolyte.

[0089] (3) Battery assembly

[0090] Leads were installed on the positive electrode and the Li metal counter electrode obtained above. The electrode body was prepared in such a way that the positive electrode and the Li metal counter electrode were facing each other with a separator containing PP and PE having a thickness of 0.015 mm sandwiched therebetween. The electrode body was sealed in an outer casing made of an aluminum laminate film together with a non-aqueous electrolyte to assemble a secondary battery A1.

[0091] (4) Overdischarge treatment

[0092] The secondary battery A1 was over-discharged at a constant current of 13 mA / g (relative to the mass of the positive electrode active material) until the closed circuit voltage of the battery reached 2.0 V (Li counter electrode reference).

[0093] The positive electrode was taken out from the secondary battery A1 after the overdischarge treatment, and the non-aqueous electrolyte was fully rinsed with dimethyl carbonate, dried, and then the surface XPS analysis was performed. As a result, the oxygen (O-1s) spectrum that appeared in the binding energy range of 525 to 536 eV, the carbon (C-1s) spectrum that appeared in the binding energy range of 280 to 295 eV, and the fluorine (F-1s) spectrum that appeared in the binding energy range of 680 to 690 eV were detected. From the oxygen spectrum, the peak caused by the combination of transition metals and oxygen derived from the positive electrode active material was confirmed in the range of 528 to 530 eV, and the peak caused by carbon-oxygen bonds was confirmed in the range of 530 to 536 eV. From the carbon spectrum, the peaks caused by carbon-carbon bonds and carbon-hydrogen bonds were confirmed in the range of 282 to 288 eV, and the peak caused by carbon-fluorine bonds was confirmed in the range of 288 to 293 eV. In addition, from the fluorine spectrum, a peak due to a fluorine-carbon bond was confirmed in the range of 686 to 690 eV, and a peak due to a fluorine-lithium bond was confirmed in the range of 683 to 686 eV.

[0094] (5) Evaluation

[0095] [Evaluation 1: Internal resistance measurement]

[0096] Initial charge and discharge were performed under the conditions shown in the following charge 1 and discharge 1. The charge and discharge were performed in an environment of 25°C.

[0097] (Charging 1)

[0098] The battery was charged at a constant current of 80 mA / g (relative to the mass of the positive electrode active material) until the closed circuit voltage reached 4.2 V. Thereafter, the battery was charged at a constant voltage of 4.2 V until the current value was less than 13 mA / g (relative to the mass of the positive electrode active material).

[0099] (Discharge 1)

[0100] The battery was discharged at a constant current of 130 mA / g (relative to the mass of the positive electrode active material) until the closed circuit voltage of the battery reached 2.5 V. Thereafter, the battery was discharged again at a constant current of 13 mA / g (relative to the mass of the positive electrode active material) until the closed circuit voltage of the battery reached 2.5 V.

[0101] The battery after the initial charge and discharge was charged again under the same conditions as in charge 1, and then connected to an LCR meter to measure the absolute value of impedance |Z| at 1 Hz. The impedance per unit electrode area was evaluated by multiplying the measured value by the electrode area.

[0102] [Evaluation 2: Cycle characteristics]

[0103] After the initial charge and discharge, the charge and discharge were repeated multiple times under the conditions shown in the following charge 2 and discharge 2. The charge and discharge were performed at 45° C. As described below, the deterioration of the positive electrode was accelerated by charging under higher voltage conditions than usual in charge 2.

[0104] (Charging 2)

[0105] The battery was charged at a constant current of 80 mA / g (relative to the mass of the positive electrode active material) until the closed circuit voltage reached 4.8 V. Thereafter, the battery was charged at a constant voltage of 4.8 V until the current value was less than 13 mA / g (relative to the mass of the positive electrode active material).

[0106] (Discharge 2)

[0107] The battery was discharged at a constant current of 130 mA / g (relative to the mass of the positive electrode active material) until the closed circuit voltage of the battery reached 2.5 V. Thereafter, the battery was discharged again at a constant current of 13 mA / g (relative to the mass of the positive electrode active material) until the closed circuit voltage of the battery reached 2.5 V.

[0108] The above charge and discharge cycle was repeated 30 times, and the ratio (%) of the 30th discharge capacity to the initial discharge capacity was calculated as the capacity retention rate X. 30 to make an evaluation.

[0109] Comparative Example 1

[0110] Secondary battery B1 was assembled in the same manner as in Example 1 except that trifluoromethylmaleic anhydride was not added in the preparation of the nonaqueous electrolyte. In addition, overdischarge treatment was not performed.

[0111] The assembled secondary battery B1 was evaluated in the same manner as in Example 1.

[0112] Comparative Example 2

[0113] In the preparation of the nonaqueous electrolyte, 1 part by mass of maleic anhydride was added instead of trifluoromethylmaleic anhydride. A secondary battery B2 was prepared in the same manner as in Example 1 except for the above. The secondary battery B2 after the overdischarge treatment was evaluated in the same manner as in Example 1.

[0114] The evaluation results of Example 1 and Comparative Examples 1 and 2 are shown in Table 1. Figure 2 The capacity retention rate X in each charge and discharge cycle is shown in n changes.

[0115] [Table 1]

[0116]

[0117] As shown in Table 1, the secondary battery A1 of Example 1 has a high capacity retention rate and a low resistance when compared with the secondary batteries B1 and B2 of Comparative Examples 1 and 2.

[0118] The capacity retention rate of battery B2 after 30 cycles is comparable to that of battery B1 in which the film is not formed using the film-forming compound. Figure 2 As shown in FIG. 1 , the capacity maintenance rates of batteries B1 and B2 show almost the same change in capacity maintenance rate as the charge and discharge cycles are repeated. The reason for this is considered to be as follows.

[0119] In battery B2, a coating which is a reduction decomposition product of maleic anhydride is formed on the positive electrode by overdischarge treatment. However, it is believed that the coating does not contain fluorine, so the oxidation resistance is low, and the coating is oxidatively decomposed at the beginning of the charge and discharge cycle, and it is believed that the capacity retention rate is not improved. In addition, it is inferred that the low-resistance coating remains at the beginning of the charge cycle, so the initial impedance decreases.

[0120] In contrast, in battery A1, a coating formed on the positive electrode surface is derived from the reductive decomposition of trifluoromethylmaleic anhydride caused by overdischarge treatment. This coating has oxidation resistance and excellent lithium ion conductivity. As a result, the decrease in capacity retention rate is suppressed, and it is believed that the internal resistance can be lowered.

[0121] The present invention has been described with respect to the preferred embodiments at this stage, but these disclosures are not interpreted restrictively. Various modifications and changes should be obvious to those skilled in the art of the present invention by reading the above disclosures. Therefore, it should be interpreted that the scope of the attached claims includes all modifications and changes without departing from the true spirit and scope of the present invention.

[0122] Industrial Applicability

[0123] The secondary battery disclosed herein is useful as a driving power source for personal computers, mobile phones, mobile devices, portable information terminals (PDAs), portable game devices, video recorders, etc., as a main power source or auxiliary power source for driving motors of hybrid vehicles, plug-in HEVs, etc., as a driving power source for power tools, vacuum cleaners, robots, etc., and the like.

[0124] Description of Reference Numerals

[0125] 1: Secondary battery, 10: Wound electrode group, 11: Square battery case, 12: Sealing plate, 13: Negative terminal, 14: Positive lead, 15: Negative lead, 16: Gasket, 17: Sealing plug, 17a: Liquid injection hole, 18: Frame

Claims

1. A secondary battery comprising a positive electrode containing a positive electrode active material, a negative electrode and an electrolyte, The electrolyte comprises a solvent, a lithium salt dissolved in the solvent, and a coating-forming compound. The film-forming compound has an unsaturated carbon-carbon bond and fluorine, The film-forming compound comprises trifluoromethylmaleic anhydride, At least a portion of the surface of the positive electrode active material is covered with a film containing lithium, oxygen, carbon and fluorine. The film containing fluorine contains a reduction decomposition product of the film-forming compound, The film-forming compound is a compound that is reduced at a potential of +2.0 V or higher based on Li.

2. The secondary battery according to claim 1, in, The negative electrode includes a lithium-containing material having a lithium ion release potential in the range of +2.0 V to +3.5 V based on Li.

3. The secondary battery according to claim 2, in, The lithium-containing material includes at least one of a phosphate belonging to the space group Pnma and containing lithium and a transition metal element and a composite oxide belonging to the space group Immm and containing lithium and a transition metal element.

4. The secondary battery according to claim 1 or 2, in, The positive electrode active material includes Li a Ni b M 1 1-b O 2 The lithium nickel composite oxide shown, M 1 is at least one selected from the group consisting of Mn, Co and Al, Satisfies 0.95≤a≤1.2 and 0.5≤b≤1.

5. The secondary battery according to claim 4, in, The lithium nickel composite oxide is Li a Ni b Mn c Co 1-b-c O 2 express, Satisfies 0.1≤c≤0.

4.

6. The secondary battery according to claim 4, in, The compressive strength of the lithium nickel composite oxide particles is 250 MPa or more and 1500 MPa or less.

7. The secondary battery according to claim 1 or 2, in, The solvent comprises a fluorinated solvent containing fluorine, oxygen and carbon, The ratio of the fluorinated solvent in 100 parts by mass of the solvent is 30 parts by mass or more and 100 parts by mass or less.

8. The secondary battery according to claim 7, in, The fluorinated solvent is at least one selected from the group consisting of fluoroethylene carbonate, methyl 3,3,3-trifluoropropionate, and 2,2,2-trifluoroethyl acetate.

9. A method for manufacturing a secondary battery, comprising the following steps: an assembly step of assembling a secondary battery having a positive electrode, a negative electrode and an electrolyte; and a coating forming step of immersing the positive electrode in a solution containing a coating forming compound having an unsaturated carbon-carbon bond and fluorine and a lithium salt, and covering the surface of the positive electrode with a coating formed by reductive decomposition of the coating forming compound, The film-forming compound includes trifluoromethylmaleic anhydride.

10. The manufacturing method according to claim 9, in, The solution is the electrolyte, The film forming step includes the step of: after the step of assembling the secondary battery, overdischarging the secondary battery until the potential of the positive electrode reaches or below the reduction potential of the film forming compound.

Citation Information

Patent Citations

  • Organic electrolytic solution and lithium battery using the same

    JP2007317647A

  • Nonaqueous electrolyte secondary battery and manufacturing method thereof

    CN101483256A

  • Nonaqueous electrolyte secondary battery, and manufacturing method thereof

    JP2009164082A

  • Positive electrode for nonaqueous electrolyte battery, nonaqueous electrolyte battery, and manufacturing method of nonaqueous electrolyte battery

    JP2011096551A

  • Secondary battery

    JP2013016347A