Writing feeling improvement tablets

By using a specially made writing sense improvement piece on the touch panel, the problem that writing sense cannot be reproduced in the prior art is solved, and the writing sense on the contact surface of the stylus is improved, and the writing experience and the durability of the panel are improved. sex.

CN112625616BActive Publication Date: 2024-11-05LINTEC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011007961.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-09-24
Filing Date
2020-09-23
Publication Date
2024-11-05
Estimated Expiration
2040-09-23

AI Technical Summary

Technical Problem

The writing sense on the existing touch panel cannot fully reproduce the writing sense when using writing utensils on paper, especially the writing sense of ballpoint pens.

Method used

A writing-sensation improvement piece is adopted, characterized by pressing the triangular conical indentation head with a front end curvature radius of 100nm and an inter-edge angle of 115° on the contact surface of the stylus at a load speed of 1mN/s, and pressing when reaching 1961mN The depth is 10μm or more and 30μm or less, and a writing-sensation improvement layer and an adhesive layer are provided on the contact surface of the stylus to ensure that the dynamic friction coefficient is above 0.11 or less and 0.62 or less, the static friction coefficient is above 0.12 or less and 0.65 or less, and the standard deviation of friction force It is 5 mN or more and 60 mN or less, and has suitable optical properties and scratch resistance.

Benefits of technology

It realizes the dent and vibration feeling of writing utensils when writing on paper on the touch panel, improves the excellence of writing, and has high transparency, anti-glare and scratch resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0002696612430000271
    Figure BDA0002696612430000271
  • Figure BDA0002696612430000281
    Figure BDA0002696612430000281
  • Figure BDA0002696612430000291
    Figure BDA0002696612430000291
Patent Text Reader

Abstract

The present invention provides a writing feel improving sheet, which can well reproduce the writing feel when writing on paper with a writing utensil. The writing feel improving sheet has a stylus contact surface with which a stylus touches, and when a tip of a triangular pyramid indenter having a tip curvature radius of 100 nm and an edge angle of 115° is pressed at a load speed of 1 mN / s, the pressing depth is 10 μm or more and 30 μm or less when the test load reaches 1961 mN.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a writing feel improving sheet capable of improving the writing feel of a touch pen on a touch panel or the like. Background Art

[0002] In recent years, in various electronic devices, image display devices (touch panels) with position detection functions that serve as both display devices and input means have been widely used. In such a touch panel, in addition to using fingers for input, a stylus can also be used for input. If a stylus is used, more delicate and high-precision input operations can be performed than with fingers. However, the display module of the touch panel is usually hard. Therefore, the writing feel of using a stylus is different from the writing feel of using a writing tool on paper, and it is difficult to say how good it is.

[0003] In order to solve the problem of writing feel caused by the stylus on the touch panel, research is being conducted on controlling the physical properties of the surface of the touch panel. For example, Patent Document 1 discloses a resistive film touch panel having an input operation surface that adjusts the pencil hardness, surface energy, and elastic deformability within a specified range. In addition, as a sheet disposed on the outermost surface of the touch panel for improving the writing feel (hereinafter sometimes referred to as a "writing feel improvement sheet"), Patent Document 2 discloses a transparent laminate, which is sequentially laminated with a surface treatment layer, a transparent rigid layer, and a transparent relaxation layer having a thickness of 0.2 to 2 mm.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Laid-Open No. 2001-243016

[0007] Patent Document 2: Japanese Patent Application Laid-Open No. 2004-259256 Summary of the invention

[0008] Technical Problems to be Solved by the Invention

[0009] However, the invention disclosed in Patent Document 1 or Patent Document 2 cannot fully provide the writing feeling when writing on paper using a writing utensil (particularly a ballpoint pen). Therefore, it is desired to develop a writing feeling improving sheet that further reproduces the writing feeling when writing on paper using a writing utensil.

[0010] The present invention has been made in view of the above-mentioned actual situation, and an object of the present invention is to provide a writing feel-improving sheet that can well reproduce the writing feel when writing on paper using a writing instrument.

[0011] Technical means to solve technical problems

[0012] In order to achieve the above-mentioned objectives, first, the present invention provides a writing feel improving sheet, which has a stylus contact surface contacted by a stylus, characterized in that, for the stylus contact surface, when the front end of a triangular cone-shaped indenter with a front end curvature radius of 100nm and an edge angle of 115° is pressed at a load speed of 1mN / s, the pressing depth when the test load reaches 1961mN is greater than 10μm and less than 30μm (Invention 1).

[0013] By satisfying the above-mentioned pressing depth, the writing feel improving sheet of the above-mentioned invention (Invention 1) can well reproduce the concave feeling of paper when writing on paper using a writing utensil (especially a ballpoint pen), thereby well reproducing the writing feel when writing on paper using a writing utensil.

[0014] In the above invention (Invention 1), it is preferred that: after the tip of a stylus having a tip of 0.5 mm in diameter is brought into contact with the stylus contact surface, a load of 200 g is applied to the stylus, while maintaining the angle between the stylus and the stylus contact surface at 45°, the dynamic friction coefficient of the stylus when sliding linearly at a speed of 1.6 mm / sec is greater than 0.11 and less than 0.62 (Invention 2).

[0015] In the above inventions (Inventions 1 and 2), it is preferred that: the writing feel improving sheet comprises a writing feel improving layer, a substrate arranged on one side of the writing feel improving layer, and an adhesive layer arranged on the side of the substrate opposite to the writing feel improving layer, and the side of the writing feel improving layer opposite to the substrate is the stylus contact surface (Invention 3).

[0016] In the above invention (Invention 3), it is preferred that the writing feel-improving layer is directly laminated on one surface of the substrate (Invention 4).

[0017] In the above inventions (Inventions 3 and 4), it is preferred that the writing feel-improving layer is a hard coat layer (Invention 5).

[0018] Effects of the Invention

[0019] The writing feel-improving sheet of the present invention can well reproduce the writing feel when writing on paper using a writing instrument. DETAILED DESCRIPTION

[0020] Hereinafter, embodiments of the present invention will be described.

[0021] The writing feel improving sheet of this embodiment has a stylus contact surface that is contacted by a stylus. Both sides of the writing feel improving sheet of this embodiment can be stylus contact surfaces, but usually only one side of the writing feel improving sheet is the stylus contact surface, and the other side is a surface for attaching to a touch panel or the like.

[0022] 1. Physical properties of writing feel improving sheet

[0023] (1) Compression depth

[0024] Regarding the writing feel improving sheet of this embodiment, when the tip of a triangular pyramid indenter with a tip curvature radius of 100nm and an edge angle of 115° is pressed on the stylus contact surface at a load speed of 1mN / s, the pressing depth is 10μm or more and 30μm or less when the test load reaches 1961mN. By making the pressing depth within this range, the concave feeling when writing on the stylus contact surface with a stylus is very close to the concave feeling when writing on paper with a writing utensil, and an excellent writing feel can be achieved.

[0025] From the perspective of further improving the reproducibility of the above-mentioned feeling of depression, the above-mentioned pressing depth is preferably 12 μm or more, and particularly preferably 16.5 μm or more. In addition, from the same perspective, the above-mentioned pressing depth is preferably 25 μm or less, and particularly preferably 20 μm or less. In addition, the details of the method for measuring the above-mentioned pressing depth are shown in the description of the test examples described later.

[0026] (2) Friction coefficient

[0027] For the writing feel improving sheet of this embodiment, after the pen tip of a stylus having a 0.5 mm diameter pen tip is brought into contact with the stylus contact surface, and while a load of 200 g is applied to the stylus, the stylus is slid linearly at a speed of 1.6 mm / sec while maintaining the angle between the stylus and the stylus contact surface at 45°. The dynamic friction coefficient is preferably 0.11 or more, particularly preferably 0.18 or more, and further preferably 0.23 or more. In addition, the above-mentioned dynamic friction coefficient is preferably 0.62 or less, more preferably 0.52 or less, particularly preferably 0.42 or less, and further preferably 0.32 or less.

[0028] By setting the dynamic friction coefficient within the above range, when a stylus pen is used on a touch panel to which the writing feel improving sheet is attached, the vibration sense transmitted to the hand holding the stylus pen is very close to the vibration sense obtained when writing on paper using a writing utensil (especially a ballpoint pen). Thus, the vibration sense is combined with the above-mentioned concave sense to easily achieve a better writing feel.

[0029] For the writing feel improving sheet of the present embodiment, after the tip of a stylus pen having a tip of 0.5 mm in diameter is brought into contact with the stylus pen contact surface, the static friction coefficient when the stylus pen is linearly slid at a speed of 1.6 mm / sec while a load of 200 g is applied to the stylus pen while maintaining the angle between the stylus pen and the stylus pen contact surface at 45° is preferably 0.12 or more, particularly preferably 0.20 or more, and further preferably 0.25 or more. In addition, the static friction coefficient is preferably 0.65 or less, more preferably 0.55 or less, particularly preferably 0.45 or less, and further preferably 0.35 or less.

[0030] By setting the static friction coefficient within the above range, when a stylus pen is used on a touch panel having a writing feel improving sheet attached thereto, the vibration feeling at the beginning of writing is very close to the vibration feeling obtained when writing on paper using a writing utensil (especially a ballpoint pen). Thus, the vibration feeling is combined with the above-mentioned concave feeling to easily achieve a better writing feel.

[0031] (3) Standard deviation of friction force

[0032] For the writing feel improving sheet of the present embodiment, after the tip of a stylus having a 0.5 mm diameter tip is brought into contact with the stylus contact surface, a load of 200 g is applied to the stylus, while the angle between the stylus and the surface is maintained at 45°, and the stylus is slid linearly at a speed of 1.6 mm / sec, the standard deviation of the friction force generated between the tip and the surface measured between a position where the sliding distance is 10 mm and a position where the sliding distance is 20 mm is preferably 5 mN or more, more preferably 8 mN or more, and particularly preferably 11 mN or more. In addition, the standard deviation is preferably 60 mN or less, more preferably 40 mN or less, and particularly preferably 30 mN or less. By setting the standard deviation within the above range, the vibration feeling when using the stylus on the touch panel with the writing feel improving sheet attached is very close to the vibration feeling when writing on paper using a writing utensil (especially a ballpoint pen).

[0033] The details of the method for measuring the dynamic friction coefficient, the static friction coefficient, and the standard deviation of the friction force are as described in the test examples described later.

[0034] (4) Optical properties

[0035] The haze value of the writing feel improving sheet of the present embodiment is not particularly limited, but is preferably 0.5% or more, more preferably 1% or more, and particularly preferably 15% or more, and further preferably 22% or more from the perspective of obtaining sufficient anti-glare properties. On the other hand, the haze value is preferably 95% or less, particularly preferably 65% ​​or less, and further preferably 40% or less. By making the haze value 95% or less, the transparency of the writing feel improving sheet of the present embodiment becomes higher. In addition, the haze value is measured in accordance with JIS K7136:2000, and the detailed measurement method is shown in the description of the test example described later.

[0036] The total light transmittance of the writing feel improving sheet of the present embodiment is preferably 70% or more, particularly preferably 80% or more, and further preferably 88% or more. By making the total light transmittance 70% or more, the transparency of the writing feel improving sheet of the present embodiment becomes higher. On the other hand, the upper limit of the total light transmittance is not particularly limited, for example, it is preferably 100% or less, particularly preferably 96% or less, and further preferably 92% or less. In addition, the total light transmittance is measured in accordance with JIS K7361-1:1997, and the detailed measurement method is shown in the description of the test example described later.

[0037] The glossiness of the stylus contact surface of the writing feel improving sheet of the present embodiment at a measurement angle of 60° is preferably 1% or more, particularly preferably 10% or more, and further preferably 20% or more. In addition, the glossiness is preferably 130% or less, particularly preferably 90% or less, and further preferably 60% or less. By making the glossiness within the above range, it is easy to achieve anti-glare properties suitable for the use of a touch panel with a writing feel improving sheet. In addition, the glossiness is measured in accordance with JIS K 8741:1997, and the detailed measurement method is shown in the description of the test example described later.

[0038] (5) Scratch resistance

[0039] For the writing feel improving sheet of this embodiment, 0000# steel wool was used at 250 g / cm 2 The number of scratches produced when the stylus contact surface is wiped 10 times back and forth at a speed of 10 cm with a load of 10 is preferably 10 or less, particularly preferably 5 or less, and further preferably 0. As a result, the stylus contact surface of the writing feel improving sheet of the present embodiment can exhibit good hard coat property and excellent abrasion resistance. In addition, the abrasion resistance based on the evaluation of the hardness of the steel wool is easily achieved when the writing feel improving sheet of the present embodiment has a hard coating layer as a writing feel improving layer as described later. In addition, the detailed method for measuring the above-mentioned abrasion resistance is shown in the description of the test example described later.

[0040] (6) Pencil hardness

[0041] For the writing feel improving sheet of the present embodiment, the scratch hardness (pencil hardness) based on the pencil method measured according to JIS K5600-5-4:1999 on the stylus contact surface is preferably 3B or more, and particularly preferably HB or more. By making the stylus contact surface of the writing feel improving sheet of the present embodiment have such a pencil hardness, it is easy to exert the required hardness and scratch resistance. In addition, the detailed measurement method of the above pencil hardness is shown in the description of the test example described later.

[0042] 2. Layer composition of the writing feel improving sheet

[0043] The layer structure of the writing feel improving sheet of the present embodiment is not particularly limited as long as it satisfies the aforementioned pressing depth with respect to the stylus pen contact surface and can be applied to a touch panel using a stylus pen.

[0044] From the perspective of being easy to achieve the aforementioned pressing depth and easy to adjust other physical properties, the writing feel improving sheet of this embodiment preferably comprises a writing feel improving layer, a substrate provided on one side of the writing feel improving layer, and an adhesive layer provided on the side of the substrate opposite to the writing feel improving layer. When having such a layer structure, the side of the writing feel improving layer opposite to the substrate is preferably a stylus contact surface.

[0045] (1) Base material

[0046] The substrate may be appropriately selected from substrates suitable for a touch panel using a stylus pen. For example, a plastic film, a glass plate, etc. may be used as the substrate, and a plastic film is preferably used from the perspective of good affinity with the writing feel improving layer.

[0047] Examples of the plastic film include polyester films such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate; polyolefin films such as polyethylene films and polypropylene films; celluloid, diacetylcellulose films, triacetylcellulose films, butyl acetylcellulose films, polyvinyl chloride films, polyvinylidene chloride films, polyvinyl alcohol films, ethylene-vinyl acetate copolymer films, polystyrene films, polycarbonate films, polymethylpentene films, polysulfone films, polyetheretherketone films, polyethersulfone films, polyetherimide films, fluororesin films, polyamide films, acrylic resin films, polyurethane resin films, norbornene polymer films, cyclic olefin polymer films, cyclic conjugated diene polymer films, vinyl alicyclic hydrocarbon polymer films, and other plastic films or laminated films thereof. Among them, from the perspective of easily achieving the aforementioned pressing depth, a polyester film is preferably used, and polyethylene terephthalate is particularly preferably used.

[0048] In addition, for the purpose of improving the adhesion with the layer (writing feeling improvement layer, adhesive layer, intermediate layer described later, etc.) provided on the surface thereof, an easy-adhesive layer formed by primer treatment, etc., or a surface treatment layer obtained by oxidation method, embossing method, etc., may be provided on one or both sides of the above-mentioned substrate as required. Examples of the above-mentioned oxidation method include corona discharge treatment, chromic acid treatment, flame treatment, hot air treatment, ozone / ultraviolet treatment, etc. In addition, examples of the above-mentioned embossing method include sandblasting method, solvent treatment method, etc.

[0049] In addition, in this specification, the easy-adhesive layer or the surface-treated layer is defined as a part of the substrate. Therefore, for example, when a writing feel improving sheet is assumed in which a writing feel improving layer is directly laminated on a substrate, the possibility that the easy-adhesive layer or the surface-treated layer exists in the substrate of such a writing feel improving sheet is not excluded.

[0050] The thickness of the substrate is preferably 5 μm or more, particularly preferably 10 μm or more, and further preferably 15 μm or more. By making the lower limit of the thickness of the substrate within the above range, the writing feel improving sheet of the present embodiment is easy to have sufficient strength. In addition, the thickness of the substrate is preferably 300 μm or less, more preferably 200 μm or less, particularly preferably 150 μm or less, and further preferably 100 μm or less. By making the upper limit of the thickness of the substrate within the above range, the writing feel improving sheet of the present embodiment is easy to achieve the aforementioned pressing depth.

[0051] (2) Writing feel improvement layer

[0052] The material used to form the writing feel improving layer is not particularly limited as long as it can achieve the aforementioned pressing depth. The writing feel improving layer can be a hard coating layer having hard coating properties. In this case, the stylus contact surface is likely to have good scratch resistance.

[0053] The writing feeling improvement layer is preferably formed by curing the coating composition described below. In particular, the coating composition preferably contains a curable component, microparticles, a surface conditioner, and silicon dioxide nanoparticles. According to such a coating composition, it is easy to form the above-mentioned hard coating with good hard coating properties.

[0054] (2-1) Curable Component

[0055] The curable component is a component that is cured by a trigger such as active energy rays or heat, and examples thereof include active energy ray-curable components and thermosetting components. In the present embodiment, active energy ray-curable components are preferably used from the perspective of the hardness of the writing feel improving layer formed or the heat resistance of the substrate (plastic film).

[0056] As the active energy ray-curable component, it is preferable to use a component that can be cured by irradiation with active energy rays to exhibit a predetermined hardness and achieve the above-mentioned physical properties.

[0057] As specific active energy ray-curable components, multifunctional (meth)acrylate monomers, (meth)acrylate prepolymers, active energy ray-curable polymers, etc. can be listed, among which multifunctional (meth)acrylate monomers and / or (meth)acrylate prepolymers are preferred. Multifunctional (meth)acrylate monomers and (meth)acrylate prepolymers can be used alone or simultaneously. In addition, in this specification, (meth)acrylate refers to acrylate and methacrylate. Other similar terms are also the same.

[0058] Examples of the polyfunctional (meth)acrylate monomer include 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, hydroxypivalate neopentyl glycol di(meth)acrylate, dicyclopentyl di(meth)acrylate, caprolactone-modified dicyclopentenyl di(meth)acrylate, ethylene oxide-modified phosphoric acid di(meth)acrylate, allylated cyclohexyl di(meth)acrylate, isocyanurate di(meth)acrylate, and trimethylolpropane tri(meth)acrylate. The present invention also includes polyfunctional (meth)acrylates such as (meth)acrylate, dipentaerythritol tri(meth)acrylate, propionic acid-modified dipentaerythritol tri(meth)acrylate, pentaerythritol tri(meth)acrylate, propylene oxide-modified trimethylolpropane tri(meth)acrylate, tri(acryloxyethyl)isocyanurate, pentaerythritol tetra(meth)acrylate, propionic acid-modified dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, ethylene oxide-modified dipentaerythritol hexa(meth)acrylate, and caprolactone-modified dipentaerythritol hexa(meth)acrylate. These polyfunctional (meth)acrylate monomers may be used alone or in combination of two or more.

[0059] On the other hand, as (meth)acrylate prepolymers, for example, urethane acrylate, polyester acrylate, epoxy acrylate, polyol acrylate, etc. can be cited. Among them, urethane acrylate prepolymers are preferably used from the perspective of easily achieving the aforementioned pressing depth.

[0060] Examples of the urethane acrylate prepolymer include a reaction product obtained by esterifying a hydroxyl group of a polyurethane pre-oligomer obtained from a polyether polyol or a polyester polyol and a polyisocyanate with (meth)acrylic acid; a reaction product obtained by reacting an isocyanate-terminated polyurethane oligomer obtained by reacting a polyether polyol or a polyester polyol with a polyisocyanate with a hydroxyl-containing (meth)acrylic acid; and the like.

[0061] (2-2) Microparticles

[0062] By containing fine particles in the coating composition, the surface of the formed writing feel improving layer becomes moderately rough, making it easy to adjust the haze value or 60° glossiness to the above-mentioned values, and at the same time, to achieve the above-mentioned standard deviation of the friction coefficient and friction force.

[0063] In addition, the above-mentioned microparticles refer to microparticles having an average particle diameter greater than the silica nanoparticles described later. For example, the average particle diameter of the above-mentioned microparticles is preferably 1 μm or more, particularly preferably 2 μm or more, and further preferably 3 μm or more. In addition, the average particle diameter of the above-mentioned microparticles is preferably 20 μm or less, more preferably 16 μm or less, particularly preferably 12 μm or less, and further preferably 6 μm or less. By making the average particle diameter of the above-mentioned microparticles within the above-mentioned range, it is easy to achieve the above-mentioned haze value, 60° gloss, friction coefficient and standard deviation of friction.

[0064] In addition, the coefficient of variation (CV value) of the particle size represented by the following formula of the above-mentioned particles is preferably 3% or more, particularly preferably 8% or more, and further preferably 13% or more. On the other hand, the coefficient of variation (CV value) of the particle size is preferably 70% or less, particularly preferably 45% or less, and further preferably 25% or less. By making the CV value of the above-mentioned particles within the above-mentioned range, it becomes easy to adjust the concavo-convex shape of the surface, and it is easy to achieve the standard deviation of the friction force mentioned above.

[0065] Coefficient of variation of particle size (CV value) = (standard deviation particle size / average particle size) × 100

[0066] The average particle size and coefficient of variation (CV value) of the particle size of the fine particles are measured using a laser diffraction scattering particle size distribution analyzer using a few drops of a 5 mass % dispersion prepared using methyl ethyl ketone as a dispersion medium as a sample.

[0067] The above-mentioned fine particles may be organic fine particles, inorganic fine particles, or resin fine particles having both inorganic and organic properties. From the perspective of easily achieving the above-mentioned standard deviation of frictional force, organic fine particles or resin fine particles having both inorganic and organic properties are preferred.

[0068] As organic particles, for example, acrylic resin particles (e.g., polymethyl methacrylate particles, etc.), silicone particles, melamine resin particles, acrylic-styrene copolymer particles, polycarbonate particles, polyethylene particles, polystyrene particles, benzoguanamine resin particles, etc. can be listed, and these resins may be cross-linked. Among the above particles, acrylic resin particles and silicone particles are preferred from the perspective of easily achieving the standard deviation of the friction force described above. As acrylic resin particles, polymethyl methacrylate particles are particularly preferred, and cross-linked polymethyl methacrylate particles are more preferred.

[0069] Examples of the inorganic fine particles include fine particles composed of silicon dioxide, aluminum oxide, titanium dioxide, zirconium oxide, tin oxide, indium oxide, cadmium oxide, antimony oxide, and the like.

[0070] As the resin fine particles having both inorganic and organic properties, silicone fine particles (for example, Tospearl series manufactured by Momentive Performance Materials Japan Inc.) are particularly preferred.

[0071] The above-mentioned fine particles may be used alone or in combination of two or more.

[0072] The microparticles may be subjected to desired surface modification. In addition, the shape of the microparticles may be a regular shape such as a sphere, or an irregular shape with no particular shape. From the perspective of easily achieving the standard deviation of the friction force described above, a regular shape is preferred, and a sphere is particularly preferred.

[0073] Relative to 100 parts by mass of curable components, the content of the microparticles in the coating composition is preferably 0.01 parts by mass or more, more preferably 0.1 parts by mass or more, particularly preferably 1 parts by mass or more, and further preferably 7 parts by mass or more. In addition, relative to 100 parts by mass of curable components, the content of the microparticles in the coating composition is preferably 50 parts by mass or less, particularly preferably 30 parts by mass or less, and further preferably 15 parts by mass or less. By making the content of microparticles within the above range, it is easy to achieve the standard deviation of the aforementioned coefficient of friction and frictional force.

[0074] (2-3) Surface Conditioner

[0075] By making the coating composition contain a surface conditioner, it is possible to suppress the occurrence of stripe-like defects or unevenness on the formed writing feel improving layer. As a result, the film thickness becomes uniform, the writing feel improving sheet is easy to present a more excellent appearance, and has the required optical properties (haze value and total light transmittance, etc.). In addition, since the surface of the writing feel improving layer of the writing feel improving sheet is easy to be in a good surface state, the writing feel improving layer is easy to achieve the above-mentioned standard deviation of the friction coefficient and friction force.

[0076] As the surface conditioner, for example, fluorine-based, silicone-based, acrylic-based, vinyl-based surface conditioners can be listed, among which fluorine-based surface conditioners are preferred from the perspective of surface conditioning performance or compatibility with other components. In addition, the surface conditioner can be used alone or in combination of two or more.

[0077] As the fluorine-based surface conditioner, preferably a compound having a perfluoroalkyl group or a fluorinated alkenyl group on the main chain or the side chain can be listed. As commercially available products, preferably BYK-340 manufactured by BYK Japan KK., Fitter 650A manufactured by Neos Co., Ltd., MEGAFACE RS-75 manufactured by DIC CORPORATION, V-8FM manufactured by OSAKA ORGANIC CHEMICAL INDUSTRY LTD., etc. can be listed, but it is not limited thereto. As the silicone-based surface conditioner, preferably polydimethylsiloxane or modified polydimethylsiloxane, particularly preferably polydimethylsiloxane.

[0078] Relative to 100 parts by mass of curable components, the content of the surface conditioning agent in the coating composition is preferably 0.01 parts by mass or more, particularly preferably 0.1 parts by mass or more, and further preferably 0.2 parts by mass or more. In addition, relative to 100 parts by mass of curable components, the content of the surface conditioning agent in the coating composition is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, particularly preferably 3 parts by mass or less, and further preferably 1 part by mass or less. By making the content of the surface conditioning agent within the above range, the appearance of the writing feeling improvement sheet can be effectively improved. In addition, it is easy to adjust the optical properties (haze value and total light transmittance, etc.) within the aforementioned range. Further, the writing feeling improvement layer is easy to achieve the aforementioned coefficient of friction.

[0079] (2-4) Silica Nanoparticles

[0080] By making the coating composition contain silica nanoparticles, the hardness of the formed writing feel improving layer can be effectively increased.

[0081] The average particle size of the silicon dioxide nanoparticles is preferably 1 nm or more, particularly preferably 5 nm or more, and more preferably 10 nm or more. In addition, the average particle size of the silicon dioxide nanoparticles is preferably 300 nm or less, particularly preferably 100 nm or less, and more preferably 50 nm or less. In addition, the average particle size of the silicon dioxide nanoparticles is set to a value measured by a laser diffraction scattering particle size distribution measuring device.

[0082] For the purpose of improving dispersibility, organic matter can be used to modify the silicon dioxide nanoparticles. In addition, the silicon dioxide nanoparticles are preferably in the form of organosol (colloidal). By being in the form of organosol, the dispersibility of the silicon dioxide nanoparticles becomes good, improves the homogeneity and light transmittance of the formed writing feeling improvement layer.

[0083] As the silica nanoparticles, commercially available products may be used, and examples thereof include organosilica sol MEK-ST and MIBK-ST manufactured by Nissan Chemical Corporation.

[0084] Relative to 100 parts by mass of curable components, the content of the silica nanoparticles in the coating composition is preferably 5 parts by mass or more, particularly preferably 10 parts by mass or more, and more preferably 15 parts by mass or more. In addition, relative to 100 parts by mass of curable components, the content of the silica nanoparticles in the coating composition is preferably 50 parts by mass or less, particularly preferably 35 parts by mass or less, and more preferably 25 parts by mass or less. By making the content of the silica nanoparticles 5 parts by mass or more, the hardness of the formed writing feeling improvement layer can be more effectively improved, and at the same time, the generation of glare can be more effectively suppressed. On the other hand, by making the blending ratio of the silica nanoparticles 50 parts by mass or less, the aggregation of the silica nanoparticles can be suppressed, and the homogeneity and light transmittance of the formed writing feeling improvement layer can be well maintained.

[0085] (2-5) Other ingredients

[0086] In addition to the above-mentioned components, the coating composition of the present embodiment may also contain various additives. As various additives, for example, photopolymerization initiator, ultraviolet light absorber, antioxidant, light stabilizer, antistatic agent, silane coupling agent, anti-aging agent, thermal polymerization inhibitor, colorant, surfactant, storage stabilizer, plasticizer, lubricant, defoamer, organic filling material, wettability improver, coating surface improver etc. may be listed.

[0087] Examples of the photopolymerization initiator include benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin n-butyl ether, benzoin isobutyl ether, acetophenone, dimethylaminoacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 2-hydroxy-2-methyl-1-phenylpropane-1-one, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-1-propanone, 4- (2-hydroxyethoxy)phenyl-2(hydroxy-2-propyl)ketone, benzophenone, p-phenylbenzophenone, 4,4'-diethylaminobenzophenone, dichlorobenzophenone, 2-methylanthraquinone, 2-ethylanthraquinone, 2-tert-butylanthraquinone, 2-aminoanthraquinone, 2-methylthioxanthone, 2-ethylthioxanthone, 2-chlorothioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, benzil dimethyl ketal, acetophenone dimethyl ketal, p-dimethylaminobenzoate, etc. These photopolymerization initiators may be used alone or in combination of two or more.

[0088] The content of the photopolymerization initiator in the coating composition is preferably 1 part by mass or more, particularly preferably 2 parts by mass or more, relative to 100 parts by mass of the curable component. In addition, the content of the photopolymerization initiator in the coating composition is preferably 10 parts by mass or less, particularly preferably 5 parts by mass or less, relative to 100 parts by mass of the curable component.

[0089] (2-6)Thickness

[0090] The thickness of the writing feel improving layer is preferably 0.1 μm or more, particularly preferably 1 μm or more, and further preferably 2 μm or more. In addition, the thickness of the writing feel improving layer is preferably 30 μm or less, more preferably 20 μm or less, particularly preferably 10 μm or less, and further preferably 4 μm or less. By making the thickness of the writing feel improving layer within the above range, the writing feel improving sheet of the present embodiment can easily achieve the above-mentioned pressing depth.

[0091] (3)Adhesive layer

[0092] The adhesive used to form the above-mentioned adhesive layer is not particularly limited as long as it can achieve the aforementioned pressing depth. As the adhesive, it is preferred to use an adhesive commonly used for optical purposes, for example, acrylic adhesives, rubber adhesives, silicone adhesives, urethane adhesives, polyester adhesives, polyvinyl ether adhesives, etc. can be listed. Among them, it is preferred to show the required adhesiveness, optical properties and excellent durability of acrylic adhesives.

[0093] Examples of the acrylic adhesive include an adhesive obtained by cross-linking an adhesive composition containing a (meth)acrylic acid ester polymer and a cross-linking agent. In the present specification, the term "polymer" also includes the concept of "copolymer".

[0094] (Meth) acrylate polymer preferably contains a reactive group-containing monomer having a reactive group that reacts with a crosslinking agent in the molecule as the monomer unit constituting the polymer. Through the reaction of the reactive group and the crosslinking agent described later, it is easy to control the cohesive force of the adhesive obtained within the required range, and as a result, it is easy to reach the aforementioned pressing depth. As the functional group-containing monomer, it is preferably a monomer having a polymerizable double bond and a hydroxyl, a carboxyl, an amino group and other functional groups in the molecule, wherein, preferably using at least one of a monomer (carboxyl-containing monomer) containing a carboxyl group as a functional group and a monomer (hydroxyl-containing monomer) containing a hydroxyl group as a functional group.

[0095] Examples of the above-mentioned carboxyl group-containing monomers include ethylenically unsaturated carboxylic acids such as acrylic acid and methacrylic acid, among which acrylic acid is preferred. In addition, preferred examples of the above-mentioned hydroxyl group-containing monomers include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate. These monomers may be used alone or in combination of two or more.

[0096] The (meth)acrylate polymer preferably contains 1% by mass or more, particularly preferably 3% by mass or more, of the structural unit derived from the functional group-containing monomer. The polymer preferably contains 40% by mass or less, particularly preferably 20% by mass or less of the structural unit.

[0097] From the perspective of exhibiting the desired adhesive force, the (meth)acrylate polymer preferably contains an alkyl (meth)acrylate as a monomer unit constituting the polymer, and it is particularly preferred to use an alkyl acrylate having an alkyl group with 1 to 18 carbon atoms. Specific examples thereof include methyl (meth)acrylate, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, etc., among which n-butyl (meth)acrylate is preferred. These alkyl (meth)acrylates may be used alone or in combination of two or more.

[0098] The (meth)acrylate polymer preferably contains 50% by mass or more, particularly preferably 80% by mass or more of the structural unit derived from the (meth)acrylate alkyl ester. The polymer preferably contains 99% by mass or less, particularly preferably 97% by mass or less of the structural unit.

[0099] The (meth)acrylate polymer may be copolymerized with the above-mentioned functional group-containing monomer and (meth) alkyl acrylate, and may also be copolymerized with other monomers. In addition, the polymerized form of the polymer may be a random copolymer or a block copolymer. In addition, the polymer may be used alone or in combination of two or more.

[0100] The weight average molecular weight of the (meth)acrylate polymer is preferably 300,000 or more, and particularly preferably 1,000,000 or more. In addition, the weight average molecular weight is preferably 2,500,000 or less, and particularly preferably 2,000,000 or less. By making the weight average molecular weight of the (meth)acrylate polymer within the above range, it is easy to satisfy the storage modulus described later and to achieve the aforementioned pressing depth.

[0101] The crosslinking agent may react with the reactive functional group of the (meth)acrylate polymer, and preferably, for example, an epoxy crosslinking agent, an isocyanate crosslinking agent, etc. The crosslinking agent may be used alone or in combination of two or more.

[0102] The content of the crosslinking agent in the adhesive composition is preferably 0.01 parts by mass or more, particularly preferably 0.1 parts by mass or more, relative to 100 parts by mass of the (meth)acrylate polymer, and is preferably 10 parts by mass or less, particularly preferably 5 parts by mass or less.

[0103] To the adhesive composition, various additives commonly used in acrylic adhesives may be added as needed, for example, active energy ray-curable components, photopolymerization initiators, silane coupling agents, antistatic agents, tackifiers, antioxidants, light stabilizers, softeners, fillers, refractive index adjusters, light scattering agents, etc.

[0104] The adhesive composition can be prepared by preparing a (meth)acrylate polymer, and mixing the obtained (meth)acrylate polymer, a crosslinking agent, and additives as needed. The (meth)acrylate polymer can be prepared by polymerizing a mixture of monomers constituting the polymer using a conventional free radical polymerization method. The polymerization of the (meth)acrylate polymer is preferably carried out by a solution polymerization method using a polymerization initiator as required. The adhesive composition can be prepared into a coating solution of the adhesive composition by adding a diluting solvent and mixing thoroughly.

[0105] The lower limit of the gel fraction of the adhesive constituting the adhesive layer is preferably 40% or more, particularly preferably 60% or more, and more particularly preferably 70% or more. In addition, the upper limit of the gel fraction of the above-mentioned adhesive is preferably 99% or less, particularly preferably 90% or less, and more particularly preferably 85% or less. By making the gel fraction of the adhesive within the above range, it is easy to achieve the above-mentioned pressing depth.

[0106] In addition, the gel fraction of the above-mentioned adhesive can be measured by a common method, for example, the adhesive can be immersed in ethyl acetate at room temperature (23° C.) for 72 hours, and the gel fraction can be calculated based on the mass of the adhesive before and after the immersion. That is, when the mass of the adhesive before immersion is set as M1 and the mass of the adhesive after immersion and sufficient drying is set as M2, the gel fraction can be obtained by the calculation formula (M2 / M1)×100.

[0107] The storage modulus of the adhesive layer at 23°C is preferably 0.02MPa or more, particularly preferably 0.06MPa or more, and more preferably 0.09MPa or more. In addition, the storage modulus is preferably 0.50MPa or less, particularly preferably 0.20MPa or less, and more preferably 0.14MPa or less. By making the storage modulus of the adhesive layer at 23°C within the above range, it is easy to achieve the above-mentioned pressing depth.

[0108] The storage modulus is measured in accordance with JIS K7244-6:1999 using a viscoelasticity tester (e.g., manufactured by REOMETRIC, product name "DYNAMIC ANALYZER") at a measurement frequency of 1 Hz and a measurement temperature of 23°C by a torsional shear method.

[0109] The lower limit of the thickness of the adhesive layer is preferably 20 μm or more, particularly preferably 40 μm or more, and more preferably 70 μm or more. By making the lower limit of the thickness of the adhesive layer as described above, it is easy to achieve the aforementioned pressing depth, and at the same time it is easy to exert the required adhesion. In addition, the upper limit of the thickness of the adhesive layer is preferably 300 μm or less, particularly preferably 200 μm or less, and more preferably 150 μm or less. By making the upper limit of the thickness of the adhesive layer as described above, it is easy to achieve the thinning of the touch panel with a writing feeling improvement sheet.

[0110] In addition, the lower limit of the ratio of the thickness of the adhesive layer to the thickness of the base material and the writing feeling improvement layer is preferably more than 0.2 times, particularly preferably more than 0.5 times, and more preferably more than 1 times. By making the lower limit of the above-mentioned ratio as described above, it is easy to reach the aforementioned pressing depth. In addition, the upper limit of the above-mentioned ratio is preferably less than 5.0 times, particularly preferably less than 3.5 times, and more preferably less than 2.0 times. By making the upper limit of the above-mentioned ratio as described above, even when the adhesive layer is thicker (for example, when the thickness of the adhesive layer is more than 150 μm), there is sufficient pencil hardness.

[0111] (4) Other components

[0112] The writing feel improving sheet of this embodiment may further include a layer other than the aforementioned writing feel improving layer, substrate and adhesive layer. For example, an intermediate layer having a lower elastic modulus than the writing feel improving layer may be provided between the writing feel improving layer and the substrate. In addition, a release sheet may be laminated on the surface of the adhesive layer opposite to the substrate.

[0113] The intermediate layer may be provided from the viewpoint of facilitating the above-mentioned pressing depth. As the material of the intermediate layer, the same material as the writing feel improving layer may be used, and it is particularly preferred to form the intermediate layer using the above-mentioned coating composition.

[0114] When the intermediate layer is provided, from the perspective of facilitating the aforementioned pressing depth, its thickness is preferably 5 μm or more, particularly preferably 10 μm or more, and further preferably 20 μm or more. In addition, from the same perspective, the thickness of the intermediate layer is preferably 50 μm or less, particularly preferably 40 μm or less, and further preferably 35 μm or less.

[0115] In addition, when the writing feel improving sheet has the above-mentioned intermediate layer, there is a tendency that the writing feel improving layer is easily broken when using a stylus. Such a tendency becomes higher especially when the writing feel improving layer is a hard coating layer. From such a perspective, the writing feel improving sheet of the present embodiment preferably does not have an intermediate layer, that is, the writing feel improving layer is preferably directly laminated on one side of the substrate. In addition, in this specification, even when the writing feel improving layer is directly laminated on one side of the substrate, as described above, the aforementioned easy-adhesive layer or surface treatment layer may be present on the writing feel improving layer side of the substrate.

[0116] As the release sheet, for example, polyethylene film, polypropylene film, polybutylene film, polybutadiene film, polymethylpentene film, polyvinyl chloride film, vinyl chloride copolymer film, polyethylene terephthalate film, polyethylene naphthalate film, polybutylene terephthalate film, polyurethane film, ethylene vinyl acetate film, ionomer resin film, ethylene-(methyl) acrylic acid copolymer film, ethylene-(methyl) acrylic acid ester copolymer film, polystyrene film, polycarbonate film, polyimide film, fluororesin film, liquid crystal polymer film, etc. can be used. In addition, crosslinked films of these films can also be used. Further, laminated films of these films can also be used.

[0117] The release surface (surface in contact with the adhesive layer) of the release sheet is preferably subjected to a release treatment. Examples of release agents used for the release treatment include alkyd-based, silicone-based, fluorine-based, unsaturated polyester-based, polyolefin-based, and wax-based release agents.

[0118] The thickness of the release sheet is not particularly limited, but is generally about 20 to 150 μm.

[0119] 3. Method for producing writing feel improving sheet

[0120] As long as the writing feel improving sheet can achieve the aforementioned pressing depth, the manufacturing method of the writing feel improving sheet of the present embodiment is not particularly limited. For example, after a laminate consisting of a writing feel improving layer and a substrate, and a laminate consisting of an adhesive layer and a release sheet are separately manufactured, these laminates are attached in a manner that the substrate and the adhesive layer are in contact, thereby obtaining a writing feel improving sheet having the writing feel improving layer, the substrate, the adhesive layer, and the release sheet laminated in sequence.

[0121] The laminate composed of the writing feel improving layer and the substrate can be obtained, for example, by applying a coating liquid containing the coating composition and a desired solvent to one surface of the substrate and curing the obtained coating film to form the writing feel improving layer.

[0122] The above solvent can be used for improving coating properties, adjusting viscosity, adjusting solid content concentration, etc., and any solvent can be used without particular limitation as long as it can dissolve curable components, etc., and disperse fine particles, etc.

[0123] Specific examples of the solvent include alcohols such as methanol, ethanol, isopropanol, butanol, and octanol; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; esters such as ethyl acetate, butyl acetate, ethyl lactate, and γ-butyrolactone; ethers such as ethylene glycol monomethyl ether (methyl cellosolve), ethylene glycol monoethyl ether (ethyl cellosolve), diethylene glycol monobutyl ether (butyl cellosolve), and propylene glycol monomethyl ether; aromatic hydrocarbons such as benzene, toluene, and xylene; amides such as dimethylformamide, dimethylacetamide, and N-methylpyrrolidone, and the like.

[0124] The coating liquid of the coating composition can be applied by conventional methods, such as rod coating, knife coating, roll coating, blade coating, die coating, or gravure coating. After applying the coating liquid of the coating composition, the coating film is preferably dried at 40 to 120° C. for about 30 seconds to 5 minutes.

[0125] When the coating composition has active energy ray curing properties, the coating composition is cured by irradiating the coating film of the coating composition with active energy rays such as ultraviolet rays, electron beams, etc. Ultraviolet irradiation can be performed using a high-pressure mercury lamp, a FUSION H lamp, a xenon lamp, etc. The irradiation amount of ultraviolet rays is preferably 50 to 1000 mW / cm 2 , light intensity is 50~1000mJ / cm 2 The illumination is preferably 100 to 500 mW / cm 2 , light intensity is 100~500mJ / cm 2On the other hand, electron beam irradiation can be performed using an electron beam accelerator or the like, and the irradiation amount of the electron beam is preferably about 10 to 1000 krad.

[0126] The laminate composed of the adhesive layer and the release sheet can be obtained, for example, by the following method: the release surface of the release sheet is coated with a coating liquid containing the aforementioned adhesive composition and a desired solvent, and the coating film thus obtained is dried, etc., thereby forming an adhesive layer. The solvent is not particularly limited, and various solvents can be used, for example, the aforementioned solvent for preparing the coating liquid of the coating composition can be used. In addition, the coating method of the coating liquid can use, for example, the same method as the coating liquid of the coating composition. The drying of the coating film of the adhesive composition can be carried out, for example, by heating the coating film at a temperature of more than 80°C and less than 180°C for more than 10 seconds and less than 5 minutes. Furthermore, after such a heat treatment, a aging period of about 1 to 2 weeks can be set at room temperature (for example, 23°C, 50%RH).

[0127] 4. Use of writing feeling improvement tablets

[0128] The writing feel improving sheet of this embodiment can be used as a sheet constituting the outermost layer of a touch panel (image display device with position detection function) using a stylus pen. Specifically, it is preferably laminated on a covering material of a touch panel having a display module such as a liquid crystal (LCD) module, a light emitting diode (LED) module, an organic electroluminescent (organic EL) module, or a contact sensor. It is preferably laminated on the covering material of the writing feel improving sheet by attaching it via the above-mentioned adhesive layer.

[0129] In addition, the stylus pen used for the writing feel improvement sheet in the present embodiment is not particularly limited, and a conventionally known stylus pen can be used. For example, as the stylus pen, a stylus pen with a polyacetal pen tip, a stylus pen with a hard felt pen tip, a stylus pen with an elastic pen tip, etc. can be used. In addition, the shape of the stylus pen tip is not particularly limited, and can be appropriately selected from a disc-shaped pen tip, a round pen tip, a polygonal pen tip, etc. From the perspective of being able to obtain a sense of vibration when writing with a ballpoint pen, a round pen tip is preferred. When the shape of the stylus pen tip is round, the diameter of the pen tip is preferably 0.1 mm or more, particularly preferably 0.2 mm or more, and more preferably 0.3 mm or more. In addition, the above diameter is preferably 5 mm or less, particularly preferably 2 mm or less, and more preferably 1 mm or less.

[0130] The writing feel improving sheet of this embodiment can well reproduce the concave feeling of paper when writing on paper with a writing utensil (especially a ballpoint pen) by satisfying the above-mentioned pressing depth. Thus, the writing feel when writing on paper with a writing utensil can be well reproduced.

[0131] 5. Touch panel with writing feel improvement sheet

[0132] By laminating the writing feel improving sheet of this embodiment on a touch panel, a touch panel with a writing feel improving sheet can be obtained. Specifically, the touch panel with a writing feel improving sheet comprises: a writing feel improving sheet having a stylus contact surface to be contacted by a stylus and a touch panel, and on the display surface side of the touch panel, the writing feel improving sheet is laminated on the surface side opposite to the stylus contact surface. The writing feel improving sheet can be laminated directly on the display surface of the touch panel, or can be laminated on the display surface side of the touch panel via other components or layers.

[0133] The type and method of the touch panel are not particularly limited, for example, electrostatic capacitance, electromagnetic induction, resistive film, surface elastic wave (ultrasonic), infrared and other touch panels can be used. Among them, from the perspective of easy reproduction of excellent writing feeling, electrostatic capacitance touch panels are preferred, and if the reproducibility of text written by a stylus is taken into account, electrostatic capacitance touch panels with electromagnetic induction are particularly preferred. The specific structure of electrostatic capacitance and electromagnetic induction touch panels is not particularly limited, and previously known touch panels can be used.

[0134] The embodiments described above are described to facilitate understanding of the present invention, and are not described to limit the present invention. Therefore, each element disclosed in the above embodiments includes all design changes or equivalents within the technical scope of the present invention.

[0135] Example

[0136] The present invention will be described in more detail below with reference to Examples and the like, but the scope of the present invention is not limited to these Examples and the like.

[0137] [Preparation Example]

[0138] The materials described in Table 1 were mixed in the composition shown in Table 2 to obtain coating compositions C1 to C4. In addition, the blending ratio shown in Table 2 is a ratio based on the solid content conversion value. Furthermore, the obtained coating compositions were diluted with propylene glycol monomethyl ether to obtain coating solutions of coating compositions C1 to C4. In addition, the solid content concentrations of the obtained coating solutions are shown in Table 2.

[0139] [Example 1]

[0140] (1) Formation of a writing feel improving layer

[0141] The coating composition C1 obtained in the above preparation example was coated on one side of a polyethylene terephthalate (PET) film (manufactured by TORAY INDUSTRIES, INC., product name "Lumirror U48", thickness 125 μm) as a substrate having an adhesive layer on both sides using a Meyer bar to form a coating film, and then the coating film was dried by heating at 70° C. for 1 minute in an oven.

[0142] Then, in a nitrogen atmosphere, ultraviolet rays were irradiated under the following conditions using an ultraviolet irradiation device (manufactured by GS Yuasa International Ltd., product name: "Nitrogen Purge Small Conveyor UV Irradiation Device CSN2-40") to cure the coating film and form a writing feel improving layer with a thickness of 3 μm.

[0143] [Ultraviolet irradiation conditions]

[0144] Light source: high pressure mercury lamp

[0145] Lamp power: 1.4kW

[0146] Conveyor belt speed: 1.2m / min

[0147] Illuminance: 100mW / cm 2

[0148] Light intensity: 240mJ / cm 2

[0149] Oxygen concentration: less than 1%

[0150] (2) Formation of Adhesive Layer

[0151] A (meth)acrylate copolymer was prepared by copolymerizing 95 parts by mass of n-butyl acrylate and 5 parts by mass of acrylic acid by solution polymerization. The molecular weight of the (meth)acrylate copolymer was measured by the method described below, and the weight average molecular weight (Mw) was 1.5 million.

[0152] 99.8 parts by mass (solid content conversion value; the same applies hereinafter) of the obtained (meth)acrylate copolymer and 0.2 parts by mass of 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane as a crosslinking agent were mixed and stirred thoroughly, and diluted with toluene to obtain a coating liquid of an adhesive composition.

[0153] Then, using an applicator, a release sheet (Lintec Corporation, product name "SP-PET381031") having a silicone release layer formed on one surface of a polyethylene terephthalate film having a thickness of 38 μm was coated with the coating liquid of the adhesive composition obtained above to form a coating film. Further, an oven was used to heat at 100° C. for 3 minutes to dry the coating film, and an adhesive layer having a thickness of 50 μm, a gel fraction of 80%, and a storage modulus of 0.12 MPa at 23° C. was formed on the release sheet by aging at 23° C. and 50% RH for 7 days.

[0154] Here, the weight average molecular weight (Mw) is a polystyrene-equivalent weight average molecular weight measured by gel permeation chromatography (GPC) under the following conditions (GPC measurement).

[0155] <Measurement Conditions>

[0156] ·GPC measuring apparatus: manufactured by TOSOH CORPORATION, HLC-8320

[0157] ·GPC column (passed in the following order): manufactured by TOSOH CORPORATION

[0158] TSK gel superH-H

[0159] TSK gel superHM-H

[0160] TSK gel superH2000

[0161] ·Test solvent: tetrahydrofuran

[0162] ·Measurement temperature: 40℃

[0163] (3) Formation of a writing feel improving sheet

[0164] The surface on the substrate side of the laminate of the substrate and the writing feel improving layer obtained in the above step (1) is bonded to the surface on the adhesive layer side of the laminate of the release sheet and the adhesive layer obtained in the above step (2), thereby obtaining a writing feel improving sheet having the writing feel improving layer, the substrate, the adhesive layer and the release sheet laminated in this order.

[0165] [Examples 2 to 15, Comparative Example 1]

[0166] A writing feel improving sheet was produced in the same manner as in Example 1 except that the type of coating composition used, the thickness of the writing feel improving layer, the type and thickness of the substrate used, and the thickness of the adhesive layer were changed as shown in Table 3.

[0167] [Example 16]

[0168] Using a Meyer rod, the coating liquid of the coating composition C4 obtained in the above preparation example was applied to one side of a polyethylene terephthalate (PET) film (Toray Industries, Inc. manufactured, product name "Lumirror U48", thickness 125 μm) having an easy-adhesive layer on both sides as a substrate, thereby forming a coating film, and then using an oven, heating at 70° C. for 1 minute to dry the above coating film. Then, the above coating film was irradiated with ultraviolet rays under the aforementioned ultraviolet irradiation conditions to cure the above coating film. Thus, an intermediate layer with a thickness of 30 μm was formed.

[0169] Furthermore, the coating composition C1 obtained in the above preparation example was coated on the surface of the intermediate layer side in the laminated body having the intermediate layer formed on one surface of the substrate obtained above using a Meyer rod to form a coating film, and then the coating film was dried by heating at 70° C. for 1 minute using an oven. Then, the coating film was irradiated with ultraviolet rays under the above ultraviolet irradiation conditions to cure the coating film. Thus, a writing feel improving layer with a thickness of 3 μm was formed.

[0170] The surface on the substrate side of the laminated body obtained in the order of the writing feel improving layer, the intermediate layer and the substrate was adhered to the surface on the adhesive layer side of the laminated body of the release sheet and the adhesive layer obtained in the same manner as in step (2) of the aforementioned Example 1, thereby obtaining a writing feel improving sheet in which the writing feel improving layer, the intermediate layer, the substrate, the adhesive layer and the release sheet were laminated in the order.

[0171] [Test Example 1] (Measurement of optical properties)

[0172] The release sheet was peeled off from the writing feel improving sheet produced in Examples and Comparative Examples, and the exposed surface (adhesive surface) of the exposed adhesive layer was bonded to a glass plate (thickness: 1.2 mm) to prepare a measurement sample.

[0173] Then, after background measurement was performed using only the glass plate, the haze value (%) of the writing feel improving sheet was measured using a haze meter (manufactured by Nippon Denshoku Industries Co., Ltd., product name "NDH-5000") for the above-mentioned measurement sample in accordance with JIS K7136:2000, and the total light transmittance (%) of the writing feel improving sheet was measured in accordance with JIS Z 8741:1997. These results are shown in Table 3.

[0174] In addition, for the surface (the contact surface of the stylus) on the writing feeling improvement layer side in the measurement sample obtained in the same manner as above, in accordance with JIS Z8741:1997, using a gloss meter (manufactured by Nippon Denshoku Industries Co., Ltd., product name "VG7000"), the gloss at a measurement angle of 60° was measured. The results are shown in Table 3.

[0175] [Test Example 2] (Measurement of Pressing Depth)

[0176] The release sheet was peeled off from the writing feeling improvement sheet manufactured in the examples and comparative examples, and the exposed surface (adhesive surface) of the exposed adhesive layer was adhered to a glass plate (thickness: 1.2 mm), which was used as a measurement sample.

[0177] After setting the above measurement sample on a micro surface hardness tester (manufactured by Shimadzu Corporation, product name "Shimadzu Dynamic Ultra Micro Surface Hardness Tester W201S"), for the surface (the contact surface of the stylus) on the writing feeling improvement layer side in the above measurement sample, the front end of a triangular pyramid indenter (Berkovich indenter, front end curvature radius: 100 nm, included angle between edges: 115°) was pressed at a load speed of 1 mN / s, and the pressing depth (μm) when the test load reached 1961 mN was measured. The results are shown in Table 3.

[0178] In addition, for reference, the pressing depth on paper was measured. Specifically, commercially available paper (manufactured by KOKUYO Co., Ltd., product name "Campus loose leaf しっかり書ける", product model "NO-S836BT", size: B5, line spacing: type B) was set on the support table of the above micro surface hardness tester in a state of overlapping 20 sheets, and then the pressing depth (μm) of the outermost surface of the overlapping paper was measured under the same conditions as above. As a result, a measured value of 17.8 μm was obtained.

[0179] [Test Example 3] (Friction Measurement)

[0180] The release sheet was peeled off from the writing feeling improvement sheet manufactured in the examples and comparative examples, and the exposed surface (adhesive surface) of the exposed adhesive layer was adhered to a glass plate (thickness: 1.2 mm), which was used as a measurement sample.

[0181] The above-mentioned measurement sample was set on the dedicated bogie for measurement of a static and kinetic friction measuring machine (manufactured by Trinity Lab Inc., product name "Tri Lab Master TL201Ts") with the side of the writing feel improvement layer (the contact surface of the stylus) facing upward. In addition, as the static and kinetic friction measuring machine is used, the dedicated bogie for measurement moves back and forth in a specified direction while maintaining the horizontal state of the setting surface of the measurement sample.

[0182] Then, the stylus was fixed to the above-mentioned static and kinetic friction measuring machine in such a way that the tip of the stylus touches the contact surface of the stylus. At this time, the stylus was tilted at an angle of 45° with respect to the contact surface of the stylus and fixed. In addition, at this time, the tilting direction was set to tilt toward the traveling direction side of the dedicated bogie for measurement and to be parallel to the traveling direction at the same time. As the stylus, a stylus (manufactured by Wacom Inc., product name "ACK-20001", diameter of the tip: 0.5 mm) having a tip made of polyoxymethylene (POM) was used.

[0183] Then, under the condition of applying a load of 200 g to the stylus, the dedicated bogie for measurement was moved at a speed of 1.6 mm / second, so that the stylus slid on the contact surface of the stylus (sliding distance: 100 mm). Based on the friction force measured at this time, the static friction coefficient and the kinetic friction coefficient were calculated, and for the friction force measured between the position where the sliding distance is 10 mm and the position where the sliding distance is 20 mm, the standard deviation (mN) of the friction force was calculated. The results are shown in Table 3.

[0184] In addition, for reference, the static friction coefficient and the kinetic friction coefficient when writing on paper with a ballpoint pen were measured. Specifically, 20 sheets of commercially available paper (manufactured by KOKUYO Co., Ltd., product name "Campus loose leaf しっかり書ける", product model "NO-S836BT", size: B5, line spacing: B type) were overlapped and set on the dedicated bogie for measurement of the above-mentioned static and kinetic friction measuring machine. Then, a ballpoint pen (manufactured by BIC Corporation, product name "Orange EG 1.0", oil-based ballpoint pen, diameter of the tip: 1.0 mm) was fixed to the above-mentioned static and kinetic friction measuring machine in such a way that the tip of the pen touches the outermost surface of the overlapped paper. Then, the ballpoint pen was slid on the surface of the paper under the same conditions as above, and the static friction coefficient, the kinetic friction coefficient, and the standard deviation of the friction force were calculated based on the friction force measured at this time. As a result, the static friction coefficient was 0.28, the kinetic friction coefficient was 0.27, and the standard deviation of the friction force was 30 mN.

[0185] [Test Example 4] (Evaluation of writing feel)

[0186] The release sheet was peeled off from the writing feel improving sheet produced in Examples and Comparative Examples, and the exposed surface (adhesive surface) of the exposed adhesive layer was bonded to a glass plate (thickness: 1.2 mm) to prepare a measurement sample.

[0187] For the surface of the writing feel improving layer side (stylus pen contact surface) in the above-mentioned measurement sample, the evaluator simulated a predetermined writing operation using a stylus pen having a polyacetal (POM) pen tip (manufactured by Wacom Inc., product name "ACK-20001", pen tip diameter: 0.5 mm) to evaluate the following writing feel. The results are shown in Table 3.

[0188] (1) Vibration

[0189] The following criteria were used to evaluate whether the vibration feeling when writing on paper with a ballpoint pen could be reproduced.

[0190] A: The vibration feeling can be reproduced very well.

[0191] B+: The vibration is slightly loud, but can be reproduced well.

[0192] B-: The vibration is slightly weak, but can be reproduced well.

[0193] C+: The vibration is too strong and cannot be reproduced well.

[0194] C-: The vibration is too small to be reproduced well.

[0195] (2) Feeling of depression

[0196] Whether or not the concave feeling when writing on paper with a ballpoint pen can be reproduced was evaluated based on the following criteria.

[0197] A: The feeling of depression can be reproduced very well.

[0198] B+: The depression is slightly large, but can be reproduced well.

[0199] B-: The feeling of depression is slightly small, but can be reproduced well.

[0200] C+: The depression is too large, but the image is reproduced well.

[0201] C-: The feeling of depression is too small, but can be reproduced well.

[0202] D+: The feeling of depression is too large and cannot be reproduced well.

[0203] D-: The depression is too small to be reproduced well.

[0204] [Test Example 5] (Evaluation of anti-glare properties)

[0205] The release sheet was peeled off from the writing feel improving sheet produced in Examples and Comparative Examples, and the exposed surface (adhesive surface) of the adhesive layer was bonded to one surface of a black acrylic plate (Mitsubishi Rayon Co., Ltd., product name: "Acrylite L502") to prepare a measurement sample.

[0206] Then, a three-wavelength fluorescent lamp was turned on above the writing feel improving sheet, and the light was reflected by the writing feel improving sheet. The reflected light was visually observed, and the anti-glare property was evaluated according to the following criteria. The results are shown in Table 3.

[0207] A: The outline of the fluorescent light recognized by the reflection of the writing feel improving sheet is blurred and cannot be discerned.

[0208] B: The outline of the fluorescent light recognized by the reflection of the writing feel improving sheet is slightly blurred, and the outline can be roughly recognized, but it is very difficult.

[0209] C: The outline of the fluorescent lamp recognized by the reflection of the writing feel improving sheet is not blurred and the outline can be easily recognized.

[0210] [Test Example 6] (Evaluation of scratch resistance)

[0211] The release sheet was peeled off from the writing feel improving sheet produced in Examples and Comparative Examples, and the exposed surface (adhesive surface) of the exposed adhesive layer was bonded to a glass plate (thickness: 1.2 mm) to prepare a measurement sample.

[0212] The writing feel improving layer side (stylus pen contact surface) of the measurement sample was rubbed with 0000# steel wool at 250 g / cm 2 The writing feel improving layer was rubbed back and forth 10 times with a load of 10 cm. The surface of the writing feel improving layer was visually checked under a three-wavelength fluorescent lamp, and the scratch resistance was evaluated according to the following criteria. The results are shown in Table 3.

[0213] A: No injuries were found.

[0214] B: Less than 10 scars were confirmed.

[0215] C: 11 or more scars were confirmed.

[0216] [Test Example 7] (Measurement of pencil hardness)

[0217] The release sheet was peeled off from the writing feel improving sheet produced in Examples and Comparative Examples, and the exposed surface (adhesive surface) of the exposed adhesive layer was bonded to a glass plate (thickness: 1.2 mm) to prepare a measurement sample.

[0218] The surface of the writing feel improving layer side (stylus pen contact surface) in the above-mentioned measurement sample was measured for scratch hardness by the pencil method using a pencil scratch hardness tester (manufactured by TOYOSEIKI Co., Ltd., product name "NP") under the conditions of a load of 750 g and a speed of 1.0 mm / s in accordance with JIS K5600-5-4:1999. The measurement results were classified according to the following criteria and are shown in Table 3.

[0219] A: Pencil hardness is HB or higher.

[0220] B: The pencil hardness is less than HB and 3B or more.

[0221] C: Pencil hardness is less than 3B.

[0222] In addition, the details of the abbreviations in Table 3 are as follows.

[0223] Lumirror U48: Polyethylene terephthalate (PET) film having an easy-adhesive layer on both sides (manufactured by Toray Industries, Inc., product name "Lumirror U48", thickness of 50 μm, 75 μm, 100 μm or 125 μm)

[0224] Lumirror U40: Polyethylene terephthalate (PET) film having an easy-adhesive layer on both sides (manufactured by Toray Industries, Inc., product name "Lumirror U40", thickness 23 μm)

[0225] [Table 1]

[0226]

[0227] [Table 2]

[0228]

[0229]

[0230] As can be seen from Table 3, the writing feel improving sheet produced in the examples can well reproduce the concave feeling when writing on paper using a writing utensil, and achieves excellent writing feel in combination with good reproducibility of the vibration feeling. In addition, the writing feel improving sheet produced in the examples also obtained good results in the evaluation of various optical properties, anti-glare properties, scratch resistance and pencil hardness.

[0231] Industrial Applicability

[0232] The writing feel improving sheet of the present invention can be suitably used as the outermost layer of a touch panel using a stylus pen.

Claims

1. A writing feel improving sheet having a stylus contact surface to be contacted by a stylus, characterized in that: The writing feel improving sheet comprises a writing feel improving layer, a substrate provided on one side of the writing feel improving layer, and an adhesive layer provided on the side of the substrate opposite to the writing feel improving layer. The writing feel improving layer is formed by curing a coating composition containing a curable component, fine particles, a surface conditioner and silica nanoparticles. The average particle size of the microparticles is 3 μm or more and 20 μm or less. The surface of the writing feel improving layer opposite to the substrate is the stylus pen contact surface. For the stylus contact surface, when the tip of a triangular pyramid indenter with a tip curvature radius of 100 nm and an edge angle of 115° is pressed at a load speed of 1 mN / s, the pressing depth is 10 μm to 30 μm when the test load reaches 1961 mN.

2. The writing feel improving sheet according to claim 1, wherein: After the tip of a stylus having a tip of 0.5 mm in diameter is brought into contact with the stylus contact surface, a load of 200 g is applied to the stylus, while the angle between the stylus and the stylus contact surface is maintained at 45°, and the dynamic friction coefficient of the stylus when sliding linearly at a speed of 1.6 mm / sec is greater than 0.11 and less than 0.

62.

3. The writing feel improving sheet according to claim 1, wherein: The writing feel-improving layer is directly laminated on one surface of the substrate.

4. The writing feel improving sheet according to claim 1, wherein: The writing feel improving layer is a hard coating layer.