Method for manufacturing single-crystal thin film on insulator and laminated structure
By forming a single-crystal grain array on an insulator and using a low-mobility material as a seed layer, combined with epitaxy of a high-mobility material, the problems of high cost and low yield in the preparation of single-crystal thin films in the prior art have been solved, and low-cost, high-quality preparation of single-crystal thin films has been achieved.
Patent Information
- Application Number
- CN202111200484.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-14
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2041-10-14
AI Technical Summary
Existing technologies for preparing single-crystal thin films on insulators are costly and have low yields, making them unsuitable for large-scale production.
A high-quality single-crystal thin film is formed by forming a single-crystal seed layer on an insulating substrate, using a low-mobility material as the first epitaxial material, and then epitaxially forming a high-mobility material on it.
It has achieved low-cost, high-quality preparation of single-crystal thin films, which are suitable for large-scale production.
Smart Images

Figure CN113964020B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor fabrication technology, and in particular to a method for preparing single-crystal thin films on insulators and a stacked structure thereof. Background Technology
[0002] Fabricating single-crystal thin films on insulators is of great significance, for example, as they can be used as substrate materials for device fabrication or as top silicon materials for three-dimensional integrated devices. In existing technologies, the fabrication of single-crystal thin films on insulators is mainly achieved through bonding technology. The laminated structures of insulators and single-crystal thin films prepared using bonding technology have high material quality and can be used to fabricate high-performance semiconductor devices. However, the laminated structures prepared by bonding technology are costly and have low yields, which is not conducive to large-scale fabrication. Summary of the Invention
[0003] The method and stacked structure for preparing single-crystal thin films on insulators provided by this invention can prepare high-quality single-crystal thin film stacked structures at low cost, which is beneficial for large-scale preparation of single-crystal thin film stacked structures.
[0004] In a first aspect, the present invention provides a method for preparing a single-crystal thin film on an insulator, comprising:
[0005] An insulating substrate is prepared, the insulating substrate comprising an insulating layer and an array of single-crystal grains distributed on the insulating layer;
[0006] Epitaxy is performed on the insulating substrate using a first epitaxial material to obtain a single crystal seed layer;
[0007] A single-crystal thin film layer is obtained by epitaxy with a second epitaxial material on the single-crystal seed layer; wherein the mobility of the second epitaxial material is greater than that of the first epitaxial material.
[0008] Optionally, the preparation of the insulating substrate includes:
[0009] Multiple recessed structures are formed on the insulating layer, the recessed structures being used to obtain a single crystal orientation;
[0010] An amorphous thin film is formed on the insulating layer;
[0011] The amorphous thin film is annealed to form a regular polycrystalline thin film;
[0012] The regular polycrystalline thin film is subjected to crystal orientation etching to preserve the single-crystal grain array;
[0013] An insulating medium is filled into the grooves formed by etching in the single-crystal grain array.
[0014] Optionally, the crystal orientation etching of the regular polycrystalline thin film includes: using a mixed aqueous solution of hydrofluoric acid and potassium dichromate to perform crystal orientation etching on the regular polycrystalline thin film.
[0015] Optionally, annealing the amorphous thin film includes:
[0016] A crystallization inhibition film is formed on the surface of the amorphous thin film to induce lateral crystallization of the amorphous thin film during annealing.
[0017] The amorphous thin film was annealed using laser annealing.
[0018] When the thickness of the amorphous thin film is less than 500 angstroms, a laser wavelength below 355 nanometers is selected for laser annealing.
[0019] When the thickness of the amorphous thin film is not less than 500 angstroms, laser annealing is performed using a laser wavelength of 475 nanometers or higher.
[0020] Optionally, forming multiple recessed structures on the insulating layer includes:
[0021] A periodically arranged recessed structure is formed on an insulating medium, wherein the size of the recessed structure is less than 0.5 micrometers and the distance between adjacent recessed structures is less than 10 micrometers.
[0022] Optionally, forming an amorphous thin film on the insulating layer includes forming an amorphous thin film material on the insulating layer using physical vapor deposition or chemical vapor deposition.
[0023] Optionally, filling the grooves formed by etching in the single-crystal grain array with an insulating medium includes: filling the grooves formed by etching in the single-crystal grain array with an insulating medium by atomic layer deposition; or, performing silicon oxidation on the single-crystal grain array to expand the surface of the single-crystal grains and fill the grooves.
[0024] Optionally, forming multiple recessed structures on the insulating layer includes forming multiple blind holes or multiple grooves on the insulating layer.
[0025] In a second aspect, the present invention provides a single-crystal thin film stacked structure on an insulator, comprising:
[0026] An insulating substrate, a first epitaxial material, and a second epitaxial material are stacked sequentially from bottom to top; wherein,
[0027] The insulating substrate includes an insulating layer and a single-crystal grain array disposed on the insulating layer;
[0028] The migration rate of the second epitaxial material is greater than that of the first epitaxial material.
[0029] Optionally, the insulating substrate is provided with a plurality of recessed structures, and the single crystal grains in the single crystal grain array are integrally formed with the recessed structures in a one-to-one correspondence.
[0030] In the technical solution provided by this invention, an array of multiple single-crystal grains is used as a seed layer. Epitaxy is performed on the single-crystal grain array to form a single-crystal seed layer. A second epitaxy is then performed on the single-crystal seed layer to form a high-quality single-crystal thin film material. Since the second epitaxial material is a high-mobility material, it is difficult to obtain a good single-crystal thin film if the second epitaxial material is directly epitaxially performed on the single-crystal grain array. Therefore, in the technical solution provided by this invention, a low-mobility material is first used as the first epitaxial material to form a single-crystal seed layer. The single-crystal seed layer has good crystal orientation. When the second epitaxial material is then used on the single-crystal seed layer for epitaxy, a good single-crystal thin film can be obtained. Attached Figure Description
[0031] Figure 1a This is a schematic diagram illustrating the formation of an amorphous material using a method for preparing a single-crystal thin film on an insulator according to an embodiment of the present invention;
[0032] Figure 1b This is a cross-sectional schematic diagram of an embodiment of the method for preparing a single-crystal thin films on an insulator according to the present invention, showing the formation of an amorphous material.
[0033] Figure 2a This is a schematic diagram illustrating the crystal orientation etching process in another embodiment of the present invention for preparing a single-crystal thin film on an insulator.
[0034] Figure 2b This is a cross-sectional schematic diagram of crystal orientation etching performed in another embodiment of the method for preparing a single-crystal thin film on an insulator according to the present invention;
[0035] Figure 3a This is a schematic diagram illustrating the grain boundary filling process in a method for preparing a single-crystal thin film on an insulator according to another embodiment of the present invention.
[0036] Figure 3b This is a cross-sectional schematic diagram of grain boundary filling in a method for preparing a single-crystal thin film on an insulator according to another embodiment of the present invention;
[0037] Figure 4a This is a schematic diagram illustrating the epitaxy of a first epitaxial material in another embodiment of the method for preparing a single crystal thin film on an insulator according to the present invention.
[0038] Figure 4b This is a cross-sectional schematic diagram of the epitaxial process of a first epitaxial material in another embodiment of the method for preparing a single crystal thin film on an insulator according to the present invention.
[0039] Figure 5a This is a schematic diagram illustrating the epitaxy of a second epitaxial material in another embodiment of the method for preparing a single crystal thin film on an insulator according to the present invention.
[0040] Figure 5b This is a cross-sectional schematic diagram of the epitaxial growth of a second epitaxial material in another embodiment of the method for preparing a single crystal thin film on an insulator according to the present invention. Detailed Implementation
[0041] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0042] This invention provides a method for preparing a single-crystal thin film on an insulator, comprising:
[0043] An insulating substrate is prepared, the insulating substrate comprising an insulating layer 100 and a single-crystal grain array 200 distributed on the insulating layer 100; in some embodiments, the insulating substrate includes the insulating layer 100, for example, a thin film prepared of silicon oxide as the insulating layer 100, or an insulating layer 100 formed of silicon nitride or aluminum oxide, wherein an amorphous material is formed on the insulating layer 100, such as... Figures 1a to 1b As shown; after annealing, amorphous materials form polycrystalline thin films. The polycrystalline thin films are then subjected to crystal orientation etching to remove grain boundaries, defects, and regions with undesirable crystal orientations, thereby preserving the single-crystal grain array 200, as shown. Figure 2a and Figure 2b As shown. In the single-crystal grain array 200, each individual grain is a single-crystal grain, and the entire array is formed by arranging multiple single-crystal grains in a periodic manner.
[0044] Epitaxial growth is performed on the insulating substrate using a first epitaxial material to obtain a single-crystal seed layer 300. In some embodiments, since trenches 210 exist between the grains of the single-crystal grain array 200 after crystal orientation etching, a flat plane is required to achieve the epitaxy of the first epitaxial material. Therefore, the trenches 210 need to be filled first. For example, silicon oxide can be used to fill and planarize the trenches 210 to obtain a seed layer 300. Figure 3a and Figure 3b The structure is shown. Epitaxy is performed on the obtained plane using the first epitaxial material to form a single-crystal seed layer 300, as shown. Figure 4a and Figure 4bAs shown. The first epitaxial material can usually be silicon. Since silicon is a low-mobility epitaxial material, it can form a good single-crystal seed layer 300 on the single-crystal grain array 200. At the same time, it has good lattice compatibility with the subsequent high-mobility second epitaxial material, which is conducive to the formation of a high-quality single-crystal thin film layer 400 by the subsequent second epitaxial material.
[0045] A single-crystal thin film layer 400 is obtained by epitaxy on the single-crystal seed layer 300 using a second epitaxial material; wherein the mobility of the second epitaxial material is greater than the mobility of the first epitaxial material. In some embodiments, such as Figure 5a and Figure 5b As shown, the single crystal seed layer 300 formed by the first epitaxial material can obtain a predetermined crystal orientation, and the second epitaxial material formed on the single crystal seed layer 300 can obtain a large area of high-quality single crystal thin film layer 400.
[0046] In the technical solution provided in this embodiment, an array of multiple single-crystal grains is used as a seed layer. A single-crystal seed layer 300 is formed on the single-crystal grain array 200 via epitaxy. A second epitaxy is then performed on the single-crystal seed layer 300 to form a high-quality single-crystal thin film material. Since the second epitaxial material is a high-mobility material, it is difficult to obtain a good single-crystal thin film if the second epitaxial material is directly epitaxially performed on the single-crystal grain array 200. Therefore, in the technical solution provided by this invention, a low-mobility material is first used as the first epitaxial material to form the single-crystal seed layer 300. The single-crystal seed layer 300 has good crystal orientation. When the second epitaxial material is then used on the single-crystal seed layer 300 for epitaxy, a good single-crystal thin film can be obtained.
[0047] As an optional implementation method, the preparation of the insulating substrate includes:
[0048] A plurality of recessed structures 110 are formed on the insulating layer 100, the recessed structures 110 being used to obtain a single crystal orientation; in some embodiments, such as Figure 1a and Figure 1b As shown, multiple recessed structures 110 are provided on the insulating layer 100. During the subsequent annealing process of the amorphous material, the amorphous material in the recessed structure 110 will be restricted by the recessed structure 110, thereby forming a single crystal orientation. As the annealing process progresses, the amorphous film will be transformed into a single crystal grain with the same crystal orientation as the recessed structure 110.
[0049] An amorphous thin film is formed on the insulating layer 100; in some embodiments, such as Figure 1a and Figure 1bAs shown, an amorphous thin film is formed on the insulating layer 100 with the recess 110 structure. During the formation process, the recess 110 structure on the insulating layer 100 is filled. Those skilled in the art should understand that during the formation of the amorphous thin film, a conformal structure corresponding to the recess 110 structure is formed. Therefore, after the amorphous thin film is formed, planarization treatment is required.
[0050] The amorphous thin film is annealed to form a regular polycrystalline thin film; in some embodiments, such as Figure 1a and Figure 1b As shown, due to the presence of multiple recessed structures 110 on the insulating layer 100, during the conversion of the amorphous thin film into single-crystal grains, the crystal orientation within the recessed structures 110 is used as the predetermined crystal orientation for generation. Grain boundaries are formed between adjacent single-crystal grains; therefore, the entire polycrystalline thin film is a polycrystalline thin film.
[0051] The regular polycrystalline thin film is subjected to crystal orientation etching to retain the single-crystal grain array 200; in some embodiments, such as Figure 2a and Figure 2b As shown, during crystal orientation etching, the grain boundaries, defects, and non-expected crystal orientations are etched, thereby removing the non-expected crystal orientations and dividing multiple single crystal grains. Thus, each grain is a single crystal grain, and multiple single crystal grains are arranged in a periodic manner to form a single crystal grain array 200.
[0052] An insulating medium 220 is filled into the grooves formed by etching in the single-crystal grain array 200. In some embodiments, such as Figure 3a and Figure 3b As shown, since the subsequent epitaxial growth of the first epitaxial material needs to be performed on a flat plane, the groove is filled in this embodiment. The insulating medium used for filling can be, for example, an insulating medium 220 formed of silicon material, or an insulating medium 220 formed of silicon nitride or aluminum oxide.
[0053] In this embodiment, a recessed 110 structure is used to restrict the crystal orientation. Therefore, during the annealing process, the entire amorphous thin film forms multiple single-crystal grains based on the crystal orientation of the recessed 110 structure. This provides a seed layer with a single crystal orientation for the subsequent epitaxy of the first epitaxial material, which is beneficial for controlling the crystal orientation of the subsequent first epitaxial material.
[0054] As an optional implementation, crystal orientation etching of the regular polycrystalline thin film includes: etching the regular polycrystalline thin film with a mixed aqueous solution of hydrofluoric acid and potassium dichromate. In some embodiments, the mixed aqueous solution of hydrofluoric acid and potassium dichromate can etch grain boundaries, defects, and non-desired crystal orientations in the polycrystalline thin film, thereby preserving only the array of single-crystal grains.
[0055] As an optional implementation, annealing the amorphous thin film includes:
[0056] A crystallization inhibition film is formed on the surface of the amorphous thin film to induce lateral crystallization during annealing. In some embodiments, a 300-500 Å silicon oxide or silicon nitride film is deposited on the surface before laser annealing. This serves to suppress longitudinal growth during crystallization and improve laser absorption efficiency.
[0057] The amorphous thin film is annealed using laser annealing. In some embodiments, laser annealing can heat the amorphous thin film quickly and uniformly, improving heating efficiency and uniformity.
[0058] When the thickness of the amorphous thin film is less than 500 angstroms, a laser wavelength below 355 nm is selected for laser annealing; when the thickness of the amorphous thin film is not less than 500 angstroms, a laser wavelength above 475 nm is selected for laser annealing. In some embodiments, since the smaller the laser wavelength, the higher the energy, the faster the heat dissipation rate is when the film thickness is small. Therefore, heating with a higher energy density is required, and a smaller laser wavelength is selected. When the film thickness is large, a longer laser wavelength is selected.
[0059] As an optional implementation, forming a plurality of recessed structures 110 on the insulating layer 100 includes: forming periodically arranged recessed structures 110 on the insulating medium, wherein the size of the recessed structures 110 is less than 0.5 micrometers, and the distance between adjacent recessed structures 110 is less than 10 micrometers. In some embodiments, in order to limit the crystal orientation formed during annealing in the recessed structures 110, the size of the recessed structures 110 is set to be less than 0.5 micrometers in this embodiment. To ensure the quality of the single crystal grains, it is necessary to set an appropriate spacing between adjacent recessed structures 110; in this embodiment, a spacing of less than 10 micrometers is selected.
[0060] As an optional implementation, forming an amorphous thin film on the insulating layer 100 includes forming an amorphous thin film material on the insulating layer 100 using a physical vapor deposition (PVD) or chemical vapor deposition (CVD) method. In some embodiments, since PVD or CVD has the characteristics of low cost and high efficiency, in order to reduce the preparation cost of the thin film material, in this embodiment, an amorphous thin film material is formed by a PVD or CVD method.
[0061] As an optional implementation, filling the grooves etched in the single-crystal grain array 200 with an insulating medium includes filling the grooves etched in the single-crystal grain array 200 with an insulating medium 220 using atomic layer deposition. In this embodiment, since the grooves etched in the single-crystal grain array 200 are extremely small, in order to obtain a good filling effect, the grooves etched in the single-crystal grain array 200 are filled with a medium using atomic layer deposition. Alternatively, the single-crystal grain array is oxidized with silicon to cause the surface of the single-crystal grains to expand and fill the grooves. In some embodiments, during the oxidation process, silicon becomes silicon oxide. Due to the increase in oxygen atoms, the oxide particles expand, thus filling the grain boundaries through the expansion effect of silicon oxidation. The oxidation process can be thermal oxidation or low-temperature ozone oxidation.
[0062] As an optional implementation, forming a plurality of recesses 110 on the insulating layer 100 includes forming a plurality of blind holes or a plurality of grooves on the insulating layer 100. In some embodiments, the recesses 110 are configured as blind holes, and during annealing, the amorphous material in the blind holes is confined by the blind holes and transforms into a single-crystal material with a single crystal orientation; for example, the crystal orientation formed can be [0,0,1]. Similarly, the recesses 110 can also be configured as grooves, and during annealing, the amorphous material in the grooves is confined by the grooves and transforms into a single-crystal material with a single crystal orientation.
[0063] This invention also provides a 400-layer structure of a single-crystal thin film layer on an insulator, comprising:
[0064] An insulating substrate, a first epitaxial material, and a second epitaxial material are stacked sequentially from bottom to top; wherein,
[0065] The insulating substrate includes an insulating layer 100 and a single-crystal grain array 200 disposed on the insulating layer 100;
[0066] The migration rate of the second epitaxial material is greater than that of the first epitaxial material.
[0067] In some embodiments, the insulating substrate includes an insulating layer 100, which may be a thin film made of silicon oxide as the insulating layer 100, on which an amorphous material is formed, such as... Figures 1a to 1b As shown; after annealing, amorphous materials form polycrystalline thin films. The polycrystalline thin films are then subjected to crystal orientation etching to remove grain boundaries, defects, and regions with undesirable crystal orientations, thereby preserving the single-crystal grain array 200, as shown. Figure 2a and Figure 2bAs shown. In the single-crystal grain array 200, each individual grain is a single-crystal grain, and the entire array is formed by arranging multiple single-crystal grains in a periodic manner. Since trenches 210 exist between the grains of the single-crystal grain array 200 after crystal orientation etching, a flat plane is needed to achieve the epitaxy of the first epitaxial material. Therefore, the trenches 210 need to be filled first. For example, silicon oxide can be used to fill and planarize the trenches 210, resulting in... Figure 3a and Figure 3b The structure is shown. Epitaxy is performed on the obtained plane using the first epitaxial material to form a single-crystal seed layer 300, as shown. Figure 4a and Figure 4b As shown. The first epitaxial material is typically silicon. Because silicon is a low-mobility epitaxial material, it can form a good single-crystal seed layer 300 on the single-crystal grain array 200. Simultaneously, it has good lattice compatibility with the subsequent high-mobility second epitaxial material, which is beneficial for the formation of a high-quality single-crystal thin film layer 400 by the subsequent second epitaxial material. For example... Figure 5a and Figure 5b As shown, the single crystal seed layer 300 formed by the first epitaxial material can obtain a predetermined crystal orientation, and the second epitaxial material formed on the single crystal seed layer 300 can obtain a large area of high-quality single crystal thin film layer 400.
[0068] In the technical solution provided in this embodiment, an array of multiple single-crystal grains is used as a seed layer. A single-crystal seed layer 300 is formed on the single-crystal grain array 200 via epitaxy. A second epitaxy is then performed on the single-crystal seed layer 300 to form a high-quality single-crystal thin film material. Since the second epitaxial material is a high-mobility material, it is difficult to obtain a good single-crystal thin film if the second epitaxial material is directly epitaxially performed on the single-crystal grain array 200. Therefore, in the technical solution provided by this invention, a low-mobility material is first used as the first epitaxial material to form the single-crystal seed layer 300. The single-crystal seed layer 300 has good crystal orientation. When the second epitaxial material is then used on the single-crystal seed layer 300 for epitaxy, a good single-crystal thin film can be obtained.
[0069] As an optional implementation, the insulating substrate has a plurality of recessed structures 110, and the single crystal grains in the single crystal grain array 200 are integrally formed with the recessed structures 110 in a one-to-one correspondence. In some embodiments, such as Figure 1a and Figure 1bAs shown, an amorphous thin film is formed on an insulating layer 100 with recessed structures 110. During the formation process, the recessed structures 110 on the insulating layer 100 are filled. Those skilled in the art should understand that during the formation of the amorphous thin film, a conformal structure corresponding to the recessed structures 110 is formed. Therefore, planarization is required after the amorphous thin film is formed. Since the insulating layer 100 has multiple recessed structures 110, during the conversion of the amorphous thin film into single-crystal grains, the crystal orientation in the recessed structures 110 is used as the predetermined crystal orientation for generation. Grain boundaries are formed between adjacent single-crystal grains; therefore, the entire polycrystalline thin film is a polycrystalline thin film. Figure 2a and Figure 2b As shown, during crystal orientation etching, the grain boundaries, defects, and non-expected crystal orientations are etched, thereby removing the non-expected crystal orientations and dividing multiple single crystal grains. Thus, each grain is a single crystal grain, and multiple single crystal grains are arranged in a periodic manner to form a single crystal grain array 200. Each single crystal grain corresponds to a recess 110 structure.
[0070] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention should be included within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be determined by the scope of the claims.
Claims
1. A method for preparing a single-crystal thin film on an insulator, characterized in that, include: An insulating substrate is prepared, the insulating substrate comprising an insulating layer and a single-crystal grain array distributed on the insulating layer; wherein, trenches are formed between the grains of the single-crystal grain array, and silicon oxide is used to fill and planarize the trenches; Epitaxy is performed on the insulating substrate using a first epitaxial material to obtain a single crystal seed layer; A single-crystal thin film layer is obtained by epitaxy with a second epitaxial material on the single-crystal seed layer; wherein the mobility of the second epitaxial material is greater than that of the first epitaxial material. The preparation of the insulating substrate includes: Multiple recessed structures are formed on the insulating layer, the recessed structures being used to obtain a single crystal orientation; An amorphous thin film is formed on the insulating layer; The amorphous thin film is annealed to form a regular polycrystalline thin film; The regular polycrystalline thin film is subjected to crystal orientation etching to preserve the single-crystal grain array; An insulating medium is filled into the grooves formed by etching in the single-crystal grain array.
2. The method for preparing a single-crystal thin film on an insulator according to claim 1, characterized in that, The crystal orientation etching of the regular polycrystalline thin film includes: using a mixed aqueous solution of hydrofluoric acid and potassium dichromate to perform crystal orientation etching on the regular polycrystalline thin film.
3. The method for preparing a single-crystal thin film on an insulator according to claim 1, characterized in that, Annealing the amorphous thin film includes: A crystallization inhibition film is formed on the surface of the amorphous thin film to induce lateral crystallization of the amorphous thin film during annealing. The amorphous thin film was annealed using laser annealing. When the thickness of the amorphous thin film is less than 500 angstroms, a laser wavelength below 355 nanometers is selected for laser annealing. When the thickness of the amorphous thin film is not less than 500 angstroms, laser annealing is performed using a laser wavelength of 475 nanometers or higher.
4. The method for preparing a single-crystal thin film on an insulator according to claim 1, characterized in that, Forming multiple recessed structures on the insulating layer includes: A periodically arranged recessed structure is formed on an insulating medium, wherein the size of the recessed structure is less than 0.5 micrometers and the distance between adjacent recessed structures is less than 10 micrometers.
5. The method for preparing a single-crystal thin film on an insulator according to claim 1, characterized in that, Forming an amorphous thin film on the insulating layer includes forming an amorphous thin film material on the insulating layer using physical vapor deposition or chemical vapor deposition methods.
6. The method for preparing a single-crystal thin film on an insulator according to claim 1, characterized in that, Filling the grooves formed by etching in the single-crystal grain array with an insulating medium includes: filling the grooves formed by etching in the single-crystal grain array with an insulating medium by atomic layer deposition; or, performing silicon oxidation on the single-crystal grain array to expand the surface of the single-crystal grains and fill the grooves.
7. The method for preparing a single-crystal thin film on an insulator according to claim 1, characterized in that, Forming multiple recessed structures on the insulating layer includes forming multiple blind holes or multiple grooves on the insulating layer.
8. A single-crystal thin film stacked structure on an insulator, characterized in that, include: An insulating substrate, a first epitaxial material, and a second epitaxial material are stacked sequentially from bottom to top; wherein the first epitaxial material forms a single crystal seed layer, and the second epitaxial material forms a single crystal thin film layer. The insulating substrate includes an insulating layer and a single-crystal grain array disposed on the insulating layer; The mobility of the second epitaxial material is greater than that of the first epitaxial material; Among them, there are trenches between the grains of the single crystal grain array, and silicon oxide is used to fill the trenches and planarize them; The preparation of the insulating substrate includes: Multiple recessed structures are formed on the insulating layer, the recessed structures being used to obtain a single crystal orientation; An amorphous thin film is formed on the insulating layer; The amorphous thin film is annealed to form a regular polycrystalline thin film; The regular polycrystalline thin film is subjected to crystal orientation etching to preserve the single-crystal grain array; An insulating medium is filled into the grooves formed by etching in the single-crystal grain array.
9. The single-crystal thin film stacked structure on an insulator according to claim 8, characterized in that, The insulating substrate has multiple recessed structures, and the single crystal grains in the single crystal grain array are integrally formed with the recessed structures in a one-to-one correspondence.
Citation Information
Patent Citations
GaN layer transfer single crystal thin film preparation method based on silicon heterogeneous substrate
CN108242420A