Color-changing materials based on metal nanoparticles and their applications

By complexing metal nanoparticles with hygroscopic expanded carboxy compound, the color and transparency of intelligent optical materials under moisture stimulation under low energy consumption is achieved, and multi-mode response modulation and high energy consumption in the prior art are solved. The problem has expanded the application of intelligent optical materials.

CN114088702BActive Publication Date: 2024-11-15WUHAN TEXTILE UNIV
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
CN202111370059.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-18
Publication Date
2024-11-15
Estimated Expiration
2041-11-18

Smart Images

  • Figure CN114088702B_ABST
    Figure CN114088702B_ABST
Patent Text Reader

Abstract

The present invention provides a color-changing material based on metal nanoparticles and its application. The color-changing material includes carboxyl-complexed metal nanoparticles; the carboxyl-complexed metal nanoparticles include carboxyl-containing compounds and metal nanoparticles complexed with the carboxyl-containing compounds; the color-changing material based on metal nanoparticles undergoes a reversible change in color and / or transparency as humidity changes. After a carboxyl-containing polymer material with a high hygroscopic expansion rate is complexed with metal nanoparticles, it can be used as a filler and added to a polymer composite material with a highly similar refractive index and a small hygroscopic expansion rate, so as to achieve a reversible tuning of the color and transparency of the moisture response. The color-changing material provided by the present invention can be prepared into a variety of forms such as films, gels, fibers, etc., and can also be used as a filler for moisture-responsive color evolution, and is expected to be applied in the field of smart materials such as optical response windows with low energy consumption and humidity decoding paper.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of optical response smart materials, and in particular to a color-changing material based on metal nanoparticles and applications thereof. Background Art

[0002] In recent years, smart optical materials based on optical modulation in response to external stimuli have great application prospects in optical switches, sensors, smart windows, etc., and have attracted widespread interest. Usually, such smart optical materials refer to materials that can produce reversible optical responses such as color, transmittance, polarization, etc. under additional environmental stimuli such as electric field, temperature, humidity, pressure, etc.

[0003] The physical coloring of plasmons causes unique color rendering due to light scattering or light transmission caused by their selective absorption, and is even used in optical devices because its color regulation under additional stimulation can bring rich visual enjoyment. However, with the development of optical devices, a single mode of light response can no longer meet the needs of visualization, and there are few studies that can simultaneously achieve optical multi-mode response modulation of the visual system. Moreover, once the structure of traditional plasmon metal materials is fixed, it has always been a huge challenge to achieve reversible color conversion under environmental stimulation through wavelength depth modulation that is highly dependent on the shape of the nanoparticles. Even some stimuli require additional power consumption.

[0004] In view of this, it is necessary to design an improved color-changing material based on metal nanoparticles to solve the above problems. Summary of the invention

[0005] In order to overcome the above-mentioned deficiencies of the prior art, the purpose of the present invention is to provide a color-changing material based on metal nanoparticles and its application. The color-changing material complexes metal nanoparticles with a hygroscopic and swellable carboxyl compound, and the hygroscopic and swellable function of the hygroscopic carboxyl compound causes the refractive index of the surrounding medium of the metal nanoparticles to change, and further causes the change of the electron density of the metal nanoparticles complexed therewith, thereby producing a color change, and has the characteristics of simple structure, sensitive color change response, and reversibility.

[0006] To achieve the above-mentioned purpose of the invention, the present invention provides a color-changing material based on metal nanoparticles, including carboxyl-complexed metal nanoparticles; the carboxyl-complexed metal nanoparticles include carboxyl-containing compounds and metal nanoparticles complexed with the carboxyl-containing compounds; the color-changing material based on metal nanoparticles undergoes a reversible change in color and / or transparency as humidity changes.

[0007] As a further improvement of the present invention, the color-changing material based on metal nanoparticles further comprises a second component having a different hygroscopic expansion coefficient from that of the carboxyl-containing compound and a similar refractive index in a dry state.

[0008] As a further improvement of the present invention, the hygroscopic expansion rate of the carboxyl-containing compound is greater than 50%, and the difference between the hygroscopic expansion rate of the second component and the carboxyl-containing compound is greater than 30%.

[0009] As a further improvement of the present invention, the second component is polyvinyl alcohol-ethylene copolymer; the carboxyl-containing compound is a carboxyl-containing polymer, and the carboxyl-containing polymer includes but is not limited to one or more of hyaluronic acid, carboxylated chitosan, carboxylated cellulose, carboxylated agarose, and protein.

[0010] As a further improvement of the present invention, the metal nanoparticles include but are not limited to gold nanorods, silver nanodisks, aluminum nanoparticles, and one or more metal nanoparticles in the shape of a triangle, a circle, a square, etc., which are plasmonic materials.

[0011] As a further improvement of the present invention, the metal nanoparticles are surface-modified metal nanoparticles, and the surface modifier used includes but is not limited to trisodium citrate or polyvinyl pyrrolidone.

[0012] As a further improvement of the present invention, the preparation method of the surface-modified metal nanoparticles includes: adding a water-soluble metal salt solution, the surface modifier and the reducing agent to deionized water, reacting at 25-40°C for a preset time, and then centrifuging to obtain the surface-modified metal nanoparticles.

[0013] As a further improvement of the present invention, the color-changing material based on metal nanoparticles is a color-changing film material, a color-changing gel material, a color-changing fiber material, or a color-changing fabric or a color-changing filler.

[0014] As a further improvement of the present invention, the method for preparing the color-changing film material comprises: preparing a solution containing the carboxyl complex metal nanoparticles, and coating the solution to form a film to obtain the color-changing film material;

[0015] The preparation method of the color-changing gel material comprises: filling the solution into a mold and solidifying and molding the solution to obtain the color-changing gel material;

[0016] The method for preparing the color-changing fiber material comprises: wet spinning the solution to obtain the color-changing fiber material.

[0017] The present invention also provides an application of the color-changing material based on metal nanoparticles as described in any one of the above items, wherein the color-changing material based on metal nanoparticles is used in intelligent optical response and intelligent driving materials based on humidity changes.

[0018] The beneficial effects of the present invention are:

[0019] 1. The color-changing material based on metal nanoparticles provided by the present invention complexes a carboxyl compound with good hygroscopicity with metal nanoparticles, and induces the dielectric constant of the silver nanoparticles to change and the electron density to change due to electron transfer through the hygroscopic expansion of the hygroscopic carboxyl compound, so that under the action of moisture, the plasmons of the silver nanoparticles reversibly move over 50nm, thereby achieving reversible color adjustment.

[0020] 2. The present invention strategically designs a composite optical film, disperses triangular metal nanoparticles functionalized with carboxyl compounds into another component with a different hygroscopic expansion rate but a similar refractive index in a dry state, to prepare a composite color-changing material, which can achieve a new breakthrough in the dual-light response modulation mode stimulated by moisture, that is, to achieve the reversible tuning of color and transparency.

[0021] 3. The present invention obtains the dynamic evolution of the total refractive index and the microscopic surface roughness structure under moisture stimulation through the different hygroscopic expansion ratios of the two polymers in the composite system of hyaluronic acid and polyvinyl alcohol-ethylene copolymer nanofibers and the highly similar refractive index in the dry state, and develops a moisture-responsive and transparency-adjustable optical material. This intelligent optical material with light transmittance and color changes under external stimulation is expected to be applied in the field of intelligent materials such as optical response windows with low energy consumption and humidity decoding paper.

[0022] 4. The silver / hyaluronic acid / polyvinyl alcohol-ethylene copolymer nanofiber composite film of the present invention has a significant color change effect under humidity stimulation, which expands the application of fixed structure plasmonic materials (such as silver triangular disks) in optical color display devices. Specifically, the evolution of the extinction wavelength of the silver triangular disk in response to moisture leads to color switching, and the reversible recovery of color is achieved after removing moisture and drying.

[0023] 5. The present invention realizes the stimulus-responsive application of color-changing materials under the demand of low energy consumption, which is more energy-saving and environmentally friendly; it also realizes the changes in three modes under moisture response: the optical changes of color and transparency, and the joint changes of bending deformation behavior, which has richer visual stimulation.

[0024] 6. The color-changing material of the present invention can be prepared into various forms such as films, gels, fibers, etc., and can also be used as fillers for color evolution in response to moisture. It can also be expanded to moisture color-changing fillers formed by composites of plasmon materials (such as precious metals, semiconductors) and polymers with hygroscopic expansion functions (such as absorbent resins, etc.), and their applications (such as lipsticks, jewelry coatings, food packaging, humidity sensors, etc.). BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1From left to right in the figure are the moisture response color change diagrams of the silver / hyaluronic acid composite film materials prepared in Examples 1-4.

[0026] Figure 2 From left to right in the figure are the moisture response color change diagrams of the silver / hyaluronic acid composite film materials prepared in Examples 5-8.

[0027] Figure 3 This is a graph showing the transparency change in response to moisture of the hyaluronic acid / polyvinyl alcohol-ethylene copolymer nanofiber composite film material.

[0028] Figure 4 (a) is a graph showing the moisture response transparency change of the silver / hyaluronic acid / polyvinyl alcohol-ethylene copolymer nanofiber composite film prepared in Example 12; (b) is a graph showing the transparency change at different moisture response times; (c) is a real picture showing the application of the color-changing material prepared in Example 12 in diapers; and (d) is a real picture showing the application of the color-changing material prepared in Example 12 in a mask.

[0029] Figure 5 (a) and (b) are actual pictures of the silver / hyaluronic acid / polyvinyl alcohol-ethylene copolymer nanofiber composite film prepared in Example 12 before and after moisture stimulation.

[0030] Figure 6 The transmittance of the silver / hyaluronic acid composite film material prepared in Example 4 to light of different wavelengths at different humidity levels.

[0031] Figure 7 This is the moisture-stimulated color response of the gold nanorod / hyaluronic acid composite film material prepared in Example 13. DETAILED DESCRIPTION

[0032] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in detail below in conjunction with specific embodiments.

[0033] It should also be noted that, in order to avoid obscuring the present invention due to unnecessary details, only structures and / or processing steps closely related to the scheme of the present invention are shown in the specific embodiments, while other details that are not closely related to the present invention are omitted.

[0034] In addition, it should be noted that the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.

[0035] The present invention provides a color-changing material based on metal nanoparticles, including carboxyl complexed metal nanoparticles; the carboxyl complexed metal nanoparticles include carboxyl compounds and metal nanoparticles complexed therewith; the color-changing material based on metal nanoparticles undergoes a reversible change in color and / or transparency as humidity changes. In this way, the dielectric constant of the silver nanoparticles is induced to change through the hygroscopic expansion of the hygroscopic carboxyl compound, and the electron density changes caused by the electron transfer when water is involved, so that under the action of moisture, the plasmon of the silver nanoparticles reversibly moves over 50nm, thereby achieving reversible color adjustment.

[0036] The carboxyl-containing compound is preferably a carboxyl-containing polymer, and the carboxyl-containing polymer includes but is not limited to one or more of hyaluronic acid, carboxylated chitosan, carboxylated cellulose, carboxylated agarose, and protein. For example, hyaluronic acid is preferred, which has strong hygroscopicity and contains a large number of carboxyl groups. Carboxyl complexation can be achieved without carboxyl modification. Based on the color change mechanism of the present invention, the selection of polymers that can be complexed with the silver triangular disk and have hygroscopicity can produce color changes, and the electronic density of silver is induced to change through the hygroscopic expansion of the polymer, and the electronic microstructure of the complex as a whole changes, thereby changing its light refractive index.

[0037] The metal nanoparticles include but are not limited to gold nanorods, silver nanodisks, aluminum nanoparticles, and one or more metal nanoparticles in the shape of triangle, circle, square, etc., which are plasmonic materials. Preferably, they are triangular metal nanoparticles, and more preferably, they are triangular silver nanoparticles.

[0038] The metal nanoparticles are preferably surface-modified metal nanoparticles, and the surface modifier used includes but is not limited to trisodium citrate or polyvinyl pyrrolidone. By modifying the metal nanoparticles, the color type and responsiveness can be adjusted. The preparation method of the surface-modified metal nanoparticles comprises: adding a water-soluble silver salt, a surface modifier and a reducing agent to deionized water, reacting at 25-40° C. for 0.5-2 hours, and then centrifuging to obtain a metal nanodisk.

[0039] For example, in a specific embodiment, deionized water (200mL 18.25Ω), silver nitrate (AgNO3 200μL 0.1M), trisodium citrate (Na3CA 12mL 75mM) and hydrogen peroxide (H2O2 480μL 30%) were added to a 250mL conical flask in sequence, placed in a 30°C constant temperature water bath and magnetically stirred, and after a certain period of constant temperature control, fresh sodium borohydride (NaBH4 1.2mL 0.1M) was quickly injected into the conical flask, and it can be seen that the solution quickly turns yellow, orange, red, and finally turns blue. At this time, the constant temperature water bath is continued to stir for 15min, and then placed in a 30°C constant temperature box for two hours. After the reaction is completed, the suspension of the silver triangular disk is centrifuged to obtain trisodium citrate capping agent-silver triangular disk (TSCAg).

[0040] In particular, further secondary growth can be performed, that is, the TSCAg obtained above is dispersed in 40 mL of aqueous solution, and 10 mL of a mixed solution containing ascorbic acid (AA 1.2 mM) and Na3CA (0.4 mM) is prepared and mixed with the 10 mL of the centrifuged TSCAg solution. Then, AgNO3 (10 mL 0.6 mM) solution is titrated into the mixed solution at a rate of 10 mL / h using a syringe pump under magnetic stirring, and after the titration of AgNO3 is completed, the final product is centrifuged in deionized water.

[0041] The preparation method of carboxyl-containing complex metal nanoparticles comprises: mixing a carboxyl-containing compound and metal nanoparticles in a solution to make the two complex.

[0042] The color-changing material based on metal nanoparticles can be a color-changing film material, a color-changing film material gel material, a color-changing fiber material or a color-changing fabric material, etc.

[0043] Among them, the preparation method of the color-changing film material includes: preparing a solution containing carboxyl complex metal nanoparticles (0.1wt%-2.0wt%), coating the solution into a film to obtain the color-changing film material; for example, spin coating the solution on a substrate, and tearing off the composite film after curing to obtain the color-changing film material.

[0044] The preparation method of the color-changing gel material comprises: filling a solution into a mold and solidifying and molding (such as freeze drying) to obtain the color-changing gel material.

[0045] The preparation method of the color-changing fiber material comprises: wet spinning a solution (5.0wt%-6.0wt%) to obtain the color-changing fiber material. For example, when the carboxyl-containing compound is hyaluronic acid, a 5.0wt%-6.0wt% hyaluronic acid solution is prepared, a certain amount of sodium hydroxide is added, and the mixture is stirred evenly, and a certain amount of AgNPs is added to 10mL of the hyaluronic acid solution, and stirred for 30min to obtain a spinning solution; a mixed solution of 600mL of methanol and 400mL of acetic acid is taken and placed in a glass tank as a coagulation bath for wet spinning. The spinning solution is sucked with a 10mL disposable syringe, and extruded into a methanol / acetic acid coagulation bath through an extruder for spinning, and the extrusion speed is controlled at 15mL / h to 25mL / h. The extruded fiber is soaked in the coagulation bath for 12h, and naturally air-dried after being taken out.

[0046] The color-changing material based on metal nanoparticles also includes a second component having a different hygroscopic expansion rate from the carboxyl-containing compound and a similar refractive index in a dry state (for example, a refractive index difference of less than 0.5). The hygroscopic expansion rate of the carboxyl-containing compound is greater than 50%, preferably 60%-200%, and more preferably 60%-120%. The difference between the hygroscopic expansion rate of the second component and the carboxyl-containing compound is greater than 30%, for example, 30%-100%. The hygroscopic expansion rate of the present invention refers to the ratio of the volume of the color-changing material after moisture absorption to the volume before moisture absorption.

[0047] For example, when the carboxyl-containing compound is hyaluronic acid, the second component is preferably polyvinyl alcohol-ethylene copolymer, more preferably polyvinyl alcohol-ethylene copolymer nanofiber (obtained by melt spinning and solvent phase separation). By the different hygroscopic expansion ratios of two polymers in the composite system of hyaluronic acid and polyvinyl alcohol-ethylene copolymer nanofiber (so that transparency is reduced in wet state) and the highly approximate refractive index in dry state (so that transparent state is present in dry state), the total refractive index and microscopic surface roughness structure are subjected to common dynamic evolution under moisture stimulation, thereby developing an optical material with adjustable transparency of moisture response. Meanwhile, due to the complexation of metal nanoparticles, there is also a color change function of moisture response, the intelligent optical material with light transmittance and color co-change under this external stimulation is expected to be realized in the application of intelligent material fields such as optical response windows, humidity decoding paper, etc. of low energy consumption.

[0048] Those skilled in the art can select and adjust the second component containing the carboxyl compound according to actual needs and the properties of the material itself.

[0049] The present invention also provides an application of any one of the above color-changing materials based on metal nanoparticles, and the color-changing materials based on metal nanoparticles are used in intelligent optical response and intelligent driving materials based on humidity changes, such as for the preparation of optical response windows, humidity decoding paper, diapers, masks and other products.

[0050] Examples 1-4

[0051] A color-changing composite film material based on metal nanoparticles is prepared by the following steps:

[0052] (1) Preparation of silver triangle disk (TSCAg):

[0053] Take deionized water (200mL 18.25Ω), silver nitrate (AgNO3 200μL 0.1M), trisodium citrate (Na3CA12mL 75mM), hydrogen peroxide (H2O2 480μL 30%) solution and add them to a 250mL conical flask in turn, put it in a 30℃ constant temperature water bath and stir it magnetically. After a certain period of constant temperature control, quickly inject fresh sodium borohydride (NaBH4 1.2mL 0.1M) into the conical flask, and you can see that the solution quickly turns yellow, orange, red, and finally blue. At this time, continue to stir in the constant temperature water bath for 15min, then put it in a 30℃ constant temperature box for two hours. After the reaction is completed, centrifuge the suspension of the silver triangle disk for subsequent use;

[0054] The TSCAg obtained above was dispersed in 40 mL of aqueous solution, and a 10 mL mixed solution containing ascorbic acid (AA 1.2 mM) and Na3CA (0.4 mM) was prepared and mixed with the 10 mL TSCAg solution centrifuged above. Then, AgNO3 (10 mL 0.6 mM) solution was titrated into the above mixed solution at a rate of 10 mL / h using a syringe pump under magnetic stirring. After the titration of AgNO3 was completed, the final product was centrifuged in deionized water.

[0055] (2) Preparation of silver / hyaluronic acid film with color evolution stimulated by moisture:

[0056] The prepared hyaluronic acid solution (HA) with a mass fraction of 0.1wt%-2.0wt% is mixed with AgNPs under magnetic stirring, and is compounded together through the complexation of carboxyl groups and silver. The mixed gel triangular silver disk / hyaluronic acid is spin-coated on a flat substrate to prepare a film (or filled in a mold to prepare a gel), dried at room temperature to form a film, and then removed from the film.

[0057] Table 1 Hyaluronic acid mass content of Examples 1-4

[0058] Example 1 2 3 4 Hyaluronic acid concentration (wt%) 0.2 0.5 1.0 1.5

[0059] The moisture-responsive films prepared in Examples 1-4 were subjected to a moisture sensitivity test. The test method is as follows: Take the prepared film and use a humidifier to give the film a certain humidity stimulus, and the color of the film will change immediately. The test results are as follows: Figure 1 shown.

[0060] from Figure 1 It can be seen that by changing the concentration of hyaluronic acid, the color type and depth of the color-changing film material in the dry state and the moisture-absorbed state can be controlled.

[0061] from Figure 6 It can be seen that the silver / hyaluronic acid film prepared by the present invention has a relatively large visible light transmittance in a dry state, and a slightly lower transmittance of light waves between 500-600nm. Under RH100%, the light transmittance is significantly reduced, and the transmittance of light waves between 500-600nm is most significantly reduced. It can be seen that after moisture absorption, not only the transparency of the composite film will be reduced, but the color will also change due to the difference in transmittance of different wavelengths.

[0062] Embodiment 5-8

[0063] The color-changing composite film materials based on metal nanodisks provided in Examples 5-8 are different from those in Example 4 in that silver triangular disks modified with trisodium citrate of different concentrations and silver triangular disks modified with polyvinyl alcohol pyrrolidone of different concentrations are used, and the products obtained are respectively recorded as 1TSCAg@HA, 2TSCAg@HA and 1PVPAg@HA, 2PVPAg@HA. The rest is substantially the same as in Example 4 and will not be described again.

[0064] The moisture-responsive films prepared in Examples 5-8 were subjected to a moisture sensitivity test. The test method is as follows: Take the prepared film and use a humidifier to give the film a certain humidity stimulus, and the color of the film will change immediately. The test results are as follows: Figure 2 shown.

[0065] from Figure 2 It can be seen that the TSCAg@HA material prepared in Examples 5-6 shows an evolution from rose red to orange; the PVPAg@HA material prepared in Examples 7-8 shows an evolution from gray-green to light purple. More color adjustments can be achieved by adjusting the concentration of hyaluronic acid or the concentration of surfactants TSC and PVP.

[0066] Examples 9-11

[0067] A color-changing composite fiber material based on metal nanodisks is prepared by the following steps:

[0068] Take a certain amount of hyaluronic acid powder and deionized water, stir vigorously at room temperature to prepare a 5.5wt% hyaluronic acid solution, add a certain amount of sodium hydroxide, stir until it is evenly stirred, take a certain amount of AgNPs, TSCAg and PVPAg and add them to 10mL of hyaluronic acid solution, stir for 30min, and the spinning solution is ready.

[0069] Take 600mL of methanol and 400mL of acetic acid mixture and place it in a glass tank as a coagulation bath for wet spinning. Use a disposable 10mL syringe to absorb the spinning solution and squeeze it into the methanol / acetic acid coagulation bath through an extruder for spinning. The extrusion speed is controlled at 20mL / h. Soak the extruded fiber in the coagulation bath for 12h, take it out and let it air dry naturally.

[0070] The test method of the prepared moisture-responsive color-changing fiber is as follows: take the prepared dry Ag@HA fiber, use a humidifier to give the color-changing fiber a certain humidity, the fiber will expand to different degrees, and show a color-changing effect. The addition of AgNPs can prepare orange fibers; the addition of TSCAg can prepare rose-red fibers; the addition of PVPAg can prepare blue fibers.

[0071] Example 12

[0072] Preparation of a moisture-stimulated color and transmittance-responsive silver / hyaluronic acid / polyvinyl alcohol-ethylene copolymer nanofiber composite film:

[0073] Polyvinyl alcohol-ethylene copolymer / cellulose acetate butyrate composite fibers were obtained by melt extrusion; acetone was then used to completely remove cellulose acetate butyrate from the composite fibers to obtain polyvinyl alcohol-ethylene copolymer nanofibers; secondly, a polyvinyl alcohol-ethylene copolymer nanofiber suspension with a fiber content of 3.5 wt% was prepared by dispersing the nanofibers in an isopropanol solution using a high-speed shearing machine.

[0074] The silver / hyaluronic acid suspension prepared in Example 12 above is added to the polyvinyl alcohol-ethylene copolymer nanofiber suspension and fully dispersed, and the mixed solution is sprayed on the polyethylene terephthalate non-woven fabric. After the solvent evaporates, the silver / hyaluronic acid / polyvinyl alcohol-ethylene copolymer nanofiber composite film can be directly demolded and used.

[0075] The prepared moisture-responsive color-transparency co-modulated moisture-sensitive test method is as follows: take the prepared dry silver / hyaluronic acid / polyvinyl alcohol-ethylene copolymer nanofiber composite film, stimulate it with a humidifier, and obtain the effect of color-transmittance co-changing. Figure 4 As shown in (a), it can be seen that before moisture stimulation, the silver / hyaluronic acid / polyvinyl alcohol-ethylene copolymer nanofiber composite film has high transparency and is purple. After moisture stimulation, the transparency decreases and turns light purple. This is because the dry refractive index of hyaluronic acid and polyvinyl alcohol-ethylene copolymer nanofiber is similar, so the composite has high transparency. After moisture absorption, the difference in the moisture absorption expansion rate between the two makes the refractive index significantly different, which is optically similar to partitioning, so the transparency decreases. The transparency can be restored after drying. Figure 4As can be seen from (b), the moisture response time of the present invention is short, indicating that the optical response sensitivity is high. As can be seen from (c) and (d), the present invention can be used for intelligent moisture color display of diapers or masks to visualize the moisture of the material.

[0076] from Figure 3 It can be seen that when hyaluronic acid is not complexed with silver triangular disc silver, the obtained hyaluronic acid / polyvinyl alcohol-ethylene copolymer nanofiber composite film only produces a conversion of transparency when stimulated by moisture.

[0077] from Figure 5 It can be seen that the silver / hyaluronic acid / polyvinyl alcohol-ethylene copolymer nanofiber composite film prepared by the present invention will curl inward under moisture stimulation, that is, moisture-driven deformation occurs. This is caused by the difference in the hygroscopic expansion rate of hyaluronic acid and polyvinyl alcohol-ethylene copolymer nanofiber.

[0078] Example 13

[0079] A color-changing composite film material based on metal nanoparticles is different from Example 4 in that the silver triangular disk is replaced with gold nanorods to obtain a gold nanorod / hyaluronic acid composite film material. The rest is substantially the same as Example 4 and will not be described again.

[0080] from Figure 7 It can be seen that the color of the composite membrane material prepared in this embodiment changes from dark gray to light gray as the humidity increases.

[0081] In summary, the color-changing material based on metal nanodisks provided by the present invention complexes a carboxyl compound with good hygroscopicity with a metal nanodisk, and induces a change in the dielectric constant of the silver nanoparticles through the hygroscopic expansion of the hygroscopic carboxyl compound, and the electron transfer when water is involved causes a change in the electron density, so that under the action of moisture, the plasmon of the silver nanoparticles reversibly moves over 50nm, thereby achieving reversible color adjustment. The present invention also disperses the triangular silver nanoparticles functionalized with a carboxyl compound into another component with a different hygroscopic expansion rate but a similar refractive index in a dry state to prepare a composite color-changing material, which can achieve a new breakthrough in the dual-light response modulation mode stimulated by moisture, that is, to achieve the common reversible tuning of color and transparency.

[0082] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention.

Claims

1. A color-changing material based on metal nanoparticles, characterized in that: The invention comprises carboxyl complexed metal nanoparticles; the carboxyl complexed metal nanoparticles comprise carboxyl compounds and metal nanoparticles complexed with the carboxyl compounds; the color-changing material based on the metal nanoparticles undergoes a reversible change in color and / or transparency as humidity changes; The color-changing material based on metal nanoparticles further comprises a second component having a different hygroscopic expansion rate from the carboxyl-containing compound and a similar refractive index in a dry state; The hygroscopic expansion rate of the carboxyl-containing compound is greater than 50%, and the difference between the hygroscopic expansion rate of the second component and the carboxyl-containing compound is greater than 30%; The second component is polyvinyl alcohol-ethylene copolymer; the carboxyl-containing compound is a carboxyl-containing polymer, and the carboxyl-containing polymer includes one or more of hyaluronic acid, carboxylated chitosan, carboxylated cellulose, carboxylated agarose, and protein.

2. The color-changing material based on metal nanoparticles according to claim 1, characterized in that: The metal nanoparticles are one or more metal nanoparticles in the shape of triangle, circle, or square.

3. The color-changing material based on metal nanoparticles according to claim 1, characterized in that: The metal nanoparticles are surface-modified metal nanoparticles, and the surface modifier used is trisodium citrate or polyvinyl pyrrolidone.

4. The color-changing material based on metal nanoparticles according to claim 3, characterized in that: The preparation method of the surface-modified metal nanoparticles comprises: adding a water-soluble metal salt solution, the surface modifier and the reducing agent into deionized water, reacting at 25-40° C. for a preset time, and then centrifuging to obtain the surface-modified metal nanoparticles.

5. The color-changing material based on metal nanoparticles according to any one of claims 1 to 4, characterized in that: The color-changing material based on metal nanoparticles is a color-changing film material, a color-changing gel material, a color-changing fiber material, a color-changing fabric or a color-changing filler.

6. The color-changing material based on metal nanoparticles according to claim 5, characterized in that: The preparation method of the color-changing film material comprises: preparing a solution containing the carboxyl complex metal nanoparticles, and coating the solution to form a film to obtain the color-changing film material; The preparation method of the color-changing gel material comprises: filling the solution into a mold and solidifying and molding the solution to obtain the color-changing gel material; The method for preparing the color-changing fiber material comprises: wet spinning the solution to obtain the color-changing fiber material.

7. Use of a color-changing material based on metal nanoparticles according to any one of claims 1 to 6, characterized in that: The color-changing material based on metal nanoparticles is used in intelligent optical response and intelligent driving materials based on humidity changes.

Citation Information

Patent Citations

  • Applications of multi-component super-molecule hydrogel as stress response material and self-healing material

    CN103272540A

  • Insoluble nano humidity indicating material, preparation and application thereof

    CN105784703A

  • Photonic crystal nano-composite gel membrane with temperature / humidity dual responses and preparation method of photonic crystal nano-composite gel membrane

    CN107915856A

  • High-sensitivity flexible humidity sensor and preparation method thereof

    CN109975370A

  • Fiber-based humidity sensor based on moisture absorption and color change, and preparation method thereof

    CN112964650A