Method for manufacturing a solid electrolyte

By mixing lithium, sulfur, and phosphorus raw materials with a complexing agent using a liquid-phase method, a crystalline solid electrolyte with a PS₄³⁻ structure is formed, solving the problem of difficulty in balancing particle size and conductivity in existing technologies, and realizing the efficient manufacturing of electrolytes with small particle size and high conductivity.

CN114245945BActive Publication Date: 2026-11-24IDEMITSU KOSAN CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202080056934.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-09-20
Filing Date
2020-09-17
Publication Date
2026-11-24
Estimated Expiration
2040-09-17

AI Technical Summary

Technical Problem

Existing technologies make it difficult to simultaneously manufacture sulfide solid electrolytes with small particle size and high ionic conductivity. In particular, manufacturing at high temperatures can easily lead to grain growth, and the solvent is difficult to remove after the reaction, which affects the conductivity.

Method used

A crystalline solid electrolyte with a PS₄³⁻ structure is formed by mixing lithium, sulfur, and phosphorus raw materials with a complexing agent using a liquid-phase method, heating the mixture in a pressure vessel to form a precursor, and then crystallizing it under reflux conditions.

Benefits of technology

This invention enables the fabrication of sulfide solid electrolytes with small particle size and high ionic conductivity, avoiding the problems of grain growth and solvent residue at high temperatures, and improving the performance of the electrolyte.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114245945B_ABST
    Figure CN114245945B_ABST
Patent Text Reader

Abstract

This invention provides a method for manufacturing a crystalline solid electrolyte, wherein the crystalline solid electrolyte has a small particle size and high ionic conductivity, and contains lithium, sulfur, phosphorus, and halogen elements. The method is characterized by comprising: a mixing step, including a complexing step of mixing solid electrolyte raw materials and a complexing agent in a liquid phase to obtain a precursor containing lithium, sulfur, and phosphorus; and a crystallization step, wherein the precursor is heated in a solvent using a pressure vessel or during reflux.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for manufacturing solid electrolytes. Background Technology

[0002] In recent years, with the rapid popularization of information-related devices and communication equipment such as computers, cameras, and mobile phones, the development of batteries used as their power source has also gained attention. Previously, batteries used for such applications employed electrolytes containing flammable organic solvents. However, by making the battery entirely solid-state, safety devices are simplified due to the absence of flammable organic solvents within the battery, and manufacturing costs and productivity are significantly improved. Therefore, the development of batteries that replace the electrolyte with a solid electrolyte layer has been undertaken.

[0003] As solid electrolytes, sulfide solid electrolytes and oxide solid electrolytes are known, and the sulfide solid electrolyte obtained by the method described in Patent Document 1 is known to have high ionic conductivity. Crystal structures of sulfide solid electrolytes include, for example, Li4P2S6, Li7PS6, and Li7P3S6. 11 Beyond crystal structure, as a device capable of possessing PS4 3- Crystal structures, such as the Li3PS4 crystal structure and Li... 4-x Ge 1- x P x S4 type sulfide crystalline lithium superionic conductor thio-LISICON Region II crystal structure, and Li 4-x Ge 1- x P x S4 type sulfide crystalline lithium superionic conductors with similar crystal structures to the thio-LISICON Region II type, and Argyrodite crystal structures, etc.

[0004] Sulfide solid electrolytes containing a sulfide-germanium sulfide crystal structure are known to have relatively high ionic conductivity. As a manufacturing method, for example, Non-Patent Documents 1 and 2 disclose a method of mechanically grinding the electrolyte using a planetary ball mill followed by heat treatment at a high temperature of 550°C. Furthermore, Patent Document 2 discloses a method of mixing lithium sulfide (LiS2) powder and sulfide powder using a ball mill or similar device, and then calcining the mixture in a hydrogen sulfide atmosphere at 600–800°C.

[0005] From the perspective of performance and manufacturing of all-solid-state lithium batteries, solid electrolytes with small particle sizes are required. For example, smaller particle sizes facilitate the formation of a contact interface between the active material and the solid electrolyte when using solid electrolytes to fabricate electrodes. However, to obtain sulfide solid electrolytes with excellent ionic conductivity and containing a sulfide-germanium sulfide crystal structure, calcination at relatively high temperatures is necessary, requiring heating in a gas atmosphere conducive to grain growth. Furthermore, Patent Documents 3 and 4 disclose methods for pulverizing granulated solid electrolytes after heating, but these methods sometimes result in a decrease in ionic conductivity.

[0006] Furthermore, Patent Document 5 discloses a method for manufacturing sulfide solid electrolytes by heating in a solvent to prevent granulation. However, in the prior art, sulfide solid electrolytes containing sulfide-germanium ore-type crystal structures require high-temperature heating treatment at 550°C to 800°C during manufacturing, and therefore are difficult to heat in a solvent due to their boiling points.

[0007] Therefore, it is difficult to manufacture sulfide solid electrolytes with small particle size and high ionic conductivity.

[0008] Patent Document 6 describes a method for manufacturing a sulfide-based solid electrolyte, including a step of contacting an alkali metal sulfide with a sulfur compound in a mixed solvent of a hydrocarbon solvent and a polar aprotic solvent. Patent Document 7 describes a method for manufacturing a lithium-ion conductive solid electrolyte, including a step of contacting a compound such as phosphorus sulfide with lithium sulfide in a hydrocarbon solvent. However, in both methods, only a glassy sulfide-based solid electrolyte can be obtained in the solvent. To obtain a crystalline sulfide-based solid electrolyte, drying and heating steps are required after the contacting step. Therefore, it is difficult to easily manufacture sulfide-based solid electrolytes with small particle sizes and high ionic conductivity.

[0009] Patent Document 8 describes a method for manufacturing a solid electrolyte containing a sulfide-germanium ore-type crystal structure, comprising: heat-treating a mixture of raw materials containing lithium, sulfur, phosphorus, and halogens in a solvent using a pressure vessel or during reflux; removing the solvent; and calcining the processed product obtained by the heat treatment. The method described in Patent Document 7, like that in Patent Document 6, does not yield a crystallizable solid electrolyte in a solvent and requires calcination of the processed product, thus making it difficult to easily manufacture sulfide solid electrolytes with small particle sizes and high ionic conductivity.

[0010] Furthermore, Non-Patent Document 3 describes a method of dissolving Li₂S, LiBr, and Li₃PS₄ in an ethanol solvent and reacting them in solution to synthesize Li₆PS₅Br crystals as argillaceous sulfide-germanium ore-type crystals. In this method, since the raw materials such as Li₂S, LiBr, and Li₃PS₄ are dissolved in an ethanol solvent, the reaction of these raw materials is equivalent to a homogenization method in liquid-phase processes. However, in the homogenization method, since precipitation proceeds based on the inherent solubility of each component, the components separate and precipitate, or the affinity of Li for the solvent is too strong, making it difficult to remove the solvent even after drying after precipitation. For these main reasons, the ionic conductivity of the solid electrolyte can sometimes decrease significantly.

[0011] Existing technical documents

[0012] Patent documents

[0013] Patent Document 1: International Publication No. 2017 / 159667

[0014] Patent Document 2: Japanese Patent Application Publication No. 2013-211171

[0015] Patent Document 3: International Publication No. 2018 / 164224

[0016] Patent Document 4: International Publication No. 2019 / 031436

[0017] Patent Document 5: Japanese Patent Application Publication No. 2014-096391

[0018] Patent Document 6: International Publication No. 2014 / 192309

[0019] Patent Document 7: International Publication No. 2009 / 047977

[0020] Patent Document 8: Japanese Patent Application Publication No. 2020-95953

[0021] Non-patent literature

[0022] Non-patent literature 1: Angewandte Chemie International Edition, No. 47 (2008), pp. 755-758

[0023] Non-patent literature 2: Condensed Matter Physics, Issue 208 (2011), No. 8, pp. 1804-1807

[0024] Non-patent literature 3: Journal of Colour Materials (J. Jpn. Soc. Colour Mater), No. 89, No. 9 (2016), pp. 139-143 Summary of the Invention

[0025] The technical problem that the invention aims to solve

[0026] The present invention was made in view of the following circumstances, and its object is to provide a method for manufacturing solid electrolytes with small particle size and high ionic conductivity.

[0027] Solution to the above technical problems

[0028] In order to solve the above-mentioned technical problem, the inventors conducted in-depth research and found that the technical problem can be solved by the following invention.

[0029] 1. A method for manufacturing a crystalline solid electrolyte, the crystalline solid electrolyte comprising lithium, sulfur, phosphorus and halogen elements, comprising: a mixing step, including a complexing step of mixing solid electrolyte raw materials and a complexing agent in a liquid phase to obtain a precursor comprising lithium, sulfur and phosphorus elements; and a crystallization step, wherein the precursor is heated in a solvent using a pressure vessel or during reflux.

[0030] Invention Effects

[0031] According to the present invention, a method for manufacturing a solid electrolyte with small particle size and high ionic conductivity can be provided. Attached Figure Description

[0032] Figure 1 The X-ray diffraction spectrum is that of the precursor, solid electrolyte, obtained in Example 1.

[0033] Figure 2 The X-ray diffraction spectrum is that of the solid electrolyte obtained in Comparative Example 1.

[0034] Figure 3 The X-ray diffraction spectrum is that of the solid electrolyte obtained in Comparative Example 2.

[0035] Figure 4 The X-ray diffraction spectra of the precursor and pulverized material were obtained in Reference Example 1.

[0036] Figure 5 The X-ray diffraction spectra of the precursor and pulverized material were obtained in Reference Example 2. Detailed Implementation

[0037] Hereinafter, embodiments of the present invention (hereinafter sometimes referred to as "this embodiment") will be described. Furthermore, in this specification, the upper and lower limits of the numerical ranges referred to by "above," "below," and "~" are values ​​that can be arbitrarily combined; additionally, the values ​​of the embodiments can also be used as the upper and lower limits.

[0038] In the method for manufacturing a crystalline solid electrolyte according to this embodiment, the crystalline solid electrolyte contains lithium, sulfur, phosphorus, and halogen elements. The method is characterized by comprising: a mixing step, including a complexing step in which a solid electrolyte raw material and a complexing agent are mixed in a liquid phase to obtain a precursor containing lithium, sulfur, and phosphorus; and a heating step, in which the precursor is heated in a solvent using a pressure vessel or during reflux (this step may also be referred to as a "crystallization step" as described later).

[0039] In this specification, "solid electrolyte" refers to an electrolyte that remains solid at 25°C under a nitrogen atmosphere. The solid electrolyte obtained by the manufacturing method of this embodiment is a solid electrolyte having ionic conductivity, containing at least sulfur and phosphorus elements and may also contain lithium elements as elements that embody ionic conductivity.

[0040] Solid electrolytes can be broadly categorized into amorphous and crystalline solid electrolytes. The solid electrolyte obtained through this invention is a crystalline solid electrolyte. Whether a solid electrolyte is crystalline can be determined by X-ray diffraction measurement. 31 The determination can be made based on measurements such as P-NMR. For example, in X-ray diffraction measurements, when peaks originating from solid electrolytes are observed in the X-ray diffraction pattern, especially in crystal structures such as Li6PS5X and Li... 7-x PS 6-x X x In the case of sulforaphane-germanium-type crystals (X = Cl, Br, I, x = 0.0–1.8), the solid electrolyte can be considered a crystalline solid electrolyte. The diffraction peaks of these sulforaphane-germanium-type crystal structures appear, for example, near 2θ = 15.3°, 17.7°, 31.1°, 44.9°, and 47.7°. Furthermore, when using… 31 If the crystallinity measured by P-NMR is above 80%, the solid electrolyte can be considered a crystalline solid electrolyte. Specifically, the degree of crystallinity is a value obtained by measuring the solid... 31 For the obtained P-NMR spectra, the resonance lines observed in the 70-120 ppm range are separated into Gaussian curves using the nonlinear least squares method, and the area ratio of each curve is calculated.

[0041] [Mixed Process]

[0042] The method for manufacturing a crystalline solid electrolyte according to this embodiment includes a mixing step to obtain a precursor containing lithium, sulfur, and phosphorus. This mixing step includes a complexing step in which a solid electrolyte raw material and a complexing agent are mixed in a liquid phase. The precursor containing lithium, sulfur, and phosphorus obtained through this mixing step is fed to a subsequent heating step (crystallization step).

[0043] (Solid electrolyte raw materials)

[0044] From the viewpoint of obtaining a crystalline solid electrolyte containing lithium, sulfur, phosphorus and halogen elements, it is preferable to use a raw material containing one element selected from lithium, sulfur, phosphorus and halogen elements as the solid electrolyte raw material used in this embodiment. A raw material containing lithium, sulfur, phosphorus and halogen elements can be prepared by combining one or more raw materials.

[0045] Examples of such raw materials include: lithium sulfide (Li2S); phosphorus trisulfide (P2S3), phosphorus pentasulfide (P2S5), and other phosphorus sulfides.

[0046] Lithium sulfide is preferably in particles.

[0047] The average particle size (D) of lithium sulfide particles 50 The average particle size is preferably 0.1 μm to 300 μm, more preferably 1 μm to 100 μm, even more preferably 3 μm to 50 μm, and particularly preferably 5 μm to 30 μm. In this specification, the average particle size (D...) 50 The particle size distribution is the particle size at which 50% of the total particle size is accumulated from the smallest particle when plotting the cumulative particle size distribution curve. The volume distribution is, for example, the average particle size that can be measured using a laser diffraction / scattering particle size distribution measuring device. Furthermore, for other solid raw materials used in this embodiment, it is preferable to use solid raw materials with an average particle size similar to that of the lithium sulfide particles described above; that is, it is preferable to use solid raw materials with an average particle size within the same range as the average particle size of the lithium sulfide particles described above.

[0048] Furthermore, from the viewpoint of improving ionic conductivity, raw materials containing halogen elements are used as raw materials for solid electrolytes.

[0049] Examples of raw materials containing halogen elements include: lithium halides such as lithium fluoride, lithium chloride, lithium bromide, and lithium iodide; phosphorus halides such as various phosphorus fluorides (PF3, PF5), various phosphorus chlorides (PCl3, PCl5, P2Cl4), various phosphorus bromides (PBr3, PBr5), and various phosphorus iodides (PI3, P2I4); thiophosphoric fluoride (PSF3), thiophosphoric chloride (PSCl3), thiophosphoric bromide (PSBr3), thiophosphoric iodide (PSI3), thiophosphoric fluoride dichloride (PSCl2F), and thiophosphoric fluoride dibromide (PSBr2F); raw materials composed of at least two elements selected from the above four elements, namely lithium, phosphorus, and sulfur, as well as the preferred halogen elements; halogen monomers such as fluorine (F2), chlorine (Cl2), bromine (Br2), and iodine (I2), with chlorine (Cl2), bromine (Br2), and iodine (I2) being preferred.

[0050] Other substances that can be used as raw materials besides those mentioned above include, for example, raw materials containing at least one element selected from lithium, phosphorus, and sulfur, and containing elements other than these three elements. More specifically, examples include: lithium compounds such as lithium oxide, lithium hydroxide, and lithium carbonate; alkali metal sulfides such as sodium sulfide, potassium sulfide, rubidium sulfide, and cesium sulfide; metal sulfides such as silicon sulfide, germanium sulfide, boron sulfide, gallium sulfide, tin sulfide (SnS, SnS2), aluminum sulfide, and zinc sulfide; phosphoric acid compounds such as sodium phosphate and lithium phosphate; alkali metal halides other than lithium such as sodium iodide, sodium fluoride, sodium chloride, and sodium bromide; metal halides such as aluminum halide, silicon halide, germanium halide, arsenic halide, selenium halide, tin halide, antimony halide, tellurium halide, and bismuth halide; phosphorus oxychloride (POCl3) and phosphorus tribromide (POBr3); etc.

[0051] In this embodiment, from the viewpoint of improving ionic conductivity, the precursor containing lithium, sulfur, and phosphorus obtained through this mixing process is preferably containing PS4. 3- The precursor to the structure, details of which will be described later, includes PS4. 3- The precursors of the structure include, for example, amorphous Li3PS4, crystalline Li3PS4, and complexes of amorphous Li3PS4 and crystalline Li3PS4 obtained through complexation decomposition, etc. 3- Structure. In addition to these PS4s... 3- Besides the structural component, it may also be a mixture containing unreacted solid electrolyte raw materials (raw materials mainly containing halogen elements) or raw materials containing halogen elements that are mixed in after the complexation process described later. Therefore, in this specification, PS4 will be included. 3- The precursor to the structure is called "PS4" 3- Structures, etc.

[0052] In this case, phosphorus sulfides such as lithium sulfide (Li2S), phosphorus trisulfide (P2S3), and phosphorus pentasulfide (P2S5) are preferably used as raw materials.

[0053] In this case, as long as it can form a PS4 3- Within a certain range of structural ratios, there are no particular restrictions on the mixing ratio of lithium sulfide to phosphorus sulfide, thus enabling efficient formation of PS4. 3- From a structural point of view, when using phosphorus pentasulfide as phosphorus sulfide, the ratio of the molar number of lithium sulfide to the total molar number of lithium sulfide and phosphorus pentasulfide is preferably in the range of 60 to 90%, more preferably in the range of 65 to 85%, further preferably in the range of 70 to 80%, even more preferably in the range of 72 to 78%, and particularly preferably in the range of 73 to 77%.

[0054] Furthermore, in this embodiment, PS4 is easily formed. 3- From the perspective of structure and improved ionic conductivity, it is preferable to use raw materials containing halogen elements in addition to phosphorus sulfides such as lithium sulfide (Li₂S), phosphorus trisulfide (P₂S₃), and phosphorus pentasulfide (P₂S₅). When using raw materials containing halogen elements, in this mixing process, in addition to the raw materials containing lithium, phosphorus, and sulfur such as lithium sulfide and phosphorus sulfide, the raw materials containing halogen elements are preferably lithium halides such as lithium fluoride, lithium chloride, lithium bromide, and lithium iodide, and halogen monomers such as fluorine (F₂), chlorine (Cl₂), bromine (Br₂), and iodine (I₂). Among the lithium halides, lithium chloride, lithium bromide, and lithium iodide are preferred, and lithium chloride and lithium bromide are more preferred. Among the halogen monomers, chlorine (Cl₂), bromine (Br₂), and iodine (I₂) are preferred, and chlorine (Cl₂) and bromine (Br₂) are more preferred.

[0055] When using raw materials containing halogens, the combination of raw materials may preferably include, for example: a combination of lithium sulfide, phosphorus pentasulfide and lithium halide; a combination of lithium sulfide, phosphorus pentasulfide and halogen monomer; a combination of lithium sulfide, phosphorus pentasulfide, lithium halide and halogen monomer, more preferably a combination of lithium sulfide, phosphorus pentasulfide and lithium halide; a combination of lithium sulfide, phosphorus pentasulfide and halogen monomer, and even more preferably a combination of lithium sulfide, phosphorus pentasulfide and lithium halide.

[0056] Furthermore, in this case, lithium chloride, lithium bromide, and lithium iodide are preferred as lithium halides, and lithium chloride and lithium bromide are more preferred as lithium halides. As halogen monomers, chlorine, bromine, and iodine are preferred, and chlorine and bromine are more preferred as halides.

[0057] When using raw materials containing halogen elements, these raw materials can be blended in this mixing process, or they can be blended together from the beginning with materials such as lithium sulfide and phosphorus pentasulfide, or they can be blended after the complexation process described later. In this case, the raw materials containing halogen elements can, for example, be used in this mixing process with lithium sulfide and phosphorus sulfide to synthesize PS4. 3- The structure is then blended.

[0058] The blending ratio of the raw material when using a halogen-containing raw material will be described later.

[0059] (Complexing process)

[0060] The mixing process includes a complexing step in which the aforementioned solid electrolyte raw material and the complexing agent are mixed in a liquid phase. In addition to this complexing step of mixing the electrolyte raw material and the complexing agent in a liquid phase, the mixing process in this embodiment may also include a heating step and a pulverizing step, which are different from the drying step and heating step (crystallization step) described later. Furthermore, in this specification, the complexing agent refers to a substance that can complex with lithium, and is preferably a precursor containing lithium, sulfur, and phosphorus that can react with the lithium-containing sulfide contained in the aforementioned solid electrolyte raw material to promote the formation of a precursor containing lithium, sulfur, and phosphorus. 3- A complexing agent that forms the structure. The complex obtained by complexing with lithium is a complex containing lithium, sulfur, phosphorus, and the complexing agent. Preferably, it is a complex obtained by decomposing the complex to obtain amorphous Li3PS4 or crystalline Li3PS4. PS4 is obtained by removing the complexing agent from the complex (also referred to as "complex decomposition"). 3- Amorphous Li3PS4 and crystalline Li3PS4 in the structure.

[0061] As a complexing agent, any compound possessing the aforementioned properties can be used without particular limitations. In particular, compounds containing heteroelements such as nitrogen, oxygen, and chlorine, which have a high affinity for lithium, are preferred examples. Compounds containing groups containing these heteroelements are even more preferred examples. This is because these heteroelements and the groups containing them can coordinate (bond) with lithium.

[0062] Examples of heteroelements include nitrogen, oxygen, chlorine, and other halogen elements, and examples of complexing agents containing these elements are preferred.

[0063] Specifically, examples include: ester solvents such as ethyl acetate and butyl acetate; aldehyde solvents such as formaldehyde, acetaldehyde, and dimethylformamide; ketone solvents such as acetone and methyl ethyl ketone; ether solvents such as diethyl ether, diisopropyl ether, dibutyl ether, tetrahydrofuran, dimethoxyethane, cyclopentylmethyl ether, tert-butylmethyl ether, and anisole; halogenated aromatic hydrocarbon solvents such as trifluorotoluene, nitrobenzene, chlorobenzene, chlorotoluene, and bromobenzene; amine solvents such as tetramethylethylenediamine, tetraethylethylenediamine, tetramethyldiaminopropane, tetraethyldiaminopropane, cyclopropylenediamine, toluenediamine, and tetraethylenepentamine; nitrile solvents such as acetonitrile, methoxyacetonitrile, propionitrile, methoxypropionitrile, and benzyl nitrile; and solvents containing carbon atoms and heteroatoms such as dimethyl sulfoxide and carbon disulfide.

[0064] Among these, amine solvents, ether solvents, and nitrile solvents are preferred as complexing agents, with ether solvents being more preferred, particularly diethyl ether, diisopropyl ether, dibutyl ether, and tetrahydrofuran, with tetrahydrofuran being more preferred. Furthermore, as complexing agents, those that are insoluble or difficult to dissolve in the solid electrolyte raw material are preferred; from this perspective, amine solvents and ether solvents are preferred. Using such solvents allows the raw material to react in a non-homogeneous manner in a liquid-phase process to obtain the precursor, which is readily obtained as a monomer, thus improving ionic conductivity.

[0065] In addition to the complexing agents mentioned above, various solvents can also be used, such as: aliphatic hydrocarbon solvents such as hexane, pentane, 2-ethylhexane, heptane, octane, decane, undecane, dodecane, and tridecane; alicyclic hydrocarbon solvents such as cyclohexane and methylcyclohexane; aromatic hydrocarbon solvents such as benzene, toluene, xylene, mesitylene, ethylbenzene, and tert-butylbenzene; oligomers obtained by polymerizing at least one of n-paraffinic hydrocarbons such as n-butene and n-propylene with a degree of polymerization of about 3 to 10, and their hydrides, i.e., n-paraffinic hydrocarbon solvents; oligomers obtained by polymerizing at least one of paraffinic hydrocarbons such as isobutene, n-butene, n-propylene, and isopropylene with a degree of polymerization of about 3 to 10, and their hydrides, i.e., isoparaffinic hydrocarbon solvents, etc.

[0066] When a solid electrolyte raw material and a complexing agent are mixed in a liquid phase, the amount of the complexing agent relative to the solid electrolyte raw material is such that the content of the solid electrolyte raw material in the liquid phase is preferably 1 to 50% by mass, more preferably 2 to 30% by mass, further preferably 3 to 20% by mass, and even more preferably 5 to 15% by mass.

[0067] Precursors containing lithium, sulfur, and phosphorus, preferably containing PS4 3- The precursor to the structure (PS4) 3-The structure, etc., can be synthesized by mixing the above-mentioned solid electrolyte raw materials and complexing agents. In addition to mixing, it can also be synthesized by, for example, crushing, kneading, or a combination of these processes. Mixing, crushing, kneading, etc., are events that can occur simultaneously, so it is sometimes difficult to distinguish them clearly. This is because if solid or powdered raw materials, which are examples of raw materials that can be included in the above-mentioned solid electrolyte raw materials, are mixed, kneading may sometimes occur. At the same time, the solid electrolyte raw materials may collide with each other and crush or knead each other. In addition, crushing itself may also serve as mixing or kneading. The synthesis of the precursor in this mixing process is carried out by applying forces such as rotation and vibration to the various raw materials contained in the solid electrolyte raw materials, thereby repeatedly contacting the raw materials with each other. This contact only needs to include at least the mixing process, and may also be accompanied by other processes such as crushing, kneading, etc. In addition, the above-mentioned processing in the complexing process is used to obtain PS4 containing a complex containing lithium, sulfur, phosphorus and the complexing agent. 3- The precursor of the structure is processed in a complexation process as a form of mixing, and is different from the pulverization process that pulverizes the precursor obtained through the complexation process described later.

[0068] In this embodiment, the processes of mixing, crushing, kneading, or combining them can be carried out, for example, by a mechanically stirred mixer equipped with stirring blades in a tank.

[0069] Examples of mechanical mixing machines include high-speed mixing machines and twin-arm mixing machines. From the viewpoint of promoting more uniform contact and reaction among the various raw materials contained in the raw material composition, resulting in higher ionic conductivity, high-speed mixing machines are preferred. In addition, examples of high-speed mixing machines include vertical axis rotary mixers and horizontal axis rotary mixers, or any type of mixer can be used.

[0070] Examples of the shapes of stirring blades used in mechanical mixing mixers include blade type, arm type, belt type, multi-stage blade type, double-arm type, bucket type, biaxial blade type, flat blade type, and C-type blade type. From the viewpoint of promoting more uniform contact between the various raw materials contained in the raw material contents and achieving higher ionic conductivity, bucket type, flat blade type, and C-type blade type are preferred.

[0071] In addition, the above-mentioned processing can also be carried out using a media pulverizer, for example.

[0072] Media mills are broadly classified into container-driven mills and media-stirring mills. Container-driven mills include, for example, stirring tanks, grinding tanks, or combinations thereof, such as ball mills and bead mills. Ball mills and bead mills can be of various types, including rotary, rolling, vibrating, and planetary types.

[0073] Examples of media-stirred pulverizers include: impact pulverizers such as shredders, hammer mills, and needle mills; tower pulverizers such as tower mills; trough pulverizers such as grinding mills, wet sand mills (aquamizers), and sand mills; flow-through trough pulverizers such as adhesive mills and coarse crushers; flow-through tube pulverizers; annular pulverizers such as combined ball mills; continuous dynamic pulverizers; and various other pulverizers.

[0074] In addition, it can also be done using single-axis or multi-axis kneaders, for example.

[0075] In the complexation process, to more effectively synthesize components containing PS4 3- The precursor to the structure (PS4) 3- From the viewpoint that complexes containing lithium, sulfur, phosphorus, and the aforementioned complexing agent are preferred, and that amorphous Li3PS4 and crystalline Li3PS4 complexes are preferably obtained through the aforementioned complexation decomposition, a process using a mechanically stirred mixer is preferred. This is also preferred from the viewpoint of manufacturing efficiency. On the other hand, from the same viewpoint, in the complexation process, it is preferable to avoid using media mills such as ball mills, bead mills, and media stirring mills, which are commonly referred to as pulverizers, or kneaders.

[0076] There are no particular limitations on the temperature during the synthesis of the aforementioned precursors in the complexation process; for example, it can be adjusted within the range of 20 to 100°C. It can be around room temperature (23°C), or it can be heated to accelerate the synthesis reaction in a short time. A higher temperature is preferred as long as it is under conditions that do not dry out, such as reflux. For example, it can be set to 50 to 90°C, more preferably around 80°C.

[0077] Furthermore, the synthesis time can be set to approximately 0.5 to 100 hours, but considering manufacturing efficiency, it is preferable to set it to 1 to 90 hours, and more preferably 3 to 75 hours.

[0078] The substance obtained by the above synthesis can be said to be a precursor containing lithium, sulfur and phosphorus, that is, a complex containing lithium, sulfur, phosphorus and the above complexing agent. Preferably, it is a complex of amorphous Li3PS4 and crystalline Li3PS4 obtained by the above complexation decomposition.

[0079] (Drying process)

[0080] In the mixing process, in order to remove the complexing agent and solvent mentioned above, the manufacturing method of this embodiment may also include a drying process (also referred to as the "drying process"). In the mixing process, if a slurry containing a complex of amorphous and crystalline Li3PS4 is obtained as described above, the complexing agent and solvent can be removed from the slurry by drying in the drying process to obtain complex crystals.

[0081] By removing the complexing agent and solvent, impurities are reduced, and an increase in ionic conductivity can be expected. On the other hand, when the complexation process described above is carried out in the liquid phase, the resulting substance is a slurry containing the precursor. If this slurry is dried, it is prone to forming aggregates. If these aggregates are subjected to heating as required (described later), they become larger calcined bodies, thus making it impossible to obtain a solid electrolyte with a small particle size. In such cases, from the viewpoint of manufacturing efficiency of solid electrolytes, it is preferable not to include a drying process in the mixing process when the pulverization or heating process described later is involved.

[0082] Therefore, the decision on whether or not a drying process is necessary can be made by considering factors such as the desired solid electrolyte and the raw materials used, as there are both advantages and disadvantages.

[0083] The drying of the precursors accompanying the complexing agent and solvent can be carried out at a temperature corresponding to the type of residual complexing agent and solvent, for example, at a temperature above the boiling point of the residual complexing agent and solvent. The drying temperature is typically set to 5–100°C, preferably 10–90°C, and more preferably 20–85°C. In addition, vacuum drying (vacuum drying) can also be carried out using a vacuum pump or the like.

[0084] There is no particular limitation on the drying time, but it is preferably 1 minute or more, more preferably 10 minutes or more, further preferably 30 minutes or more, and even more preferably 1 hour or more. Furthermore, there is no particular limitation on the upper limit of the drying time, but it is preferably 24 hours or less, more preferably 12 hours or less, further preferably 6 hours or less, and even more preferably 3 hours or less.

[0085] Alternatively, the drying of the precursors accompanying the complexing agent and solvent can be performed by filtration using a glass filter, solid-liquid separation by decantation, or solid-liquid separation using a centrifuge. In this embodiment, drying based on the aforementioned temperature conditions can also be performed after solid-liquid separation.

[0086] Specifically, in solid-liquid separation, it is relatively easy to transfer the precursor, which is accompanied by a complexing agent and solvent, into a container, and after the precursor precipitates, remove the solvent to become the supernatant by decantation or by filtration using, for example, a glass filter with a pore size of about 10 to 200 μm, preferably 20 to 150 μm.

[0087] (heating)

[0088] In addition to the heating process (crystallization process) described later, the precursor obtained by the above mixing process can also be heated during the mixing process. For example, to prepare a precursor containing amorphous or crystalline Li3PS4 as PS4. 3- Heating is effective for the structure. For example, after removing the complexing agent and solvent from a slurry containing a complex that yields both amorphous and crystalline Li3PS4 through the complexing and drying processes described above, and obtaining a complex crystal, the complex crystal can be heated to remove (decompose) the complexing agent, yielding amorphous Li3PS4. Alternatively, after obtaining a complex crystal or amorphous Li3PS4, heating can be performed while adjusting the heating temperature to obtain crystalline Li3PS4. Thus, in the manufacturing method of this embodiment, the heating in the mixing process (not the heating process (crystallization process) described later) can include a complex decomposition process to remove the complexing agent from the complex crystal to obtain amorphous Li3PS4, and a process to heat the complex crystal or amorphous Li3PS4 to obtain crystalline Li3PS4. That is, in the manufacturing method of this embodiment, the mixing process can preferably include a complex decomposition process and a process to obtain crystalline Li3PS4 as the heating process.

[0089] Typically, heating solid electrolytes can sometimes cause them to expand and enlarge in size. In this embodiment, the aforementioned precursor (PS4) is generated prior to the pulverization process described later. 3- (Structure, etc.), thereby enabling the obtained solid electrolyte to have a smaller particle size, thus simultaneously achieving particle size reduction and ionic conductivity improvement.

[0090] The heating process temperature in the mixing step only needs to be able to achieve the desired temperature for PS4. 3- The precursor to the structure (PS4) 3- There are no particular limitations on the temperature of the structure, etc. For example, it is preferred to be above 140°C, more preferably above 145°C, further preferably above 150°C, and even more preferably above 170°C. There is no particular upper limit, but it is preferred to be below 300°C, more preferably below 275°C, further preferably below 225°C, and even more preferably below 200°C. As long as it is within the above temperature range, it is possible to manufacture components including the PS4 more efficiently. 3- The precursor to the structure (PS4) 3- (Structures, etc.), and mainly crystalline Li3PS4 can be obtained.

[0091] Furthermore, when the main goal is to obtain amorphous Li3PS4, the upper limit can be set to below 150°C, preferably below 140°C, and more preferably below 135°C. The lower limit is not particularly limited and can be set to around 100°C or above, preferably above 105°C.

[0092] The heating process in the mixing step only needs to be sufficient to obtain PS4. 3- The precursor to the structure (PS4) 3- There are no particular restrictions on the heating time (such as for structures), but it is preferred to be 10 minutes or more, more preferably 30 minutes or more, further preferably 1 hour or more, and even more preferably 4 hours or more. In addition, there are no particular restrictions on the upper limit of the heating time, but it is preferred to be 24 hours or less, more preferably 18 hours or less, further preferably 12 hours or less, and even more preferably 10 hours or less.

[0093] Heating during the mixing process can be carried out in an inert gas atmosphere (e.g., nitrogen or argon) or under a reduced pressure atmosphere (especially in a vacuum). This is to prevent the degradation (e.g., oxidation) of the precursors obtained through the above synthesis and mixing.

[0094] Furthermore, there are no particular limitations on the heating method; for example, methods such as using heating plates, autoclaves, vacuum heating devices, argon atmosphere furnaces, and firing furnaces can be used. In addition, in industrial applications, horizontal dryers and horizontal vibrating flow dryers with heating units and feeding mechanisms can also be used, depending on the processing capacity.

[0095] Thus, the product containing PS4 obtained through any of the following steps: complexation, drying, and heating (which may include a complexation decomposition step to obtain crystalline Li3PS4). 3- The precursor to the structure (PS4) 3- (structures, etc.), specifically including PS4 3- The structure of the structure (PS4) 3- The material of the structure, as PS4 3- The structure can be representatively exemplified by complexes of amorphous and crystalline Li3PS4 obtained through complexation decomposition, amorphous Li3PS4, crystalline Li3PS4 (β-Li3PS4), etc. Furthermore, in the presence of PS4... 3- These PS4s exist in the precursor of the structure. 3- There are cases where a structure is contained in a single type, and there are also cases where multiple types coexist and are contained within each other.

[0096] In this embodiment, a PS4 is first formed. 3-The structure is supplied to subsequent processes, thereby obtaining a solid electrolyte with small particle size and high ionic conductivity.

[0097] The complexes of amorphous and crystalline Li3PS4 are obtained through complexation decomposition and are prepared as a slurry containing a complexing agent, solvent, etc. The complexing agent and solvent are removed from the slurry by drying, resulting in a complex crystal. By heating the complex crystal (not the heating process (crystallization process)), the complexing agent can be removed from the complex crystal (complexation decomposition), yielding amorphous Li3PS4. Furthermore, during this heating, crystalline Li3PS4 can be obtained directly from the complex crystal or obtained through amorphous Li3PS4. In the manufacturing method of this embodiment, the aforementioned Li3PS4 containing PS4 is finally processed through the heating process (crystallization process) described later. 3- The precursor to the structure (PS4) 3- (Structures, etc.) crystallize to obtain a crystalline solid electrolyte containing lithium, sulfur, phosphorus and halogen elements.

[0098] Therefore, the manufacturing method of this embodiment is preferably one or more of the following steps after the complexation step: a drying step to obtain a complex crystal, a complexation decomposition step to remove the complexing agent contained in the complex crystal to obtain the amorphous Li3PS4, and a step to heat at least one of the complex crystal and the amorphous Li3PS4 to obtain crystalline Li3PS4.

[0099] The precursor includes PS4 3- Structures can be built through solids 31 Observation was performed using P-NMR measurements.

[0100] The preferred product obtained in this mixing process contains PS4 3- The precursor of the structure exhibits characteristics of PS4 3- Peaks generated by the structure. From the viewpoint of ionic conductivity, a crystal structure composed of phosphorus and sulfur is preferably free of PS4. 3- Structures other than the structure, such as P2S7 4- Structure, P2S6 4- Structure (P) x S y a- Crystal structures such as PS4 are readily obtained using the above synthesis method. 3- The precursor to a structure.

[0101] The precursor obtained in this mixing process is preferably pre-formed with PS4 3-The main framework of the structure is supplied to various processes such as the crushing process and the heating process (crystallization process) described later. This is because it is easy to obtain solid electrolytes with smaller particle sizes by suppressing the increase in particle size.

[0102] In the manufacturing method of this embodiment, a PS4 is pre-formed. 3- The main framework of the structure was thus created to include the PS4. 3- The precursor to the structure (PS4) 3- In a crystallization process involving heating the precursor (such as structural components) in a solvent, the PS4 contained in the precursor is simultaneously crystallized. 3- The reaction of the structure with raw materials containing halogens yields a crystalline solid electrolyte containing lithium, sulfur, phosphorus, and halogens.

[0103] (The blending of raw materials containing halogen elements)

[0104] As described above, in this embodiment, a raw material containing a halogen element can be used. In this case, the raw material containing the halogen element can be blended in the complexation step of the mixing process, or blended after the complexation step. Blending after the complexation step means that after obtaining the precursor obtained through the complexation step, i.e., the aforementioned raw material containing PS4... 3- Precursor blending of the structure specifically includes blending after the complexation process and before the pulverization process, or blending during the pulverization process. When a raw material containing a halogen element is blended during the complexation process, PS4 can be obtained in that complexation process. 3- A precursor to a mixture of a structural component and a raw material containing a halogen element. Furthermore, if a raw material containing a halogen element is incorporated after this complexation step, i.e., during the synthesis of PS4... 3- After the structure is formed, the raw material containing halogen elements is mixed in the same way as the complexation process described above, or it is pulverized in a pulverization process, thereby obtaining a product containing PS4. 3- A precursor to a mixture of structures, raw materials containing halogen elements, etc.

[0105] In the manufacturing method of this embodiment, the raw material containing halogen elements can be added together with other solid electrolyte raw materials to perform the complexation process described above, or it can be added after the complexation process, but this will result in a more reliable formation of PS4. 3- From the viewpoint of improving the structure, achieving higher ionic conductivity, and more reliably reducing particle size, it is preferable to blend raw materials containing halogen elements after the complexation process, and more preferably to blend raw materials containing halogen elements after the complexation process and before the pulverization process.

[0106] Furthermore, raw materials containing lithium sulfide can be further blended during or before the pulverization process, similarly to raw materials containing halogen elements. Lithium sulfide is a preferred raw material used in the aforementioned complexation process, for example, in the case of raw materials containing PS4 obtained through the pulverization process. 3- The amount of lithium sulfide required in the manufacture of the precursor of the structure differs from the amount of lithium sulfide required in the crystalline solid electrolyte obtained by the manufacturing method of this embodiment. When compensating for the deficiency of lithium sulfide used in the complexation process relative to the amount required for the manufacture of the desired crystalline solid electrolyte, it is effective to incorporate raw materials containing lithium sulfide.

[0107] In this pulverizing process, the raw materials containing halogen elements and the raw materials containing lithium sulfide are pulverized and dispersed together with the precursor obtained in the complexing process to form a precursor.

[0108] Therefore, in this embodiment, it is sufficient to achieve the desired mixing ratio of various elements contained in the crystalline solid electrolyte at the time point between the pulverization process and the crystallization process.

[0109] In this embodiment, the blending ratios of various raw materials used in the solid electrolyte raw material can be appropriately determined according to the desired crystal structure. As an example, the blending ratios of various raw materials in a crystalline solid electrolyte having a sulforaphite-germanium-type crystal structure, which is one of the preferred crystalline solid electrolytes obtained by the manufacturing method of this embodiment, will be described below. Furthermore, crystalline solid electrolytes having a sulforaphite-germanium-type crystal structure will be described later.

[0110] For example, when the crystalline Li3PS4 (β-Li3PS4) obtained in the complexation process is blended with lithium sulfide and lithium halide, the molar ratio of these raw materials (Li3PS4:Li2S:lithium halide) is preferably 15-55:3-25:20-80, more preferably 20-45:5-20:30-70, even more preferably 25-40:8-18:40-60, and even more preferably 30-35:10-15:50-55.

[0111] Furthermore, for example, when lithium sulfide, phosphorus pentasulfide, and lithium halide are mixed in the complexation process, the molar ratio of these raw materials (Li2S:P2S5:lithium halide) is preferably 15-75:3-25:10-70, more preferably 25-65:5-20:20-60, even more preferably 35-55:8-18:30-50, and even more preferably 45-50:10-15:35-45.

[0112] Furthermore, when lithium chloride and lithium bromide are used together as lithium halides, the molar ratio of lithium bromide to the total molar ratio of lithium chloride and lithium bromide is preferably 1 to 70%, more preferably 10 to 60%, even more preferably 20 to 50%, and even more preferably 30 to 40%.

[0113] (Grinding process)

[0114] The mixing step in the manufacturing method of this embodiment preferably includes a pulverizing step. The substance obtained by pulverizing the complexing step described above is a precursor containing lithium, sulfur, and phosphorus elements, and preferably contains PS4. 3- Precursor of the structure (PS4) 3- (Structures, etc.). By heating the pulverized material obtained from this pulverizing process in the heating process (crystallization process) described later, the diffusion distance of each element in the particles can be shortened. Therefore, even with a lower heating temperature, it is easy to obtain the desired crystalline solid electrolyte (therefore, the "heating process" can also be called the "crystallization process"). Therefore, in the manufacturing method of this embodiment, in the above-mentioned mixing process, after the complexation process, the material is pulverized by this pulverizing process and then heated by the heating process (crystallization process), thereby efficiently obtaining a solid electrolyte with a small particle size and high ionic conductivity. In addition, in this embodiment, the pulverizing process is usually performed after the complexation process. However, since it can be performed by the same process as mechanical grinding, although there may be cases where the processing conditions need to be adjusted, the complexation process and the pulverizing process can be performed simultaneously, that is, the pulverizing process can be omitted.

[0115] As described above, the product containing PS4 is obtained by a drying process and heating after a mixing process (complexing process) or a complexing process. 3- Precursor of the structure (PS4) 3- The structure (etc.) includes amorphous Li3PS4, crystalline Li3PS4 (β-Li3PS4), and complexes of the amorphous and crystalline Li3PS4 obtained through complexation decomposition, etc. 3- Structure. If crystalline Li3PS4 is supplied to the pulverization process, it can be amorphized to become amorphous Li3PS4. Therefore, when the precursor contains amorphous Li3PS4, the amorphous Li3PS4 contained in the precursor is either amorphized amorphous Li3PS4 through heating of the complex or amorphized amorphous Li3PS4 through pulverization of crystalline Li3PS4.

[0116] The grinding process can be carried out using any known method and is not particularly limited. However, from the viewpoint of more efficient grinding, mechanical grinding is preferred. Furthermore, by employing mechanical grinding, when raw materials containing halogen elements are mixed in after the complexation process, or when raw materials containing lithium sulfide are mixed in during or before the grinding process, the reaction of these raw materials is promoted, making it easier to obtain a solid electrolyte with high ionic conductivity.

[0117] Mechanical grinding is an example of a method that uses a media mill as a precursor to the above-mentioned mixing process. Media mills are generally classified into container-driven mills and media-stirring mills, with container-driven mills such as ball mills and bead mills being preferred. Various forms of ball mills and bead mills can be used, including rotary, rolling, vibrating, and planetary types.

[0118] In this pulverization process, pulverization can be carried out in the liquid phase. Pulverization in the liquid phase can sometimes be accelerated. Therefore, in the manufacturing method of this embodiment, the pulverization process can be carried out directly without removing the complexing agent and solvent used in the above-mentioned mixing process, or the complexing agent and solvent can be removed after the above-mentioned mixing process is completed, and then a new solvent can be added to carry out pulverization in the liquid phase.

[0119] As the solvent used in this pulverization process, for example, solvents exemplified as complexing agents and solvents that can be used in the synthesis of precursors in the complexation process described above can be used. Preferred solvents are aromatic solvents, ether solvents, and nitrile solvents, more preferably aromatic solvents and nitrile solvents, further preferably toluene, xylene, ethylbenzene, tert-butylbenzene, and isobutyronitrile, and even more preferably toluene and isobutyronitrile.

[0120] Furthermore, the amount of solvent used relative to the solid electrolyte raw material in this case is the same as the amount of complexing agent used in the complexing process described above.

[0121] The average particle size (D) of the pulverized material obtained in this pulverizing process 50 The average particle size is preferably 0.01 μm to 100 μm, more preferably 0.03 μm to 50 μm, even more preferably 0.05 μm to 10 μm, and even more preferably 0.1 μm to 3 μm. When the average particle size of the pulverized material is set within the above range, the diffusion distance of each element in the particles is shortened during heating in the heating process (crystallization process). Therefore, even with a lower heating temperature, the desired crystalline solid electrolyte can be easily obtained. Furthermore, since a lower heating temperature can be achieved, the progression of grain growth can be suppressed, maintaining a smaller particle size. As a result, crystalline solid electrolytes with smaller particle sizes can be obtained more efficiently.

[0122] In this embodiment, by adjusting the pulverization processing conditions, the average particle size of the pulverized material can be set within the aforementioned range. For example, in the case of mechanical grinding using a media pulverizer during the pulverization process, the particle size, shape, and amount of zirconia balls, zirconia beads, etc., used in the pulverizer, as well as the operating conditions (speed, etc.) of the pulverizer, can be adjusted. Furthermore, in the case of pulverization in the liquid phase, the amount of solvent relative to the precursor can be adjusted.

[0123] [Heating process (crystallization process)]

[0124] The method for manufacturing a crystalline solid electrolyte according to this embodiment includes a heating step ("crystallization step"), in which a precursor containing lithium, sulfur, and lithium elements is heated in a solvent using a pressure vessel or during reflux. As described above, the precursor containing lithium, sulfur, and lithium elements preferably contains PS4. 3- The precursor of the structure. In addition, as mentioned above, the precursor containing lithium, sulfur and phosphorus is preferably a pulverized material that has undergone the above-described pulverization process.

[0125] In the manufacturing method of this embodiment, a heating process (crystallization process) is performed using a precursor containing lithium, sulfur, and phosphorus, preferably containing PS4. 3- The precursor to the structure (PS4) 3- PS4 included in structures, etc. 3- The reaction between the structure and a raw material containing halogen elements introduces halogen elements into the PS4. 3- The structure is crystallized to obtain a crystalline solid electrolyte containing lithium, sulfur, phosphorus, and halogen elements.

[0126] By heating the pulverized material obtained in the mixing process, preferably the pulverizing process, through a heating process (crystallization process), the diffusion distance of each element in the particles is shortened. Therefore, even if the heating temperature is set to a lower temperature, the desired crystalline solid electrolyte can be easily obtained. Thus, the "heating process" can also be called the "crystallization process." In the manufacturing method of this embodiment, by employing a heating process (crystallization process), the solid electrolyte is crystallized using a pressure vessel or by heating in a solvent during reflux, thereby promoting the crystallization of the solid electrolyte and suppressing the increase in particle size.

[0127] On the other hand, if a crystalline solid electrolyte with a desired crystal structure is manufactured in this heating step (crystallization step), and then a pulverization step is performed, the crystal structure may be damaged, resulting in a decrease in ionic conductivity. From this viewpoint, in the manufacturing method of this embodiment, it is preferable that there is no pulverization step after the heating step (crystallization step).

[0128] As for the method of heating the precursor obtained in the mixing process, preferably the pulverized material obtained in the pulverizing process, there are no particular limitations as long as a pressure vessel is used or the process is carried out simultaneously with reflux; any method can be adopted. For example, among the methods described for heating the precursor in the above-mentioned mixing process, methods using pressure vessels such as autoclaves, argon atmosphere furnaces, firing furnaces, or vacuum heating devices that can be heated under negative pressure (vacuum) can be adopted, or methods using industrially available horizontal dryers, horizontal vibrating flow dryers, etc., can be adopted. Among these, from the viewpoint of suppressing particle size increase in the heating process (crystallization process), an autoclave is preferred. Furthermore, as for the method of carrying out reflux simultaneously, examples can be given of reflux methods using small devices such as Demroth condensers and Liebig condensers, to medium to large industrial reflux cooling devices, depending on the scale.

[0129] The heating temperature in the heating process (crystallization process) can be adjusted appropriately according to the desired solid electrolyte. For example, in the case of manufacturing a solid electrolyte with a sulforaphane-germanium crystal structure, it is preferably 200°C to 425°C, more preferably 225°C to 340°C, even more preferably 275°C to 385°C, and even more preferably 325°C to 370°C. Until now, high temperatures such as 550°C and 600–800°C are required in the manufacture of solid electrolytes with a sulforaphane-germanium crystal structure, but according to the manufacturing method of this embodiment, a low temperature can be set as described above. From the viewpoint of such effect, the manufacturing method of this embodiment is suitable for manufacturing solid electrolytes with a sulforaphane-germanium crystal structure.

[0130] The heating time in the heating process (crystallization process) can be adjusted appropriately according to the desired solid electrolyte. For example, it is preferably more than 1 minute, more preferably more than 10 minutes, further preferably more than 30 minutes, and even more preferably more than 1 hour. In addition, there is no particular upper limit to the heating time, but it is preferably less than 24 hours, more preferably less than 10 hours, further preferably less than 5 hours, and even more preferably less than 3 hours.

[0131] Furthermore, heating can be carried out in an inert gas atmosphere (e.g., nitrogen atmosphere, argon atmosphere) or in a reduced pressure atmosphere (especially in a vacuum). This prevents the degradation (e.g., oxidation) of the resulting solid electrolyte.

[0132] During the heating process (crystallization process), it is not preferable to pre-dry or to dry simultaneously with crystallization. This is because the average particle size may increase during drying, and in the manufacturing method of this embodiment, it is preferable to avoid drying as much as possible.

[0133] During the heating process (crystallization process), the complexing agent and solvent used in the mixing and pulverizing processes can be used without removing them. Instead, the precursors containing the complexing agent and solvent obtained in these processes can be directly heated. Alternatively, the complexing agent and solvent accompanying the precursors can be replaced with a high-boiling-point solvent beforehand. In this case, solvents described as those that can be used in the mixing process can be used. Preferably, a solvent with a boiling point higher than that of the complexing agent and solvent used in the complexing process is used. Among these, paraffinic solvents, such as n-paraffinic hydrocarbon solvents and isoparaffinic hydrocarbon solvents, which are commonly used as high-boiling-point solvents, are preferred. Similarly, the solvent used in the heating process (crystallization process) is preferably a solvent that does not dissolve or is difficult to solvent the precursors. From this point of view, paraffinic solvents are also preferred. The crystalline solid electrolyte obtained through the heating process (crystallization process) is less likely to contain impurities such as solvents, and a high-quality (high ionic conductivity) crystalline solid electrolyte is easily obtained.

[0134] Furthermore, the above-mentioned drying can be performed when solvent replacement is carried out.

[0135] (Crystal structure of solid electrolytes)

[0136] Examples of solid electrolytes obtained by the manufacturing method of this embodiment include Li6PS5X and Li 7- x PS 6-x X x (X = Cl, Br, I, x = 0.0–1.8) and other silver-germanium sulfide crystal structures (Japanese Patent Application Publication No. 2011-096630, Japanese Patent Application Publication No. 2013-211171, etc.). The diffraction peaks of these silver-germanium sulfide crystal structures appear, for example, near 2θ = 15.3°, 17.7°, 31.1°, 44.9°, and 47.7°.

[0137] In addition, the following crystal structures can be cited as examples of sulfosilver germanite crystal structures.

[0138] The aforementioned Li 7-x P 1- y Si y S6 and Li 7+x P 1-y Si y S6 (where x is -0.6 to 0.6, y is 0.1 to 0.6) has a cubic crystal or orthorhombic crystal structure, preferably a cubic crystal structure, and in X-ray diffraction measurement using CuKα rays, it mainly has peaks at positions 2θ = 15.5°, 18.0°, 25.0°, 30.0°, 31.4°, 45.3°, 47.0°, and 52.0°.

[0139] The aforementioned Li 7-x-2y PS 6-x-y Cl x The crystal structure represented by (0.8≤x≤1.7, 0<y≤-0.25x+0.5) is preferably a cubic crystal, and in X-ray diffraction measurement using CuKα rays, it mainly has peaks at positions 2θ = 15.5°, 18.0°, 25.0°, 30.0°, 31.4°, 45.3°, 47.0°, and 52.0°.

[0140] The aforementioned Li 7-x PS 6-x Ha x The crystal structure represented by (Ha is Cl or Br, x is preferably 0.2 to 1.8) is preferably a cubic crystal, and in X-ray diffraction measurement using CuKα rays, it mainly has peaks at positions 2θ = 15.5°, 18.0°, 25.0°, 30.0°, 31.4°, 45.3°, 47.0°, and 52.0°.

[0141] In addition, these peak positions can shift within a range of ±0.5°.

[0142] From the viewpoint of obtaining higher ionic conductivity, the crystal structure of the solid electrolyte obtained by the production method of this embodiment is preferably an argyrodite-type crystal structure. Furthermore, from the viewpoint of the effect of being able to set the heating temperature in step 3 to a low temperature, the production method of this embodiment is suitable for producing a solid electrolyte having an argyrodite-type crystal structure.

[0143] The solid electrolyte obtained by the manufacturing method of this embodiment can be a solid electrolyte having the above-described silver-germanium sulfide crystal structure, or it can have a silver-germanium sulfide crystal structure as the host crystal. From the viewpoint of obtaining higher ionic conductivity, it is preferable to have a silver-germanium sulfide crystal structure as the host crystal. In this specification, "having as the host crystal" means that the proportion of the crystal structure to be targeted in the crystal structure is 80% or more, preferably 90% or more, and more preferably 95% or more.

[0144] Furthermore, from the viewpoint of obtaining higher ionic conductivity, the crystalline solid electrolyte obtained by the manufacturing method of this embodiment is preferably a crystalline solid electrolyte that does not contain crystalline Li3PS4 (β-Li3PS4). Whether or not crystalline Li3PS4 (β-Li3PS4) is present can be confirmed by the presence or absence of diffraction peaks at 2θ = 17.5° and 26.1° observed in crystalline Li3PS4. In this specification, if such diffraction peaks are not present, or even if such diffraction peaks are present but only to the extent that they are extremely small compared to the diffraction peaks of the argyrophthalite-type crystal structure, then it is defined as a crystalline solid electrolyte that does not contain crystalline Li3PS4 (β-Li3PS4).

[0145] The shape of the solid electrolyte obtained by the manufacturing method of this embodiment is not particularly limited; for example, a particulate shape can be cited. The average particle size (D) of the particulate solid electrolyte... 50 Preferably, the micrometer is 0.01 μm or more and 100 μm or less, more preferably 0.03 μm or more and 50 μm or less, even more preferably 0.05 μm or more and 10 μm or less, and even more preferably 0.1 μm or more and 3 μm or less.

[0146] Example

[0147] The invention will now be described in detail by way of examples, but the invention is not limited to these examples.

[0148] (Example 1)

[0149] In a reaction vessel equipped with stirring blades, lithium sulfide and phosphorus pentasulfide were weighed and added under a nitrogen atmosphere to achieve a molar ratio of 75:25. While cooling with methanol / liquid nitrogen, the stirring blades were operated, and then dehydrated tetrahydrofuran (dehydrated THF), also pre-cooled to -20°C with methanol / liquid nitrogen, was added using a Teflon tube to achieve a total feedstock concentration of 10% by mass. The mixture was then stirred at room temperature (23°C) for 72 hours. Next, the tetrahydrofuran was removed using a canula, followed by the addition of dehydrated THF to achieve a total feedstock concentration of 10% by mass, followed by stirring for 30 minutes and then removal. This process was repeated at least three times to obtain a product containing PS4.3- The 3THF adduct (complex) of the structure Li3PS4.

[0150] Next, the PS4 was subjected to a temperature of 80°C. 3- The 3THF adduct of Li3PS4 with the PS4 structure was subjected to vacuum drying for 2 hours, followed by heat treatment at 180°C for 8 hours to obtain the PS4-like compound. 3- The structure of crystalline Li3PS4 (β-Li3PS4) was confirmed by powder X-ray diffraction (XRD) measurements using an X-ray diffraction (XRD) apparatus (SmartLab apparatus, manufactured by Rigaku Corporation), which showed diffraction peaks at 17.5° and 26.1°.

[0151] The obtained PS4 3- In the crystalline Li3PS4 (β-Li3PS4) structure, based on the above-mentioned molar ratio of lithium sulfide to phosphorus pentasulfide of 75:25, Li2S, LiCl, and LiBr were weighed and added in molar ratios of 40, 100, and 60, respectively, to bring the total amount of these to 10% by mass. Dehydrated toluene was then added, followed by isobutyronitrile. The mixture was then pulverized for 1 hour using a bead mill ("Lab Star Mini LMZ015 (model)", manufactured by Ashizawa Finetech Co., Ltd.) to obtain a slurry containing the pulverized precursors. Furthermore, in this pulverization process, zirconia beads with a diameter of 0.5 mm were added to bring the total amount of the above-mentioned precursors to 80% by volume.

[0152] The particle size distribution of the pulverized material after grinding was measured, and the average particle size (D) was obtained. 50 The value is 0.2 μm.

[0153] Next, an isoparaffinic hydrocarbon solvent ("IP2830 (trade name)", manufactured by Idemitsu Kosan Co., Ltd.) was added to the slurry-like pulverized material, and the material was dried under reduced pressure at 100°C for 6 hours to replace the solvent with a high-boiling-point solvent (isoparaffinic hydrocarbon solvent). The pulverized material was then heated in the solvent at 340°C for 2 hours using an autoclave.

[0154] Subsequently, the solvent was removed using a sleeve, and dehydrated toluene was added and stirred. High-boiling-point solvents (isomeric paraffinic hydrocarbon solvents) were removed by decantation, followed by drying at 100°C for 2 hours to obtain a solid electrolyte with a sulforaphite-germanium-type crystal structure. Powder X-ray diffraction (XRD) measurements confirmed the solid electrolyte's sulforaphite-germanium-type crystal structure by showing diffraction peaks at 15.3°, 17.7°, 31.1°, 44.9°, and 47.7°.

[0155] The average particle size (D) of the obtained solid electrolyte 50 The particle size was measured to be 0.3 μm, and the ionic conductivity was measured to be 3.3 mS / cm, confirming that the particle size is small and has high ionic conductivity.

[0156] In addition, in this embodiment, the ionic conductivity is measured as described below.

[0157] The obtained crystalline solid electrolyte was shaped into a piece with a diameter of 10 mm (cross-sectional area S: 0.785 cm²). 2 A sample was prepared from spherical particles with a height (L) of 0.1–0.3 cm. The top and bottom of the sample were used as electrode terminals, and measurements were taken at 25°C using AC impedance spectroscopy (frequency range: 5 MHz–0.5 Hz, amplitude: 10 mV) to obtain a Cole-Cole diagram. Near the right end of the arc observed in the high-frequency region, the real part Z'(Ω) at the point where -Z"(Ω) is minimum was taken as the volume resistance R(Ω) of the electrolyte, and the ionic conductivity σ(S / cm) was calculated according to the following formula.

[0158] R = ρ(L / S)

[0159] σ=1 / ρ

[0160] exist Figure 1 The X-ray diffraction spectra of the precursor and solid electrolyte obtained in Example 1 are shown by powder X-ray diffraction (XRD) measurement.

[0161] (Comparative Example 1)

[0162] The slurry-like powder obtained in Example 1 was subjected to reduced pressure drying to remove the solvent, thereby obtaining a mixed powder. Subsequently, it was heated in an electric furnace (“F-1404-A (model)”, manufactured by Tokyo Glass Equipment Co., Ltd.) inside a glove box under a nitrogen atmosphere. Specifically, an Al2O3 crucible (“999-60S (model)”, manufactured by Tokyo Glass Equipment Co., Ltd.) was placed inside the electric furnace and kept at 340°C for at least 1 hour. Afterward, the furnace door was opened, 1g of the mixed powder was quickly poured into the crucible, and the door was immediately closed, and heating was carried out for 10 minutes. The crucible was then removed from the furnace and slowly cooled to obtain a solid electrolyte with a sulforaphite-germanium type crystal structure.

[0163] The average particle size (D) of the obtained solid electrolyte 50 Measurements were performed, and the result was 67 μm. Furthermore, the ionic conductivity was measured, and the result was 7.2 (mS / cm). It was confirmed that although the ionic conductivity was high, the average particle size was very large compared to the average particle size of the examples, indicating significant granulation was performed. In addition, in... Figure 2The X-ray diffraction spectrum of the solid electrolyte obtained in Comparative Example 1 is shown by powder X-ray diffraction (XRD) measurement.

[0164] (Comparative Example 2)

[0165] Lithium sulfide, phosphorus pentasulfide, lithium chloride, and lithium bromide were weighed in the manner described in Example 1, bringing the total weight to 100g. Dehydrated toluene was added to a weight of 10% by mass, followed by isobutyronitrile. The mixture was then pulverized for 1 hour using a bead mill (LabStar Mini LMZ015, manufactured by Ashizawa Finetech Co., Ltd.) to obtain a slurry containing the pulverized material. Furthermore, in this pulverization process, zirconia beads with a diameter of 0.5mm were incorporated to a weight of 80% by volume.

[0166] The obtained slurry was dried under reduced pressure to remove the solvent, resulting in a pulverized raw material mixture powder. Subsequently, it was calcined in an electric furnace within a glove box under a nitrogen atmosphere at 400°C for 1 hour. Specifically, 30g of the pulverized mixture was weighed into a sagger made of Al₂O₃, as used in Comparative Example 1, and placed in the electric furnace. The temperature was increased from room temperature to 400°C over 1.5 hours, then maintained at 400°C for 1 hour. After natural cooling, the sagger was removed to obtain the calcined powder. This process was repeated to obtain 100g of calcined powder.

[0167] To the aforementioned 100g of calcined powder, dehydrated toluene was added in an amount of 10% by mass, followed by isobutyronitrile. The mixture was then pulverized for 1 hour using a bead mill (Lab Star Mini LMZ015, manufactured by Ashizawa Finetech Co., Ltd.) to obtain a slurry containing the pulverized material. Furthermore, during this pulverization process, zirconia beads with a diameter of 0.5mm were added in an amount of 80% by volume. The resulting slurry was dried under reduced pressure at 100°C to obtain a solid electrolyte.

[0168] The average particle size (D) of the obtained solid electrolyte 50 Measurements were performed, and the result was 0.5 μm. Furthermore, the ionic conductivity was measured, and the result was 1.0 (mS / cm), confirming that although pulverization was achieved, the ionic conductivity was low. Additionally, in... Figure 3 The X-ray diffraction spectrum of the solid electrolyte obtained in Comparative Example 2 is shown by powder X-ray diffraction (XRD) measurement.

[0169] (Refer to Example 1)

[0170] In a reaction vessel equipped with stirring blades, lithium sulfide and phosphorus pentasulfide were weighed and added under a nitrogen atmosphere to achieve a molar ratio of 75:25. Further, based on the aforementioned 75:25 molar ratio of lithium sulfide to phosphorus pentasulfide, lithium sulfide, lithium chloride, and lithium bromide were weighed and added to achieve molar ratios of 40, 100, and 60 respectively. While cooling with methanol / liquid nitrogen, the stirring blades were operated. Then, using a Teflon tube, dehydrated tetrahydrofuran (dehydrated THF), also pre-cooled to -20°C with methanol / liquid nitrogen, was added to achieve a total mass of 10% of the raw materials (lithium sulfide, phosphorus pentasulfide, lithium chloride, and lithium bromide). The mixture was then stirred at room temperature (23°C) for 72 hours. Next, the tetrahydrofuran was removed using a sleeve, followed by the addition of dehydrated THF to achieve a total mass of 10% of the raw materials. The mixture was stirred for 30 minutes and then removed again. This process was repeated at least three times.

[0171] Next, the obtained material was subjected to vacuum drying at 80°C for 2 hours, followed by heat treatment at 180°C for 8 hours to obtain the precursor. The precursor was subjected to powder X-ray diffraction (XRD) measurements in the same manner as in Example 1, and the results are as follows: Figure 4 As shown in (a), in addition to lithium sulfide, lithium bromide, and lithium chloride, crystalline Li3PS4 (β-Li3PS4) was also identified.

[0172] Furthermore, the obtained precursor was further processed by adding dehydrated toluene to a mass of 10% by weight, followed by the addition of isobutyronitrile, and then pulverizing the mixture for 1 hour using a bead mill ("Lab Star Mini LMZ015 (model)", manufactured by Ashizawa Finetech Co., Ltd.) to obtain a slurry containing the pulverized material. In addition, during this pulverization process, zirconia beads with a diameter of 0.5 mm were added to a mass of 80% by weight.

[0173] The slurry containing the pulverized material was dried at 100°C under reduced pressure to obtain a powder. The obtained powder was subjected to powder X-ray diffraction (XRD) measurements in the same manner as in Example 1, and the results are as follows. Figure 4 As shown in (b), in addition to lithium sulfide, lithium bromide and lithium chloride, a broad peak also appears, confirming that crystalline Li3PS4 (β-Li3PS4) has become amorphous Li3PS4.

[0174] (See Example 2 for reference)

[0175] A slurry containing pulverized material was obtained in the same manner as in Example 1. The obtained slurry containing pulverized material was dried at 100°C under reduced pressure to obtain powder of pulverized material.

[0176] The obtained precursor before pulverization was subjected to powder X-ray diffraction (XRD) measurements in the same manner as in Example 1, and the results are as follows: Figure 5 As shown in (a), crystalline Li3PS4 (β-Li3PS4) was confirmed, in addition to a small amount of unreacted lithium sulfide. Furthermore, powder X-ray diffraction (XRD) measurements were performed on the powders obtained by adding lithium sulfide, lithium chloride, and lithium bromide using the same method as described above, and the results are as follows. Figure 5 As shown in (b), in addition to lithium sulfide, lithium bromide, and lithium chloride, broad peaks also appeared, confirming that crystalline Li3PS4 (β-Li3PS4) had become amorphous Li3PS4. Thus, as can be seen from Reference Examples 1 and 2, the mixing of raw materials containing halogen elements is independent of the timing of the complexation process; the same precursor can be obtained at the stage after the pulverization process and before the crystallization process.

[0177] Industrial availability

[0178] According to the method for manufacturing crystalline solid electrolytes of this embodiment, it is possible to manufacture solid electrolytes with small particle size and high ionic conductivity, and it is particularly preferred for manufacturing solid electrolytes with a sulforaphite-germanium type crystal structure.

[0179] Furthermore, the solid electrolyte obtained by the manufacturing method of this embodiment is preferably used in batteries, especially in batteries used in information-related devices or communication devices such as computers, cameras, and mobile phones.

Claims

1. A method for manufacturing a crystalline solid electrolyte, wherein the crystalline solid electrolyte comprises lithium, sulfur, phosphorus, and halogen elements, characterized in that, The crystalline solid electrolyte has a sulforaphite-germanium ore-type crystal structure, and the manufacturing method comprises: The mixing process includes a complexing process of mixing solid electrolyte raw materials and complexing agents in the liquid phase to obtain a precursor containing lithium, sulfur and phosphorus elements; In the crystallization process, the precursor is heated in a solvent using a pressure vessel or during reflux. The complexing agent is at least one solvent selected from amine solvents, ether solvents, and nitrile solvents. In the crystallization process, at least one solvent selected from aliphatic hydrocarbon solvents, alicyclic hydrocarbon solvents, aromatic hydrocarbon solvents, and paraffin solvents is used. The crystallization process is carried out at a temperature above 200°C and below 425°C.

2. The method for manufacturing the crystalline solid electrolyte as described in claim 1, characterized in that, The mixing process includes a crushing process for the precursor.

3. The method for manufacturing the crystalline solid electrolyte as described in claim 1, characterized in that, In the complexing process, a complex containing lithium, sulfur, phosphorus and the complexing agent is obtained.

4. The method for manufacturing the crystalline solid electrolyte as described in claim 1, characterized in that, In the mixing process, raw materials containing halogen elements are mixed in after the complexing process.

5. The method for manufacturing the crystalline solid electrolyte as described in claim 4, characterized in that, The halogen element is at least one of chlorine, bromine, and iodine.

6. The method for manufacturing a crystalline solid electrolyte as described in claim 5, characterized in that, The halogen elements are chlorine and bromine.

7. The method for manufacturing the crystalline solid electrolyte as described in claim 4, characterized in that, The raw material containing the halogen element is selected from at least one of lithium halides and halogen monomers.

8. The method for manufacturing a crystalline solid electrolyte as described in claim 1, characterized in that, The solid electrolyte raw material includes lithium halide as a raw material.

9. The method for manufacturing a crystalline solid electrolyte as described in claim 8, characterized in that, The lithium halide is at least one selected from lithium chloride, lithium bromide, and lithium iodide.

10. The method for manufacturing a crystalline solid electrolyte as described in claim 9, characterized in that, The lithium halide is lithium chloride and lithium bromide.

11. The method for manufacturing a crystalline solid electrolyte as described in claim 7, characterized in that, The halogen monomer is at least one selected from chlorine, bromine, and iodine.

12. The method for manufacturing the crystalline solid electrolyte as described in claim 11, characterized in that, The halogen monomers are chlorine and bromine.

13. The method for manufacturing a crystalline solid electrolyte as described in claim 1, characterized in that, The solid electrolyte raw material includes lithium sulfide and phosphorus sulfide.

14. The method for manufacturing the crystalline solid electrolyte as described in claim 13, characterized in that, The phosphorus sulfide is phosphorus pentasulfide.

15. The method for manufacturing a crystalline solid electrolyte as described in claim 1, characterized in that, The mixing in the complexation process is carried out using a mechanical stirring mixer.

16. The method for manufacturing a crystalline solid electrolyte as described in claim 15, characterized in that, The mixing in the complexing process is performed without using a pulverizer or kneader.

17. The method for manufacturing a crystalline solid electrolyte as described in claim 1, characterized in that, The precursor includes a PS4 3- Structure.

18. The method for manufacturing a crystalline solid electrolyte as described in claim 17, characterized in that, The PS4 3- The structure is amorphous Li3PS4, crystalline Li3PS4, or a complex of said amorphous Li3PS4 or crystalline Li3PS4 obtained by complexation decomposition.

19. The method for manufacturing a crystalline solid electrolyte as described in claim 18, characterized in that, In the mixing process, after the complexing process, there are one or more of the following processes: a drying process to obtain a complex crystal, a complexing decomposition process to remove the complexing agent contained in the complex crystal to obtain the amorphous Li3PS4, and a process of heating at least one of the complex crystal and the amorphous Li3PS4 to obtain crystalline Li3PS4.

20. The method for manufacturing a crystalline solid electrolyte as described in claim 19, characterized in that, The mixing process includes the drying process, the complexation decomposition process, and the process of obtaining crystalline Li3PS4.

21. The method for manufacturing a crystalline solid electrolyte as described in claim 19, characterized in that, The drying process is carried out at a drying temperature of 5–100°C.

22. The method for manufacturing a crystalline solid electrolyte as described in claim 21, characterized in that, The drying process is carried out at a drying temperature of 20–85°C.

23. The method for manufacturing a crystalline solid electrolyte as described in claim 19, characterized in that, The drying process is carried out by vacuum drying.

24. The method for manufacturing a crystalline solid electrolyte as described in claim 19, characterized in that, The heating temperature in the complexation decomposition process and the process of obtaining crystalline Li3PS4 is above 140°C and below 300°C.

25. The method for manufacturing a crystalline solid electrolyte as described in claim 24, characterized in that, The heating temperature is above 170℃ and below 200℃.

26. The method for manufacturing a crystalline solid electrolyte as described in claim 1, characterized in that, The crystallization process is carried out at a temperature above 325°C and below 370°C.

27. The method for manufacturing a crystalline solid electrolyte as described in claim 1, characterized in that, The crystallization process is carried out using an autoclave.

28. The method for manufacturing a crystalline solid electrolyte as described in claim 1, characterized in that, There is no pulverization process following the crystallization process.

29. The method for manufacturing a crystalline solid electrolyte as described in claim 1, characterized in that, A drying process is not included before the crystallization process.

30. The method for manufacturing a crystalline solid electrolyte as described in claim 1, characterized in that, The complexing agent is an ether solvent.

31. The method for manufacturing a crystalline solid electrolyte as described in claim 30, characterized in that, The ether solvent is selected from at least one of diethyl ether, diisopropyl ether, dibutyl ether, and tetrahydrofuran.

32. The method for manufacturing a crystalline solid electrolyte as described in claim 31, characterized in that, The ether solvent is tetrahydrofuran.

33. The method for manufacturing a crystalline solid electrolyte as described in claim 1, characterized in that, In the complexation process, at least one solvent selected from aliphatic hydrocarbon solvents, alicyclic hydrocarbon solvents, aromatic hydrocarbon solvents, and paraffin solvents is used.

34. The method for manufacturing a crystalline solid electrolyte as described in claim 1, characterized in that, The amount of the complexing agent used is such that the content of the solid electrolyte raw material reaches 1 to 50% by mass.

35. The method for manufacturing a crystalline solid electrolyte as described in claim 34, characterized in that, The amount of complexing agent used is such that the content of the solid electrolyte raw material reaches 5-15% by mass.

36. The method for manufacturing a crystalline solid electrolyte as described in claim 33, characterized in that, The solvent is a paraffin-based solvent.

37. The method for manufacturing a crystalline solid electrolyte as described in claim 36, characterized in that, The paraffin solvent is an isoparaffin hydrocarbon solvent.

Citation Information

Patent Citations

  • Solid-state lithium secondary battery, and method for producing the same

    JP2011096630A

  • Method of manufacturing sulfide-based solid electrolyte

    JP2013211171A

  • Manufacturing method of lithium ion conductive solid electrolyte

    JP2014096391A

  • Method for producing solid electrolyte having argyrodite type crystal structure

    JP2020095953A

  • Method for producing lithium ion conductive solid electrolyte

    WO2009047977A1