Aqueous dispersion composition
The water-borne vinyl acetate copolymer dispersion composition prepared by the extruder continuous phase conversion method solves the problems of wide particle size distribution and poor coating stability in the existing technology, and achieves small particle size, narrow particle size distribution and good coating. Layer uniformity, suitable for food and industrial packaging, improves bond strength and hot tack.
Patent Information
- Application Number
- CN202080036986.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-04-17
- Filing Date
- 2020-03-02
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2040-03-02
AI Technical Summary
The low-temperature heat-sealing composition prepared by the existing emulsification method has problems such as wide particle size distribution, coating appearance problems, and poor storage stability, making it difficult to meet the needs of food and industrial packaging.
A water-borne vinyl acetate copolymer dispersion composition with small particle size and narrow particle size distribution was prepared using an extruder-based continuous phase conversion method, including vinyl acetate copolymer, compatibilizer, dispersant, alkali and water addition substance, forming a stable aqueous continuous dispersion through neutralization and phase conversion.
It achieves smaller particle size, narrower particle size distribution, good coating uniformity and better storage stability. It is suitable for food and industrial packaging and improves bonding strength and hot tack.
Smart Images

Figure BDA0003361351750000111 
Figure BDA0003361351750000121 
Figure BDA0003361351750000122
Abstract
Description
Technical Field
[0001] The present invention relates to an aqueous dispersion composition for use as a heat seal coating (HSC); more particularly, the present invention relates to an aqueous dispersion composition for use as a HSC produced by an extruder-based continuous phase inversion process. Background Art
[0002] In the food and industrial packaging industries, adhesive compositions are often used to heat seal polymer packaging at low temperatures (e.g., less than [<] 150 degrees Celsius [°C]); at low temperatures, the adhesive composition should: (1) be stable, (2) have a reasonable particle size and particle size distribution, (3) have viscosity and rheological properties that allow the composition to be easily applied to a substrate and can be coated on the substrate to provide a uniform heat-seal coating; (4) be environmentally friendly, and (5) comply with food contact regulations, and therefore be suitable for use in food packaging.
[0003] So far, various emulsification methods under various method conditions (e.g., under high temperature and high pressure) have been used to prepare low-temperature heat-sealing compositions used as emulsion adhesive products, such as disclosed in CN108084370A, CN108148215A, and CN108102472A. In addition, a continuous direct dispersion method based on an extruder has also been used to prepare a water-based heat-sealing product based on ethylene-vinyl acetate copolymer (EVA copolymer), wherein the polymer melt blend is contacted with an aqueous stream including a neutralizing agent, water, and a surfactant in the emulsification zone of the extruder to form a dispersion. However, there are one or more problems in the above direct emulsification method, such as the emulsion produced by the method has a wider particle size distribution, which can lead to potential coating appearance problems, such as yellowing, shelf life stability potentially reduced, particle and particle composition uneven problems. In view of the above existing problems of the prior art emulsion and method, it is desirable to provide a dispersion composition that can be used as a heat-sealing coating without the above problems. Summary of the invention
[0004] The present invention relates to a novel waterborne vinyl acetate copolymer dispersion composition used as HSC. According to a preferred embodiment of the present invention, the vinyl acetate copolymer may include, for example, an ethylene vinyl acetate (EVA) copolymer dispersion composition. In another preferred embodiment, the dispersion composition may include the following components: (a) at least one vinyl acetate copolymer; (b) at least one compatibilizer; (c) at least one alkyl carboxylic acid as a dispersant after neutralization; (d) a first water addition to provide a polymer continuous dispersion; (e) at least one base added to neutralize the effective acid and separate the water addition that continuously produces the polymer continuous system; and (f) a second water addition to achieve phase conversion to a water continuous dispersion.
[0005] In another embodiment, the present invention includes a method of making a waterborne vinyl acetate copolymer dispersion composition for use as a HSC, wherein the method includes producing the dispersion using an extruder-based continuous phase inversion process. The method is advantageous in that the method is capable of producing a dispersion having a smaller particle size and a narrower particle size distribution and a lower amount (e.g., <1.5 weight percent [wt %]) of surfactant compared to a direct emulsification process using a continuous extruder. The use of increased amounts (e.g., greater than [>] 2 wt %) of surfactant can adversely affect the application properties of the resulting dispersion product, such as lower water resistance and lower durability due to surfactant surface migration.
[0006] In yet another embodiment, the present invention includes a HSC prepared from the above dispersion composition; and a substrate containing the HSC on at least a portion of a surface of the substrate.
[0007] In yet another embodiment, the present invention includes food and industrial packaging materials heat-sealed with the above HSC; and heat-sealed articles prepared from the above HSC composition. DETAILED DESCRIPTION
[0008] The term "compatibilizer" as used herein refers to a resin having a viscosity of >1 Pascal-second (Pa·s) at 170°C, an acid value between 50 mg KOH per gram of resin (mg KOH / g resin) and 200 mg KOH / g resin; and a melting point above 100°C.
[0009] By "dispersant" herein is meant fatty acids, soaps generated in situ.
[0010] "Neutralizing agent" herein means a compound used to neutralize an acid (eg, an alkyl carboxylic acid described herein). Examples of neutralizing agents include, for example, KOH, ammonia, NaOH, amines, and mixtures thereof.
[0011] Water herein means deionized (DI) water used to make the aqueous dispersion of the present invention.
[0012] In a broad embodiment, the dispersion composition of the present invention comprises: (a) at least one vinyl acetate copolymer, such as EVA; (b) at least one compatibilizer; (c) at least one dispersant; (d) a first water addition to provide a polymer continuous dispersion; (e) at least one base added to neutralize the effective acid and separate the water addition to continuously produce the polymer continuous system; and (f) a second water addition to achieve a phase inversion to a water continuous dispersion.
[0013] The vinyl acetate copolymer compound used to prepare the dispersion composition of the present invention includes, for example, one or more vinyl acetate copolymer compounds known in the art. For example, the copolymer compound includes ethylene vinyl acetate copolymer (EVA); vinyl acetate ethylene copolymer (VAE); other vinyl acetate copolymers, such as vinyl acetate acrylate copolymer and vinyl acetate-ethylene-styrene copolymer, etc.; and mixtures thereof.
[0014] The amount of copolymer compound used to prepare the dispersion composition of the present invention is, for example, 50 to 90 wt % in one embodiment, 80 to 90 wt % in another embodiment, and 85 to 90 wt % in yet another embodiment, based on the total solids content.
[0015] Some exemplary advantageous properties exhibited by vinyl acetate copolymer compounds may include better adhesion to polyethylene terephthalate (PET), foils, and other substrates.
[0016] In another embodiment, a copolymer is produced using, for example, a monomer containing an oxygen element as one of the monomers (i.e., a comonomer and a vinyl acetate comonomer). For example, in addition to an olefin such as ethylene, the comonomer is selected from one or more of the following compounds: vinyl acetate, acrylate, methacrylate, acrylic acid nitrile, etc.; and mixtures thereof.
[0017] The amount of the comonomer compound when used with the vinyl acetate comonomer is, for example, 5 to 70 wt % in one embodiment, 10 to 50 wt % in another embodiment, 15 to 40 wt % in yet another embodiment, and 15 to 30 wt % in yet another embodiment.
[0018] The compatibilizer compound used to prepare the dispersion composition of the present invention includes, for example, one or more compatibilizer compounds known in the art. For example, in one embodiment, the compatibilizer compound includes rosin acid, rosin ester, terpene phenolic resin, pure monomer resin and phenolic resin or a mixture thereof.
[0019] Generally, the viscosity of the compatibilizer compound at 170° C. is >1 Pa·s in one embodiment, 1 Pa·s to 20 Pa·s in another embodiment, and 5 Pa·s to 8 Pa·s in yet another embodiment. The viscosity of the compatibilizer is measured by any well-known means, such as by using a conventional viscometer, such as a Brookfield Thermosel.
[0020] Generally, the compatibilizer compound has an acid value of 10 mg KOH / g resin to 250 mg KOH / g resin in one embodiment, 50 mg KOH / g resin to 200 mg KOH / g resin in another embodiment, 100 mg KOH / g resin to 200 mg KOH / g resin in yet another embodiment, 125 mg KOH / g resin to 200 mg KOH / g resin in yet another embodiment, and 140 mg KOH / g resin to 180 mg KOH / g resin in even yet another embodiment. The acid value of the compatibilizer can be measured by any conventional titration method.
[0021] The melting point of the compatibilizer compound includes, for example, above 40°C in one embodiment, 50°C to 200°C in another embodiment, 100°C to 200°C in yet another embodiment, and 120°C to 180°C in yet another embodiment. The melting point of the compatibilizer can be measured by any well-known means. For example, the melting point of the compatibilizer of the present invention is measured by conventional differential scanning calorimetry (DSC) methods.
[0022] The amount of compatibilizer compound used to prepare the dispersion composition of the present invention includes, for example, 5 to 30 wt % of the total solids content in one embodiment, 9 to 20 wt % in another embodiment, 9 to 15 wt % in yet another embodiment, and 9 to 12 wt % in yet another embodiment.
[0023] Some benefits of using a compatibilizer compound include, for example, that the compatibilizer facilitates the interaction of the EVA polymer with the dispersant, and that the compatibilizer facilitates the interaction of the EVA polymer with the substrate, thereby enhancing adhesion properties.
[0024] Dispersants or dispersant compounds used to prepare the dispersion compositions of the present invention include, for example, one or more dispersants known in the art. For example, in one embodiment, the dispersant includes alkyl carboxylic acids; oleic acid (fatty acid, soap generated in situ); dimer acid; other alkyl carboxylic acids having >12 to <20 carbon atoms per acid; and mixtures thereof.
[0025] Concentrations of dispersants used to prepare the dispersion compositions of the present invention include, for example, <2 wt % of formulation solids in one embodiment, <1.5 wt % in another embodiment, <1 wt % in yet another embodiment, 0.66 wt % to 1 wt % in yet another embodiment, and 0.66 wt % to 0.75 wt % in yet another embodiment.
[0026] When the appropriate amount of dispersant is properly selected, some exemplary advantageous properties include (1) providing stability to the polymer particles in the dispersion, and (2) providing a balance of surface tension and wetting ability of the dispersion to the substrate.
[0027] The method of making the dispersion composition of the present invention may include adding one or more water additives to the composition. For example, in a preferred embodiment, a first water additive is added to the composition in an amount sufficient to form a continuous dispersion of the polymer.
[0028] For example, the amount of the first water addition is 3.5 to 6 wt % in one embodiment, 3.5 to 5 wt % in another embodiment, and 3.5 to 4.5 wt % in yet another embodiment based on total solids and water.
[0029] The dispersion composition of the present invention includes a base to neutralize the effective acid in the composition and separate the water additive of the continuous system of continuously producing the polymer. The base compound used to prepare the dispersion composition of the present invention includes, for example, one or more bases known in the art. For example, the neutralizing agent or base compound includes potassium hydroxide aqueous solution (KOH), sodium hydroxide (NaOH), ammonia and mixtures thereof. In a preferred embodiment, the base compound is, for example: KOH with a concentration of 10% to 90% by weight, 20% to 90% by weight in another embodiment, and 40% to 50% by weight in another embodiment.
[0030] The amount of base used to prepare the dispersion composition of the present invention is, for example, such that the theoretical neutralized acid value of the component is 70 percent (%) to 130% in one embodiment, 80% to 120% in another embodiment, 90% to 110% in yet another embodiment, and 90% to 100% in yet another embodiment.
[0031] Some exemplary beneficial properties exhibited by the base may include neutralization that stabilizes the polymer particles.
[0032] As previously described, the method of making the dispersion composition of the present invention includes adding one or more waters to the composition. In a preferred embodiment, a second water addition is added to the composition, for example in an amount sufficient to effect a phase inversion to a water continuous dispersion.
[0033] For example, based on (1) total solids, (2) first water addition, and (3) second water addition, the amount of second water addition is >3.5 wt % in one embodiment, 20 wt % to 90 wt % in another embodiment, 30 wt % to 70 wt % in yet another embodiment, and 40 wt % to 60 wt % in yet another embodiment.
[0034] The dispersion composition of the present invention may also include other optional additional compounds or additives; and the optional compounds may be added to the composition in combination with one or more of components (a)-(f). Optional additives or agents that can be used to prepare the dispersion composition of the present invention include, for example, optional one or more compounds known in the art for their use or function. For example, optional additives include, but are not limited to, defoamers, rheology modifiers, wetting agents, and mixtures thereof.
[0035] When used to prepare the dispersion compositions of the present invention, the amounts of optional compounds include, for example, 0 wt % to 5 wt % in one embodiment, 0.001 wt % to 3 wt % in another embodiment, 0.01 wt % to 2 wt % in yet another embodiment, and 0.1 wt % to 1 wt % in yet another embodiment.
[0036] In a general embodiment, the method for preparing the dispersion composition of the present invention comprises the steps of mixing (e.g., melt blending) the following: (a) at least one vinyl acetate copolymer, such as EVA; (b) at least one compatibilizer; (c) at least one dispersant; (d) a first water addition to provide a polymer continuous dispersion; (e) at least one base added to neutralize the effective acid and separate the water addition to continuously produce the polymer continuous system; and (f) a second water addition to achieve a phase inversion to a water continuous dispersion.
[0037] Generally speaking, the process apparatus and ancillary equipment suitable for use in the present invention for forming a homogenous melt blend may include any components; and any conditions commonly used for melt blending thermoplastic resins and known to those familiar with extruder-based processes. For example, apparatus that may be used in the present invention include heat exchangers, back pressure regulators, melt pumps, gear pumps; kneaders, Mixers, rotor-stator mixers, single-screw extruders, twin-screw extruders, multi-screw extruders and other devices.
[0038] In addition, various schemes can be used to set up the process equipment. For example, in one embodiment, the first mixing device is used in combination with the second mixing device. For example, in some embodiments, the first mixing device is a kneader, The first mixing device is a mixer, a single screw extruder or a multi-screw extruder; and the second mixing device is, for example, an extruder, such as a twin-screw extruder with multiple heating zones. For example, in other embodiments, the first mixing device is, for example, an extruder, such as a twin-screw extruder; and the second mixing device is a rotor stator mixer.
[0039] In another embodiment, a single extruder (e.g., a twin-screw extruder with multiple heating zones, with auxiliary equipment such as a back pressure regulator, a melt pump, or a gear pump) is used to produce the aqueous dispersion composition of the present invention. For example, in various embodiments, the extruder may have various zones, including, for example, (1) a conveying, melting and mixing zone, (2) an emulsification zone, and (3) a dilution zone; and the different zones may be operated at a predetermined temperature. In some embodiments, the conveying, melting and mixing zone portion of the extruder may have a barrel of length "L" and diameter "D", and the length-to-diameter ratio (L / D) used is: for example, in a preferred embodiment, not less than 12:1, such as 12:1 to 60:1. In some preferred embodiments, the above-mentioned method based on the extruder used in the present invention is described in more detail, for example, in U.S. Provisional Patent Application No. 62 / 579,354 filed by Escobar Marin et al. on October 31, 2017.
[0040] In another embodiment, the aqueous dispersion composition is prepared, for example, using a continuous process based on an extruder, according to the following general method: the above components (a)-(f) of the composition of the present invention are fed into an extruder using, for example, a controlled rate feeder. As described above, any conventional extruder can be used in the present invention. In one embodiment, the extruder includes, for example, a 25 millimeter (mm) diameter twin screw extruder having an L / D ratio as described above. In one embodiment, the feed rate (grams / minute (g / min)) of components (a)-(f) is, for example, 60 g / min to 150 g / min. The components of the present invention are transferred and melted via an extruder to form a liquid molten material.
[0041] The extruder temperature profile can be gradually increased to a predetermined temperature. For example, in one embodiment, the gradually increased temperature is 70°C to 240°C, and in another embodiment, 120°C to 150°C. In one embodiment, water is then fed into the extruder at a predetermined rate (e.g., at a rate of 1.0 g / min to 2.0 g / min). After feeding the water, in one embodiment, a second introduction site in the extruder is used to feed the neutralizer into the extruder at a predetermined rate (e.g., at a rate of 1.4 g / min to 2.4 g / min). In one embodiment, after the neutralizer, phase conversion water is fed into the extruder via the inlet position of the extruder; and water is fed into the extruder at a predetermined rate (e.g., at a rate of 1.0 g / min to 8.0 g / min). In one embodiment, two independent pumps are also used to feed dilution water into the extruder at one or two inlet positions (first and second inlet positions) of the extruder at a predetermined rate (e.g., at a rate of 20 g / min to 90 g / min). The extruder temperature profile is recooled to a temperature of, for example, less than 100° C. near the end of the extruder. At the extruder exit, a back pressure regulator is used to adjust the pressure inside the extruder barrel to a pressure suitable for reducing steam formation. Generally, in one embodiment, the pressure inside the extruder barrel is, for example, 2 megapascals [MPa] to 4 MPa.
[0042] After the above process steps, the resulting aqueous dispersion product exits the extruder. In a preferred embodiment, the aqueous dispersion is then filtered through a 200 micron (μm) filter. The resulting filtered aqueous dispersion has a solid content measured in weight percent (wt%); and the solid particles of the dispersion have a volume average particle size measured in microns. For example, in one embodiment, the solid content of the dispersion is 30 wt% to 50 wt%; and in one embodiment, the particle size of the particles in the dispersion is 0.9 μm to 2.0 μm. In some embodiments, the particle size modulus value can also be recorded. The solid content of the aqueous dispersion is measured using conventional instruments, such as MB45 infrared solid analyzer (purchased from Ohaus Corporation); and conventional instruments (such as The particle size of the solid particles of the aqueous dispersion is measured using an LS-230 particle size analyzer (available from Beckman Coulter Corporation). In a preferred embodiment, the solid content and average particle size (PS) of the solid particles of the dispersion are as described in Table IV of the Examples.
[0043] In one embodiment, the aqueous dispersion composition is, for example, a wax-free aqueous dispersion composition. In a preferred embodiment, the wax-free aqueous dispersion composition is manufactured, for example, using an extruder-based continuous process. The process steps include, for example, the following process steps:
[0044] (A) providing an extruder;
[0045] (B) feeding into the extruder a mixture of: (i) at least one vinyl acetate copolymer; (ii) at least one compatibilizer; and a dispersant;
[0046] (C) feeding a first water addition to the mixture of step (B) in the extruder to provide a continuous polymer dispersion;
[0047] (D) feeding at least one base into the mixture of step (C) in the extruder to neutralize any effective acid present in the mixture of step (C); and
[0048] (E) feeding a second addition of water to the mixture of step (D) in the extruder to effect phase inversion, thereby forming a water continuous dispersion.
[0049] In another embodiment, step (B) of the above method can be divided into two steps. For example, (i) at least one vinyl acetate copolymer and (ii) at least one compatibilizer are first mixed together to form a mixture, and then the mixture is fed into an extruder in a stream; and at least one dispersant is fed into the extruder in a separate material stream.
[0050] The dispersion composition of the present invention prepared according to the method described above has several beneficial properties, including, for example, smaller particle size and narrower particle distribution, and such properties advantageously result in, for example, good coating appearance; good coating uniformity; more preferably storage stability and preferred solids content.
[0051] For example, in one embodiment, the solids content of the dispersion of the present invention is 20% solids to 80% solids; in another embodiment, 30% solids to 70% solids, and in yet another embodiment, 35% solids to 55% solids. The solids content of the dispersion can be measured, for example, by an Ohaus MB45 infrared moisture analyzer (available from Ohaus Corporation) or by a thermal oven. In a preferred embodiment, the solids content of the dispersion is measured by the above moisture analyzer.
[0052] For example, the viscosity characteristics of the dispersion of the present invention are 10 millipascal-seconds (mPa.s) to 100 mPa.s in one embodiment; 20 mPa.s to 60 mPa.s in another embodiment, and 30 mPa.s to 50 mPa.s in yet another embodiment. The viscosity characteristics of the dispersion are measured, for example, using a Brookfield DV-II+ (available from Brookfield).
[0053] For example, the particle size of the particles in the dispersion of the present invention is 0.2 micrometers (μm) to 6 μm in one embodiment; 0.3 μm to 4 μm in another embodiment, and 0.4 μm to 2 μm in yet another embodiment. The particle size of the dispersion can be measured by any well-known particle size measuring instrument. In one embodiment, the particle size of the dispersion is measured, for example, using a Beckman Coulter LS 13 320 instrument.
[0054] In addition to the above properties, the performance of the dispersion composition is evaluated in terms of, for example, shelf stability and is tested by accelerated temperature aging at 45°C and refrigerated conditions. For example, the shelf stability of the dispersion of the present invention is evaluated by aging in: (1) a refrigerated (4°C) environment and (2) a heated (45°C) oven, by tracking the phase separation and viscosity of the dispersion weekly. If the dispersion settles and separates into two layers; the viscosity changes significantly by more than 100%; or becomes gelatinous (i.e., gelling occurs), then the dispersion is not shelf stable.
[0055] The overall stability of the dispersion can then be compared to a commercial product produced using a batch process. In one embodiment, a dispersion is rated as having "good" shelf stability or "worse" shelf stability, for example, compared to a batch process product. For example, "good" shelf stability means a dispersion that performs the same as or better than a batch process commercial product; and "worse shelf stability" means a dispersion that performs worse than a batch process commercial product.
[0056] As mentioned above, after the dispersion composition of the present invention is prepared, the dispersion composition can be used as HSC for various applications immediately. For example, in one embodiment, the HSC dispersion composition can be used to produce HSC on a substrate such as a food packaging film, and then the film substrate can be heat sealed.
[0057] The HSC dispersion composition can be applied to a substrate using various conventional coating methods such as gravure coating, Meyer rod coating, curtain coating, air knife coating method, flexographic relief method, and lithographic printing method.
[0058] The dispersion compositions of the present invention provide HSCs that can be advantageously used in a variety of applications, such as for heat sealing food and industrial packaging. The HSCs of the present invention also exhibit several beneficial properties, including, for example, good coating appearance, high bond strength and high hot tack, and no yellowing.
[0059] For example, in one embodiment, the appearance of a coating formed from a HSC dispersion of the present invention is evaluated by visually observing the coating of the present invention and comparing the HSC of the present invention with a batch process HSC coated on a PET film. The HSC appearance can be reported, for example, according to the following rating system: HSC with a "good" coating appearance as determined by visual observation versus HSC with an "oily" coating appearance as determined by visual observation. An HSC with a "good" coating appearance is one where the coating gloss is acceptable and the smoothness is good; and an "oily" coating appearance is one where the HSC is observed to have an ugly appearance and is unacceptable. In addition, by visual observation, HSCs made using conventional batch processes may also appear undesirably "yellow" or opaque, whereas HSCs made according to the present invention do not have a "yellowing" appearance, but are observed to have a clear coating.
[0060] For example, in one embodiment, the sealing performance of the HSC of the present invention is better than the batch method in terms of bonding strength. For example, the bonding strength of the HSC of the present invention is: 20% to 300% better than the batch method in one embodiment, 50% to 200% better than the batch method in another embodiment, 60% to 150% better than the batch method in another embodiment; and 70% to 100% better than the batch method in another embodiment. The sealing properties of the HSC are measured, for example, by bonding tests as described below in the Examples.
[0061] For example, in one embodiment, the hot tack properties of the HSC of the present invention are better than the batch process. For example, the hot tack properties of the HSC of the present invention are: 10% to 200% better than the batch process in one embodiment, 20% to 150% better than the batch process in another embodiment, 25% to 100% better than the batch process in yet another embodiment; and 30% to 80% better than the batch process in yet another embodiment. The hot tack properties of the HSC are measured, for example, according to ASTM F1921 Test Method B using a temperature controlled Instron testing instrument operating at a speed of 200 millimeters per second (mm / s).
[0062] As previously mentioned, the dispersion composition can be used to make HSC for food packaging articles. Other applications in which the dispersion composition can be used include applications such as industrial skin packaging and medical packaging applications.
[0063] Examples
[0064] The following examples are presented to further illustrate the present invention, but should not be construed as limiting the scope of the claims. Unless otherwise indicated, all parts and percentages are by weight.
[0065] Various terms and designations used in the following inventive examples (Inv.Ex.) and comparative examples (Comp.Ex.); and raw materials or components are described in Table I.
[0066] Table I - List of compounds
[0067]
[0068] Table II - Component Characteristics
[0069]
[0070] Table III - Dispersion Formulations
[0071]
[0072] Table IV - Dispersion Conditions
[0073]
[0074] Notes to Table IV: (1) “V 平均 "PS" stands for "volume average particle size".
[0075] (2) “NA” stands for “Not Applicable”.
[0076] (3) "ND" stands for "Not Dispersed".
[0077] (4) "NM" stands for "not measured".
[0078] Comparative Example AD
[0079] General procedure for preparing dispersions
[0080] The aqueous dispersions were prepared in Comparative Examples AD using the following general procedure:
[0081] Components 1-3 as described in Table IV were fed into a 25 mm diameter twin screw extruder using a controlled rate feeder and using the feed rates (g / min) described in Table IV. Components 1-3 were conveyed through the extruder and melted to form a liquid molten material.
[0082] The extruder temperature profile was ramped up to the temperature described in the "Polymer Melt Zone" column of Table IV. Water was mixed with the neutralizing agent and fed into the extruder at the feed rate described in Table IV so as to neutralize at the initial water introduction point. Next, dilution water was fed into the extruder at one inlet location or two separate inlet locations (first and second inlet locations) at the feed rate described in Table IV using two separate pumps. The extruder temperature profile was cooled back to a temperature of less than 100° C. near the end of the extruder. At the extruder exit, a back pressure regulator was used to adjust the pressure inside the extruder barrel to a pressure suitable for reducing steam formation.
[0083] The aqueous dispersion product exits the extruder. The aqueous dispersion is filtered through a 200 μm filter. The resulting filtered aqueous dispersion has a solid content measured in weight percent (wt %); and the solid particles of the dispersion have a volume average particle size measured in microns (V 平均 The solid content of the aqueous dispersion was measured using an infrared solid analyzer; and the particle size of the solid particles of the aqueous dispersion was measured using a Coulter LS-230 particle size analyzer (available from Beckman Coulter). The solid content and average particle size (PS) of the solid particles of the dispersion are described in Table IV.
[0084] Example 1 and Example 2 and Comparative Example EI
[0085] In Inventive Examples 1 and 2 and Comparative Example EI, aqueous dispersions were prepared using the general dispersion preparation procedure described above in Comparative Examples AD, except that water and neutralizing agent were fed separately to the extruder after the extruder temperature profile was ramped up to the temperature described in the "Polymer Melting Zone" column of Table IV. Water was fed to the extruder at the rate described in Table IV, followed by addition of the neutralizing agent at the second introduction point at the rate described in Table IV. Phase inversion water was fed to the extruder after the neutralizing agent at the inlet location of the extruder.
[0086] Characteristic measurement
[0087] Solid content measurement
[0088] The solids content of the dispersion was measured by an Ohaus MB45 infrared moisture analyzer. The analyzer was set to 150°C with measurement completion set to a loss of <1 milligram (mg) in 90 seconds (s).
[0089] Viscosity measurement
[0090] The viscosity of the dispersion was tested by Brookfield DV-II+. The measurement was performed at 20 revolutions per minute (RPM) and 25°C using an RV spindle.
[0091] Particle size measurement
[0092] Particle size measurements of the dispersions were performed with a Beckman Coulter LS 13 320 instrument. The instrument was equipped with a universal liquid module containing DI water, and the data were analyzed using an optical model with a fluid refractive index of 1.332 and a sample refractive index of 1.5 real and 0 imaginary.
[0093] Performance evaluation test
[0094] The performance of all dispersion compositions was evaluated by comparing the performance of the dispersions with that of a commercial product made in a batch process. The "batch process commercial product" is available from the Dow Chemical Company as Adcote 37JD1198.
[0095] The dispersion samples were applied to the substrate by hand using a Mayer rod pull-down rod and pull-down method; and the dry coating weight was adjusted to about 5.5-6.0 g / m 2 After drawdown, the wet coating was dried in an oven at 90°C for about 2 minutes (min).
[0096] Storage stability
[0097] The shelf stability of the dispersions was evaluated under (1) refrigerated (4°C) environment and (2) oven heat (45°C) aging conditions by tracking phase separation and viscosity weekly. The overall stability of each dispersion was compared to the batch commercial product; and the results were reported according to the following rating system: a dispersion with "good" shelf stability means a dispersion that performs the same as the batch commercial product; and a dispersion with "worse" shelf stability means a dispersion that performs worse than the batch commercial product.
[0098] Coating appearance
[0099] The appearance of HSC formed from the dispersion on PET film was visually observed and compared with Adcote 37JD 1198. The coating appearance was reported according to the following rating system: HSC with "good" coating appearance was observed to have a coating with acceptable gloss and good smoothness; while "oily" coating appearance was observed to have an ugly oily appearance and was unacceptable.
[0100] Heat seal substrate
[0101] The heat-sealed substrate is prepared by heat sealing the primed substrate to the second substrate using the following method:
[0102] The primed substrate comprised commercially available 92 g PET, pre-laminated PET-aluminum foil edges.
[0103] The second substrate included commercially available 92 g PET, 4 mil polyvinyl chloride (PVC) sheet, 4 mil polyethylene terephthalate glycol (PETG) sheet, 4 mil low density polyethylene (LDPE) sheet, aluminum (Al) foil.
[0104] The dispersion composition of the present invention was applied to the surface of the primed substrate using a manual pull-down procedure. The primed substrate coated with the wet dispersion composition was then contacted with a second substrate. The wet-coated primed substrate and second substrate were dried in a 90°C oven for approximately 2 minutes. The target coating weight for drying was adjusted to 5.5 g / m 2 Up to 6.0g / m 2 .
[0105] Adhesion testing of heat seal substrates
[0106] Adhesion testing of the heat-seal substrates was performed under the following conditions: at a pressure of 2.76 bar, for a period of 1.0 second, and at two different temperatures (93.33° C. and 121.11° C.).
[0107] Use 25.4×25.4mm 2 The strips of the sealed area were tested for adhesion at a speed of 254 mm / min. Three strips of each sample were tested and the average value was reported.
[0108] Hot tack of heat seal substrate
[0109] According to the method described in ASTM F1921 Test Method B, use a temperature controlled The testing instrument (purchased from Instron) performs hot tack measurement of the heat-sealed substrate at a speed of 200 mm / s.
[0110] Storage stability
[0111] To evaluate shelf-life stability, samples were stored at 4°C (in refrigerator) and at 45°C (in oven) for different periods of time. The samples were tested for shelf-life stability by visual inspection and the test results are summarized in Table V.
[0112] Table V - Storage Stability of Dispersions
[0113]
[0114] The shelf life stability in terms of viscosity of the dispersions after storing the samples at 4°C (in a refrigerator) and at 45°C (in an oven) for different periods of time is summarized in Table VI.
[0115] Table VI - Storage stability of dispersions - viscosity
[0116]
[0117] The samples of Comparative Example H and Comparative Example I produced a turbid oily coating appearance; therefore, no further adhesive strength testing was performed on the samples of Comparative Example H and Comparative Example I.
[0118] Table VI - Adhesion Strength of Coatings (90° Peel Test Results - Coated PET Sealed to Different Substrates
[0119]
[0120] Table VII - Adhesion Strength of Coatings (90° Peel Test Results - Coated TiVic Sealed to Different Substrates (Tyvek)
[0121]
[0122] Table VIII - Adhesion Strength of Coatings (90° Peel Test Results)
[0123]
Claims
1. A method for producing a waterborne dispersion composition using an extruder-based continuous process, the method comprising the following steps: (A) providing an extruder; (B) feeding into the extruder a mixture of: (i) at least one vinyl acetate copolymer; (ii) at least one compatibilizer; and (iii) a dispersant; (C) feeding a first addition of water to the mixture of step (B) in the extruder to provide a polymer continuous dispersion; (D) feeding at least one base into the mixture of step (C) in the extruder to neutralize any effective acid present in the mixture of step (C); and (E) feeding a second addition of water to the mixture of step (D) in the extruder to effect phase inversion to form a water continuous dispersion.
2. The method of claim 1, wherein the extruder has a first feed zone near the front end of the extruder, a second feed zone near the middle of the extruder, and a third feed zone near the back end of the extruder.
3. The process according to claim 2, wherein the temperature of the first feed zone is from 90°C to 150°C.
4. The process of claim 2, wherein the temperature of the second feed zone is from 90°C to 150°C.
5. The process of claim 2, wherein the temperature of the third feed zone is 80°C to 150°C.
6. The method of claim 1, wherein the dispersion produced by the method has a shelf stability of greater than 1 year at room temperature and a particle size of less than 2 microns.
7. The process of claim 1 wherein the at least one vinyl acetate copolymer is an ethylene vinyl acetate copolymer and is fed to the extruder at a concentration of 50% to 90% by weight of total solids.
8. The process of claim 1 wherein the at least one compatibilizer is highly dimerized rosin acid and is fed to the extruder at a concentration of 5 to 30 weight percent of total solids.
9. The process of claim 1 wherein the dispersant is oleic acid and is fed into the extruder at a concentration of 0.1 wt% to 5 wt% of total solids.
10. The process of claim 1 wherein the amount of water in the first water addition fed to the extruder is from 3.5% to 6% by weight of the total solids and the first water addition.
11. The method of claim 1 , wherein the at least one base is potassium hydroxide and is fed to the extruder at a concentration to neutralize 80% to 120% of the theoretical acid value of the components, wherein the components include the at least one vinyl acetate copolymer, the at least one compatibilizer, the dispersant, the first water addition, the at least one base, and the second water addition.
12. The method of claim 1 wherein the amount of water in the second water addition fed to the extruder is greater than or equal to 3.5 weight percent of the total solids, first and second water additions.
13. The method of claim 1, wherein the aqueous dispersion composition is free of wax.