Electrode for electrolysis
Patent Information
- Application Number
- CN202180004167.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-01-09
- Filing Date
- 2021-01-08
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-01-08
AI Technical Summary
In the existing salt water electrolysis technology, it is difficult to optimize the overvoltage and durability of the electrode at the same time. Especially on the cathode, there are problems of active material loss and reverse current degradation.
A metal-based electrode coating is used. The coating contains ruthenium oxide, cerium oxide and nickel oxide, which is formed through drying and heat treatment. The ruthenium oxide serves as the active material, the cerium oxide provides a catalyst, and the nickel oxide improves conductivity and durability. sex.
It is possible to improve the durability and conductivity of the electrode while reducing overvoltage, extending the service life of the electrode and significantly improving the electrolysis performance.
Smart Images

Figure BDA0003431547350000101 
Figure BDA0003431547350000111
Abstract
Description
Technical Field
[0002] CROSS-REFERENCE TO RELATED APPLICATIONS
[0003] This application claims priority to Korean Patent Application No. 10-2020-0003208 filed on January 9, 2020, the disclosure of which is incorporated into this specification by reference. Technical Field
[0004] The present invention relates to an electrolysis electrode capable of improving overvoltage and a method for preparing the electrolysis electrode. Background Art
[0005] The technology for producing hydroxide, hydrogen and chlorine by electrolysis of low-cost brine such as seawater is well known. This electrolysis process is also known as the chlor-alkali process and can be considered a process that has proven its performance and technical reliability in commercial operation for decades.
[0006] For the electrolysis of brine, the most widely used method at present is the ion exchange membrane method, in which an ion exchange membrane is installed in an electrolytic cell to divide the electrolytic cell into a cation chamber and an anion chamber, and brine is used as an electrolyte to obtain chlorine at the anode and hydrogen and caustic soda at the cathode.
[0007] The electrolysis of salt water is carried out by the reaction shown in the following electrochemical reaction formula.
[0008] Anode reaction: 2Cl - →Cl2+2e - (E 0 = +1.36V)
[0009] Cathode reaction: 2H2O+2e - →2OH - +H2(E 0 =-0.83V)
[0010] Overall reaction: 2Cl - +2H2O→2OH - +Cl2+H2(E 0 =-2.19V)
[0011] In the electrolysis of brine, in addition to the theoretical voltage required for brine electrolysis, the electrolysis voltage must also take into account the overvoltage of the anode, the overvoltage of the cathode, the voltage caused by the resistance of the ion exchange membrane, and the voltage caused by the distance between the anode and the cathode, and among these voltages, the overvoltage caused by the electrode is an important variable.
[0012] Therefore, methods capable of reducing overvoltage of electrodes have been studied, wherein, for example, a noble metal-based electrode called DSA (Dimensionally Stable Anode) has been developed for use as an anode, and an excellent material having durability and low overvoltage is required to be developed for a cathode.
[0013] Stainless steel or nickel has been mainly used as a cathode, and, recently, in order to reduce overvoltage, a method of using stainless steel or nickel by coating the surface of the stainless steel or nickel with nickel oxide, an alloy of nickel and tin, a combination of activated carbon and oxide, ruthenium oxide or platinum has been studied.
[0014] In addition, in order to increase the activity of the cathode by controlling the composition of the active material, a method of controlling the composition by using platinum group elements such as ruthenium and lanthanide elements such as cerium has also been studied. However, an overvoltage phenomenon occurs, and a problem of degradation due to reverse current occurs.
[0015] Prior art literature
[0016] (Patent Document 1) JP2003-277967A Summary of the invention
[0017] Technical issues
[0018] One aspect of the present invention provides an electrode for electrolysis that can reduce overvoltage by improving the electrical properties of a coating on the surface of the electrode.
[0019] Technical Solution
[0020] According to one aspect of the present invention, there is provided an electrode for electrolysis, comprising: a metal base layer; and a coating layer comprising ruthenium oxide, cerium oxide and nickel oxide, wherein the coating layer is formed on at least one surface of the base layer.
[0021] According to another aspect of the present invention, there is provided a method for preparing an electrode for electrolysis, the method comprising the steps of: applying a coating composition on at least one surface of a metal substrate; and coating the metal substrate on which the coating composition is applied by drying and heat treating, wherein the coating composition comprises a ruthenium precursor, a cerium precursor and a nickel precursor.
[0022] Beneficial Effects
[0023] The present invention provides an electrode for electrolysis which can exhibit excellent overvoltage and excellent alkaline durability while maintaining excellent conductivity by containing nickel oxide and cerium oxide together in a coating layer. DETAILED DESCRIPTION
[0024] Hereinafter, the present invention will be described in more detail.
[0025] It should be understood that the words or terms used in this specification and claims should not be understood as the meanings defined in common dictionaries. It should also be understood that the words or terms should be understood to have the same meanings as they have in the context of the relevant technology and in the technical concept of the present invention, based on the principle that the inventor can appropriately define the meanings of the words or terms in order to best explain the invention.
[0026] Electrode for electrolysis
[0027] The present invention provides an electrode for electrolysis, comprising: a metal base layer; and a coating layer, the coating layer comprising ruthenium oxide, cerium oxide and nickel oxide, wherein the coating layer is formed on at least one surface of the base layer.
[0028] The metal substrate may be nickel, titanium, tantalum, aluminum, hafnium, zirconium, molybdenum, tungsten, stainless steel or an alloy thereof, and, among these metals, the metal substrate may preferably be nickel. In the electrode for electrolysis of the present invention, when the above-mentioned type of metal substrate is used, excellent durability and mechanical strength can be provided to the electrode.
[0029] In the electrode for electrolysis of the present invention, the coating contains ruthenium oxide. Ruthenium oxide plays a role as an active material to provide ruthenium element to the coating, wherein, in the case of using ruthenium oxide in the coating of the electrode for electrolysis, the change of electrode performance over time is small, while the overvoltage phenomenon is improved, and, subsequently, the separate activation process can be minimized. Ruthenium oxide includes all types of oxides in which ruthenium element is bonded to oxygen atoms, and specifically, may be dioxide or tetraoxide.
[0030] In the electrode for electrolysis of the present invention, the coating layer contains cerium oxide, and the cerium oxide plays a role in providing cerium elements to the catalyst layer of the electrode for electrolysis. During activation or electrolysis, the cerium elements provided by the cerium oxide can minimize the loss of ruthenium elements as active materials in the coating layer of the electrode for electrolysis by improving the durability of the electrode for electrolysis.
[0031] Specifically, during the activation or electrolysis of the electrolytic electrode, the particles containing the ruthenium element in the catalyst layer become metal elements without changing their structure, or are partially hydrated and reduced to active substances. In addition, since the particles containing the cerium element in the catalyst layer change their structure to a needle shape, the particles act as protective materials to prevent the particles containing the ruthenium element in the catalyst layer from physically detaching, and, thereby, the durability of the electrolytic electrode can be improved to prevent the loss of the ruthenium element in the coating. Cerium oxide includes all types of oxides in which the cerium element is bonded to oxygen atoms, and specifically, may be oxides of (II), (III) or (IV).
[0032] The molar ratio between the ruthenium element and the cerium element contained in the coating layer may be in the range of 100:2 to 100:40, for example, in the range of 100:5 to 100:20. When the molar ratio between the ruthenium element and the cerium element contained in the coating layer is within the above range, the balance between the durability and the conductivity of the electrode for electrolysis may be excellent.
[0033] Since the above-mentioned cerium oxide shows relatively low electrical conductivity, it is necessary to maintain an excellent balance between the durability improved by the cerium oxide and the electrical conductivity reduced by the cerium oxide. In the present invention, when a part of the cerium oxide in the coating is replaced with nickel oxide having better electrical conductivity than cerium oxide, it has been found that the above-mentioned excellent balance between durability and electrical conductivity can be achieved while maintaining the durability improvement effect of cerium oxide. Therefore, the coating of the electrode for electrolysis provided by the present invention contains nickel oxide.
[0034] Since nickel oxide exhibits relatively excellent conductivity even in an oxide state, it has little effect on durability while improving the overvoltage of the electrode for electrolysis. Nickel oxide includes all types of oxides in which nickel elements are bonded to oxygen atoms, and in particular may be an oxide. In addition, since nickel oxide can suppress the reduction in conductivity caused by cerium oxide by being included in a coating together with cerium oxide, nickel oxide and cerium oxide must be included in a single coating at the same time. If nickel oxide and cerium oxide are included in coatings different from each other when multiple coatings are used, not only the above-mentioned advantages of nickel oxide cannot be obtained, but also delamination problems between coatings may also occur due to the different physical properties of nickel and cerium.
[0035] In addition, it is possible to consider using an oxide of another metal known to have excellent conductivity, for example, a metal oxide such as iron oxide to replace nickel oxide, but in the case of using the above metal oxide instead of nickel oxide, the effect of cerium oxide in preventing the loss of ruthenium element may be reduced. Specifically, if a coating composition containing a ruthenium precursor, a nickel precursor, and a cerium precursor is applied to a substrate and then sintered, since the precursors are converted into ruthenium oxide, nickel oxide, and cerium oxide, respectively, nickel does not interfere with the formation of ruthenium oxide and cerium oxide, but other metals, such as strontium (Sr), barium (Ba), vanadium (V), and praseodymium (Pr), respectively form mixed oxides, such as Sr2CeO4, BaCeO3, CeVO3, and Pr3RuO, which reduce catalytic activity.
[0036] The molar ratio between the cerium element and the nickel element contained in the coating layer may be in the range of 10:90 to 90:10, for example, 25:75 to 75:25 or 50:50 to 75:25. When the molar ratio between the cerium element and the nickel element is within the above range, the balance between the durability improvement effect of the cerium oxide and the conductivity improvement effect of the nickel oxide may be excellent.
[0037] In addition, a molar ratio between the ruthenium element and the nickel element contained in the coating layer may be in a range of 100: 2 to 100: 20, for example, 100: 5 to 100: 15. The effect of improving overvoltage by nickel oxide may be maximized within the above range.
[0038] In the electrode for electrolysis of the present invention, the coating may further contain a platinum group oxide. Platinum group oxides refer to oxides of other elements in the platinum group elements except for the above-mentioned ruthenium, and may specifically be rhodium oxide, palladium oxide, osmium oxide, iridium oxide or platinum oxide. The platinum group elements provided by the platinum group oxides may act as active materials like ruthenium elements, and, in the case where platinum group oxides and ruthenium oxides are included together in the coating, better effects may be exhibited in terms of durability and overvoltage of the electrode. Platinum group oxides include oxides of all types of platinum group elements bonded to oxygen atoms, and, specifically, may be dioxides or tetraoxides, and preferably the platinum group oxides are platinum oxides.
[0039] The molar ratio between the ruthenium element and the platinum group element contained in the coating layer may be in the range of 100:2 to 100:20, for example, in the range of 100:5 to 100:15. In the case where the molar ratio between the ruthenium element and the platinum group element contained in the coating layer is in the above range, it is desirable in terms of improving durability and overvoltage, wherein in the case where the content of the platinum group element is lower than the above range, the durability and overvoltage are reduced, and in the case where the content of the platinum group element is higher than the above range, it is disadvantageous in terms of economic efficiency.
[0040] Method for preparing electrode for electrolysis
[0041] The present invention provides a method for preparing an electrode for electrolysis, which comprises the following steps: applying a coating composition on at least one surface of a metal substrate; and coating the metal substrate on which the coating composition is applied by drying and heat treating, wherein the coating composition comprises a ruthenium precursor, a cerium precursor and a nickel precursor.
[0042] In the method for producing an electrode for electrolysis of the present invention, the metal substrate may be the same as the metal substrate of the electrode for electrolysis described previously.
[0043] In the method for preparing an electrode for electrolysis of the present invention, the coating composition may include a ruthenium precursor, a cerium precursor and a nickel precursor. After coating, the precursor is converted into an oxide by being oxidized in a heat treatment step.
[0044] The use of ruthenium precursor can be not particularly limited, as long as it is a compound that can form ruthenium oxide, can be, for example, a hydrate, hydroxide, halide or oxide of ruthenium, and can specifically be selected from at least one of ruthenium hexafluoride (RuF6), ruthenium (III) chloride (RuCl3), ruthenium (III) chloride hydrate (RuCl3 xH2O), ruthenium (III) bromide (RuBr3), ruthenium (III) bromide hydrate (RuBr3 xH2O), ruthenium iodide (RuI3) and ruthenium acetate. When using the ruthenium precursor listed above, the formation of ruthenium oxide can be easy.
[0045] The cerium precursor can be any compound capable of forming cerium oxide, without particular limitation, and can be, for example, a hydrate, hydroxide, halide or oxide of cerium element, and specifically can be at least one cerium precursor selected from cerium (III) nitrate hexahydrate (Ce (NO3) 3·6H2O), cerium (IV) sulfate tetrahydrate (Ce (SO4) 2·4H2O) and cerium (III) chloride heptahydrate (CeCl3·7H2O). When the cerium precursors listed above are used, the formation of cerium oxide can be easy.
[0046] The nickel precursor can be used without particular limitation as long as it is a compound capable of forming nickel oxide, and for example, the nickel precursor can be at least one selected from nickel chloride (II), nickel nitrate (II), nickel sulfate (II), nickel acetate (II) and nickel hydroxide (II). When the nickel precursor listed above is used, the formation of nickel oxide can be easy.
[0047] The coating composition may further include a platinum group precursor for forming a platinum group oxide in the coating. The platinum group precursor may be any compound capable of forming a platinum group oxide, without particular limitation, and may be, for example, a hydrate, hydroxide, halide or oxide of a platinum group element, and may specifically be at least one platinum precursor selected from chloroplatinic acid hexahydrate (H2PtCl6·6H2O), diamine dinitroplatinum (Pt(NH3)2(NO)2), platinum (IV) chloride (PtCl4), platinum (II) chloride (PtCl2), potassium tetrachloroplatinate (K2PtCl4) and potassium hexachloroplatinate (K2PtCl6). When the platinum group precursors listed above are used, the formation of the platinum group oxide is facilitated.
[0048] In the method for preparing an electrode for electrolysis of the present invention, the coating composition may further include an amine additive to provide strong adhesion between the coating and the metal substrate. Specifically, the amine additive may improve the bonding force between the ruthenium element, the cerium element, and the nickel element contained in the coating, and may control the oxidation state of the particles containing the ruthenium element to prepare an electrode in a form more suitable for the reaction.
[0049] The amine additive used in the present invention is particularly suitable for forming a coating because it has high solubility in water while having an amine group. The amine additive that can be used in the present invention includes melamine, ammonia, urea, 1-propylamine, 1-butylamine, 1-pentylamine, 1-heptylamine, 1-octylamine, 1-nonylamine or 1-dodecylamine, and at least one selected from them can be used.
[0050] In the electrode for electrolysis of the present invention, the ruthenium element of the ruthenium precursor and the amine additive contained in the coating layer may be contained in a molar ratio of 100:30 to 100:90, for example, 100:50 to 100:70. In the case where the amine additive is contained in a range less than the above molar ratio, the effect of improving the bonding force by the additive is not significant, and in the case where the amine additive is contained in a range greater than the above molar ratio, precipitates are easily generated in the coating liquid, so that not only the uniformity of the coating layer is reduced, but also the function of the ruthenium oxide is hindered.
[0051] In the method for preparing an electrode for electrolysis of the present invention, an alcohol solvent may be used as a solvent for the coating composition. In the case of using an alcohol solvent, the above components are easily dissolved, and even in the step of forming a coating layer after applying the coating composition, the adhesion of each component can be maintained. Preferably, at least one of isopropyl alcohol and butoxyethanol may be used as a solvent, and, more preferably, a mixture of isopropyl alcohol and butoxyethanol may be used. Compared with the case of using isopropyl alcohol and butoxyethanol alone, in the case of mixing isopropyl alcohol and butoxyethanol and using them, uniform coating can be performed.
[0052] In the preparation method of the present invention, the preparation method may include a step of pre-treating the metal substrate before coating.
[0053] The pre-treatment may include forming irregularities on the surface of the metal substrate by chemical etching, sandblasting, or thermal spraying.
[0054] The pretreatment may be performed by sandblasting the surface of the metal substrate to form fine irregularities and performing salt or acid treatment. For example, the pretreatment may be performed in the following manner: sandblasting the surface of the metal substrate with aluminum oxide to form irregularities, immersing in a sulfuric acid aqueous solution, washing, and drying to form fine irregularities on the surface of the metal substrate.
[0055] The coating is not particularly limited as long as the catalyst composition can be uniformly coated on the metal substrate and may be performed by a method known in the art.
[0056] The coating may be performed by any one method selected from blade coating, die casting, comma coating, screen printing, spray coating, electrostatic spinning, roller coating and brush coating.
[0057] The drying may be performed at 50° C. to 300° C. for 5 to 60 minutes, and may preferably be performed at 50° C. to 200° C. for 5 to 20 minutes.
[0058] When the above conditions are met, energy consumption can be minimized while the solvent can be sufficiently removed.
[0059] The heat treatment may be performed at 400° C. to 600° C. for 1 hour or less, and may preferably be performed at 450° C. to 550° C. for 5 minutes to 30 minutes.
[0060] When the above conditions are met, the strength of the metal substrate will not be affected, and impurities in the catalyst layer can be easily removed.
[0061] The coating can be performed by sequentially repeating coating, drying and heat treatment so that the coating per unit area (m 2 ) is 10 g or more of ruthenium oxide on the metal substrate. That is, after the catalyst composition is coated on at least one surface of the metal substrate, dried, and heat-treated, the preparation method according to another embodiment of the present invention can be performed by repeatedly coating, drying, and heat-treating one surface of the metal substrate coated with the first catalyst composition.
[0062] Hereinafter, the present invention will be described in more detail according to embodiments and experimental examples, but the present invention is not limited to these embodiments and experimental examples. However, the present invention can be implemented in many different forms and should not be construed as being limited to the embodiments set forth herein. Rather, these exemplary embodiments are provided so that this specification will be thorough and complete, and will fully convey the scope of the present invention to those skilled in the art.
[0063] Material
[0064] In this embodiment, a nickel mesh substrate (Ni purity of 99% or more, 200 μm) manufactured by Ildong Gold Mesh was used as a metal substrate, ruthenium (III) chloride hydrate (RuCl3·nH2O) was used as a ruthenium precursor, platinum (IV) chloride was used as a platinum group precursor, cerium (III) nitrate hexahydrate (Ce(NO3)3·6H2O) was used as a cerium precursor, and nickel chloride hexahydrate (NiCl2·6H2O) was used as a nickel precursor. Urea was used as an amine additive.
[0065] In addition, a mixture of isopropyl alcohol and 2-butoxyethanol in a volume ratio of 1:1 was used as a solvent of the coating composition.
[0066] Pretreatment of metal substrates
[0067] Before forming a coating on a metal substrate, after sandblasting the surface of the substrate with aluminum oxide (white aluminum oxide, F120) at a pressure of 0.4 MPa, the substrate was placed in a 5M H2SO4 aqueous solution heated to 80°C, treated for 3 minutes, and then washed with distilled water to complete the pretreatment.
[0068] Example 1
[0069] After 1g of ruthenium precursor, 0.3135g of cerium precursor, 0.057g of nickel precursor and 0.1625g of platinum group precursor were mixed in 10ml of a mixed solvent of the above materials at a molar ratio of 5:0.75:0.25:0.5, and the ruthenium concentration was 100g / L, 0.181g of urea was added as an amine additive at a molar ratio of 3.13. The mixed solution was stirred overnight at 50°C to prepare a coating composition. The coating composition was coated on a pretreated nickel substrate, and the coated nickel substrate was placed in a convection drying oven at 180°C for 10 minutes, and then placed in an electric heating furnace at 500°C for heat treatment for 10 minutes. After the above coating, drying and heat treatment processes were repeated 9 times, the final electrode for electrolysis was finally prepared by heat treatment at 500°C in an electric heating furnace for 1 hour.
[0070] Example 2
[0071] An electrode for electrolysis was prepared in the same manner as in Example 1, except that the molar ratio of the ruthenium precursor, the cerium precursor, the nickel precursor, and the platinum group precursor was 5:0.5:0.5:0.5.
[0072] Example 3
[0073] An electrode for electrolysis was prepared in the same manner, except that the molar ratio of the ruthenium precursor, the cerium precursor, the nickel precursor, and the platinum group precursor in Example 1 was 5:0.25:0.75:0.5.
[0074] Example 4
[0075] An electrode for electrolysis was prepared in the same manner, except that the molar ratio of the ruthenium precursor, the cerium precursor, the nickel precursor, and the platinum group precursor in Example 1 was 5:1:0.25:0.5.
[0076] Example 5
[0077] An electrode for electrolysis was prepared in the same manner, except that the molar ratio of the ruthenium precursor, the cerium precursor, the nickel precursor, and the platinum group precursor in Example 1 was 5:1:0.25:0.
[0078] Comparative Example 1
[0079] An electrode for electrolysis was prepared in the same manner, except that the molar ratio of the ruthenium precursor, the cerium precursor, the nickel precursor, and the platinum group precursor in Example 1 was 5:1:0:0.5.
[0080] Comparative Example 2
[0081] An electrode for electrolysis was prepared in the same manner, except that the molar ratio of the ruthenium precursor, the cerium precursor, the nickel precursor, and the platinum group precursor in Example 1 was 5:1:0:0.
[0082] The molar ratios of the components of the electrode coatings prepared in Examples and Comparative Examples are summarized in Table 1 below.
[0083] [Table 1]
[0084] Example 1 Example 2 Example 3 Example 4 Example 5 Comparative Example 1 Comparative Example 2 Ruthenium precursor 5 5 5 5 5 5 5 Cerium precursor 0.75 0.5 0.25 1 1 1 1 Nickel precursor 0.25 0.5 0.75 0.25 0.25 0 0 Platinum Group (Platinum) Precursors 0.5 0.5 0.5 0.5 0 0.5 0
[0085] Experimental Example 1. Performance test of prepared electrolytic electrode
[0086] In order to confirm the performance of the electrodes prepared in the examples and comparative examples, a cathode voltage measurement test was performed using a half-cell in chlor-alkali electrolysis. The electrolyte used was a 32% NaOH aqueous solution, the counter electrode used was a platinum (Pt) wire, and the reference electrode used was a Hg / HgO electrode. After the prepared electrode was placed in the electrolyte, the cathode voltage was measured at -0.62 A / cm 2 The electrodes were activated at a constant current density of 1000 Å for 1 hour, and the performance of each electrode was compared with the potential value of the first hour. The results are summarized in Table 2 below.
[0087] [Table 2]
[0088]
[0089] From the above results, it can be confirmed that when nickel oxide is further included in the coating, an effect of improving overvoltage appears, and from the comparison between Example 5 and Comparative Example 1, it can be confirmed that the nickel component exhibits a similar level of overvoltage improvement effect even when it is in a smaller amount than platinum.
[0090] Experimental Example 2. XPS Analysis of Electrode Coating
[0091] Among the electrodes prepared in Examples and Comparative Examples, the surfaces of the electrodes prepared in Examples 1, 2 and 4 and the electrode prepared in Comparative Example 1 were analyzed by X-ray photoelectron spectroscopy (XPS) to examine the amounts of the components in the coating. The results are shown in Table 3 below.
[0092] [Table 3]
[0093] Example 1 Example 2 Example 4 Comparative Example 1 Ru(%) 2.3±0.2 2.1±0.2 2.7±0.9 2.3±0.2 Ce(%) 5.1±0.3 3.0±0.5 7.2±0.2 7.5±0.1 Ni(%) 5.6±0.5 9.0±1.1 5.4±1.1 1.7±0.3 Pt(%) 3.6±0.02 3.8±0.3 3.3±0.2 3.4±0.1 C(%) 41.0±0.7 38.1±2.4 39.2±1.9 45.6±0.9 O(%) 42.4±0.2 44.0±0.9 40.3±1.3 36.3±0.4
[0094] From the above results, it can be confirmed that in the example, the surface of the electrode is smoothly coated with the nickel component. The small amount of nickel component detected in the comparative example is considered to be due to the nickel component of the substrate.
[0095] Experimental Example 3. Durability Evaluation of Electrode for Electrolysis
[0096] The ruthenium oxide in the coating of the electrode for electrolysis is converted into metallic ruthenium or ruthenium oxyhydroxide (RuO(OH)2) during the electrolysis process, and in the case of reverse current, the ruthenium oxyhydroxide is oxidized to RuO4 2- Dissolved in the electrolyte. Therefore, it can be evaluated that the later the reverse current generation condition is reached, the better the durability of the electrode. From this point of view, after activating the electrode prepared in the embodiment, the reverse current generation condition is established, and then the voltage change over time is measured. Specifically, the electrode size is set to 10mm×10mm, and at a temperature of 80°C in an electrolyte of 32wt% sodium hydroxide aqueous solution, at -0.1A / cm 2 20 minutes at a current density of -0.2A / cm 2 3 minutes at a current density of -0.3A / cm 2 3 minutes at a current density of -0.4A / cm 2 The electrode was activated by generating hydrogen gas through electrolysis at a current density of 0.05 kA / m for 30 minutes. 2 The time to reach -0.1 V was measured, and the relative reaching time was calculated based on a commercially available electrode (Asahi-Kasei Corporation). The results are shown in Table 4 below.
[0097] [Table 4]
[0098]
[0099] From the above results, it can be confirmed that the electrodes of the embodiments of the present invention exhibit excellent durability due to the longer time to reach the reverse current than conventional commercial electrodes. Specifically, the electrodes of Examples 1 to 4 all exhibited better durability than conventional commercial electrodes, and in particular, it can be confirmed that Examples 1 and 2, in which the molar ratio between nickel and cerium was 3:1 to 1:1, exhibited the best durability.
Claims
1. An electrode for electrolysis, comprising: Metal base layer; and A coating comprising ruthenium oxide, cerium oxide and nickel oxide, wherein the coating is formed on at least one surface of the metal base layer, wherein the nickel oxide and the cerium oxide are simultaneously contained in a single coating layer, The molar ratio of cerium to nickel in the coating is in the range of 10:90 to 90:
10. Wherein, the molar ratio of the ruthenium element to the nickel element contained in the coating is in the range of 100:2 to 100:
20.
2. The electrode for electrolysis according to claim 1, wherein The coating also includes a platinum group oxide.
3. The electrode for electrolysis according to claim 2, wherein: The molar ratio of the ruthenium element to the platinum group element contained in the coating is in the range of 100:2 to 100:
20.
4. A method for preparing the electrode for electrolysis according to claim 1, the method comprising: applying a coating composition to at least one surface of a metal substrate; and coating by drying and heat treating the metal substrate on which the coating composition is applied, The coating composition comprises a ruthenium precursor, a cerium precursor and a nickel precursor.
5. The method according to claim 4, wherein: The coating composition also includes a platinum group precursor.
6. The method according to claim 4, wherein: The ruthenium precursor is at least one selected from ruthenium hexafluoride (RuF6), ruthenium (III) chloride (RuCl3), ruthenium (III) chloride hydrate (RuCl3·xH2O), ruthenium (III) bromide (RuBr3), ruthenium (III) bromide hydrate (RuBr3·xH2O), ruthenium iodide (RuI3) and ruthenium acetate.
7. The method according to claim 4, wherein: The cerium precursor is at least one selected from cerium (III) nitrate hexahydrate (Ce(NO3)3·6H2O), cerium (IV) sulfate tetrahydrate (Ce(SO4)2·4H2O) and cerium (III) chloride heptahydrate (CeCl3·7H2O).
8. The method according to claim 4, wherein: The nickel precursor is at least one selected from nickel (II) chloride, nickel (II) nitrate, nickel (II) sulfate, nickel (II) acetate and nickel (II) hydroxide.
9. The method according to claim 5, wherein: The platinum group precursor is at least one selected from chloroplatinic acid hexahydrate (H2PtCl6·6H2O), diamine dinitroplatinum (Pt(NH3)2(NO)2), platinum (IV) chloride (PtCl4), platinum (II) chloride (PtCl2), potassium tetrachloroplatinate (K2PtCl4) and potassium hexachloroplatinate (K2PtCl6).
10. The method according to claim 4, wherein: The coating composition further comprises at least one amine additive selected from the group consisting of melamine, ammonia, urea, 1-propylamine, 1-butylamine, 1-pentylamine, 1-heptylamine, 1-octylamine, 1-nonylamine and 1-dodecylamine.
11. The method according to claim 10, wherein: The ruthenium element of the ruthenium precursor and the amine additive included in the coating layer are contained in a molar ratio of 100:30 to 100:90.