Sulfur-doped silicon negative electrode material, preparation method thereof, lithium secondary battery negative electrode containing the negative electrode material, and lithium secondary battery containing the negative electrode

CN112840484BActive Publication Date: 2024-10-11LG ENERGY SOLUTION LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080005694.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-03-08
Filing Date
2020-03-06
Publication Date
2024-10-11
Estimated Expiration
2040-03-06

AI Technical Summary

Technical Problem

Existing anode materials for lithium secondary batteries, especially silicon anode materials, suffer from volume expansion that leads to electrical short circuits, electrolyte decomposition and low electronic conductivity, limiting their performance in terms of high energy density and fast charging.

Method used

A sulfur-doped silicon anode material with a porous structure is prepared through a low-temperature reduction reaction, using a mixture of silicon dioxide, metal reducing agents, metal halide salts and sulfate compounds to form sulfur-doped silicon to improve its electronic conductivity and lithium ions. Diffusion rate.

Benefits of technology

It achieves the reduction of silicon volume expansion, improves electronic conductivity and lithium ion conductivity, improves the initial charge/discharge characteristics and charge/discharge life characteristics of lithium secondary batteries, and supports rapid charging and discharging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112840484B_ABST
    Figure CN112840484B_ABST
Patent Text Reader

Abstract

The present invention provides: a sulfur-doped silicon negative electrode material, the sulfur-doped silicon negative electrode material having an inner pore channel with an average width of 500nm to 3μm and an average outer diameter of 1μm to 5μm; a method for manufacturing the sulfur-doped silicon negative electrode material; a lithium secondary battery negative electrode comprising the sulfur-doped silicon negative electrode material; and a lithium secondary battery comprising the negative electrode.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2019-0027137 filed on March 8, 2019 and Korean Patent Application No. 10-2020-0028206 filed on March 6, 2020, which are hereby incorporated by reference in their entirety.

[0002] The invention relates to a sulfur-doped silicon negative electrode material, a preparation method thereof, a negative electrode for a lithium secondary battery comprising the negative electrode material, and a lithium secondary battery comprising the negative electrode. Background Art

[0003] The market for secondary batteries is expanding into various ranges such as batteries for portable electronic devices and telecommunication devices, ultra-small batteries such as batteries inserted into the human body, medium and large batteries such as those for hybrid electric vehicles (HEV / PHEV) or electric vehicles (EV), and large batteries for storing energy derived from power generation systems.

[0004] Existing carbon-based active materials commercially used as negative electrode active materials for lithium secondary batteries have excellent performance as battery active materials, but their theoretical capacity is limited to 372 mAh / g and is not suitable for satisfying such fields requiring high energy density.

[0005] Therefore, in order to solve the shortcomings of carbon-based active materials, the development of non-carbon negative electrode materials has been steadily carried out. Among them, silicon (Si) has a high discharge capacity of 4200 mAh / g and a high voltage (Li / Li) of 0.4 V. + ) has a very low lithium reaction potential, so it is expected to be used as an alternative negative electrode material. However, silicon negative electrode materials have the following disadvantages: they cause electrical short circuits due to volume expansion during charging; or increase the decomposition reaction of the electrolyte by creating new surfaces, causing the life characteristics of the battery to deteriorate rapidly. In addition, it has the disadvantage that it is not suitable for the purpose of fast charging due to low electronic conductivity and low lithium ion diffusion rate.

[0006] In order to improve the performance of silicon negative electrode materials, various attempts have been made (top-down, bottom-up or boron / nitrogen doping), such as making Si / C composite materials, but silicon negative electrode materials are still difficult to commercialize because they are prepared through complex preparation processes, are not suitable for commercialization, and exhibit low electrochemical properties (especially charging characteristics).

[0007] Prior art literature

[0008] [Patent Document]

[0009] PCT Publication No. WO2014042485A1 Summary of the invention

[0010] [Technical issues]

[0011] As a result of numerous attempts to solve the problems of the prior art as described above, the inventors of the present invention have found a method for very efficiently preparing sulfur-doped silicon having excellent properties as a negative electrode material through a low-temperature reduction reaction, thereby completing the present invention.

[0012] Therefore, an object of the present invention is to provide a method for preparing a sulfur-doped silicon negative electrode material, which can efficiently produce a sulfur-doped silicon negative electrode material having a porous structure and excellent electronic conductivity and ionic conductivity.

[0013] In addition, another object of the present invention is to provide a sulfur-doped silicon negative electrode material with a porous structure, thereby alleviating the large volume expansion of silicon, and having excellent electronic conductivity and ionic conductivity, and providing excellent initial charge / discharge characteristics, charge / discharge life characteristics, and charge / discharge characteristics according to C rate.

[0014] In addition, another object of the present invention is to provide a negative electrode comprising the sulfur-doped silicon negative electrode material and a lithium secondary battery comprising the negative electrode.

[0015] [Technical solution]

[0016] In order to achieve the above object, the present invention provides a sulfur-doped silicon negative electrode material, wherein the sulfur-doped silicon negative electrode material has an inner pore channel with an average width of 500 nm to 3 μm and an average outer diameter of 1 μm to 5 μm.

[0017] The sulfur-doped silicon negative electrode material may be characterized in that the doping amount of sulfur is 0.1 to 5 atomic %.

[0018] The sulfur-doped silicon negative electrode material may be characterized in that the electrical conductivity is 1 to 6 S / m.

[0019] The sulfur-doped silicon negative electrode material may be characterized in that the lithium ion diffusion coefficient is 10 -12 ~10 -10 cm 2 / s.

[0020] The sulfur-doped silicon negative electrode material may be characterized in that the porosity is 4% to 10%.

[0021] In addition, the present invention provides a method for preparing a sulfur-doped silicon negative electrode material, the method comprising the following steps:

[0022] (a) preparing a mixture by mixing silicon dioxide, a metal reducing agent, a metal halide salt, and a sulfate compound; and

[0023] (b) subjecting the mixture to a reduction reaction.

[0024] In addition, the present invention provides a negative electrode for a lithium secondary battery, wherein the negative electrode comprises the sulfur-doped silicon negative electrode material of the present invention.

[0025] In addition, the present invention provides a lithium secondary battery including the negative electrode for a lithium secondary battery of the present invention.

[0026] Beneficial Effects

[0027] Compared with conventional methods, the method for preparing a sulfur-doped silicon negative electrode material of the present invention provides an effect of very simply and efficiently manufacturing a sulfur-doped silicon negative electrode material having a porous structure and excellent electronic conductivity and ionic conductivity.

[0028] Because the sulfur-doped silicon negative electrode material of the present invention has a porous structure, it can alleviate the large volume expansion of silicon, and has excellent electronic conductivity and ionic conductivity, and provides the battery with excellent initial charge / discharge characteristics, charge / discharge life characteristics, and charge / discharge characteristics according to C rate. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 A scanning electron microscope (SEM) image of silica is shown.

[0030] Figure 2 A scanning electron microscope (SEM) image of sulfur-doped silicon prepared in Example 1 is shown.

[0031] Figure 3 A scanning electron microscope (SEM) image of silicon prepared in Comparative Example 1 is shown.

[0032] Figure 4 A transmission electron microscope (TEM) image of sulfur-doped silicon prepared in Example 1 is shown.

[0033] Figure 5 An elemental mapping image of the sulfur-doped silicon prepared in Example 1 obtained by energy dispersive spectroscopy (EDS) is shown.

[0034] Figure 6 A transmission electron microscope (TEM) image of silicon prepared in Comparative Example 1 is shown.

[0035] Figure 7 1 is the XRD spectrum of the sulfur-doped silicon (semi-metallic silicon) prepared in Example 1 and the silicon prepared in Comparative Example 1.

[0036] Figure 8 is a comparison graph of the electrical conductivity of sulfur-doped silicon (semi-metallic silicon) prepared in Example 1 and silicon prepared in Comparative Example 1.

[0037] Fig. 9 are initial charge / discharge curves of the coin cells prepared in Example 3 and Comparative Example 3.

[0038] Fig.10 is a graph showing the charge / discharge life characteristics of the coin cells prepared in Example 3 and Comparative Example 3.

[0039] Fig.11 is a graph showing the charge / discharge characteristics of the coin cells prepared in Example 3 and Comparative Example 3 according to the C rate. DETAILED DESCRIPTION

[0040] Hereinafter, the present invention will be described in detail.

[0041] The invention relates to a sulfur-doped silicon negative electrode material. The sulfur-doped silicon negative electrode material has an inner pore channel with an average width of 500nm to 3μm and an average outer diameter of 1μm to 5μm.

[0042] The average outer diameter of the inner pore channel is preferably 1 μm to 3 μm, more preferably 1.5 μm to 2.5 μm.

[0043] The sulfur-doped silicon negative electrode material of the present invention can be prepared by a low-temperature reduction reaction of a uniform mixture of silicon dioxide, a metal reducing agent, a metal halide salt and a sulfate compound.

[0044] According to the above-mentioned preparation method, the reduction reaction is carried out near the melting point of the metal halide salt, wherein the metal reducing agent reacts with the metal halide salt to form a metal-metal halide complex (hereinafter referred to as MHC), and the MHC selectively reduces silicon and sulfur by attacking silicon dioxide and sulfate compounds with oxygen, thereby forming small-sized silicon and sulfur seeds. In addition, the molten salt produces a clustering atmosphere, and agglomerates with each other to form silicon doped with micron-sized sulfur. Therefore, the sulfur-doped silicon negative electrode material of the present invention has a structure in which silicon and sulfur seeds agglomerate with each other in a mixed state, and has an inner pore channel formed when the seeds agglomerate with each other.

[0045] The sulfur-doped silicon negative electrode material of the present invention can alleviate the large volume expansion of silicon through a micron-sized porous structure, and enables a battery containing the sulfur-doped silicon negative electrode material to be quickly charged / discharged due to the effect of improved electronic / ionic conductivity, while providing a life improvement effect.

[0046] In the sulfur-doped silicon negative electrode material of the present invention, the inner pore channel may have a shape formed by being surrounded by sulfur-doped silicon particles, and the shape of the inner pore channel may have a shape similar to, for example, a cylindrical tube. However, the shape of the inner pore channel is not limited to these shapes, and as the inner pore channel of the present invention, any channel formed by being surrounded by sulfur-doped silicon particles may be included.

[0047] In the sulfur-doped silicon negative electrode material of the present invention, the doping amount of sulfur may be 0.1 to 5 atomic %, more preferably 0.3 to 2 atomic %.

[0048] If the doping amount of sulfur is less than the above range, it is difficult to expect improved conductivity, and if the doping amount of sulfur exceeds the above range, it is not preferred because of the problem of sulfur loss caused by the formation of excessive silicon sulfide.

[0049] The sulfur-doped silicon of the present invention has greatly improved electronic conductivity, which is comparable to the level of semi-metal (according to previous reports, when silicon is doped with sulfur to a certain level or more, a transition from an insulator to a metal occurs; Phys. Rev. Lett., 2011, 106, 178701). In addition, the lithium ion conductivity is greatly improved by the internal nanochannels formed when the individual crystal seeds are agglomerated with each other. The present invention is the first to discover a silicon negative electrode material having improved lithium ion conductivity by structurally forming channels.

[0050] The sulfur-doped silicon negative electrode material of the present invention may be characterized in that the conductivity is 1 to 6 S / m. In addition, the lithium ion diffusion coefficient is 10 -12 ~10 -10 cm 2 The sulfur-doped silicon negative electrode material of the present invention may have an electron / ion conductivity within the above range, thereby enabling rapid charge / discharge of a battery including the same and providing a lifespan improvement effect.

[0051] The sulfur-doped silicon negative electrode material may have a porosity of 4% to 10%, more preferably 5% to 8%.

[0052] In addition, the present invention relates to a method for preparing a sulfur-doped silicon negative electrode material, the method comprising the following steps:

[0053] (a) preparing a mixture by mixing silicon dioxide, a metal reducing agent, a metal halide salt, and a sulfate compound; and

[0054] (b) subjecting the mixture to a reduction reaction.

[0055] In the preparation method of the present invention, in step (a), silicon dioxide, a metal reducing agent, a metal halide salt, and a sulfate compound may be mixed in a weight ratio of 5 to 14:12 to 14:62 to 67:7 to 19.

[0056] If the amount of silica used is outside the above range, there is a problem of reduced yield due to excess unreduced silica remaining, which is not preferred.

[0057] In addition, when the amount of the metal reducing agent used is outside the above range, there is a problem that the reduction of silica and the sulfate compound does not proceed appropriately, which is not preferable.

[0058] In addition, when the amount of the metal halide salt used is outside the above range, there is a problem that the reduction of silica and the sulfate compound does not proceed appropriately, which is not preferable.

[0059] In particular, as described above, the weight ratio of the sulfate compound may be 7-19, more preferably 14-18.

[0060] If the weight ratio of the sulfate compound is less than 7, it is not preferred from the viewpoint of conductivity, and if the weight ratio of the sulfate compound exceeds 19, it is not preferred from the viewpoint of sulfur loss due to formation of excessive silicon sulfide.

[0061] In the preparation method of the present invention, the reduction reaction in step (b) can be carried out by heating to a temperature of 200 to 270° C., more preferably 220 to 250° C., under an inert atmosphere. If the reduction reaction is carried out at a temperature lower than the above range, it is difficult to induce the reduction reaction because the metal halide salt does not dissolve, which is not preferred. If the reduction reaction is carried out at a temperature exceeding the above range, the pressure in the reaction vessel is greatly increased, and the risk of explosion increases, which is not preferred.

[0062] The above reduction reaction can be carried out for 5 to 15 hours.

[0063] According to the preparation method of the present invention, if a uniform mixture of silicon dioxide, a metal reducing agent, a metal halide salt and a sulfate compound is reacted near the melting point of the metal halide salt using a low-temperature reduction reaction, the metal reducing agent reacts with the metal halide salt to form a metal-metal halide complex (hereinafter referred to as MHC). At this time, the MHC selectively reduces sulfur by attacking silicon dioxide and sulfate compounds with oxygen, thereby forming small-sized silicon and sulfur seeds, and the molten salt generates an agglomeration atmosphere and agglomerates with each other to form silicon doped with micron-sized sulfur.

[0064] In the preparation method of the present invention, the reduction reaction scheme of silicon dioxide is shown as follows:

[0065] [Reaction Scheme 1]

[0066] 3SiO 2 +4Al+2AlCl 3 →3Si+6AlOCl

[0067] In addition, the reduction reaction scheme of the sulfate compound as an additive is shown below:

[0068] [Reaction Scheme 2]

[0069] MgSO 4 +2Al+4AlCl 3 →S+MgAl 2 Cl 8 +4AlOCl

[0070] According to the preparation method of the present invention, various combinations of metal reducing agents and metal halide salts can be used for reaction, and compared with the conventional ion implantation method, uniform doping can be performed economically.

[0071] According to the preparation method of the present invention, the sulfur-doped silicon can be obtained with a high purity of 90% by weight or more.

[0072] In step (a), the sulfate compound may be at least one selected from the group consisting of: MgSO 4 、ZnSO 4 ,BaSO 4 、Na 2 SO 4 and NiSO 4 .

[0073] In step (a), the metal reducing agent may be at least one selected from the group consisting of Mg, Al, Ca and Zn, and the metal halide salt may be at least one selected from the group consisting of AlCl 3 MgCl 2 and ZnCl 2 .

[0074] After the reduction reaction of step (b) is completed, a step (c) of dispersing the reactants in water to remove unreacted metal halide salt and sulfate compound may be further performed.

[0075] In addition, after performing step (c), step (d) of removing the metal reducing agent and residual foreign matter by treating the reactant with an aqueous hydrochloric acid solution may be further performed.

[0076] In the preparation method of the present invention, 0.1% to 10% (volume / volume) of hydrofluoric acid can be used to remove unreacted silicon dioxide.

[0077] In addition, the present invention relates to a negative electrode for a lithium secondary battery and a lithium secondary battery including the negative electrode for a lithium secondary battery, wherein the negative electrode for a lithium secondary battery includes the sulfur-doped silicon negative electrode material of the present invention.

[0078] The negative electrode and the lithium secondary battery of the present invention, in addition to having the characteristics of using the sulfur-doped silicon negative electrode material to manufacture the negative electrode and using the negative electrode to manufacture the lithium secondary battery, can be constructed and manufactured by applying known techniques.

[0079] Hereinafter, a negative electrode for a lithium secondary battery and a lithium secondary battery will be described by way of examples.

[0080] The lithium secondary battery of the present invention may include: a negative electrode; a positive electrode; a separator provided between the positive electrode and the negative electrode; and an electrolyte.

[0081] The negative electrode may include a sulfur-doped silicon negative electrode material as a negative electrode active material, a binder, and a conductive material, and may be manufactured by further including a dispersant.

[0082] The negative electrode active material, binder, conductive material and / or dispersant may form a negative electrode active material layer, and the negative electrode active material layer is introduced into the negative electrode by applying a slurry containing the components to a current collector and drying it. Here, non-limiting examples of the current collector may include foil made of copper, gold, nickel or a copper alloy or a combination thereof.

[0083] There is no particular limitation on the conductive material, but conductive materials such as graphite materials such as KS6, and carbon materials such as Super-P, Denka black and carbon black; or conductive polymers such as polyaniline, polythiophene, polyacetylene and polypyrrole may be used alone or in combination.

[0084] In the lithium secondary battery of the present invention, the positive electrode may be manufactured in the form of bonding a positive electrode active material to a current collector according to a conventional method known in the art.

[0085] As the positive electrode active material, a known positive electrode active material can be used, and for example, lithium manganese oxide, lithium cobalt oxide, lithium nickel oxide, lithium iron oxide, LiNi as a three-component positive electrode material, and the like can be used. x Mn y Co z O 2 (NMC) or a lithium composite oxide obtained by combining them. In addition, examples of the current collector may include foil made of aluminum, nickel or a combination thereof. The positive electrode may further include the dispersant of the present invention.

[0086] The separator located between the positive electrode and the negative electrode is a separator that can isolate or insulate the positive electrode and the negative electrode from each other and can transfer lithium ions between the positive electrode and the negative electrode. The separator used in the present invention can be used as long as it is a porous polymer substrate commonly used in the art, for example, a polyolefin porous polymer film or a non-woven fabric, but is not particularly limited thereto.

[0087] Examples of the polyolefin-based porous polymer film may include films formed from each of polyethylene such as high-density polyethylene, linear low-density polyethylene, low-density polyethylene, and ultra-high molecular weight polyethylene; and polyolefin-based polymers such as polyethylene, polypropylene, polybutene, and polypentene, or films formed from polymers obtained by mixing them.

[0088] In addition to the polyolefin-based nonwoven fabric, the nonwoven fabric may include a nonwoven fabric formed of each of polyethylene terephthalate, polybutylene terephthalate, polyester, polyacetal, polyamide, polycarbonate, polyimide, polyetheretherketone, polyethersulfone, polyphenylene oxide, polyphenylene sulfide, polyethylene naphthalate, etc., or a nonwoven fabric formed of a polymer obtained by mixing them. The structure of the nonwoven fabric may be a spunbond nonwoven fabric or a meltblown nonwoven fabric composed of long fibers.

[0089] The thickness of the porous polymer substrate is not particularly limited but may be 5 μm to 50 μm, and the pore size and porosity present in the porous polymer substrate are not particularly limited but may be 0.01 μm to 50 μm and 10% to 95%, respectively.

[0090] In addition, in order to improve the mechanical strength of the separator and improve the safety of the lithium secondary battery, a porous coating layer containing inorganic particles and a polymer binder may be further included on at least one surface of the porous polymer substrate.

[0091] As the electrolyte, an electrolyte known in the art may be used, for example, a non-aqueous electrolyte may be used. The non-aqueous electrolyte may contain a lithium salt as an electrolyte salt. As the lithium salt, a lithium salt commonly used in an electrolyte for a lithium secondary battery may be used without limitation. For example, the anion of the lithium salt may be any one selected from the group consisting of: - , Cl - Br - ,I - 、NO 3 - 、N(CN) 2 - , BF 4 - , ClO 4 - PF 6 -, (CF 3 ) 2 PF 4 - , (CF 3 ) 3 PF 3 - , (CF 3 ) 4 PF 2 - , (CF 3 ) 5 PF - , (CF 3 ) 6 P - , CF 3 SO 3 - , CF 3 CF 2 SO 3 - , (CF 3 SO 2 ) 2 N - , (FSO 2 ) 2 N - , CF 3 CF 2 (CF 3 ) 2 CO - , (CF 3 SO 2 ) 2 CH - , (SF 5 ) 3 C - , (CF 3 SO 2 ) 3 C - , CF 3 (CF 2 ) 7 SO 3 - , CF 3 CO 2 - , CH 3 CO 2 - , SCN - , and (CF 3 CF 2 SO 2 ) 2 N - .

[0092] As the organic solvent contained in the nonaqueous electrolyte, the organic solvent commonly used in the lithium secondary battery electrolyte can be used without restriction, for example ether, ester, amide, linear carbonate, cyclic carbonate etc. can be used alone or in a combination of two or more thereof. Among them, the carbonate compound representatively being cyclic carbonate, linear carbonate or its mixture can be used.

[0093] The nonaqueous electrolyte can be injected at an appropriate stage of the lithium secondary battery manufacturing process, depending on the manufacturing process and the desired performance of the final product. That is, it can be applied before assembling the lithium secondary battery or in the final stage of assembling the lithium secondary battery.

[0094] In addition to the characteristic technology of the present invention described above, the lithium secondary battery can be constructed by applying technology known in the art.

[0095] In the case of the lithium secondary battery according to the present invention, in addition to the winding process as a general process, a stacking or laminating process of the separator and the electrode, a folding process, and a stacking / folding process may be performed.

[0096] The appearance of the lithium secondary battery is not particularly limited, but may be a cylindrical shape using a can, a square shape, a pouch shape, a coin shape, or the like.

[0097] Hereinafter, preferred embodiments of the present invention will be described to help understand the present invention. However, it will be apparent to those skilled in the art that the following embodiments illustrate the present invention, and that various changes and variations can be made within the scope and spirit of the present invention, and naturally, such changes and variations are also within the scope of the appended claims.

[0098] Example 1: Preparation of sulfur-doped silicon (semi-metallic silicon) negative electrode material

[0099] 1 g of silica, 3 g of magnesium sulfate, 2 g of aluminum metal and 10 g of aluminum chloride salt were uniformly mixed in a glove box using a mortar. After the uniformly mixed mixture was placed in a reaction container, a reduction reaction was performed by heating it at 250° C. for 10 hours in an argon atmosphere.

[0100] The semi-metallic silicon after the reduction reaction is completed is dispersed in 200 mL of water to react, and the residual magnesium sulfate and aluminum chloride are first dissolved away, and then the semi-metallic silicon is obtained through a vacuum filter.

[0101] Next, the semi-metallic silicon was put into 200 mL of 0.5 M hydrochloric acid and mixed at 35° C. for 3 hours, and the remaining aluminum metal and other foreign matters were removed.

[0102] The semi-metallic silicon is mixed with 0.1-5% (volume / volume) hydrofluoric acid for 5-30 minutes to remove the silicon dioxide remaining after the reaction, and the semi-metallic silicon is finally obtained through a vacuum filter.

[0103] Comparative Example 1: Preparation of silicon negative electrode material

[0104] A silicon negative electrode material was prepared in the same manner as in Example 1, except that magnesium sulfate as an additive was not added in Example 1.

[0105] Experimental Example 1: Evaluation of the morphology of sulfur-doped silicon (semi-metallic silicon) anode material or silicon anode material

[0106] In order to confirm the structure of the sulfur-doped silicon (semi-metal silicon) negative electrode material of the present invention, the morphologies of silicon dioxide, the sulfur-doped silicon (semi-metal silicon) prepared in Example 1, and the silicon prepared in Comparative Example 1 were photographed and compared using a scanning electron microscope (SEM) and a transmission electron microscope (TEM) ( Figures 1 to 4 ), and the width of the inner pore channel was measured. As a result of the measurement, it was confirmed that the average width of the inner pore channel was 500nm to 3μm.

[0107] In addition, the elemental mapping image ( Figure 5 ).

[0108] Specifically, Figure 1 shows a scanning electron microscope (SEM) image of silicon dioxide, Figure 2 shows a scanning electron microscope (SEM) image of sulfur-doped silicon prepared in Example 1, and Figure 3 A scanning electron microscope (SEM) image of silicon prepared in Comparative Example 1 is shown.

[0109] Figure 4 shows a transmission electron microscope (TEM) image of sulfur-doped silicon prepared in Example 1, Figure 5 shows an elemental mapping image of the sulfur-doped silicon prepared in Example 1 obtained by energy dispersive spectroscopy (EDS), and Figure 6 A transmission electron microscope (TEM) image of silicon prepared in Comparative Example 1 is shown.

[0110] from Figures 1 to 6 It can be confirmed that the sulfur-doped silicon (semi-metal silicon) negative electrode material of the present invention has a structure significantly different from that of Comparative Example 1.

[0111] Experimental Example 2: Evaluation of physical properties of sulfur-doped silicon (semi-metallic silicon) anode materials or silicon anode materials

[0112] (1) Evaluation of crystallization

[0113] The XRD patterns of the sulfur-doped silicon (semi-metallic silicon) prepared in Example 1 and the silicon prepared in Comparative Example 1 were measured by X-ray diffraction analysis using an X-ray diffractometer (Brucker, D8 ADVANCE), and the results are shown in Figure 7 middle.

[0114] As from Figure 7 It can be seen from the XRD patterns that both the sulfur-doped silicon (semi-metallic silicon) prepared in Example 1 of the present invention and the silicon prepared in Comparative Example 1 have the characteristics of crystalline silicon.

[0115] (2) Evaluation of electrical conductivity

[0116] The conductivity of the sulfur-doped silicon (semi-metallic silicon) prepared in Example 1 and the silicon prepared in Comparative Example 1 was measured by a voltage sweep method using a Keithley Soure Measure Unit (Keithley, SMU 2400). The results are shown in Figure 8 middle.

[0117] from Figure 8 It can be seen that, compared with the silicon prepared in Comparative Example 1, the sulfur-doped silicon (semi-metallic silicon) prepared in Example 1 of the present invention exhibits significantly better electrical conductivity.

[0118] Example 2: Preparation of negative electrode using sulfur-doped silicon (semi-metallic silicon) negative electrode material

[0119] A slurry composition for forming a negative electrode was prepared by mixing 1 g of the sulfur-doped silicon (semi-metallic silicon) negative electrode material prepared in the above Example 1 as a negative electrode active material, 0.05 g of PAA (manufacturer: Sigma-Aldrich) binder, 0.05 g of CMC (manufacturer: Sigma-Aldrich) binder and 0.1 g of Super P and dispersing them in an aqueous solvent.

[0120] The negative electrode was prepared by applying the slurry composition prepared above onto a copper foil and drying it.

[0121] Comparative Example 2: Preparation of negative electrode using silicon negative electrode material

[0122] A negative electrode was prepared in the same manner as in Example 2, except that the silicon negative electrode material prepared in Comparative Example 1 was used in Example 2 instead of the sulfur-doped silicon (semi-metal silicon) negative electrode material prepared in Example 1.

[0123] Example 3: Preparation of lithium secondary battery

[0124] The negative electrode prepared in Example 2 was punched out according to the size of a coin cell, and a coin cell was prepared using the negative electrode as a negative electrode.

[0125] In a glove box with argon atmosphere, the negative electrode, separator (polypropylene), lithium metal foil counter electrode, gasket, stainless steel coin, spring and stainless steel top plate were placed in order on a stainless steel bottom plate and pressurized to assemble a coin cell.

[0126] The electrolyte is a mixed solution of ethylene carbonate (EC) and diethyl carbonate (DEC), in which 1.3 M LiPF 6 , 10 wt % fluoroethylene carbonate (FEC), and the mixed solution was injected onto the stamped positive electrode.

[0127] Comparative Example 3: Preparation of lithium secondary battery

[0128] A three-electrode single cell was prepared in the same manner as in Example 3, except that the negative electrode prepared in Comparative Example 2 was used.

[0129] Experimental Example 3: Evaluation of Initial Charge / Discharge Characteristics, Charge / Discharge Life Characteristics, and Charge / Discharge Characteristics of Batteries at C Rates

[0130] Next, the batteries prepared in Example 3 and Comparative Example 3 were used to evaluate the relative capacity and area capacity of each battery.

[0131] (1) Evaluation of initial charge / discharge characteristics

[0132] The initial charge / discharge characteristics of each battery were confirmed by a constant current method (constant current measurement) using a charge / discharge device (Wonatech, WBCS3000K8), and the results are shown in Fig. 9 In. From Fig. 9 It can be seen that the initial charge / discharge efficiency of the battery prepared in Example 3 of the present invention is better than that of the battery prepared in Comparative Example 3.

[0133] (2) Evaluation of charge / discharge life characteristics

[0134] The charge / discharge life characteristics of each battery were confirmed by a constant current method (constant current measurement) using a charge / discharge device (Wonatech, WBCS3000K8), and the results are shown in Fig.10 In. From Fig.10 It can be seen that the charge / discharge life characteristics of the battery prepared in Example 3 of the present invention are better than those of the battery prepared in Comparative Example 3.

[0135] (3) Evaluation of charge / discharge characteristics based on C rate

[0136] The charge / discharge characteristics of each battery according to the C rate were confirmed by a constant current method (constant current measurement) using a charge / discharge device (Wonatech, WBCS3000K8), and the results are shown in Fig.11 In. From Fig.11 It can be seen that the charge / discharge characteristics of the battery prepared in Example 3 of the present invention according to the C rate are better than those of the battery prepared in Comparative Example 3.

Claims

1. A sulfur-doped silicon negative electrode material, the sulfur-doped silicon negative electrode material having an inner pore channel with an average width of 500 nm to 3 μm and an average outer diameter of 1 μm to 5 μm, wherein the sulfur-doped silicon negative electrode material has a structure in which silicon and sulfur seed crystals are agglomerated with each other in a mixed state, and The sulfur-doped silicon negative electrode material is a material doped with 0.1 to 5 atomic % of sulfur. 2 . The sulfur-doped silicon negative electrode material according to claim 1 , wherein the inner pore channel has a shape formed by being surrounded by sulfur-doped silicon particles. 3 . The sulfur-doped silicon negative electrode material according to claim 1 , wherein the sulfur-doped silicon negative electrode material has an electrical conductivity of 1 to 6 S / m.

4. The sulfur-doped silicon negative electrode material according to claim 1, wherein the sulfur-doped silicon negative electrode material has 10 -12 ~10 -10 cm 2 / s lithium ion diffusion coefficient. 5 . The sulfur-doped silicon negative electrode material according to claim 1 , wherein the sulfur-doped silicon negative electrode material has a porosity of 4% to 10%.

6. A method for preparing the sulfur-doped silicon negative electrode material according to claim 1, the method comprising the following steps: (a) preparing a mixture by mixing silicon dioxide, a metal reducing agent, a metal halide salt, and a sulfate compound in a weight ratio of 5 to 14:12 to 14:62 to 67:7 to 19; and (b) subjecting the mixture to a reduction reaction.

7. The method for preparing a sulfur-doped silicon negative electrode material according to claim 6, wherein in step (b), the reduction reaction is carried out by heating to a temperature of 200 to 270°C under an inert atmosphere.

8. The method for preparing a sulfur-doped silicon negative electrode material according to claim 6, wherein in step (a), the sulfate compound is at least one selected from the group consisting of: MgSO4, ZnSO4, BaSO4, Na2SO4 and NiSO4.

9. The method for preparing a sulfur-doped silicon negative electrode material according to claim 6, wherein in step (a), the metal reducing agent is at least one selected from the group consisting of: Mg, Al, Ca and Zn, and the metal halide salt is at least one selected from the group consisting of: AlCl3, MgCl2 and ZnCl2.

10. The method for preparing a sulfur-doped silicon negative electrode material according to claim 6, further comprising a step (c) of dispersing the reactants in water to remove unreacted metal halide salts and sulfate compounds after the reduction reaction of step (b) is completed.

11. The method for preparing a sulfur-doped silicon negative electrode material according to claim 10, further comprising a step (d) of removing the metal reducing agent and residual foreign matter by treating the reactants with an aqueous hydrochloric acid solution after performing step (c). 12 . The method for preparing a sulfur-doped silicon negative electrode material according to claim 6 , wherein 0.1 vol % to 10 vol % of hydrofluoric acid is used to remove unreacted silicon dioxide. 13 . A negative electrode for a lithium secondary battery, comprising the sulfur-doped silicon negative electrode material according to claim 1 . 14 . A lithium secondary battery comprising the negative electrode for a lithium secondary battery according to claim 13 .