Method for manufacturing optical laminate with adhesive layer having through hole and through hole forming device for the method
By using an end mill to cut and blow air to form through holes, the problems of insufficient adhesive and raised surfaces in optical laminates are solved, and efficient manufacturing of optical laminates is achieved.
Patent Information
- Application Number
- CN202080058479.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-05-23
- Filing Date
- 2020-12-11
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2040-12-11
AI Technical Summary
In the process of creating openings in optical laminates with adhesive layers, insufficient adhesive and/or unevenness of the surface protective film and separators can easily occur.
Through holes are formed by end mill cutting. By blowing air from the opposite direction of chip discharge during cutting, combined with clamping components and air blowing components, the cutting process is controlled to suppress missing glue and bulging.
It effectively suppresses the lack of adhesive and the protrusion of the surface protective film and separator, realizing a simple and low-cost optical laminate manufacturing process.
Smart Images

Figure CN114258333B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for manufacturing an optical laminate with an adhesive layer having through holes, and an apparatus for forming through holes in the manufacturing method. Background Technology
[0002] In image display devices such as mobile phones and laptops, various optical laminates (e.g., polarizers) are used to achieve image display and / or improve the performance of that image display. These optical laminates typically include an adhesive layer to form an optical laminate with an adhesive layer, allowing them to be attached to the image display unit. In recent years, due to the rapid proliferation of smartphones and touch-panel information processing devices, image display devices equipped with cameras have become widely used. Correspondingly, optical laminates with adhesive layers that have through-holes at positions corresponding to the camera unit are also widely used. Such through-holes can be formed, for example, by using an end mill for drilling.
[0003] Existing technical documents
[0004] Patent documents
[0005] Patent Document 1: International Publication No. 2017 / 047510 Summary of the Invention
[0006] The problem the invention aims to solve
[0007] However, in the opening process of optical laminates with adhesive layers, so-called missing adhesive (the phenomenon of missing ends of the adhesive layer) and / or protrusions in the surface protective film and / or separators used in the manufacturing process sometimes occur. The present invention was made to solve such problems, and its main objective is to provide a method for easily and inexpensively manufacturing optical laminates with adhesive layers and through holes that suppresses missing adhesive and protrusions in the surface protective film and separators.
[0008] Solution for solving the problem
[0009] A method for manufacturing an optical laminate with a through hole and an adhesive layer according to an embodiment of the present invention includes: stacking multiple optical laminates with adhesive layers to form a workpiece; and forming a through hole at a predetermined position in the workpiece by cutting with an end mill. The optical laminate with adhesive layer includes an optical film, an adhesive layer disposed on one side of the optical film, a release element temporarily bonded to the adhesive layer in a peelable manner, and a surface protective film temporarily bonded to the other side of the optical film in a peelable manner. Forming the through hole includes: cutting with an end mill against the end face of the hole; and blowing air in a direction opposite to the discharge direction of the end mill's chips during the cutting.
[0010] In one embodiment, the formation of the through hole includes: forming a pre-drilled hole; cutting with an end mill against the end face of the pre-drilled hole while simultaneously circling the end mill around the end face of the pre-drilled hole to form a next hole with a diameter a predetermined amount larger than the diameter of the pre-drilled hole; cutting with the end mill against the end face of the next hole while simultaneously circling the end face of the next hole to form yet another hole with a diameter a predetermined amount larger than the diameter of the next hole; and repeating the cutting along the end face of the hole by the circling end mill a predetermined number of times to form a through hole with a predetermined diameter, wherein air is blown during the formation of the next hole, the formation of the next hole, and the cutting by the circling end mill.
[0011] In one embodiment, the end mill's chips are discharged upwards, while the air is blown from below. In other embodiments, the end mill's chips are discharged downwards, while the air is blown from above.
[0012] In one embodiment, the air is blown from a direction within 30° of the rotation axis of the end mill.
[0013] In one embodiment, the workpiece is clamped from above and below by clamping members, and the air is blown at a distance of less than 20 mm from the upper end face of the upper clamping member or the lower end face of the lower clamping member.
[0014] In one embodiment, the formation of the through hole further includes blowing air from the chip discharge direction of the end mill and in a direction inclined relative to the rotation axis of the end mill.
[0015] According to another aspect of the present invention, a through-hole forming apparatus is provided. The through-hole forming apparatus includes: an end mill; a retaining member configured to move in a vertical direction and retain the end mill; and an air-blowing member fixed above or below the end mill and fixed in a direction within 30° of the axis of rotation of the end mill.
[0016] The effects of the invention
[0017] According to an embodiment of the present invention, in the formation of the through hole in an optical laminate with an adhesive layer having a through hole, cutting is performed while blowing air from a direction opposite to the chip discharge direction of the end mill, thereby suppressing adhesive loss and protrusion of the surface protective film and the separator. Attached Figure Description
[0018] Figure 1This is a schematic cross-sectional view illustrating an example of an optical laminate with an adhesive layer that can be used in the manufacturing method of an embodiment of the present invention.
[0019] Figure 2A This is a schematic cross-sectional view illustrating an example of a through-hole in an optical laminate with an adhesive layer that can be used in the manufacturing method of an embodiment of the present invention.
[0020] Figure 2B This is a schematic cross-sectional view illustrating other examples of through holes in an optical laminate with an adhesive layer that can be used in the manufacturing method of an embodiment of the present invention.
[0021] Figure 3 This is a schematic perspective view illustrating the general details of the formation of the through hole in the manufacturing method according to an embodiment of the present invention.
[0022] Figure 4 This is a schematic diagram illustrating the structure of an end mill with a helical cutting edge that can be used to form a through hole in the manufacturing method of an embodiment of the present invention.
[0023] Figure 5 This is a schematic diagram illustrating a representative example of the structure of an end mill with a helical cutting edge that can be used in the manufacturing method of an embodiment of the present invention, and the relationship between the chip discharge direction and the rotation direction.
[0024] Figure 6 This is a schematic top view illustrating the detailed process of forming a through hole in the manufacturing method according to an embodiment of the present invention.
[0025] Figure 7 This is a schematic top view illustrating the cutting process using an end mill in the formation of a through hole.
[0026] Figure 8 This is a schematic cross-sectional view illustrating the air jets used in the formation of the through-hole.
[0027] Figure 9 This is a microscope image showing the state of missing adhesive in the through-hole portion of the polarizer with an adhesive layer that has through-holes, obtained in Example 1.
[0028] Figure 10 This is a microscope image showing the state of the adhesive deficiency in the through-hole portion of the polarizer with an adhesive layer that has through-holes, obtained in Example 2.
[0029] Figure 11 This is a microscope image showing the state of missing adhesive in the through-hole portion of the polarizer with an adhesive layer that has through-holes, obtained in Comparative Example 1. Detailed Implementation
[0030] Hereinafter, specific embodiments of the present invention will be described with reference to the accompanying drawings, but the present invention is not limited to these embodiments. Furthermore, for ease of viewing, the drawings are shown schematically, and the proportions of length, width, thickness, and angles in the drawings differ from the actual figures.
[0031] A method for manufacturing an optical laminate with a through-hole and an adhesive layer according to an embodiment of the present invention includes: stacking multiple optical laminates with adhesive layers to form a workpiece; and forming a through-hole at a predetermined position on the workpiece by cutting with an end mill. The optical laminate with an adhesive layer includes an optical film, an adhesive layer disposed on one side of the optical film, a release element temporarily bonded to the adhesive layer in a peelable manner, and a surface protective film temporarily bonded to the other side of the optical film in a peelable manner. In an embodiment of the present invention, forming the through-hole includes: cutting by abutting the end mill against the end face of the hole; and blowing air from a direction opposite to the discharge direction of the end mill's chips during the cutting. For convenience, firstly, a specific structure of an optical laminate with an adhesive layer that can be used in the manufacturing method of an embodiment of the present invention will be described, and then, a method for manufacturing an optical laminate with a through-hole and an adhesive layer according to an embodiment of the present invention will be described.
[0032] A. Optical laminate with adhesive layer
[0033] Figure 1 This is a schematic cross-sectional view illustrating an example of an optical laminate with an adhesive layer that can be used in the manufacturing method of an embodiment of the present invention. The example optical laminate 100 with an adhesive layer includes an optical film 10, an adhesive layer 20 disposed on one side of the optical film 10, a release member 30 temporarily bonded to the adhesive layer 20 in a peelable manner, and a surface protective film 40 temporarily bonded to the other side of the optical film 10 in a peelable manner. In the case where the optical laminate with the adhesive layer is applied to an image display device, the release member 30 is typically disposed on the image display unit side. In actual use of the optical laminate with the adhesive layer, the release member 30 is peeled off, and the adhesive layer 20 can be used to adhere the optical laminate with the adhesive layer to the image display device (essentially the image display unit). The surface protective film 40 typically has a substrate 41 and an adhesive layer 42. Furthermore, to distinguish it from the adhesive layer 20, the adhesive layer 42 of the surface protective film is sometimes referred to as the "PF adhesive layer." Additionally, the surface protective film 40 is also peeled off during actual use of the optical laminate with the adhesive layer.
[0034] In an embodiment of the present invention, the optical laminate with an adhesive layer has a through hole 50 at a predetermined position. The through hole 50 can be as follows: Figure 2A As shown, one can be formed, or as shown in the diagram. Figure 2B As shown, two holes can be formed, but more than three can also be formed (not shown). For example, when two through holes are formed, it can be done as follows: Figure 2B The through-holes can be formed side-by-side along the short side, or side-by-side along the long side, or randomly. The location of the through-holes can be appropriately set according to the purpose. Through-holes are typically formed at or near the end of the optical laminate with the adhesive layer, preferably at the corner as shown in the example. By forming the through-holes at or near the end of the optical laminate with the adhesive layer, the impact on image display can be minimized when the optical laminate with the adhesive layer is applied to an image display device. In one embodiment, the through-hole can be formed at a position corresponding to the camera section of the image display device. The top view shape of the through-hole can be any suitable shape depending on the purpose and the desired structure of the image display device. As a representative example, a roughly circular shape as shown in the example can be used. The size of the through-hole (diameter in the example) is, for example, 5 mm or less, preferably 1 mm to 5 mm, more preferably 2 mm to 4 mm. Furthermore, in Figure 1 The depiction of the through hole is omitted. According to an embodiment of the present invention, as described later, during the formation of the through hole, cutting is performed while blowing air from a direction opposite to the chip discharge direction of the end mill, thereby suppressing adhesive defects and protrusions in the surface protective film and the separator. That is, according to an embodiment of the present invention, the unique problems in the manufacturing method of an optical laminate with an adhesive layer, including an adhesive layer, a separator, and a surface protective film, can be solved.
[0035] As the optical thin film 10, any suitable optical thin film for applications requiring through holes can be cited. The optical thin film can be a thin film composed of a single layer or a laminate. Specific examples of optical thin films composed of a single layer include polarizers and phase difference films. Specific examples of optical thin films configured as laminates include polarizers (representatively a laminate of a polarizer and a protective film), conductive films for touch panels, surface-treated films, and laminates formed by appropriately stacking the above-mentioned optical thin films composed of single layers and / or optical thin films configured as laminates according to the purpose (e.g., circular polarizers for anti-reflection, polarizers with conductive layers for touch panels).
[0036] The adhesive layer 20 can have any suitable structure. Specific examples of adhesives constituting the adhesive layer include acrylic adhesives, rubber adhesives, silicone adhesives, polyester adhesives, polyurethane adhesives, epoxy adhesives, and polyether adhesives. By adjusting the type, quantity, combination, and mixing ratio of the monomers in the base resin forming the adhesive, as well as the mixing amount of the crosslinking agent, reaction temperature, and reaction time, an adhesive with desired properties corresponding to the purpose can be formulated. The base resin of the adhesive can be used alone or in combination of two or more. From the viewpoints of transparency, processability, and durability, acrylic adhesives are preferred. Detailed information about the adhesive constituting the adhesive layer is described, for example, in Japanese Patent Application Publication No. 2014-115468, which is incorporated herein by reference. The thickness of the adhesive layer 20 is, for example, 10 μm to 100 μm.
[0037] The creep value of the adhesive layer 20 at 85°C is, for example, less than 500 μm, preferably 5 μm to 500 μm. In one embodiment, the creep value is preferably 200 μm to 450 μm, more preferably 220 μm to 420 μm. In other embodiments, the creep value is preferably 5 μm to 300 μm, more preferably 5 μm to 200 μm, and even more preferably 10 μm to 100 μm. If the creep value is within such a range, insufficient adhesive can be significantly suppressed when forming through-holes, and peeling under high temperature and high humidity conditions can be significantly suppressed. It is speculated that when the creep value is relatively large (e.g., above 200 μm), insufficient adhesive can also be suppressed by controlling the composition of the adhesive constituting the adhesive layer (e.g., the type of base polymer (polarity, Tg, softness), molecular weight) and crosslinking structure (e.g., the type of crosslinking agent, the distance between crosslinking points (molecular weight between crosslinking points), the crosslinking density, and the amount of uncrosslinked components (sol)). Furthermore, creep values can be measured, for example, by attaching a test sample cut from an optical laminate with an adhesive layer to a support plate with a 10mm × 10mm joint surface. With the support plate containing the test sample fixed in place, a load of 500gf is applied vertically downwards. The offset relative to the support plate is measured 1 second after the load is applied and 3600 seconds later, denoted as Cr1 and Cr, respectively. 3600 Based on Cr1 and Cr 3600 The creep value is defined as ΔCr obtained from the following formula.
[0038] ΔCr=Cr 3600 -Cr1
[0039] The energy storage modulus of the adhesive layer 20 at 85°C is preferably 1.0 × 10⁻⁶. 4 Pa or higher, preferably 2.0 × 10 Pa. 4 Pa or higher, more preferably 5.0 × 10 Pa.4 Pa or higher, more preferably 1.0 × 10 Pa 5 Pa or higher. If the energy storage modulus is within this range, the desired creep value can be easily achieved. On the other hand, the energy storage modulus is, for example, 3.0 × 10⁻⁶ Pa. 6 Below Pa. Furthermore, the storage modulus can be determined, for example, by dynamic viscoelasticity measurements.
[0040] As the separating element 30, any suitable separating element can be used. Specific examples include plastic films, non-woven fabrics, or paper coated with a release agent. Specific examples of release materials include silicone-based release agents, fluorinated release agents, and long-chain alkyl acrylate-based release agents. Specific examples of plastic films include polyethylene terephthalate (PET) films, polyethylene films, and polypropylene films. The thickness of the separating element is, for example, 10 μm to 100 μm.
[0041] As described above, the surface protective film 40 typically comprises a substrate 41 and an adhesive layer 42. Examples of materials forming the substrate 41 include ester resins such as polyethylene terephthalate resins, cyclic olefin resins such as norbornene resins, olefin resins such as polypropylene, polyamide resins, polycarbonate resins, and copolymers thereof. Ester resins (especially polyethylene terephthalate resins) are preferred. Using such a material provides the advantage of a sufficiently high elastic modulus, making it less prone to deformation even when tension is applied during transport and / or bonding.
[0042] The elastic modulus of substrate 41 is, for example, 2.2 kN / mm². 2 ~4.8kN / mm 2 If the elastic modulus of the substrate is within such a range, it has the advantage of not easily deforming even when tension is applied during transport and / or bonding. Furthermore, the elastic modulus is measured based on JIS K 6781.
[0043] The thickness of the substrate 41 is, for example, 30 μm to 70 μm.
[0044] As the adhesive layer (PF adhesive layer) 42, any suitable structure can be adopted. Specific examples include acrylic adhesives, rubber adhesives, silicone adhesives, polyester adhesives, polyurethane adhesives, epoxy adhesives, and polyether adhesives. By adjusting the type, quantity, combination, and mixing ratio of the monomers of the base resin forming the adhesive, as well as the mixing amount of the crosslinking agent, reaction temperature, and reaction time, an adhesive with desired properties corresponding to the purpose can be formulated. The base resin of the adhesive can be used alone or in combination of two or more. The adhesive constituting the PF adhesive layer is characterized by the base resin containing a polymer having active hydrogen functional groups. Using such a base resin, a PF adhesive layer with a desired storage modulus can be obtained. Detailed information about the adhesive constituting the PF adhesive layer is described, for example, in Japanese Patent Application Publication No. 2018-123281, which is incorporated herein by reference. The thickness of the PF adhesive layer 42 is, for example, 10 μm to 100 μm. The storage modulus G' of PF adhesive layer 42 at 25°C is, for example, 0.5 × 10⁻⁶. 6 (Pa)~3.0×10 6 (Pa). If the storage modulus is within this range, an adhesive layer with an excellent balance between adhesion and peelability can be obtained (resulting in a surface protective film).
[0045] The thickness of the surface protective film 40 is, for example, 40 μm to 120 μm. Furthermore, the thickness of the surface protective film refers to the total thickness of the substrate and the PF adhesive layer.
[0046] B. Method for manufacturing optical laminates with adhesive layers
[0047] The following describes a representative example of a method for manufacturing an optical laminate with an adhesive layer.
[0048] B-1. Formation of the workpiece
[0049] First, the workpiece is formed. Figure 3 This is a schematic perspective view illustrating the general details of the formation of a through hole in the manufacturing method according to an embodiment of the present invention. The workpiece W is shown in this view. Figure 3As shown, a workpiece W is formed by stacking multiple optical laminates with adhesive layers. During workpiece formation, the optical laminates with adhesive layers are typically cut into any suitable shape. Specifically, the optical laminates with adhesive layers can be cut into rectangular shapes, rectangular-like shapes, or suitable shapes corresponding to the purpose (e.g., circles). In one embodiment, the workpiece W has outer peripheral surfaces (cutting surfaces) 1a, 1b opposite each other and outer peripheral surfaces (cutting surfaces) 1c, 1d orthogonal to them. Preferably, as shown in the example, the workpiece W is held from above and below by a clamping member C including an upper clamp C1 and a lower clamp C2. The total thickness of the workpiece is preferably 3 mm or more, more preferably 5 mm to 40 mm, and even more preferably 10 mm to 30 mm. For example, when the diameter of the through hole is 2 mm to 3 mm, the total thickness of the workpiece is preferably 10 mm to 25 mm. The optical laminates with adhesive layers are stacked such that the workpiece has this total thickness. The number of optical laminates with adhesive layers constituting the workpiece can vary depending on the thickness of the optical laminate with adhesive layers. The number of optical laminates with adhesive layers is preferably 50 or more, more preferably 50 to 200, and even more preferably 75 to 150. The clamping components (e.g., jigs) can be made of either a soft or a hard material. When made of a soft material, its hardness (JIS A) is preferably 60° to 80°. If the hardness is too high, indentations may sometimes be left on the clamping components. If the hardness is too low, positional displacement may sometimes occur due to jig deformation, resulting in insufficient cutting accuracy.
[0050] B-2. Formation of through holes
[0051] Next, through holes are formed in the workpiece (essentially an optical laminate with an adhesive layer). For example... Figure 3 As shown, a through hole can be formed by cutting with an end mill. Furthermore, in Figure 3 The diagram schematically illustrates the initial pre-drilled hole and the final through hole. Below, we will first describe the end mills that can be used to form the through hole, and then explain the specific steps involved in forming the through hole.
[0052] B-2-1. Structure of an end mill
[0053] The end mill 60 may have a helical cutting edge (which may have a predetermined cutting angle), or the cutting angle may be 0°. A representative example of the end mill 60 is... Figure 3 and Figure 4As shown, it has a helical cutting edge. The effect is more pronounced when cutting with an end mill having a helical cutting edge while blowing air in the opposite direction to the chip removal direction (described later). This is because it is easy to set the chip removal direction and the air blowing direction to the desired relationship. For example... Figure 4 As shown, the end mill 60 with a helical cutting edge has: a rotation axis 61 extending along the stacking direction (vertical direction) of the workpiece W; and a cutting edge 62 configured as the outermost diameter of a main body rotating around the rotation axis 61. In the example shown, the cutting edge 62 is configured as the outermost diameter twisted along the rotation axis 61, and a right-hand helix is shown in the example. The cutting edge 62 includes a tip 62a, a rake face 62b, and a flank face 62c. The number of cutting edges 62 can be appropriately set according to the purpose. The cutting edge in the example is a three-piece structure, but the number of cutting edges can be one consecutive piece, two pieces, four pieces, or more than five pieces. The cutting edge angle of the end mill (the helix angle θ of the cutting edge in the example) is preferably 25° to 75°, more preferably 40° to 60°. The rake angle is preferably 15° to 25°, and the clearance angle is preferably 10° to 20°. The flank face of the cutting edge is preferably roughened. As a roughening treatment, any suitable treatment can be adopted. Sandblasting is a representative example. By roughening the flank face, the adhesion of the adhesive to the cutting edge can be suppressed, and as a result, adhesion can be suppressed. The outer diameter of the end mill is preferably 0.5 mm to 10 mm, more preferably 0.8 mm to 5 mm, and even more preferably 1 mm to 3 mm. The effective length of the cutting edge of the end mill is preferably 10 mm to 50 mm, more preferably 20 mm to 40 mm. Furthermore, in this specification, "adhesion" refers to the phenomenon where optical laminates with adhesive layers in a workpiece adhere to each other due to the adhesive on their end faces; chips with adhesive adhering to the end faces can promote adhesion between the optical laminates with adhesive layers. Additionally, "outer diameter of the end mill" refers to twice the distance from the rotation axis 61 to the tip 62a.
[0054] Next, we will explain the relationship between the structure of the end mill and the direction of chip discharge and rotation. Figure 5 This is a schematic diagram illustrating a representative example of the structure of an end mill with a helical cutting edge that can be used in the manufacturing method of an embodiment of the present invention. Figure 5 As shown, end mills with helical cutting edges can be broadly categorized into right-hand right-helical, right-hand left-helical, left-hand right-helical, and left-hand left-helical. For example... Figure 5 As shown, the right cutting edge refers to the structure that allows cutting when rotated clockwise as viewed from above (shank side); the left cutting edge refers to the structure that allows cutting when rotated counterclockwise as viewed from above (shank side). Figure 5As further illustrated, a right-hand helix refers to a structure in which the tip extends diagonally upward to the right when viewed from the side; a left-hand helix refers to a structure in which the tip extends diagonally upward to the left when viewed from the side. The chip discharge direction for right-hand right-hand helical cutters and left-hand left-hand helical cutters is upward; the chip discharge direction for right-hand left-hand helical cutters and left-hand right-hand helical cutters is downward. In one embodiment, the chip discharge direction of the end mill is upward. In this case, the end mill is either a right-hand right-hand helix or a left-hand left-hand helix. With such a structure, by cutting while blowing air from below, it is possible to suppress insufficient adhesive and the protrusion of the surface protective film and separators. In other embodiments, the chip discharge direction of the end mill is downward. In this case, the end mill is either a right-hand left-hand helix or a left-hand right-hand helix. With such a structure, by cutting while blowing air from above, it is possible to suppress insufficient adhesive and the protrusion of the surface protective film and separators.
[0055] B-2-2. Formation of a through hole
[0056] The following is for reference Figures 6-8 This section illustrates a representative example of forming a through hole using an end mill as described above.
[0057] First, such as Figure 6 As shown, a pre-drilled hole 51 is formed. In this specification, "pre-drilled hole" refers to a hole that serves as a basis for forming a through hole in the correct position. The pre-drilled hole 51 is typically formed by cutting with an end mill 60, whose upper end is held, moving from top to bottom. The diameter of the pre-drilled hole 51 is substantially the same as the outer diameter of the end mill 60.
[0058] Next, as Figure 7 As shown, while the end mill 60 is cutting against the end face of the pre-drilled hole 51, the end mill 60 is also moved around the end face of the pre-drilled hole 51. The result is as follows: Figure 6 and Figure 7 As shown, a next hole 52 with a diameter P larger than the diameter of the pre-drilled hole 51 is formed. While cutting one revolution to form the next hole 52, the end mill is simultaneously cut against the end face of the next hole 52, and then wound around the end face of the next hole 52 to form another next hole 53 with a diameter P larger than the diameter of the next hole 52. Hereinafter, by repeating the same steps, through holes with the desired diameter are formed (including cases where the end mill's path is a top-view spiral cut). Furthermore, in this specification, the predetermined amount P is sometimes referred to as the cutting distance.
[0059] The cutting distance P can vary depending on the size of the through hole, the outer diameter of the end mill, and the number of times the end mill rotates. The number of times the end mill rotates can also vary depending on the size of the through hole, the outer diameter of the end mill, and the cutting distance P. The cutting distance can be, for example, 5μm to 200μm, preferably 50μm to 100μm. For example, when the through hole size is 3.9mm, the outer diameter of the end mill is 2mm, and the cutting distance P is 100μm, the number of times the end mill rotates is 10.
[0060] The cutting conditions for forming the through hole can be appropriately set according to the size of the through hole, the outer diameter of the end mill, and the number of turns of the end mill. The rotational speed of the end mill is preferably 1000 rpm to 10000 rpm, more preferably 1000 rpm to 5000 rpm. The feed rate of the end mill is preferably 10 mm / min to 2000 mm / min, more preferably 50 mm / min to 500 mm / min.
[0061] A through hole 50 with a predetermined diameter is formed by repeating the cutting along the end face of the hole with an end mill as described above a predetermined number of times (i.e., cutting with an end mill a predetermined number of times around the hole). The end face of the through hole may also be finely cut as needed.
[0062] B-2-3. Air jetting
[0063] In an embodiment of the invention, air is blown from a direction opposite to the chip removal direction of the end mill while a through hole is formed (for cutting). In one embodiment, such as Figure 8 As shown, air is blown from below. In this case, the end mill's chips are discharged upwards. In other embodiments not shown, the end mill's chips are discharged downwards, and air is blown from above. The following is an example. Figure 8 The implementation method. In Figure 8 In this embodiment, an air jetting component 82 is provided below the end mill 60, which jets air upwards (essentially the through hole formed by the end mill cutting). As described above, since the chip discharge direction of the end mill is upwards, the air jetting (air supply) proceeds from the side opposite to the chip discharge direction. With this structure, chip discharge can be further improved, thus better suppressing defects in the adhesive and the protrusion of the surface protective film and the release element.
[0064] The air is typically blown from a direction within a predetermined angle θ relative to the axis of rotation (vertical direction) of the end mill 60. The angle θ is preferably within 30°, more preferably within 20°, further preferably within 10°, and particularly preferably within 5°. The angle θ can also be 0° (i.e., air can also be blown upwards in the vertical direction). Figure 8 The diagram shows an implementation where angle θ is 0°. When angle θ is 0°, chip removal is very efficient. On the other hand, when angle θ is a predetermined angle, the end mill can be fixed at both ends for cutting.
[0065] The air jetting is typically performed at a distance within a predetermined range to the workpiece. Specifically, the distance L between the upper end face of the upper clamping member C1 or the lower end face of the lower clamping member C2 and the outlet of the air jetting member 82 (in the example shown, the distance between the lower end face of the lower clamping member C2 and the outlet of the air jetting member 82) is preferably within 20 mm, more preferably within 10 mm, further preferably within 5 mm, particularly preferably within 3 mm, and especially preferably 0 mm (i.e., the lower end face of the lower clamping member C2 and the outlet of the air jetting member 82 are on the same surface). Regarding the air jetting, the shorter the distance to the workpiece, the smaller the pressure loss of the jetted air. As a result, cutting chips can be discharged very well.
[0066] The pressure of the blown air (supply pressure) is, for example, 0.05 MPa to 1 MPa, preferably 0.2 MPa to 0.5 MPa. The air velocity is, for example, 1,500 m / min to 15,000 m / min, and the air volume is, for example, 5 L / min to 1,000 L / min.
[0067] In one embodiment, in the formation of the through hole, except from the direction opposite to the direction of chip discharge from the end mill (in... Figure 8 In addition to blowing air (as shown in the example below), air can also be sprayed from the direction of chip removal of the end mill and in a direction inclined relative to the axis of rotation of the end mill (in...). Figure 8 In the example, air is sprayed from an upward angle. Figure 8In the example shown, an air jetting component 84 is provided obliquely above the hole cut by the end mill 60, and air is jetted toward the hole. By further jetting air from obliquely above, cutting chips that are discharged to the upper side of the workpiece due to the air jetting from below can be blown away and removed. As a result, cutting chips can be removed more effectively, and therefore, the defects in the adhesive, as well as the protrusion of the surface protective film and the separation parts, can be further suppressed more effectively. The pressure, velocity, and volume of the jetting air are as described above regarding the jetting from below. Furthermore, as mentioned above, when air is jetted from above the end mill (when the discharge direction of the cutting chips from the end mill is downward), air can also be jetted from obliquely below.
[0068] A typical scenario involves blowing air in the opposite direction to the chip removal direction of the end mill, at least during cutting around the end mill (i.e., the formation of the next hole and subsequent cutting). Air blowing can also occur during pre-drilling or during finish cutting.
[0069] As described above, an optical laminate with an adhesive layer and through-holes can be obtained. The optical laminate with an adhesive layer obtained by the manufacturing method of the present invention suppresses adhesive defects and protrusions in the surface protective film and separators.
[0070] C. Through-hole forming device
[0071] The manufacturing method of the embodiment of the present invention described in item B above can be performed using a through-hole forming apparatus. Therefore, embodiments of the present invention also include such a through-hole forming apparatus. Regarding the general outline of the through-hole forming apparatus of the embodiments of the present invention, as well as the through-hole forming method, please refer to... Figure 8As described in section B-2-3 above, the through-hole forming apparatus includes: an end mill 60; a holding member configured to move vertically and hold the end mill; and an air jetting member 82 fixed below the end mill and in a direction within 30° of the axis of rotation of the end mill (0° in the example, i.e., vertically downward). The air jetting member 82 can be of any suitable structure. For example, an air gun can be used. The air jetting member 82 can be mounted and fixed at any suitable position below the end mill of the apparatus (e.g., an unused lower collet). The air jetting member 82 is mounted at a predetermined angle θ relative to the axis of rotation (vertical direction) of the end mill, depending on the mounting position. Alternatively, the air jetting member 82 may not be fixed. For example, if it is a hose-shaped air jetting member, air can be manually blown from the desired position. In one embodiment, the through-hole forming apparatus may further include an air jetting member 84 obliquely above the workpiece setting portion. As described above, the air jet component 82 can also be located above the end mill. In this case, the air jet component 84 can also be located diagonally below the workpiece mounting portion, as needed.
[0072] [Example]
[0073] The present invention will now be described in detail through embodiments, but the present invention is not limited to these embodiments. The evaluation criteria for the embodiments are as follows.
[0074] (1) The raised surface of the separating part
[0075] Ten optical laminates with adhesive layers and through holes were extracted from the workpieces obtained in the Examples and Comparative Examples. These ten optical laminates were formed by randomly selecting one piece from each of the workpieces, which were then divided equally into ten parts along their thickness direction. For each of the ten optical laminates with adhesive layers, the protrusions of the separated parts were observed using a magnifying glass or microscope. If no protrusions larger than 50 μm were observed, the optical laminate with adhesive layers was considered a "protrusion-free" sample. The percentage (%) of the ten "protrusion-free" samples was used as the evaluation criterion.
[0076] A: More than 9 / 10 of the samples are "non-convex".
[0077] B: Less than 9 / 10 samples have "no convexity".
[0078] (2) The raised surface of the protective film
[0079] Similar to (1) above, the surface protective film was observed for unevenness. If no unevenness greater than 50 μm was observed, the optical laminate with the adhesive layer was considered a "non-uneven" sample. The percentage (%) of "non-uneven" samples out of 10 pieces was used as the evaluation criterion.
[0080] A: More than 9 / 10 of the samples are "non-convex".
[0081] B: Less than 9 / 10 samples have "no convexity".
[0082] (3) Lack of glue
[0083] Similar to (1) above, the lack of glue at the end of the through hole is observed using a microscope, and the image of the microscope is judged by visual inspection.
[0084] <Example 1>
[0085] A polarizer with an adhesive layer was fabricated using conventional methods. The structure consisted of a surface protective film (58 μm), a brightness enhancement film (26 μm), an adhesive layer (12 μm), a polarizing element (5 μm), an acrylic resin film (protective film, 20 μm), another adhesive layer (20 μm), and a separator (38 μm). Furthermore, a surface protective film with a structure of a PET substrate (38 μm) and a PF adhesive layer (20 μm) was used. The creep value of the adhesive layer adjacent to the separator was 94 μm. The resulting polarizer with the adhesive layer was punched to a 5.7-inch size (approximately 140 mm in length and 65 mm in width). Ninety punched polarizers were overlapped to form a workpiece (total thickness approximately 15 mm). While the workpiece was held in a fixture, a cantilevered end mill was used to cut from the surface protective film side, creating pre-drilled holes (2 mm in diameter) at the corners. During the pre-drilling process, air is blown obliquely above the workpiece (essentially the pre-drilled hole formed by cutting). Then, by utilizing methods such as... Figure 6 and Figure 7The end mill, as shown, is used for circling cutting to form a through hole with a diameter of 3.9 mm. More details are as follows. The end mill used in forming the through hole is cantilevered, with an outer diameter of 2.0 mm, an effective cutting edge length of 20 mm, a cutting edge angle of 50°, a rake angle of 18°, a clearance angle of 15°, and is a right-handed, right-hand helical cutter (chip discharge direction is upward). The cutting pitch is 100 μm, the end mill's travel speed during circling is 250 mm / min, and the rotational speed is 2500 rpm. In this embodiment, during circling cutting using the end mill, air is blown from directly below the end mill (on the end mill's axis of rotation, θ = 0°) and 10 mm from the lower end face of the lower clamp. Similarly, as when forming a pre-drilled hole, air is blown from obliquely above the workpiece. Furthermore, the blowing of air from below is performed by fixing an air gun to the lower collet. The obtained polarizers with through holes and adhesive layers were evaluated according to the above (1) to (3). The results are shown in Table 1. Furthermore, in Figure 9 The image shows the state of insufficient adhesive in the through-hole section.
[0086] <Example 2>
[0087] Air was blown from a distance of 2 mm from the lower end face of the lower clamp. Otherwise, a polarizer with a through-hole and adhesive layer was prepared in the same manner as in Example 1. The obtained polarizer with a through-hole and adhesive layer was evaluated in the same manner as in Example 1. The results are shown in Table 1. Furthermore, in Figure 10 The image shows the state of insufficient adhesive in the through-hole section.
[0088] <Example 3>
[0089] Air was blown from a distance of 0 mm from the lower end face of the lower fixture, and the number of stacked polarizers with adhesive layers was increased to make the total thickness of the workpiece approximately 25 mm. Otherwise, a polarizer with a through-hole and adhesive layer was obtained in the same manner as in Example 1. The obtained polarizer with a through-hole and adhesive layer was evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0090] <Comparative Example 1>
[0091] In the cutting process using an end mill, no air blowing from below was performed. Otherwise, a polarizer with a through-hole and adhesive layer was obtained in the same manner as in Example 1. The obtained polarizer with a through-hole and adhesive layer was evaluated in the same manner as in Example 1. The results are shown in Table 1. Furthermore, in Figure 11 The image shows the state of insufficient adhesive in the through-hole section.
[0092] [Table 1]
[0093]
[0094] <Evaluation>
[0095] As shown in Table 1, according to the embodiments of the present invention, in the formation of the through-hole of the optical laminate with the adhesive layer, cutting is performed while blowing air from a direction opposite to the chip discharge direction of the end mill, thereby suppressing insufficient adhesive and the protrusion of the surface protective film or delamination. Furthermore, in Example 3, the total thickness of the workpiece was set to approximately 25 mm, which is greater than that of Examples 1 and 2, but visual inspection confirmed that the attached foreign matter fell within the standard value of "100 μm or more and less than one," indicating no problem. In addition, in Examples 1 to 3, the following was confirmed: in all 10 samples, cracks met the standard value of "150 μm or less," attached foreign matter met the standard value of "100 μm or more and less than one," and delamination met the standard value of "150 μm or less."
[0096] Industrial availability
[0097] The manufacturing method of the present invention is suitable for manufacturing optical laminates with adhesive layers that require through holes. The optical laminates with adhesive layers obtained according to the manufacturing method of the present invention are suitable for use in automotive dashboards, smartwatches, and image display units with through holes, such as image display devices with camera units.
[0098] Explanation of reference numerals in the attached figures
[0099] W, workpiece; C, clamping component; 10, optical film; 20, adhesive layer; 30, separator; 40, surface protective film; 60, end mill; 82, air jet component; 84, air jet component; 100, optical laminate with adhesive layer.
Claims
1. A method for manufacturing an optical laminate with an adhesive layer having through holes, wherein, The manufacturing method includes: To form a workpiece by stacking multiple optical laminates with adhesive layers; and A through hole is formed at a predetermined position on the workpiece by using an end mill. The optical laminate with an adhesive layer includes an optical film, an adhesive layer disposed on one side of the optical film, a release element temporarily bonded to the adhesive layer in a peelable manner, and a surface protective film temporarily bonded to the other side of the optical film in a peelable manner. The formation of this through hole includes: Pre-drilled holes were formed; While the end mill is cutting against the inner circumferential surface of the pre-drilled hole, the end mill is also made to circle around the inner circumferential surface of the pre-drilled hole to form a next hole with a diameter that is a predetermined amount larger than the diameter of the pre-drilled hole, and a gap is formed between the end mill and the formed hole. While cutting by contacting the end mill against the inner circumferential surface of the next hole, the end mill is also moved around the inner circumferential surface of the next hole to form a further next hole with a diameter that is a predetermined amount larger than the diameter of the previous hole; and A predetermined number of cuts are made along the inner circumferential surface of the hole by using an end mill to form a through hole of a predetermined diameter. Air is blown onto the workpiece during the formation of the next hole, the next hole after that, and during cutting through the perimeter of the end mill. The end mill's chips are discharged upwards, and the air is blown from below the workpiece towards it. The angle between the rotation axis of the end mill and the direction of the air jet is within 30°.
2. The manufacturing method according to claim 1, wherein, The workpiece is clamped from above and below by clamping components. The air is blown at a distance of less than 20 mm from the lower end face of the clamping component on the lower side.
3. The manufacturing method according to claim 1 or 2, wherein, The formation of the through hole also includes blowing air toward the workpiece from the upper side of the workpiece in a direction inclined relative to the rotation axis of the end mill.
4. A through-hole forming apparatus, wherein, The through-hole forming device has the following features: An end mill, positioned above a workpiece and configured to discharge cutting chips upwards, the workpiece being formed by stacking multiple optical laminates with adhesive layers, the optical laminates with adhesive layers including an optical film, an adhesive layer disposed on one side of the optical film, a separator temporarily bonded to the adhesive layer in a peelable manner, and a surface protective film temporarily bonded to the other side of the optical film in a peelable manner. A retaining member configured to move in the vertical direction and to hold the end mill in a manner that allows it to move circumferentially along the hole; as well as An air jetting component is configured to be positioned below the workpiece and to jet air onto the workpiece in such a manner that the angle between the rotation axis of the end mill and the air jetting direction is within 30°.
Citation Information
Patent Citations
Optical film having adhesive agent on both sides, and manufacturing method of image display unit using the same
JP2014115468A
Adhesive composition, adhesive layer, surface protection film and optical member
JP2018123281A
Method for producing differently shaped polarizing plate
WO2017047510A1
Apparatus for preventing cutting chipps from adhering to drill shank
JP1997262710A
Cutting method and device thereof
JP1999197928A