Nitrogen doped-polymerized porous nano-deposition cathode material and its preparation method and application

By depositing nitrogen-doped-polymerized porous nanopowder on the surface of the sodium ion cathode material to form a multi-layer dense film, the problem of microcracks caused by the structural phase change of the cobalt-free high-nickel layered oxide cathode material during the charge and discharge process is solved, and the problem is improved. Improved electrochemical performance and cycle stability, achieving high capacity and improved mechanical properties.

CN114256458BActive Publication Date: 2024-10-18GUANGDONG BRUNP RECYCLING TECH CO LTD +2
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202111424143.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-26
Publication Date
2024-10-18
Estimated Expiration
2041-11-26

Smart Images

  • Figure CN114256458B_ABST
    Figure CN114256458B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of sodium ion batteries, and discloses a nitrogen-doped - polymer porous nano-deposited cathode material, its preparation method and application. Its general formula is Na t Li f Ni s Z 1‑s O2@aNMC - Y, where 0.8 ≤ t < 1, 0 ≤ f < 0.3, 0.5 ≤ s < 1, 0 < a < 0.1, Z is at least one of Mn, Mo, Co, Mg, Al, and Y is at least one of Cu, Ga, Zn, Cr, Zr. The nitrogen-doped - polymer porous nano-deposited cathode material prepared by the present invention obtains a multi-layer dense film on the surface of the NMC - Y deposition Na t Li f Ni s Z 1‑s O2 material. After depositing nitrogen-doped - polymer porous nano, on the one hand, the nitrogen-doped - polymer porous nano can contribute a considerable specific surface area, and on the other hand, it can also shorten the migration path of ions inside the material and improve the electrochemical performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of sodium ion batteries, and in particular relates to a nitrogen-doped-polymerized porous nano-deposition cathode material and a preparation method and application thereof. Background Art

[0002] Nickel layered oxides, whose energy density increases with the increase of high nickel content in the positive electrode material, have always been favored by battery manufacturers. In addition, cobalt is a rare metal, accounting for only 0.0025% of the earth's crust, which is much lower than the nickel content in the earth's crust. At present, the price of cobalt is much higher than that of nickel. Therefore, using high-nickel and low-cobalt layered oxides as positive electrode materials for batteries is the current main research and development direction of manufacturers.

[0003] The development of cobalt-free high-nickel layered oxides should be based on the chemical behavior of cobalt and nickel, and then explore the role of cobalt and nickel in structure and electrochemical stability, and propose feasible solutions. Unfortunately, these materials still face problems in the process of solving them, and their practical applications are limited, which is still challenging. For example, during the charge and discharge process, the cobalt-free high-nickel layered oxide positive electrode material induces the original layered spinel structure to a disordered spinel structure. However, this phase change and the deintercalation of sodium ions will cause micro-scale stress in the positive electrode material, thereby generating microcracks on the surface and inside of the positive electrode material, which will hinder the normal transmission of sodium ions, thereby reducing capacity retention, which is a more serious problem for the material. In addition, the new interface between the positive electrode material and the electrolyte causes the fluoride ions in the electrolyte to react with the exposed nickel and sodium to form fluoride salts, some of which exist in the electrolyte, and some migrate to the negative electrode with the charged sodium ions, aggravating the collapse of the structure, accelerating the electrolyte immersion channel, and destroying the mechanical integrity, which will lead to the attenuation of the electrode material and further deteriorate the cycle performance.

[0004] In order to overcome such thorny problems, the positive electrode material is improved from the perspective of composition and surface, and a sodium ion positive electrode material with high capacity, stable mechanical properties and long-cycle discharge is prepared. Summary of the invention

[0005] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention proposes a nitrogen-doped-polymerized porous nano-deposited positive electrode material and a preparation method and application thereof, and the nitrogen-doped-polymerized porous nano-deposited positive electrode material has excellent cycle performance.

[0006] To achieve the above object, the present invention adopts the following technical solutions:

[0007] A nitrogen-doped-polymerized porous nano-deposition cathode material, the general formula of which is Na t Li f Ni s Z1-s O2@aNMC-Y, where 0.8 ≤ t < 1, 0 ≤ f < 0.3, 0.5 ≤ s < 1, 0 < a < 0.1, Z is at least one of Mn, Mo, Co, Mg, and Al, and Y is at least one of Cu, Ga, Zn, Cr, and Zr; the NMC-Y is a nitrogen-doped polymerized porous nanopowder.

[0008] Preferably, the NMC is nitrogen-doped mesoporous carbon.

[0009] Preferably, the Na t Li f Ni s Z 1-s O2@aNMC-Y, where 0.8 ≤ t < 1, 0 ≤ f < 0.2, 0.7 ≤ s < 1, 0 < a < 0.1, Z is at least one of Mn, Mo, Co, Mg, and Al, and Y is at least one of Cu, Ga, Zn, Cr, and Zr.

[0010] More preferably, the Na t Li f Ni s Z 1-s O2@aNMC-Y is Na 0.8 Li 0.2 Ni 0.7 Co 0.05 Mg 0.05 Mn 0.2 O2@0.05NMC-Cu, Na 0.75 Li 0.25 Ni 0.60 Co 0.025 Mg 0.025 Mn 0.35 O2@0.025NMC-Cu, Na 0.88 Li 0.12 Ni 0.68 Co 0.065 Al 0.05 Mo 0.023 Mn 0.182 O2@0.0625NMC-Cu, Na 0.88 Li 0.12 Ni 0.765 Co 0.065 Al 0.05 Mo 0.023 Mn 0.097 One of O2@0.0875NMC-Zr.

[0011] A preparation method of a nitrogen-doped polymerized porous nano-deposited cathode material, which is used to prepare the above-mentioned nitrogen-doped polymerized porous nano-deposited cathode material.

[0012] Specifically, a method for preparing a nitrogen-doped-polymerized porous nano-deposition cathode material comprises the following steps:

[0013] (1) Mix nickel salt and Z salt, add carbonate to carry out precipitation reaction, separate solid and liquid, take solid phase, add sodium source and lithium source to mix, sinter, and obtain sodium ion positive electrode material Na t Li f Ni s Z 1-s O2;

[0014] (2) mixing 3-hexyl substituted polythiophene, a solvent, and a transition metal salt, reacting, and carbonizing to obtain nitrogen-doped-polymerized porous nanopowder NMC-Y;

[0015] (3) A protective gas and a reducing gas are introduced into the sodium ion positive electrode material for purging, and then He-loaded nitrogen doping-polymerized porous nanoparticles are used for deposition to obtain the nitrogen doped-polymerized porous nanoparticle deposited positive electrode material; the Z salt is at least one of the chlorides, nitrates, and sulfates of Mn, Mo, Co, Mg, and Al.

[0016] Preferably, in step (1), the nickel salt is at least one of nickel sulfate, nickel nitrate or nickel chloride.

[0017] Preferably, in step (1), the sodium source is at least one of sodium hydroxide, sodium acetate, sodium oxalate, sodium phosphate or sodium citrate.

[0018] Preferably, in step (1), the lithium source is at least one of lithium hydroxide, lithium acetate, lithium oxalate, lithium nitrate, lithium carbonate or lithium chloride.

[0019] Preferably, in step (1), the carbonate is at least one of sodium carbonate, sodium bicarbonate, potassium carbonate, magnesium carbonate, calcium carbonate or lithium carbonate.

[0020] Preferably, in step (1), the reaction temperature is 35-95°C.

[0021] Preferably, in step (1), the sintering temperature is 400-1100° C., and the sintering time is 3-12 hours.

[0022] Preferably, in step (2), the solvent is at least one of polyethylene glycol, ethylene glycol, ethanol, methanol, acetic acid, formic acid or triethanolamine.

[0023] Preferably, in step (2), the transition metal salt is at least one of chloride, nitrate, sulfate, bromide and iodide of Cu, Ga, Zn, Cr and Zr.

[0024] Preferably, in step (2), the solid-to-liquid ratio of the 3-hexyl substituted polythiophene, the transition metal salt and the solvent is (1-3) g: (0.01-0.5) g: (10-50) ml.

[0025] Preferably, in step (2), the carbonization step further includes allowing the reacted material to stand and dry.

[0026] More preferably, the drying temperature is 80-200°C.

[0027] Preferably, in step (2), the carbonization temperature is 200-900°C.

[0028] Preferably, in step (3), the nitrogen-doped-polymerized porous nano-deposited positive electrode material D 50 5-20μm, D max 10-50μm.

[0029] Preferably, in step (3), the sodium ion positive electrode material Na t Li f Ni s Z 1-s The mass ratio of O2 and nitrogen-doped-polymerized porous nanopowder is (70-150):(1-10).

[0030] The invention also provides a battery, comprising the nitrogen-doped-polymerized porous nano-deposition positive electrode material.

[0031] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0032] 1. The nitrogen-doped-polymerized porous nano-deposition cathode material prepared by the present invention is prepared by depositing NMC-Y with Na t Li f Ni s Z 1-s The surface of the O2 material obtained a multilayer dense film. After the deposition of nitrogen-doped-polymerized porous nanoparticles, the nitrogen-doped-polymerized porous nanoparticles can contribute a considerable specific surface area on the one hand, and on the other hand, it can also shorten the migration path of ions inside the material and improve the electrochemical performance. After 200 charge and discharge cycles, the deposition of Na t Li f Ni s Z 1-s The Coulomb efficiency of the material with O2 surface is higher, close to 100%, which proves that this material with NMC-Y deposition can effectively suppress the microcracks on the surface or inside the sodium ion positive electrode material, and correspondingly improve the recycling performance of the sodium ion positive electrode material.

[0033] 2. The NMC-Y in the nitrogen-doped-polymeric porous nano-deposition positive electrode material of the present invention not only has high conductivity and high chemical stability, but also the nitrogen-doped-polymeric porous nano-manufacturing is low-cost and simple to synthesize. Therefore, it has a positive impact on the improvement of sodium ion positive electrode materials and is beneficial to the commercial application of sodium ion positive electrode materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 This is a SEM image of the positive electrode material prepared in Example 2 of the present invention;

[0035] Figure 2 This is a SEM image of the positive electrode material prepared in Comparative Example 1 of the present invention;

[0036] Figure 3 This is a SEM image of NMC-Cu prepared in Example 2 of the present invention;

[0037] Figure 4 This is a rate performance diagram of the positive electrode materials prepared in Example 2, Example 4, and Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0038] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.

[0039] Example 1

[0040] The nitrogen-doped-polymerized porous nano-deposited positive electrode material of this embodiment has the formula Na 0.8 Li 0.2 Ni 0.7 Co 0.05 Mg 0.0 5Mn 0.2 O2@0.05NMC-Cu.

[0041] The preparation method of the nitrogen-doped-polymerized porous nano-deposition positive electrode material of this embodiment has the following specific steps:

[0042] (1) 140 ml of 0.5 mol / L nickel nitrate, 20 ml of 1.0 mol / L manganese nitrate, 10 ml of 0.5 mol / L cobalt nitrate, and 20 ml of 0.25 mol / L magnesium nitrate were mixed in a beaker, and the beaker was placed in an oil bath at 55° C., and sodium carbonate was added, stirred, and separated to obtain a nickel-containing precipitate. 80 ml of 1.01 mol / L sodium hydroxide and 20 ml of 1.0 mol / L lithium hydroxide were mixed to prepare a sodium-lithium mixture. The sodium-lithium mixture and the nickel-containing precipitate were mixed, stirred, and dried, and sent to a tubular furnace at 670° C. for calcination for 10 h, and ball milling was performed to obtain a high-nickel sodium ion positive electrode material Na 0.8 Li 0.2 Ni 0.7 Co 0.05 Mg 0.05 Mn 0.2 O2.

[0043] (2) Place the polytetrafluoroethylene cup in a 65°C oil bath, add 0.5 g of 3-hexyl-substituted polythiophene to 15 mL of polyethylene glycol in the polytetrafluoroethylene cup, then add 3 ml of 0.43 mol / L copper nitrate, stir and let stand, send to a tubular furnace, fill with nitrogen, dry at 105°C for 2 h, heat to 620°C for carbonization, and obtain 0.7 g of dark brown nitrogen-doped-polymer porous nanopowder NMC-Cu.

[0044] (3) 6gNa 0.8 Li 0.2 Ni 0.7 Co 0.05 Mg 0.05 Mn 0.2 O2 was loaded into a fixed bed reactor, filled with N2 to exclude air, heated to 125°C, and purged with N2-H2 at 50 mL / min. 0.3 g of nitrogen-doped-polymeric porous nanopowder NMC-Cu was loaded through He, reacted for 60 min, washed, demagnetized with a magnetic rod, and dried in an oven at 95°C to obtain nitrogen-doped-polymeric porous nanopowder deposition (Na 0.8 Li 0. 2Ni 0.7 Co 0.05 Mg 0.05 Mn 0.2 O2@0.05NMC-Cu).

[0045] Example 2

[0046] The nitrogen-doped-polymerized porous nano-deposited positive electrode material of this embodiment has the formula Na 0.75 Li 0.25 Ni 0.60 Co 0.025 Mg 0.025 Mn 0.35 O2@0.025NMC-Cu.

[0047] The preparation method of the nitrogen-doped-polymerized porous nano-deposition positive electrode material of this embodiment has the following specific steps:

[0048] (1) 120 ml of 0.5 mol / L nickel sulfate, 35 ml of 1.0 mol / L manganese sulfate, 5 ml of 0.5 mol / L cobalt sulfate, and 10 ml of 0.25 mol / L magnesium sulfate were mixed in a beaker, the beaker was placed in an oil bath at 55° C., sodium carbonate was added, stirred, and separated to obtain a nickel-containing precipitate, 75 ml of 1.01 mol / L sodium hydroxide and 25 ml of 1.0 mol / L lithium hydroxide were mixed to prepare a sodium-lithium mixture, the sodium-lithium mixture and the nickel-containing precipitate were mixed, stirred, and dried, and sent to a tubular furnace at 670° C. for calcination for 10 h, and ball milled to obtain a high-nickel sodium ion positive electrode material Na 0.75 Li 0.25 Ni 0.60 Co 0.025 Mg 0.025 Mn 0.35 O2.

[0049] (2) Place the polytetrafluoroethylene cup in an oil bath at 65°C, add 0.8 g of 3-hexyl-substituted polythiophene to the polytetrafluoroethylene cup containing 25 mL of polyethylene glycol, and then add 5 ml of 0.43 mol / L copper nitrate. Stir and let stand, then transfer to a tubular furnace, fill with nitrogen, dry at 105°C for 2 h, and heat to 620°C for carbonization to obtain 0.8 g of dark brown nitrogen-doped-polymer porous nanopowder NMC-Cu.

[0050] (3) 10gNa 0.75 Li 0.25 Ni 0.60 Co 0.025 Mg 0.025 Mn 0.35 O2 was loaded into a fixed bed reactor, filled with N2 to exclude air, heated to 125°C, and purged with N2-H2 at 60 mL / min. 0.25 g of nitrogen-doped-polymeric porous nanopowder NMC-Cu was loaded through He, reacted for 60 min, washed, demagnetized with a magnetic rod, and dried in an oven at 95°C to obtain nitrogen-doped-polymeric porous nanopowder deposition (Na 0.75 Li 0.25 Ni 0.60 Co 0.025 Mg 0.025 Mn 0.35 O2@0.025NMC-Cu).

[0051] Example 3

[0052] The nitrogen-doped-polymerized porous nano-deposited positive electrode material of this embodiment has the formula Na 0.88 Li0.12 Ni 0.68 Co 0.065 Al 0.05 Mo 0.023 Mn 0.182 O2@0.0625NMC-Cu.

[0053] The preparation method of the nitrogen-doped-polymerized porous nano-deposition positive electrode material of this embodiment has the following specific steps:

[0054] (1) 80 ml of 0.85 mol / L nickel sulfate, 14 ml of 1.3 mol / L manganese sulfate, 10 ml of 0.65 mol / L cobalt sulfate, 10 ml of 0.5 mol / L aluminum chloride, and 3 ml of 0.74 mol / L ammonium molybdate were mixed in a beaker, the beaker was placed in an oil bath at 60° C., sodium carbonate was added, stirred, and separated to obtain a nickel-containing precipitate, 195 ml of 0.45 mol / L sodium acetate and 20 ml of 0.61 mol / L lithium hydroxide were mixed to form a sodium-lithium mixture, the sodium-lithium mixture and the nickel-containing precipitate were mixed, stirred, and dried, and sent to a tubular furnace at 730° C. for sintering for 8 h, and ball milling to obtain a high-nickel sodium ion positive electrode material Na 0.88 Li 0.12 Ni 0.68 Co 0.065 Al 0.05 Mo 0.023 Mn 0.18 2O2.

[0055] (2) Place the polytetrafluoroethylene cup in a 70°C oil bath, add 0.5 g of 3-hexyl-substituted polythiophene to the polytetrafluoroethylene cup containing 40 mL of polyethylene glycol, and then add 8 ml of 0.66 mol / L zirconium sulfate. Stir and let stand, then send to a tubular furnace, fill with nitrogen, dry at 105°C for 2 h, and heat to 570°C for carbonization to obtain 2.8 g of dark brown nitrogen-doped-polymer porous nanopowder NMC-Zr.

[0056] (3) 8gNa 0.88 Li 0.12 Ni 0.68 Co 0.065 Al 0.05 Mo 0.023 Mn 0.182 O2 was loaded into a fixed bed reactor, filled with N2 to exclude air, heated to 135°C, and purged with N2-H2 at 50 mL / min. 0.5 g of nitrogen-doped-polymeric porous nanopowder NMC-Zr was loaded through He, reacted for 60 min, washed, demagnetized with a magnetic rod, and dried in an oven at 95°C to obtain nitrogen-doped-polymeric porous nanopowder deposition (Na 0.88 Li 0.12 Ni 0.68 Co0.065 Al 0.05 Mo 0.023 Mn 0.182 O 22 @0.0625NMC-Zr).

[0057] Example 4

[0058] The nitrogen-doped-polymerized porous nano-deposited positive electrode material of this embodiment has the formula Na 0.88 Li 0.12 Ni 0.765 Co 0.065 Al 0.05 Mo 0.023 Mn 0.097 O2@0.0875NMC-Zr.

[0059] The preparation method of the nitrogen-doped-polymerized porous nano-deposition positive electrode material of this embodiment has the following specific steps:

[0060] (1) 90 ml of 0.85 mol / L nickel sulfate, 7.5 ml of 1.3 mol / L manganese sulfate, 10 ml of 0.65 mol / L cobalt sulfate, 10 ml of 0.5 mol / L aluminum chloride, and 3 ml of 0.74 mol / L ammonium molybdate were mixed in a beaker, the beaker was placed in an oil bath at 60° C., sodium carbonate was added, stirred, and separated to obtain a nickel-containing precipitate, 8.5 ml of 1.02 mol / L sodium hydroxide and 1.5 ml of 1.0 mol / L lithium hydroxide were mixed to form a sodium-lithium mixture, the sodium-lithium mixture and the nickel-containing precipitate were mixed, stirred, dried, and sent to a tubular furnace at 730° C. for sintering for 8 h and ball milling for 6 h to obtain a high-nickel sodium ion positive electrode material Na 0.8 Li 0.2 Ni 0.7 Co 0.05 Mg 0.05 Mn 0.2 O2.

[0061] (2) Place the polytetrafluoroethylene cup in an oil bath at 70°C, add 1.0 g of 3-hexyl-substituted polythiophene to the polytetrafluoroethylene cup containing 40 mL of polyethylene glycol, and then add 10 ml of 0.66 M zirconium sulfate. Stir and let stand, then send to a tubular furnace, fill with nitrogen, dry at 105°C for 2 h, and heat to 570°C for carbonization to obtain 3.9 g of dark brown nitrogen-doped-polymer porous nanopowder NMC-Zr.

[0062] (3) 8gNa 0.8 Li 0.2 Ni 0.7 Co 0.05 Mg 0.05 Mn 0.2O2 was loaded into a fixed bed reactor, filled with N2 to exclude air, heated to 155°C, and purged with N2-H2 at 60 mL / min. 0.7 g of nitrogen-doped-polymeric porous nanopowder NMC-Zr was loaded through He, reacted for 60 min, washed, demagnetized with a magnetic rod, and dried in an oven at 95°C to obtain nitrogen-doped-polymeric porous nanopowder deposition (Na 0.88 Li 0.12 Ni 0.765 Co 0.065 Al 0.05 Mo 0.023 Mn 0.097 O2@0.0875NMC-Zr).

[0063] Comparative Example 1

[0064] The sodium ion positive electrode material of this comparative example has the formula Na 0.8 Li 0.2 Ni 0.7 Co 0.05 Mg 0.05 Mn 0.2 O2.

[0065] The preparation method of the nitrogen-doped-polymerized porous nano-deposition positive electrode material of this comparative example comprises the following specific steps:

[0066] (1) 140 ml of 0.5 mol / L nickel nitrate, 20 ml of 1.0 mol / L manganese nitrate, 10 ml of 0.5 mol / L cobalt nitrate, and 20 ml of 0.25 mol / L magnesium nitrate were mixed in a beaker, the beaker was placed in an oil bath at 55° C., sodium carbonate was added, stirred, and separated to obtain a nickel-containing precipitate, 80 ml of 1.01 mol / L sodium hydroxide and 20 ml of 1.0 mol / L lithium hydroxide were mixed to prepare a sodium-lithium mixture, the sodium-lithium mixture and the nickel-containing precipitate were mixed, stirred, and dried, and sent to a tubular furnace at 670° C. for calcination for 10 h, and ball milled to obtain a high-nickel sodium ion positive electrode material Na 0.8 Li 0.2 Ni 0.7 Co 0.05 Mg 0.05 Mn 0.2 O2.

[0067] Comparative Example 2

[0068] The nitrogen-doped-polymerized porous nano-deposited positive electrode material of this comparative example has the formula Na 0.88 Li 0.12 Ni 0.68 Co 0.065 Al 0.05 Mo 0.023 Mn 0.182 O2.

[0069] The preparation method of the nitrogen-doped-polymerized porous nano-deposition positive electrode material of this comparative example comprises the following specific steps:

[0070] (1) 80 ml of 0.85 mol / L nickel sulfate, 14 ml of 1.3 mol / L manganese sulfate, 10 ml of 0.65 mol / L cobalt sulfate, 10 ml of 0.5 mol / L aluminum chloride, and 3 ml of 0.74 mol / L ammonium molybdate were mixed in a beaker, the beaker was placed in an oil bath at 60°C, sodium carbonate was added, stirred, and a nickel-containing precipitate was separated. 195 ml of 0.45 mol / L sodium acetate and 20 ml of 0.61 mol / L lithium hydroxide were mixed to form a sodium-lithium mixture. The sodium-lithium mixture and the nickel-containing precipitate were mixed, stirred, and dried, and sent to a tubular furnace at 730°C for sintering for 8 hours and ball milling to obtain a high-nickel sodium ion positive electrode material Na 0.88 Li 0.12 Ni 0.68 Co 0.065 Al 0.05 Mo 0.023 Mn 0.182 O2.

[0071] Analysis of Examples 1-4 and Comparative Examples 1-2:

[0072] The specific surface area (BET) of the positive electrode materials in Examples 1-4 and Comparative Examples 1-2 was measured using a specific surface area pore size analyzer, and the D 10 , D 50 , D 90 , D max , the results are shown in Table 1.

[0073] Battery composition: The battery mainly includes positive and negative electrode plates, Celgard diaphragm, electrolyte (solute: 1.2 mol / L NaPF6, solvent: 5 ml EC and 5 ml EMC mixed), gasket, spring and positive and negative electrode shells. The positive electrode plate is made of the following: the positive electrode material, acetylene black and PVDF prepared in Example 1-4 and Comparative Example 1-2 are mixed into a slurry in a mass ratio of 80:10:10, and then coated on aluminum foil to make the positive electrode plate. The plate is placed in an oven at 80°C to dry, and then rolled. The sodium sheet is used as the negative electrode plate. The battery is assembled in a vacuum glove box under an argon atmosphere. The cycle performance is tested using an electrochemical workstation at room temperature. Before the test, the battery is activated with 30 mAh / g charge and discharge. The discharge range is 2.5-4.2 V. The test is performed at 0.1C, 0.2C, 0.5C, 1C, 2C, and 5C rates. The results are shown in Figure 4 (1C default is 150mAh / g), the number of cycles is 40 times, the test results at 1C rate are shown in Table 2, and the number of cycles is 200 times.

[0074] from Figure 1-Figure 3 Available, Figure 2 Prepared sodium ion cathode material Na 0.8 Li 0.2 Ni 0.7 Co 0.05 Mg 0.05 Mn 0.2 O2 particles are relatively clear. Figure 1 After the deposition of nitrogen-doped-polymerized porous nanopowder NMC-Cu, the sodium ion positive electrode material Na 0.75 Li 0.25 Ni 0.60 Co 0.025 Mg 0.025 Mn 0.35 O2@0.025NMC-Cu is rougher and covered with multi-layer thin films, and no granular structure is seen. This shows that the multi-layer thin films can provide more area and increase the contact surface. Although the deposited nitrogen-doped-polymerized porous nanopowder NMC-Cu has a greater influence on the morphology of the sodium-ion positive electrode material, the multi-layer thin film coverage can suppress the microcracks on the surface or inside the sodium-ion positive electrode material and improve the stability of the material. Figure 3 It is nitrogen-doped-polymerized porous nanopowder NMC-Cu, with a surface polymerized porous structure and particles are relatively close to each other.

[0075] Table 1 BET and particle size distribution of Examples 1-4 and Comparative Examples 1-2

[0076]

[0077] In Table 1, the BET of Examples 1-4 is between 0.34 and 0.39 m 2 / g, while the BET of Comparative Examples 1-2 is between 0.31-0.34 m 2 / g, after depositing nitrogen-doped-polymerized porous nanopowder, the BET values ​​of Examples 1-4 all increased, the D10, D50, D90, and Dmax of Examples 1-4 all increased, and the particle size of Examples 1-4 increased.

[0078] Table 2 Discharge performance of Examples 1-4 and Comparative Examples 1-2

[0079]

[0080] As shown in Table 2, Figure 4 The figure is a rate performance diagram of the positive electrode materials prepared in Example 2, Example 4, and Comparative Example 1. In Table 2, the first, 100th, and 200th discharge specific capacities of Examples 1-4 are all higher than those of Comparative Examples 1-2, and the first, 100th, and 200th discharge / charge efficiency ratios are also higher. Figure 4At 0.1C and 0.2C, the rate performance of Example 2 and Example 4 is not obviously different from that of Comparative Example 1, but at 0.5C, 1C, 2C, and 5C, the rate performance of Example 2 and Example 4 is significantly better than that of Comparative Example 1. This indicates that after the deposition of nitrogen-doped-polymerized porous nanopowder, the charge transfer resistance of the sodium ion positive electrode material is reduced, the discharge stability of the material is improved, and the rate performance of the material is improved.

[0081] The embodiments of the present invention are described in detail above in conjunction with the accompanying drawings, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present invention. In addition, the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.

Claims

1. A nitrogen-doped-polymerized porous nanopowder deposited sodium ion positive electrode material, characterized in that: The general formula of the nitrogen-doped polymer porous nanopowder-deposited sodium ion cathode material is Na t Li f Ni s Z 1-s O2@aNMC-Y, where 0.8 ≤ t < 1, 0 ≤ f < 0.3, 0.5 ≤ s < 1, 0 < a < 0.1, Z is at least one of Mn, Mo, Co, Mg, and Al, and Y is at least one of Cu, Ga, Zn, Cr, and Zr; the NMC-Y is a nitrogen-doped polymer porous nanopowder; the preparation method of the NMC-Y is: mixing 3-hexyl-substituted polythiophene, a solvent, and a transition metal salt, stirring, reacting, and carbonizing to obtain.

2. The nitrogen-doped-polymerized porous nanopowder deposited sodium ion positive electrode material according to claim 1, characterized in that: The Na t Li f Ni s Z 1-s O2@NMC-Y, where 0.8 ≤ t < 1, 0 ≤ f < 0.2, 0.7 ≤ s < 1, 0 < a < 0.1, Z is at least one of Mn, Mo, Co, Mg, and Al, and Y is at least one of Cu, Ga, Zn, Cr, and Zr.

3. The nitrogen-doped-polymerized porous nanopowder deposited sodium ion positive electrode material according to claim 1, characterized in that: The nitrogen-doped-polymerized porous nanopowder is deposited with sodium ion positive electrode material Na t Li f Ni s Z 1-s O2@aNMC-Y is Na 0.8 Li 0.2 Ni 0. 7Co 0.05 Mg 0.05 Mn 0.2 O2@0.05NMC-Cu、Na 0.75 Li 0.25 Ni 0.60 Co 0.025 Mg 0.025 Mn 0.35 O2@0.025NMC-Cu、Na 0.88 Li 0.12 Ni 0.68 Co 0.065 Al 0.05 Mo 0.023 Mn 0.182 O2@0.0625NMC-Cu、Na 0.88 Li 0.12 Ni 0.765 Co 0.065 Al 0.05 Mo 0.023 Mn 0.097 One of O2@0.0875NMC-Zr.

4. A method for preparing a nitrogen-doped-polymerized porous nanopowder deposited positive electrode material, characterized in that: The preparation method is used to prepare the nitrogen-doped-polymerized porous nanopowder deposited positive electrode material according to any one of claims 1 to 3, comprising the following steps: (1) Mix nickel salt and Z salt, add carbonate to carry out precipitation reaction, separate solid and liquid, take the solid phase, add sodium source and lithium source to mix, sinter, and obtain sodium ion positive electrode material Na t Li f Ni s Z 1-s O2; (2) mixing and stirring 3-hexyl substituted polythiophene, a solvent, and a transition metal salt, reacting, and carbonizing to obtain nitrogen-doped-polymerized porous nanopowder NMC-Y; (3) A protective gas and a reducing gas are introduced into the sodium ion positive electrode material for purging, and then He-loaded nitrogen-doped-polymerized porous nanopowder is used for deposition to obtain the nitrogen-doped-polymerized porous nanopowder deposited positive electrode material; the Z salt is at least one of the chlorides, nitrates, and sulfates of Mn, Mo, Co, Mg, and Al.

5. The preparation method according to claim 4, characterized in that: In step (1), the nickel salt is at least one of nickel sulfate, nickel nitrate or nickel chloride; in step (1), the carbonate is at least one of sodium carbonate, sodium bicarbonate, potassium carbonate, magnesium carbonate, calcium carbonate or lithium carbonate.

6. The preparation method according to claim 4, characterized in that: In step (1), the sodium source is at least one of sodium hydroxide, sodium acetate, sodium oxalate, sodium phosphate or sodium citrate; the lithium source is at least one of lithium hydroxide, lithium acetate, lithium oxalate, lithium nitrate, lithium carbonate or lithium chloride.

7. The preparation method according to claim 4, characterized in that: In step (2), the transition metal salt is at least one of chloride, nitrate, sulfate, bromide and iodide of Cu, Ga, Zn, Cr and Zr.

8. The preparation method according to claim 4, characterized in that: In step (2), the solid-liquid ratio of the 3-hexyl substituted polythiophene, transition metal salt and solvent is (1-3) g: (0.01-0.5) g: (10-50) ml; in step (3), the sodium ion positive electrode material Na t Li f Ni s Z 1-s The mass ratio of O2 and nitrogen doped-polymerized porous nanopowder is (70-150): (1-10).

9. A battery, characterized in that: The invention comprises the nitrogen-doped-polymerized porous nanopowder deposited positive electrode material as described in any one of claims 1 to 3.

Citation Information

Patent Citations

  • Olivine sodium iron phosphate with polymer coating, sodium iron battery comprising the same as cathode material, and process thereof

    KR1020160136809A

  • KR20200109991A