Shell manufacturing method, ceramic shell, and electronic device

By forming a glaze layer and engraving patterns on the surface of the ceramic shell, the problem of monotonous shell appearance is solved, and a variety of appearance effects are achieved.

CN114349538BActive Publication Date: 2026-11-24GUANGDONG OPPO MOBILE TELECOMMUNICATIONS CORP LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202210108618.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-28
Publication Date
2026-11-24
Estimated Expiration
2042-01-28

AI Technical Summary

Technical Problem

The current electronic device casings have a monotonous appearance and cannot meet users' pursuit of a richer aesthetic.

Method used

A shell with a first pattern is prepared by forming a first glaze layer on the surface of the ceramic shell body and forming a patterned layer by laser engraving.

Benefits of technology

The prepared shell has a good appearance and meets users' needs for diverse appearances.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114349538B_ABST
    Figure CN114349538B_ABST
Patent Text Reader

Abstract

This application provides a method for manufacturing a housing, a ceramic housing, and an electronic device. The housing manufacturing method includes: providing a ceramic housing body; forming a first glaze layer on at least a portion of the surface of the ceramic housing body, the first glaze layer being formed from a first glaze slurry; and engraving the first glaze layer to form a first patterned layer to obtain a housing with a first pattern. The housing manufactured by the method provided in this application has good performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of electronic technology, and in particular to a method for preparing a housing, a ceramic housing, and an electronic device. Background Technology

[0002] With the development of technology, electronic devices such as mobile phones and tablets have become indispensable tools for people. When faced with a dazzling array of electronic devices, consumers not only need to consider whether the functions of the devices meet their needs, but the appearance of the device's casing is also a crucial factor influencing their purchase decision. However, the appearance of casings in related technologies is relatively limited, failing to satisfy users' diverse aesthetic preferences. Summary of the Invention

[0003] In a first aspect, this application provides a method for preparing a shell, the method comprising:

[0004] Provides a ceramic housing body;

[0005] A first glaze layer is formed on at least a portion of the surface of the ceramic housing body, the first glaze layer being formed from a first glaze slurry; and

[0006] The first glaze layer is engraved to form a first patterned layer to obtain a shell with a first pattern.

[0007] Secondly, this application provides a housing, the housing comprising:

[0008] Ceramic shell body; and

[0009] A coloring substance is disposed within the ceramic housing body and located in at least a portion of the ceramic housing body, such that the housing has a first pattern.

[0010] Thirdly, this application provides an electronic device, which includes a housing as described in the second aspect.

[0011] The shell prepared by the shell preparation method provided in this application has a first pattern, therefore, the shell has a better appearance. Attached Figure Description

[0012] To more clearly illustrate the technical solutions of the embodiments of this application, the drawings used in the implementation will be briefly introduced below. Obviously, the drawings described below are some implementations of this application. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.

[0013] Figure 1A flowchart illustrating a shell preparation method provided in one embodiment of this application;

[0014] Figure 2 for Figure 1 A schematic diagram of the process included in S120;

[0015] Figure 3 (a)~ Figure 3 (f) is Figure 1 and Figure 2 A structural diagram corresponding to each step in the process;

[0016] Figure 4 for Figure 1 A schematic diagram of the process included in S130;

[0017] Figure 5 for Figure 1 A schematic diagram of the process included in S130;

[0018] Figure 6 for Figure 1 A schematic diagram of the process included in S110;

[0019] Figure 7 for Figure 6 A flowchart of the process included in S111;

[0020] Figure 8 for Figure 7 A schematic diagram of the process included in S1112;

[0021] Figure 9 for Figure 6 A flowchart of the process included in S112;

[0022] Figure 10 for Figure 6 A flowchart of the process included in S113;

[0023] Figure 11 A flowchart illustrating a shell preparation method provided in another embodiment of this application;

[0024] Figure 12 for Figure 11 A schematic diagram of the process included in S140;

[0025] Figure 13 (a)~ Figure 13 (f) is Figure 11 Corresponding structural diagram;

[0026] Figure 14 A schematic diagram of a housing provided according to one embodiment of this application;

[0027] Figure 15 for Figure 14Schematic diagram of the cross section along Line II;

[0028] Figure 16 A schematic diagram of a housing provided for another embodiment of this application;

[0029] Figure 17 for Figure 16 Schematic diagram of the cross section along line II-II;

[0030] Figure 18 A schematic diagram of a housing provided for another embodiment of this application;

[0031] Figure 19 A perspective view of an electronic device provided according to an embodiment of this application;

[0032] Figure 20 for Figure 19 An exploded view of the electronic device shown. Detailed Implementation

[0033] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of this application.

[0034] In this document, references to "embodiment" or "implementation" mean that a particular feature, structure, or characteristic described in connection with an embodiment or implementation may be included in at least one embodiment of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.

[0035] It should be noted that the terms "first," "second," etc., in the specification, claims, and accompanying drawings of this application are used to distinguish different objects, not to describe a specific order. Furthermore, the terms "comprising" and "having," and any variations thereof, are intended to cover non-exclusive inclusion.

[0036] This application provides a method for preparing a shell, the method being used to prepare a shell 10 (see...). Figure 14 The housing 10 can be applied to electronic device 1 (see...). Figure 19 and Figure 20The electronic device 1 can be, but is not limited to, a mobile phone, tablet computer, laptop computer, desktop computer, smart bracelet, smartwatch, e-reader, game console, or any other device with a housing 10. When the housing 10 is applied to the electronic device 1, it can be, but is not limited to, a back cover, mid-frame, or decorative component. The housing 10 can be a 2D housing, a 2.5D housing, or a 3D housing. It is understood that the above description is an introduction to one application environment of the housing 10 and should not be construed as limiting the housing 10 and housing manufacturing method provided in the embodiments of this application. In the embodiments / examples of this application, the housing is described in detail as the back cover of the electronic device, and should not be construed as limiting the housing and housing manufacturing method provided in this application.

[0037] Please see Figure 1 Figure 2 and Figure 3 , Figure 1 A flowchart illustrating a shell preparation method provided in one embodiment of this application; Figure 2 for Figure 1 A schematic diagram of the process included in S120; Figure 3 (a)~ Figure 3 (f) is Figure 1 and Figure 2 The diagram shows the structural schematics corresponding to each step. The shell preparation method includes, but is not limited to, S110, S120, and S130, which are described in detail below.

[0038] S110 provides a ceramic housing body 210.

[0039] Please see Figure 3 (a), Figure 3 (a) is Figure 1 A schematic diagram of the ceramic shell body 210 in section S110. The preparation method of the ceramic shell body 210 will be described in detail later.

[0040] Optionally, the raw material components of the ceramic shell body 210 include ceramic powder. Optionally, the ceramic powder includes at least one of zirconium oxide, alumina, silicon dioxide, titanium dioxide, silicon nitride, magnesium oxide, chromium oxide, beryllium oxide, vanadium pentoxide, boron trioxide, spinel, zinc oxide, calcium oxide, mullite, and barium titanate. In a specific embodiment, the ceramic powder is zirconium oxide powder, and the ceramic shell body 210 is a zirconium oxide ceramic shell body.

[0041] In some embodiments, the raw material components of the ceramic shell body 210 further include a binder. Optionally, the binder is at least one of epoxy binders and polyether binders. It should be noted that the decomposition or volatilization temperature of the binder is lower than the temperature during binder removal, so that the binder can be completely removed through decomposition or volatilization during binder removal, avoiding binder residue. Therefore, it can prevent residual binder from causing pores in the ceramic shell body 210 during sintering, thereby avoiding a reduction in the mechanical strength of the formed ceramic shell body 210 and avoiding affecting the appearance of the ceramic shell body 210. Optionally, the weight percentage of the binder in the raw material components of the ceramic shell body 210 ranges from 3% to 5%. Specifically, the weight percentage of the binder can be, but is not limited to, 3%, 3.5%, 4%, 4.5%, 5%, etc.

[0042] In this application embodiment, when referring to the numerical range A to B, unless otherwise specified, it means that the endpoint value A is included and the endpoint value B is included. For example, the weight percentage of the adhesive is 3% to 5%, which means that the weight percentage a of the adhesive satisfies: 3% ≤ a ≤ 5%.

[0043] In some embodiments, the raw material components of the ceramic shell body 210 further include a dispersant. The dispersant allows for more uniform mixing of the binder and ceramic powder, resulting in a more stable mixture of the binder and ceramic powder. The dispersant can be, but is not limited to, liquid paraffin. The weight percentage of the dispersant in the raw material components of the ceramic shell body 210 ranges from 1% to 5%, specifically, it can be, but is not limited to, 1%, 2%, 3%, 4%, 5%, etc.

[0044] In some embodiments, the ceramic powder in the raw material components of the ceramic shell body 210 has color, causing the ceramic body to exhibit color, such as white, beige, or gray.

[0045] In some embodiments, the raw material components of the ceramic shell body 210 further include colorants, which are used to give the ceramic shell body 210 a colored pattern or color, thereby giving the shell 10 a colored pattern or color. By controlling the color and proportion of the colorants, the ceramic shell body 210 can exhibit different appearance effects, thereby giving the shell 10 different appearance effects. Optionally, in the raw material components of the ceramic shell body 210, the weight percentage of the colorant ranges from 0.5% to 5%, specifically, it can be, but is not limited to, 0.5%, 1%, 2%, 3%, 4%, 5%, etc.

[0046] Optionally, the ceramic housing body 210 has at least one color. Further, the ceramic housing body 210 has at least two colors. In this embodiment, the ceramic housing body 210 is illustrated as a light color (e.g., white, beige, or light gray).

[0047] S120, a first glaze layer 230 is formed in at least a portion of the surface of the ceramic housing body 210, the first glaze layer 230 being formed from a first glaze slurry 220.

[0048] The first glaze layer 230 is formed by the first glaze slurry 220, and can be formed by, but is not limited to, drying, air drying, evaporating, or vacuuming the first glaze slurry 220.

[0049] Specifically, please refer to the following: Figure 2 , Figure 2 In one implementation method Figure 1 The flowchart of S120 is shown below. S120 includes S120a and S120b, which are described in detail below.

[0050] S120a, a first glaze slurry 220 is applied to at least a portion of the surface of the ceramic housing body 210. Specifically, this includes applying the first glaze slurry 220 to a portion of the surface of the ceramic housing body 210, or applying the first glaze slurry 220 to the entire surface of the ceramic housing body 210. For example, the first glaze slurry 220 is applied to a portion of one surface of the ceramic body, or to the entire surface of one surface of the ceramic housing body 210. Please refer to [link to previous section]. Figure 3 (b), Figure 3 (b) A schematic diagram showing the structure of the ceramic shell body S120a with the first glaze slurry applied to its surface. In this embodiment, the schematic diagram illustrates an example of applying the first glaze slurry 220 to the entire area of ​​one surface of the ceramic shell body 210. It should be understood that this should not be construed as limiting the shell preparation method provided in this application.

[0051] In one embodiment, the first glaze slurry 220 comprises a glaze solution and a thickener. The mass ratio of the glaze solution to the thickener ranges from 1:1 to 3:1; the glaze solution comprises a metal cation salt and a solvent, wherein the weight percentage of the metal cation salt to the solvent is 50% to 75%.

[0052] The thickener can be, but is not limited to, epoxy resin or phenolic resin. The thickener is used to give the first glaze slurry 220 a certain viscosity, facilitating the application of the first glaze slurry to the surface of the ceramic shell body.

[0053] The first glaze slurry 220 will now be described in detail. In the first glaze slurry 220, the mass ratio of the glaze solution to the thickener ranges from 1:1 to 3:1, and can be, but is not limited to, 1:1, 1.5:1, 2:1, 2.5:1, or 3:1. When the mass percentage of the glaze solution to the thickener is less than 1:1, the proportion of the thickener is too high, resulting in a high viscosity of the first glaze slurry, which is not conducive to spraying. When the mass percentage of the glaze solution to the thickener is greater than 3:1, the proportion of the thickener is too low, resulting in insufficient viscosity of the first glaze slurry. When the first glaze slurry is applied to the surface of the ceramic shell body 210, it flows more easily, leading to poor first pattern in the final shell. Therefore, in this embodiment, the mass ratio of the glaze solution to the thickener is in the range of 1:1 to 3:1, which can avoid the first pattern being poor due to the flow of the first glaze slurry on the surface of the ceramic shell body 210 caused by the viscosity of the first glaze slurry being too low, and can also improve the convenience of spraying the first glaze slurry.

[0054] In the first glaze slurry 220, the metal cation salt in the glaze solution includes, but is not limited to, one or more of iron ion salts, cobalt ion salts, and nickel ion salts. For example, the metal cation salt includes one or more of Fe2(C2O4)3, CoC2O4, NiC2O4, NiCO3, and Co(NH3)4Cl. It should be noted that "one or more" means two or more types. The cobalt ion salt may include, but is not limited to, divalent or trivalent cobalt ion salts.

[0055] The solvent may be, but is not limited to, ethyl acetate, ethylene glycol, butanol, or toluene, as long as the solvent can dissolve the metal cation salt.

[0056] The weight percentage of the metal cation salt to the solvent is 50% to 75%, and can be, but is not limited to, 50%, 55%, 60%, 65%, 70%, or 75%. When the weight percentage of the metal cation salt to the solvent is less than 50%, the proportion of the metal cation salt is small, which will result in a lighter color (i.e., lower grayscale) or even an indistinct color in the final prepared first pattern. When the weight percentage of the metal cation salt to the solvent is greater than 75%, there is too much metal cation salt, and the solvent may not be able to completely dissolve the metal cation salt. Therefore, in this embodiment, the weight percentage of the metal cation salt to the solvent is 50% to 75%, which balances the grayscale of the final prepared first pattern with the solvent's ability to dissolve the metal cation salt.

[0057] The first glaze slurry 220 can be applied to at least a portion of the surface of the ceramic housing body 210 by means of, but not limited to, spraying, coating, printing, brushing, etc.

[0058] The thickness of the first glaze slurry 220 is related to the weight percentage of the metal salt to the solvent in the glaze solution, and the mass ratio of the glaze solution to the thickener in the first glaze slurry 220. When the weight percentage of the metal cation salt to the solvent in the glaze solution is 50% to 75%, and the mass ratio of the glaze solution to the thickener in the first glaze slurry 220 is in the range of 1:1 to 3:1, the thickness of the first glaze slurry 220 is less than or equal to 20 μm. For example, the thickness of the first glaze slurry 220 can be, but is not limited to, 2 μm, 5 μm, 7 μm, 10 μm, 12 μm, 15 μm, 17 μm, or 20 μm.

[0059] When the thickness of the first glaze slurry 220 and the weight percentage of the metal salt to the solvent in the glaze solution, as well as the mass ratio of the glaze solution to the thickener in the first glaze slurry 220 are constant, the thickness of the first glaze slurry 220 is related to the maximum gray value of the first pattern 130 in the finally prepared shell 10.

[0060] When the thickness of the first glaze slurry 220, the weight percentage of the metal salt to the solvent in the glaze solution, and the mass ratio of the glaze solution to the thickener in the first glaze slurry 220 are constant: when the thickness of the first glaze slurry 220 is less than the threshold thickness, and the thicker the first glaze slurry 220 is, the larger the maximum gray value of the first pattern 130 of the shell 10 is finally prepared; correspondingly, when the thickness of the first glaze slurry 220 is less than the threshold thickness, and the thinner the first glaze slurry 220 is, the smaller the maximum gray value of the first pattern 130 of the shell 10 is finally prepared.

[0061] Understandably, when the thickness of the first glaze slurry 220, the weight percentage of the metal salt to the solvent in the glaze solution, and the mass ratio of the glaze solution to the thickener in the first glaze slurry 220 are constant: when the thickness of the first glaze slurry 220 is greater than or equal to the threshold thickness, the maximum grayscale variation of the first pattern 130 of the finally prepared shell 10 changes little with the change in the thickness of the first glaze slurry 220, or even stops changing. For example, in this embodiment, the threshold thickness can be, but is not limited to, 20 μm, 25 μm, or 30 μm.

[0062] When the thickness of the first glaze slurry 220 is greater than or equal to the threshold thickness, the time required to engrave the first glaze layer 230 obtained by laser on the first glaze slurry 220 is longer. Therefore, the time required to prepare the shell 10 is longer and the preparation efficiency is reduced.

[0063] In this embodiment, when the weight percentage of the metal cation salt to the solvent in the glaze solution is 50% to 75%, and the mass ratio of the glaze solution to the thickener in the first glaze slurry 220 is in the range of 1:1 to 3:1, the thickness of the first glaze slurry 220 is less than or equal to 20 μm. On the one hand, this satisfies the grayscale requirement of the first preset pattern of the final prepared shell 10, and on the other hand, it takes into account the time required for subsequent laser engraving of the first glaze layer 230 obtained from the first glaze slurry 220, resulting in a better effect in preparing the shell 10.

[0064] S120b, the ceramic shell body 210 on which the first glaze slurry 220 is disposed is dried to form a first glaze layer 230 on the ceramic shell body 210.

[0065] Please see Figure 3 (c), Figure 3(c) is a schematic diagram of the structure after S120b. The ceramic shell body 210 disposed in the first glaze slurry 220 is dried, the solvent in the glaze solution in the first glaze slurry 220 evaporates, and the remaining metal cation salt and the thickener form the first glaze layer 230.

[0066] The time and temperature required to dry the ceramic shell body 210 on which the first glaze slurry 220 is applied are related to the thickness of the first glaze slurry 220. Specifically, in one embodiment, the thickness of the first glaze slurry 220 is less than or equal to 20 μm. Drying the ceramic shell body 210 on which the first glaze slurry 220 is applied to form a first glaze layer 230 on the ceramic shell body 210 includes baking at 80°C to 150°C for 20 to 50 minutes to form the first glaze layer 230 on the ceramic shell body 210.

[0067] The baking temperature is 80°C to 150°C, which includes, but is not limited to, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, or 150°C.

[0068] The baking time is 20 to 50 minutes, which includes, but is not limited to, 20 minutes, 25 minutes, 30 minutes, 35 minutes, 40 minutes, 45 minutes, or 50 minutes.

[0069] Drying the ceramic shell body 210, which is coated with the first glaze slurry 220, is to allow the solvent in the first glaze slurry 220 to evaporate, thereby fixing the metal cation salt onto the surface of the ceramic shell body 210, facilitating subsequent laser engraving. For the same first glaze slurry 220, a higher baking temperature results in a shorter baking time; conversely, a lower baking temperature results in a longer baking time.

[0070] In other words, S120b specifically includes: baking at 80°C to 150°C for 20 to 50 minutes to form the first glaze layer 230 on the ceramic shell body 210.

[0071] S130, the first glaze layer 230 is patterned to form a first patterned layer 240 to obtain a shell 10 having the first pattern 130.

[0072] Patterning the first glaze layer 230 to form a first patterned layer 240 can be done, but is not limited to, laser engraving, texture imprinting, masking, and etching.

[0073] Please see Figure 3 (d), Figure 3 (d) is a schematic diagram of the formation of the first patterned layer 240. Figure 3 (e) is a schematic diagram of the shell structure obtained after S130; Figure 3 (f) is Figure 3 (e) Cross-sectional view along AA. In this embodiment, the first pattern 130 is used as a texture pattern for illustration. It should be understood that this should not be construed as a limitation on the shell preparation method provided in this application. Next, the specific process of S130 in one embodiment will be described in detail.

[0074] Please refer to the following: Figure 4 , Figure 4 for Figure 1 The flowchart included in S130 is shown below. In this embodiment, S130 includes S131, S132 and S133, which are described in detail below.

[0075] S131 outputs the preset pattern to the laser engraving device.

[0076] The style of the preset pattern determines the style of the first pattern 130 of the final manufactured shell 10. In this embodiment, the style of the preset pattern and the style of the first pattern 130 of the final manufactured shell 10 are the same, and have the same grayscale. In other embodiments, the style of the preset pattern and the style of the first pattern 130 of the final manufactured shell 10 are similar, for example, the style of the preset pattern and the style of the first pattern 130 of the final manufactured shell 10 are proportional (e.g., magnified by a preset factor, or reduced by a preset factor). In other embodiments, the grayscale of the preset pattern is similar to the grayscale of the first pattern 130 of the final manufactured shell 10.

[0077] For example, the preset pattern includes a textured pattern or a gradient pattern. Therefore, the first pattern 130 of the prepared housing 10 includes a textured pattern or a gradient pattern. In other words, the effect of the first pattern 130 includes a textured effect or a gradient effect.

[0078] When the preset pattern includes a textured pattern, the preset pattern may include multiple textures arranged according to a preset rule, such as multiple lines arranged according to a preset rule (e.g., straight line segments, curved ends, or hyperbolic segments), or multiple shapes arranged according to a preset rule (e.g., triangles, quadrilaterals, circles, or annexes). When the preset pattern includes a gradient pattern, it may include an ink wash gradient pattern, or a marble gradient pattern, etc.

[0079] To balance the manufacturing efficiency of the housing 10 and the precision of the first pattern 130, the laser engraving equipment can be, but is not limited to, an infrared laser engraving equipment or an ultraviolet laser engraving equipment. Accordingly, the laser output by the laser engraving equipment is an infrared laser or an ultraviolet laser.

[0080] The precision of the laser engraving equipment determines the precision of the final pattern 130. When the laser engraving equipment is an infrared laser engraving equipment, the laser output by the equipment is an infrared laser. For example, the spot diameter of the infrared laser is 0.08 mm, or approximately 0.08 mm. When the laser engraving equipment is an ultraviolet laser engraving equipment, the laser output by the equipment is an ultraviolet laser. For example, the spot diameter of the ultraviolet laser is 0.03 mm, or approximately 0.03 mm. Therefore, the spot diameter of the ultraviolet laser is smaller than that of the infrared laser. That is, the precision of the ultraviolet engraving equipment is higher than that of the infrared engraving equipment. Understandably, although the precision of the ultraviolet engraving equipment is higher than that of the infrared engraving equipment, both the ultraviolet engraving equipment and the infrared engraving equipment can meet the precision requirements for manufacturing the housing 10.

[0081] Furthermore, the shell fabrication method provided in this application can also adjust the laser spot according to the desired fineness of each part of the first pattern 130. For example, the fineness of a portion P and another portion P' in the first pattern 130 to be fabricated is different. The fineness of portion P is a first fineness, and the fineness of the other portion P' is a second fineness; if the first fineness is greater than the second fineness, then the size of the laser spot used to carve portion P is smaller than the size of the laser spot used to carve the other portion P'.

[0082] S132, control the power of the laser output by the laser engraving device according to the preset pattern. Different gray levels in the preset pattern correspond to different laser powers, wherein the larger the gray level, the smaller the laser power.

[0083] The smaller the grayscale value in the preset pattern, the greater the power of the corresponding laser; correspondingly, the larger the grayscale value in the preset pattern, the smaller the power of the corresponding laser.

[0084] Specifically, the smaller the grayscale value of a region in the preset pattern, the higher the power of the corresponding laser. Therefore, when the laser engraves the corresponding portion of the first glaze layer 230, more of it is removed, leaving less remaining material. Less remaining material means fewer cations, resulting in a smaller grayscale value for the corresponding region in the first pattern 130 of the prepared shell 10. Conversely, the larger the grayscale value of a region in the preset pattern, the lower the power of the corresponding laser. Therefore, when the laser engraves the corresponding portion of the first glaze layer 230, less of it is removed, leaving more remaining material. More remaining material means more cations, resulting in a larger grayscale value for the corresponding region in the first pattern 130 of the prepared shell 10.

[0085] Therefore, by irradiating each part of the first glaze layer 230 with the laser, and selecting the corresponding laser power according to the different gray levels of the preset pattern, a first patterned layer 240 corresponding to the gray level of the preset pattern is formed. The thicker parts of the first patterned layer 240 correspond to the gray level of the preset pattern, and the thinner parts of the first patterned layer 240 correspond to the gray level of the preset pattern.

[0086] In one embodiment, when the laser irradiates various portions of the first glaze layer 230, the portion of the first glaze layer 230 corresponding to the part with the highest grayscale in the preset pattern may or may not be irradiated. Whether irradiation is required depends on the thickness of the first glaze layer 230 and the amount of metal cations in it. Similarly, the portion of the first glaze layer 230 corresponding to the part with the lowest grayscale in the preset pattern may or may not be irradiated. Again, whether irradiation is required depends on the thickness of the first glaze layer 230 and the amount of metal cations in it. As long as the grayscale of the first pattern 130 in the final manufactured shell 10 matches the grayscale of the preset pattern, the desired outcome is achieved.

[0087] In this embodiment, when the first glaze layer 230 is irradiated with a laser, the laser power output by the laser engraving device corresponding to the part with the highest gray level in the preset pattern is 0%; the laser power output by the laser engraving device corresponding to the part with the lowest gray level in the preset pattern is 100%.

[0088] S133, the first glaze layer 230 is irradiated with the laser to remove part of the glaze in the first glaze layer 230 to form the first patterned layer 240.

[0089] In one embodiment, when the laser is used to irradiate the first glaze layer 230, the irradiation can be carried out along a preset path. For example, if the first glaze layer 230 includes one end and the other end facing away from each other, then the preset path can be from one end of the first glaze layer 230 to the other end of the first glaze layer 230.

[0090] In another embodiment, the laser is used to irradiate the first glaze layer 230. Irradiation can be performed according to the different gray levels of the preset pattern. For example, the first glaze layer 230 can be irradiated first based on the area with the highest gray level in the preset pattern, and then the corresponding areas in the first glaze layer 230 can be irradiated gradually according to the decrease in gray level in the preset pattern. Understandably, in other embodiments, the first glaze layer 230 can also be irradiated first based on the area with the lowest gray level in the preset pattern, and then the corresponding areas in the first glaze layer 230 can be irradiated gradually according to the increase in gray level in the preset pattern.

[0091] In one embodiment, obtaining the shell 10 having the first pattern 130 in S130 includes: sintering a ceramic shell body 210 having a first patterned layer 240 to obtain the shell 10 having the first pattern 130.

[0092] The ceramic shell body 210 with the first patterned layer 240 is sintered. During the sintering process, the viscous agent in the first patterned layer 240 volatilizes, and the metal cations in the first patterned layer 240 permeate into the interior of the ceramic shell body 210 through the surface. Under constant sintering temperature and time, the thicker the portion of the first patterned layer 240 in the ceramic shell body 210, the more metal cations permeate into the interior of the ceramic shell body 210, resulting in a higher grayscale value for the corresponding portion of the final shell 10. Conversely, the thinner the portion of the first patterned layer 240 in the ceramic shell body 210, the fewer metal cations permeate into the interior of the ceramic shell body 210, resulting in a lower grayscale value for the corresponding portion of the final shell 10. Therefore, when the first patterned layer 240 changes according to the thickness gradient, after sintering the ceramic shell body 210 and the first patterned layer 240, metal cations penetrate into the ceramic shell body 210 and develop color, thereby forming an effect of having a certain color (such as the first pattern 130 having a first color) changing according to the grayscale gradient.

[0093] In one embodiment, a ceramic shell body 210 having a first patterned layer 240 is sintered to obtain a shell 10 with a first pattern 130 having a thickness of 0.2 mm to 1.0 mm. For example, the thickness of the shell 10 may be 0.2 mm, 0.25 mm, 0.3 mm, 0.35 mm, 0.4 mm, 0.45 mm, 0.5 mm, 0.55 mm, 0.6 mm, 0.65 mm, 0.7 mm, 0.75 mm, 0.8 mm, 0.85 mm, 0.9 mm, 0.95 mm, or 1.0 mm. Correspondingly, the thickness of the portion of the shell 10 infiltrated by the metal cation is 1 μm to 300 μm. For example, the thickness of the portion of the shell 10 infiltrated by the metal cation is 1 μm, or 1.5 μm, or 2 μm, or 5 μm, or 10 μm, or 15 μm, or 20 μm, or 30 μm, or 40 μm, or 50 μm, or 60 μm, or 70 μm, or 80 μm, or 90 μm, or 100 μm, or 110 μm, or 120 μm. μm, or 130μm, or 140μm, or 150μm, or 160μm, or 170μm, or 180μm, or 190μm, or 200μm, or 210μm, or 220μm, or 230μm, or 240μm, or 250μm, or 260μm, or 270μm, or 280μm, or 290μm, or 300μm.

[0094] In one embodiment, a ceramic shell body 210 having a first patterned layer 240 is sintered to obtain a shell 10 with a first pattern 130 having a thickness of 0.4 mm to 0.5 mm. For example, the thickness of the shell 10 is 0.4 mm, 0.42 mm, 0.45 mm, 0.48 mm, or 0.5 mm. Correspondingly, the thickness of the portion of the shell 10 infiltrated by the metal cation is 1 μm to 200 μm. For example, the thickness of the portion of the shell 10 infiltrated by the metal cation is 1 μm, or 1.5 μm, or 2 μm, or 5 μm, or 10 μm, or 15 μm, or 20 μm, or 30 μm, or 40 μm, or 50 μm, or 60 μm, or 70 μm, or 80 μm, or 90 μm, or 100 μm, or 110 μm, or 120 μm, or 130 μm, or 140 μm, or 150 μm, or 160 μm, or 170 μm, or 180 μm, or 190 μm, or 200 μm. The thickness of the portion of the shell 10 infiltrated by the metal cation with the lowest gray level is 1 μm to 2 μm, and the thickness of the portion of the shell 10 infiltrated by the metal cation with the highest gray level is 100 μm to 200 μm. For example, the thickness of the portion of the shell 10 in which the metal cations have diffused and where the grayness is minimal is 1 μm, or 1.2 μm, or 1.5 μm, or 1.8 μm, or 2 μm; correspondingly, the thickness of the portion of the shell 10 in which the metal cations have diffused and where the grayness is maximum is 100 μm, or 105 μm, or 110 μm, or 115 μm, or 120 μm, or 125 μm, or 130 μm, or 135 μm, or 140 μm, or 145 μm, or 150 μm, or 155 μm, or 160 μm, or 165 μm, or 170 μm, or 175 μm, or 180 μm, or 185 μm, or 190 μm, or 195 μm, or 200 μm.

[0095] Please refer to the following: Figure 5 , Figure 5 for Figure 1 The flowchart included in S130 is shown below. S130 specifically includes: S130a, which is described in detail below.

[0096] S130a, a ceramic blank having a first patterned layer 240 is sintered at 950°C to 1200°C for a time ranging from 2h to 3h to obtain a shell 10 having the first pattern 130.

[0097] When the temperature is below 950℃, the sintering temperature is too low, and the metal cations in the first patterned layer 240 cannot penetrate well or even penetrate into the shell formed by the ceramic blank. Furthermore, when the temperature is below 950℃, the ceramic blank cannot be properly vitrified, affecting the structural strength of the final shell 10. When the temperature is above 1200℃, the crystals formed during sintering of the ceramic blank will grow excessively large, further affecting the strength of the final shell 10. Therefore, in this embodiment, the sintering temperature selected for sintering the ceramic blank with the first patterned layer 240 is between 950℃ and 1200℃, which allows the metal cations in the first patterned layer 240 to penetrate well into the shell 10 formed by the ceramic blank, and gives the shell 10 good structural strength.

[0098] When sintering the ceramic blank with the first patterned layer 240, the selected temperature is 950°C to 1200°C. For example, the temperature can be, but is not limited to, 950°C, 1000°C, 1050°C, 1100°C, 1150°C, or 1200°C.

[0099] The sintering time ranges from 2 hours to 3 hours. For example, the sintering time ranges from 2 hours, or 2 hours and 10 minutes, or 2 hours and 20 minutes, or 2 hours and 30 minutes, or 2 hours and 40 minutes, or 2 hours and 50 minutes, or 3 hours.

[0100] Understandably, given a fixed thickness of the first glaze layer 230, a fixed thickness of the ceramic blank, and a fixed mass of the final shell 10 and parameters of the first pattern 130: the higher the sintering temperature, the shorter the required sintering time; correspondingly, the lower the sintering temperature, the longer the required sintering time.

[0101] In this embodiment of the application, the sintering temperature of the ceramic blank with the first patterned layer 240 is 950°C to 1200°C and the sintering time is 2h to 3h. On the one hand, this can ensure the quality of the shell 10 and the first pattern 130 obtained by sintering, and on the other hand, it can shorten the sintering time and improve the efficiency of the preparation of the shell 10.

[0102] The shell preparation method provided in this application can prepare a shell 10 with a first pattern 130. Therefore, the shell 10 prepared by the shell preparation method provided in this application has a better appearance.

[0103] The steps included in S110 are described in detail below. Please refer to [link / reference needed]. Figure 6 , Figure 6 for Figure 1A schematic diagram of the process included in S110 is shown. S110 includes S111, S112, and S113. S111, S112, and S113 are described in detail below.

[0104] S111, ceramic granules are shaped to obtain a shell green body.

[0105] Specifically, please refer to the following: Figure 7 , Figure 7 for Figure 6 The flowchart included in S111 is shown below. In one embodiment, S111 includes S1111 and S1112, which are described in detail below.

[0106] S1111, ceramic powder is mixed with a binder and granulated to obtain ceramic granules, wherein the particle size of the ceramic powder ranges from 0.2 μm to 0.8 μm, the mesh size of the ceramic granules ranges from 40 mesh to 100 mesh, and the BET specific surface area of ​​the granules is 6 m². 2 / g to 10m 2 / g, wherein the binder is at least one of epoxy binder and polyether binder, and the weight percentage of the binder in the ceramic granules ranges from 3% to 5%.

[0107] Specifically, ceramic powder and binder are weighed according to a preset weight ratio, the ceramic powder and binder are mixed evenly, and granulation is carried out using granulation equipment to obtain granules.

[0108] Optionally, the average particle size d of the ceramic powder ranges from 0.2 μm ≤ d ≤ 0.8 μm. Specifically, the average particle size of the ceramic powder can be, but is not limited to, 0.2 μm, 0.3 μm, 0.4 μm, 0.5 μm, 0.6 μm, 0.7 μm, and 0.8 μm. If the particle size of the ceramic powder is too small, the preparation difficulty increases, thus increasing the cost. When the particle size of the ceramic powder is as small as the nanometer level, the ceramic powder is prone to agglomeration, forming large particles, which reduces the mechanical strength of the obtained ceramic green body, and consequently reduces the mechanical strength of the finally prepared shell 10. Similarly, if the particle size of the ceramic powder is too large, for example, greater than 0.8 μm, it also reduces the mechanical strength of the obtained ceramic green body, and consequently reduces the mechanical strength of the finally prepared shell 10. Therefore, when the particle size of the ceramic powder ranges from 0.2 μm to 0.8 μm, the obtained ceramic green body can have good mechanical strength, thus resulting in good mechanical strength of the finally prepared shell 10, while also having a lower preparation cost. "Average particle size" refers to the average particle size of all particles in ceramic powder.

[0109] Please refer to the previous description of the ceramic powder and the binder, which will not be repeated here.

[0110] When the raw material components of the ceramic shell body 210 also include dispersants, colorants, etc., the preparation method further includes mixing the dispersants, colorants, etc. with ceramic powder and binder before granulation. Please refer to the previous description for the dispersants and colorants; they will not be repeated here.

[0111] Optionally, the mesh size of the ceramic granules ranges from 40 mesh to 100 mesh. Specifically, the mesh size of the ceramic granules can be, but is not limited to, 40 mesh, 50 mesh, 60 mesh, 70 mesh, 80 mesh, 90 mesh, 100 mesh, etc. In other words, the particle size of the ceramic granules ranges from 150 μm to 380 μm; specifically, the particle size of the ceramic granules can be, but is not limited to, 150 μm, 180 μm, 200 μm, 220 μm, 250 μm, 280 μm, 300 μm, 330 μm, 350 μm, 380 μm, etc. If the particle size of the ceramic granules is too small, the preparation difficulty increases, thus increasing the cost. When the particle size is as small as the nanometer level, the ceramic granules are prone to agglomeration, forming large particles, which reduces the mechanical strength of the resulting shell 10. If the particle size is too large, for example, greater than 0.8 μm, gaps and air bubbles are easily left during green body forming, which also reduces the mechanical strength of the resulting shell 10. Therefore, when the particle size of the ceramic granules is in the range of 0.2 μm to 0.8 μm, the resulting shell 10 can have good mechanical strength while maintaining a low preparation cost.

[0112] Optionally, the BET specific surface area of ​​the ceramic granules is 6m². 2 / g to 10m 2 / g. Specifically, the BET specific surface area of ​​the ceramic particles can be, but is not limited to, 6m². 2 / g, 6.5m 2 / g、7m 2 / g, 7.5m 2 / g、8m 2 / g, 8.5m 2 / g、9m 2 / g, 9.5m 2 / g, 10m 2 / g etc. The larger the specific surface area, the smaller the ceramic particles, and the easier it is for the ceramic particles to agglomerate and form large particles, which will reduce the mechanical strength of the shell 10. The smaller the specific surface area, the larger the ceramic particles, and during green body forming, gaps and air bubbles are more likely to remain, which will also reduce the mechanical strength of the shell 10.

[0113] It should be noted that the decomposition or volatilization temperature of the binder is lower than the temperature during binder removal, so that the binder can be completely removed through decomposition or volatilization during binder removal, avoiding binder residue. Therefore, it avoids the formation of residual pores in the ceramic shell body 210 during sintering, thereby preventing a reduction in the mechanical strength of the formed ceramic shell body 210 and avoiding affecting its appearance. Optionally, the weight percentage of the binder in the raw material composition of the ceramic shell body 210 ranges from 3% to 5%. Specifically, the weight percentage of the binder can be, but is not limited to, 3%, 3.5%, 4%, 4.5%, 5%, etc.

[0114] Optionally, the binder in the ceramic granules comprises a weight percentage ranging from 3% to 5%. For a detailed description of the ceramic powder and binder, please refer to the description in the corresponding section of the above embodiments.

[0115] S1112, The ceramic particles are shaped to obtain a shell green body.

[0116] In S1112, the molding process includes compression molding or injection molding; when the molding process is compression molding, S1112 specifically includes S1112', which is described in detail below. Please refer to [link to relevant documentation]. Figure 8 , Figure 8 for Figure 7 A schematic diagram of the process included in S1112.

[0117] S1112', the molding pressure ranges from 10MPa to 15MPa, and the pressure is held for 10s to 20s to form the ceramic particles to obtain a shell green body.

[0118] Optionally, the compression molding pressure can range from 10 MPa, 11 MPa, 12 MPa, 13 MPa, 14 MPa, or 15 MPa. If the compression molding pressure is too low, it affects the density of the resulting shell preform, and may even prevent it from forming a shell preform with a complete shape. Higher compression molding pressure results in a denser shell preform, which is beneficial for improving the mechanical properties of the produced shell preform. However, excessive compression molding pressure increases the requirements for the equipment.

[0119] Optionally, the holding time can be 10 seconds, 12 seconds, 14 seconds, 16 seconds, 18 seconds, or 20 seconds, etc. The longer the holding time, the better the density and forming condition of the resulting shell blank. However, if the holding time is too long, it will affect the production efficiency.

[0120] In one embodiment, the molding temperature is room temperature. It should be noted that, in the embodiments of this application, room temperature refers to 25°C, or approximately equal to 25°C.

[0121] In other embodiments, the granules can be placed in an injection molding machine to produce a shell preform by injection molding.

[0122] S112, the shell blank is debonded and sintered to obtain the shell blank.

[0123] Please refer to the following: Figure 9 , Figure 9 for Figure 6 The flowchart included in S112 is shown below. S112 includes, but is not limited to, S1121, S1122, and S1123. S1121, S1122, and S1123 are described in detail below.

[0124] S1121, the shell blank is gradually heated to 800°C to 950°C to remove the adhesive, and the adhesive removal time is from 2h to 3h, so that the adhesive in the shell blank is removed.

[0125] The binder in the shell blank can be discharged through volatilization or decomposition.

[0126] When the raw material components of the shell 10 also include a dispersant, the dispersant will also decompose or volatilize during the dispensing process and thus be eliminated.

[0127] In one embodiment, the pressure during glue removal is atmospheric pressure. It should be noted that the atmospheric pressure referred to in the embodiments of this application generally refers to standard atmospheric pressure.

[0128] S1122, gradually heat to 1350℃ to 1500℃ for sintering, the sintering time being 8h to 10h.

[0129] S1123, cool down to room temperature to obtain the shell blank.

[0130] It should be noted that the glue removal time and sintering time do not include the time required for heating and cooling.

[0131] Optionally, the adhesive removal temperature is between 800℃ and 950℃, specifically, but not limited to, 800℃, 820℃, 840℃, 860℃, 880℃, 900℃, 920℃, 940℃, and 950℃. If the adhesive removal temperature is too low, the adhesive removal time will be too long, affecting production efficiency, or even failing to remove it completely. This can easily leave pores on the shell blank during sintering, affecting the mechanical strength of the resulting shell blank. If the adhesive removal temperature is too high, the adhesive decomposes or volatilizes too violently, easily leaving air bubbles in the shell blank, affecting the mechanical strength of the resulting shell blank. In addition, if the adhesive removal temperature is too high, the ceramic may crystallize prematurely, which will also reduce the mechanical strength of the shell blank.

[0132] Optionally, the glue removal time is 2 hours to 3 hours, specifically, it can be, but is not limited to, 120 minutes, 130 minutes, 140 minutes, 150 minutes, 160 minutes, 170 minutes, 180 minutes, etc. If the glue removal time is too short, the glue removal will be incomplete, which may result in residual air bubbles in the finished shell blank. A short glue removal time also affects production efficiency.

[0133] Optionally, the sintering temperature ranges from 1350℃ to 1500℃; specifically, it can be, but is not limited to, 1350℃, 1380℃, 1400℃, 1420℃, 1450℃, 1480℃, 1500℃, etc. If the sintering temperature is too low, the shell blank will not be ceramicized; if the sintering temperature is too high, it is easy to overheat, affecting the mechanical strength of the obtained shell blank.

[0134] Optionally, the sintering time can range from 8 hours to 10 hours; specifically, it can be, but is not limited to, 8 hours, 8.5 hours, 9 hours, 9.5 hours, 10 hours, etc. If the sintering time of the shell green body is too long, the ceramic grains may grow too large, which is not conducive to improving the mechanical strength of the shell green body. If the sintering time of the shell green body is too short, the density between the ceramic powders will be insufficient, which may result in incomplete ceramic formation and will also affect the mechanical strength of the obtained shell green body.

[0135] S113, The shell blank is processed and polished to obtain the ceramic shell body 210.

[0136] Please refer to the following: Figure 10 , Figure 10 for Figure 6 The flowchart included in S113 is shown below. S113 includes S1131 and S1132, which are described in detail below.

[0137] S1131, The shell blank is processed to obtain a shell blank of a preset size.

[0138] Specifically, processing the shell blank may include performing computerized numerical control (CNC) processing on the shell blank to obtain a shell blank of a preset size.

[0139] S1132, Grinding and polishing the shell blank of the preset size to obtain the ceramic shell body 210, wherein the surface gloss of the ceramic shell body 210 is 130Gu to 160Gu.

[0140] A pre-sized shell blank is ground and polished to obtain a high-gloss ceramic shell body 210. Optionally, the gloss level (60° angle test) of the ceramic shell body 210 surface is between 130 Gu and 160 Gu. Specifically, the gloss level of the ceramic shell body 210 can be, but is not limited to, 130 Gu, 135 Gu, 140 Gu, 145 Gu, 150 Gu, 155 Gu, 160 Gu, etc. When the gloss level of the ceramic shell body 210 surface is too low (e.g., below 110 Gu), the gloss of the surface of the ceramic shell body 210 is not obvious, affecting the texture of the shell 10; when the gloss level of the ceramic shell body 210 surface is too high (e.g., above 160 Gu), it increases the cost and process difficulty of preparing the surface of the ceramic shell body 210. When the gloss level of the ceramic shell body 210 surface is between 110 Gu and 160 Gu, the surface of the shell 10 has good gloss and is easy to produce.

[0141] Optionally, the Vickers hardness of the ceramic shell body 210 of this application can be, but is not limited to, 1200 HV to 1400 HV. Specifically, it can be, but is not limited to, 1200 HV, 1230 HV, 1250 HV, 1280 HV, 1300 HV, 1320 HV, 1350 HV, 1380 HV, 1400 HV, etc. The higher the Vickers hardness of the ceramic shell body 210, the higher the hardness of the resulting shell 10.

[0142] Therefore, the shell preparation method provided in this application grinds and polishes a shell blank of a preset size to obtain the ceramic shell body 210. It should be noted that the metal cations in the first patterned layer 240 penetrate into the ceramic shell body 210 as a colorant 120 to produce color. When the metal cations penetrate into the ceramic shell body 210, they do not reduce the high gloss effect of the ceramic shell body 210. Therefore, the surface of the shell 10 prepared subsequently has a high gloss, that is, the appearance of the prepared shell 10 has a high gloss state and high gloss effect.

[0143] Furthermore, since the metal cations in the first patterned layer 240 penetrate (infiltrate) into the ceramic shell body 210 as colorant 120, the infiltration of metal cations has a relatively small impact on the structural strength of the ceramic shell body 210. In other words, the hardness of the portion of the ceramic shell body 210 in which the metal cations have infiltrated is comparable to the hardness of the portion of the ceramic shell body 210 in which the metal cations have not infiltrated, thereby ensuring that the strength of each part of the finally prepared shell 10 is comparable.

[0144] As described above, the shell preparation method provided in this application, after completing the preparation of the ceramic shell body 210, then applies a first glaze slurry 220 to at least a portion of the surface of the ceramic shell body 210, and uses a laser to engrave the first glaze layer 230 formed by drying, so as to achieve the refinement and repeatability of the pattern in the engraved first patterned layer 240. When the ceramic shell body 210 with the first patterned layer 240 is sintered, the metal cations in the first patterned layer 240 penetrate (diffused) into the ceramic shell body 210 as coloring substances 120, thus developing color. When the sintering temperature and time of the ceramic shell body 210 are constant, the thicker the portion of the corresponding first patterned layer 240 in the ceramic shell body 210, the more metal cations penetrate into the interior of the ceramic shell body 210. Therefore, the grayscale of the corresponding part in the final prepared shell 10 is greater. Conversely, the thinner the portion of the corresponding first patterned layer 240 in the ceramic shell body 210, the fewer metal cations penetrate into the interior of the ceramic shell body 210. Therefore, the grayscale of the corresponding part in the final prepared shell 10 is smaller. Therefore, the shell preparation method provided in this application can control the thickness of each part of the first patterned layer 240, that is, control the content of metal cations penetrating into the ceramic shell body 210, thereby forming an effect with a certain color (such as the first pattern 130 having a first color) changing according to a grayscale gradient.

[0145] In summary, the shell preparation method provided in this application can simultaneously improve the color grayscale variation, fineness, hardness, and surface gloss of the first pattern 130 in the shell 10 when forming the first pattern 130, thereby producing a shell 10 with a better appearance.

[0146] Please refer to the following: Figure 11 , Figure 12 and Figure 13 , Figure 11 A flowchart illustrating a shell preparation method provided in another embodiment of this application; Figure 12 for Figure 11 A schematic diagram of the process included in S140; Figure 13 (a)~ Figure 13 (f) is Figure 11 The corresponding structural schematic diagram is shown below. In this embodiment, the shell preparation method includes steps S110, S120, S130, S140, and S150, as described above and will not be repeated here. Steps S140 and S150 are detailed below. It can be understood that in the flowchart of this embodiment, the shell preparation method includes steps S140 and S150 combined with... Figure 1The shell preparation method described in the above embodiments is illustrated by example. In other embodiments, the shell preparation method including S140 can also be combined with the shell preparation method provided in any of the preceding embodiments.

[0147] The first pattern 130 has a first color. S140 and S150 are described in detail below.

[0148] S140, a second glaze layer 270 is provided in at least a portion of the surface of the housing 10, the second glaze layer 270 being formed of a second glaze slurry 250.

[0149] The second glaze layer 270 is formed from the first glaze slurry 250, and can be formed by, but is not limited to, drying, air drying, evaporating, or vacuuming the second glaze slurry 250.

[0150] Specifically, please refer to the following: Figure 12 , Figure 12 In one implementation method Figure 11 The flowchart of S140 is shown below. S140 includes S140a and S140b, which are described in detail below.

[0151] S140a, a second glaze slurry 250 is applied to at least a portion of the surface of the housing 10.

[0152] Specifically, please refer to the following: Figure 13 (a) and Figure 13 (b), Figure 13 (a) is a schematic diagram of a shell with a first pattern; Figure 13 (b) is a schematic diagram of the structure after S140a. The second glaze slurry 250 will be described in detail below.

[0153] The second glaze slurry 250 can be applied to the entire surface of the housing 10, or to a portion of the surface of the housing 10. For example, the second glaze slurry 250 can be applied to the entire surface of the housing 10, or to a portion of the surface of the housing 10. When the second glaze slurry 250 is applied to a portion of the surface of the housing 10, the second glaze slurry 250 can be applied to the area corresponding to the first pattern 130, or to the area other than the first pattern 130; this is not limited in this embodiment. In the schematic diagram of this embodiment, the example of the second glaze slurry 250 being applied to the entire surface of the housing 10 is used for illustration.

[0154] The method of applying the second glaze slurry 250 to at least a portion of the surface of the housing 10 may be the same as or different from the method of applying the first glaze slurry 220 to at least a portion of the surface of the ceramic housing body 210, and is not limited in this embodiment.

[0155] The second glaze slurry 250 includes a glaze solution and a thickener. The mass ratio of the glaze solution to the thickener in the second glaze slurry 250 ranges from 1:1 to 3:1. The glaze solution contains a metal cation salt and a solvent, wherein the weight percentage of the metal cation salt to the solvent is 50% to 75%.

[0156] In the second glaze slurry 250, the mass ratio of the glaze solution to the thickener ranges from 1:1 to 3:1, and can be, but is not limited to, 1:1, 1.5:1, 2:1, 2.5:1, or 3:1.

[0157] In the second glaze slurry 250, the metal cation salt in the glaze solution includes, but is not limited to, one or more of iron ion salts, cobalt ion salts, and nickel ion salts. For example, the metal cation salt includes one or more of Fe2(C2O4)3, CoC2O4, NiC2O4, NiCO3, and Co(NH3)4Cl. It should be noted that "one or more" means two or more types.

[0158] In this embodiment, the metal cation salts in the glaze solution of the second glaze slurry 250 are different from the metal cation salts in the glaze solution of the first glaze slurry 220, which makes the first color of the final first pattern 130 different from the second color of the second pattern 140.

[0159] The solvent may be, but is not limited to, ethyl acetate, ethylene glycol, butanol, or toluene, as long as the solvent can dissolve the metal cation salt.

[0160] The weight percentage of the metal cation salt to the solvent is 50% to 75%, and may be, but is not limited to: 50%, 55%, 60%, 65%, 70%, or 75%.

[0161] The second glaze slurry 250 can be applied to at least a portion of the surface of the housing 10 by methods including, but not limited to, spraying, coating, printing, brushing, etc. The method of applying the second glaze slurry 250 to at least a portion of the surface of the housing 10 can be the same as, or different from, the method of applying the first glaze slurry 220 to at least a portion of the surface of the ceramic housing body 210.

[0162] The thickness of the second glaze slurry 250 is related to the weight percentage of the metal salt to the solvent in the glaze solution, and the mass ratio of the glaze solution to the thickener in the second glaze slurry 250. When the weight percentage of the metal cation salt to the solvent in the glaze solution is 50% to 75%, and the mass ratio of the glaze solution to the thickener in the second glaze slurry 250 is in the range of 1:1 to 3:1, the thickness of the second glaze slurry 250 is less than or equal to 20 μm. For example, the thickness of the second glaze slurry 250 can be, but is not limited to, 2 μm, 5 μm, 7 μm, 10 μm, 12 μm, 15 μm, 17 μm, or 20 μm.

[0163] When the thickness of the second glaze slurry 250 and the weight percentage of the metal salt to the solvent in the glaze solution, as well as the mass ratio of the glaze solution to the thickener in the second glaze slurry 250 are constant, the thickness of the second glaze slurry 250 is related to the maximum gray value of the second pattern 140 in the finally prepared shell 10.

[0164] When the thickness of the second glaze slurry 250, the weight percentage of the metal salt to the solvent in the glaze solution, and the mass ratio of the glaze solution to the thickener in the second glaze slurry 250 are constant: when the thickness of the second glaze slurry 250 is less than the threshold thickness, and the thicker the second glaze slurry 250 is, the larger the maximum gray value of the second pattern 140 of the final prepared shell 10 is; correspondingly, when the thickness of the second glaze slurry 250 is less than the threshold thickness, and the thinner the second glaze slurry 250 is, the smaller the maximum gray value of the second pattern 140 of the final prepared shell 10 is.

[0165] Understandably, when the thickness of the second glaze slurry 250, the weight percentage of the metal salt to the solvent in the glaze solution, and the mass ratio of the glaze solution to the thickener in the second glaze slurry 250 are constant: when the thickness of the second glaze slurry 250 is greater than or equal to the threshold thickness, the maximum grayscale variation of the second pattern 140 of the finally prepared shell 10 changes little with the change in the thickness of the second glaze slurry 250, or even stops changing. For example, in this embodiment, the threshold thickness can be, but is not limited to, 20 μm, 25 μm, or 30 μm.

[0166] When the thickness of the second glaze slurry 250 is greater than or equal to the threshold thickness, the time required to engrave the second glaze layer 260 obtained by laser on the second glaze slurry 250 is longer. Therefore, the time required to prepare the shell 10 is longer and the preparation efficiency is reduced.

[0167] In this embodiment, when the weight percentage of the metal cation salt to the solvent in the glaze solution is 50% to 75%, and the mass ratio of the glaze solution to the thickener in the second glaze slurry 250 is in the range of 1:1 to 3:1, the thickness of the second glaze slurry 250 is less than or equal to 20 μm. On the one hand, this satisfies the grayscale requirement of the second preset pattern of the final prepared shell 10, and on the other hand, it takes into account the time required for subsequent laser engraving of the second glaze layer 260 obtained from the second glaze slurry 250, resulting in a better effect in preparing the shell 10.

[0168] S140b, the shell 10 on which the second glaze slurry 250 is disposed is dried to form a second glaze layer 260 on the shell 10.

[0169] After S140b, please refer to the specific structure. Figure 13 (c) The shell 10 disposed in the second glaze slurry 250 is dried, the solvent in the glaze solution in the second glaze slurry 250 evaporates, and the remaining metal cation salt and the thickener form the second glaze layer 260.

[0170] The time and temperature required to dry the shell 10 to which the second glaze slurry 250 is applied are related to the thickness of the second glaze slurry 250. Specifically, in one embodiment, the thickness of the second glaze slurry 250 is less than or equal to 20 μm.

[0171] The step of drying the shell 10 on which the second glaze slurry 250 is disposed to form a second glaze layer 260 on the shell 10 includes: baking at 80°C to 150°C for 20 minutes to 50 minutes to form the second glaze layer 260 on the shell 10.

[0172] S150, the second glaze layer 260 is patterned to form a second patterned layer 270 to obtain a housing 10 having a first pattern 130 and a second pattern 140, wherein the second pattern 140 has a second color.

[0173] Patterning the second glaze layer 260 to form a second patterned layer 270 can be done, but is not limited to, laser engraving, texture imprinting, masking, and etching.

[0174] After S150, please refer to the specific structure. Figure 13(d) In one embodiment, the second glaze layer 260 is patterned with a laser to form a second patterned layer 270. The method of patterning the second glaze layer 260 with a laser to form the second patterned layer 270 can be the same as the method of patterning the first glaze layer 230 with a laser to form the first patterned layer 240. For details, please refer to the above description of the method of patterning the first glaze layer 230 to form the first patterned layer 240, which will not be repeated here.

[0175] In S150, obtaining a housing 10 having a first pattern 130 and a second pattern 140 includes, but is not limited to, sintering the housing 10 having a second patterned layer 270 to obtain a housing 10 having a first pattern 130 and a second pattern 140, wherein the second pattern 140 has a second color.

[0176] In one embodiment, the shell 10 having the second patterned layer 270 is sintered at 950°C to 1200°C for a period of 2 to 3 hours to obtain a shell 10 having a first pattern 130 and a second pattern 140.

[0177] After S150, please refer to the specific structure. Figure 13 (e) and Figure 13 (f), Figure 13 (e) is a schematic diagram of the structure after S150; Figure 13 (f) is Figure 13 (e) is a schematic diagram along the cross section of BB. In one embodiment, the shell 10 with the second patterned layer 270 is sintered in the same way as the first patterned layer 240, as described above, and will not be repeated here.

[0178] The shell preparation method provided in this application can form a first pattern 130 with a first color using a first glaze slurry 220, and can also form a second pattern 140 with a second color using a second glaze slurry 250. Therefore, the shell 10 prepared by the shell preparation method provided in this application has a better appearance.

[0179] As can be seen from the above analysis, the first color is different from the second color. Correspondingly, the first glaze slurry 220 is different from the second glaze slurry 250. The sintering temperature for sintering the first patterned layer 240 obtained from the first glaze slurry 220 is different from the sintering temperature for sintering the second patterned layer 270 obtained from the second glaze slurry 250.

[0180] If the first patterned layer 240 obtained from the first glaze slurry 220 and the second patterned layer 270 obtained from the second glaze slurry 250 are sintered in the same sintering process at a sintering temperature T0, when the sintering temperature T0 is compatible with the sintering temperature T1 of the first glaze slurry 220, the sintering temperature T0 may not be compatible with the sintering temperature T2 of the second glaze slurry 250; correspondingly, when the sintering temperature T0 is compatible with the sintering temperature T2 of the second glaze slurry 250, it may not be compatible with the sintering temperature T1 of the first glaze slurry 220. Therefore, when the first patterned layer 240 and the second patterned layer 270 are sintered in the same sintering process at a sintering temperature T0, the formed first pattern 130 or second pattern 140 may be distorted.

[0181] The shell preparation method provided in this application involves sintering the first patterned layer 240 at a sintering temperature (named the first sintering temperature) adapted to the first glaze slurry 220 to form a shell 10 with a first pattern 130, and then sintering the second patterned layer 270 at a sintering temperature (named the second sintering temperature) adapted to the second glaze slurry 250 to form a second pattern 140. This method can reduce the risk of distortion in the first pattern 130 and the second pattern 140 that have been prepared.

[0182] Furthermore, when it is necessary to prepare a pattern with more than two colors, a first pattern 130 with a first color, a second pattern 140 with a second color, and an Nth pattern with an Nth color can be prepared sequentially, where N≥3. This allows the prepared housing 10 to have a pattern with multiple colors. For example, the prepared housing 10 can have a multi-color texture effect. This application also provides a housing 10, which can be prepared by the housing preparation method described above; the housing preparation method can prepare the housing 10 provided in this application. The housing 10 can be applied to an electronic device 1 (see...). Figure 19 and Figure 20 The electronic device 1 can be, but is not limited to, a mobile phone, tablet computer, laptop computer, desktop computer, smart bracelet, smartwatch, e-reader, game console, or any other device with a housing 10. When the housing 10 is applied to the electronic device 1, it can be, but is not limited to, a back cover, mid-frame, or component of the electronic device 1. The housing 10 can be a 2D housing, a 2.5D housing, or a 3D housing.

[0183] Please refer to the following: Figure 14 and Figure 15 , Figure 14 A schematic diagram of a housing provided according to one embodiment of this application; Figure 15 for Figure 14A cross-sectional view along line II. The ceramic housing 10 includes a ceramic housing body 110 and a colorant 120. The colorant 120 is disposed within the ceramic housing body 110 and located in at least a portion of the ceramic housing body 110, such that the housing 10 has a first pattern 130.

[0184] In this embodiment, the raw material components of the ceramic shell body 110 include ceramic powder. In other words, the shell 10 is a ceramic shell, and the ceramic shell body 110 is made of ceramic material. Optionally, the ceramic powder includes at least one of zirconium oxide, alumina, silicon dioxide, titanium dioxide, silicon nitride, magnesium oxide, chromium oxide, beryllium oxide, vanadium pentoxide, boron trioxide, spinel, zinc oxide, calcium oxide, mullite, and barium titanate. In a specific embodiment, the ceramic powder is zirconium oxide powder, and the ceramic shell body 110 is a zirconium oxide ceramic shell body.

[0185] The color-developing substance 120 is disposed within the ceramic housing body 110. The at least part of the area where the color-developing substance 120 is disposed and the other areas where the color-developing substance 120 is not disposed exhibit different colors or different gray levels, thereby giving the housing 10 a first pattern 130.

[0186] In one embodiment, the color-developing substance 120 is a metal cation disposed in at least a portion of the ceramic housing body 110, and the metal cation will be described in detail later.

[0187] In this embodiment, the ceramic shell body 110 of the shell 10 is formed by sintering the ceramic shell body 210 in the previous shell preparation method.

[0188] The housing 10 provided in this application embodiment has a first pattern 130. Therefore, the housing 10 has the effect that when the housing 10 is applied to the electronic device 1, the electronic device 1 has a better appearance and better distinguishability.

[0189] The effect of the first pattern 130 includes at least one of a texture effect and a gradient effect. Figure 14 and Figure 15 The effect of the first pattern 130 is used as an example to illustrate the texture effect. Please refer to the attached document. Figure 16 and Figure 17 , Figure 16 A schematic diagram of a housing provided for another embodiment of this application; Figure 17 for Figure 16 A schematic cross-sectional view along line II-II. Figure 16 and Figure 17 In the example shown, the effect of the first pattern is a gradient effect.

[0190] When the effect of the first pattern 130 includes a texture effect, the first pattern 130 is a texture pattern. For example, the first pattern 130 includes multiple textures arranged according to a preset rule, such as multiple lines arranged according to a preset rule (e.g., straight line segments, curved ends, or hyperbolic segments), or multiple shapes arranged according to a preset rule (e.g., triangles, quadrilaterals, circles, or annular rings). When the effect of the first pattern 130 includes a gradient effect, for example, it may include a watercolor gradient pattern or a marble gradient pattern, etc. It should be noted that the gradient effect is manifested in the gradient change of the metal cations along one or more directions in the shell 10. Figure 16 and Figure 17 The first pattern 130 is a heart pattern with a gradient effect, which is used as an example for illustration and should not be construed as a limitation on the gradient effect and pattern of the shell 10 provided in the embodiments of this application.

[0191] In one embodiment, the ceramic housing body 110 has a first surface 111 and a second surface 112 disposed opposite to each other. The first surface 111 is the outer surface of the housing 10. The colorant 120 is disposed within the ceramic housing body 110 and distributed on the first surface 111 (see further details). Figures 14 to 17 The ceramic housing body 110 has an outer surface, and the coloring substance 120 is disposed inside the ceramic housing body 110 adjacent to the first surface 111 and distributed in the portion where the outer surface is located.

[0192] As described above in the preparation method of the shell 10, the ceramic shell body 210 with the first patterned layer 240 is sintered to obtain a shell 10 with the first pattern 130. It can be seen that the metal cations enter the interior of the ceramic blank from the surface where the first patterned layer 240 is located. After sintering, the ceramic shell body 110 is obtained, and the surface of the ceramic blank with the first patterned layer 240 becomes the outer surface of the ceramic shell body 110 after sintering. Therefore, the colorant 120 is disposed inside the ceramic shell body 110 and adjacent to the outer surface (first surface 111).

[0193] In one embodiment, the gloss of the first surface 111 is greater than that of the second surface 112.

[0194] The gloss of the first surface 111 is greater than that of the second surface 112, which makes the appearance of the housing 10 more glossy and gives the housing 10 a better texture.

[0195] In this embodiment, the second surface 112 is disposed opposite to the first surface 111. Therefore, the second surface 112 is usually used as the inner surface of the housing 10. The second surface 112 is usually not observed. Therefore, when manufacturing the housing 10, there is no need to perform high-precision polishing on the second surface 112, or even to polish the second surface 112, thereby saving the cost of manufacturing the housing 10.

[0196] In one embodiment, the gloss level (60° angle test) of the first surface 111 is 130 Gu to 160 Gu. Specifically, the gloss level of the ceramic housing body 210 can be, but is not limited to, 130 Gu, 135 Gu, 140 Gu, 145 Gu, 150 Gu, 155 Gu, 160 Gu, etc.

[0197] When the gloss level of the first surface 111 of the housing 10 is too low (e.g., below 110 Gu), the gloss of the surface of the housing 10 is not obvious, affecting the texture of the surface. When the gloss level of the first surface 111 of the housing 10 is too high (e.g., above 160 Gu), the cost and process difficulty of manufacturing the first surface 111 of the housing 10 are increased. When the gloss level of the first surface 111 of the housing 10 is between 110 Gu and 160 Gu, the surface of the housing 10 has good gloss and is easy to manufacture.

[0198] Optionally, the Vickers hardness of the housing 10 in this application can be, but is not limited to, 1200 HV to 1400 HV, so that the housing 10 has a high hardness. Specifically, it can be, but is not limited to, 1200 HV, 1230 HV, 1250 HV, 1280 HV, 1300 HV, 1320 HV, 1350 HV, 1380 HV, 1400 HV, etc.

[0199] In one implementation, please refer to the following: Figures 14 to 17 The thickness d1 of the ceramic shell body 110 satisfies: 0.2mm≤d1≤1.0mm; the dispersion thickness d2 of the colorimetric substance 120 satisfies: 1μm≤d2≤300μm.

[0200] For example, the thickness of the shell 10 is 0.2 mm, or 0.25 mm, or 0.3 mm, or 0.35 mm, or 0.4 mm, or 0.45 mm, or 0.5 mm, or 0.55 mm, or 0.6 mm, or 0.65 mm, or 0.7 mm, or 0.75 mm, or 0.8 mm, or 0.85 mm, or 0.9 mm, or 0.95 mm, or 1.0 mm. Accordingly, the thickness of the portion of the shell 10 infiltrated by the metal cation is from 1 μm to 300 μm. For example, the thickness of the portion of the shell 10 infiltrated by the metal cation is 1 μm, or 1.5 μm, or 2 μm, or 5 μm, or 10 μm, or 15 μm, or 20 μm, or 30 μm, or 40 μm, or 50 μm, or 60 μm, or 70 μm, or 80 μm, or 90 μm, or 100 μm, or 110 μm, or 120 μm. μm, or 130μm, or 140μm, or 150μm, or 160μm, or 170μm, or 180μm, or 190μm, or 200μm, or 210μm, or 220μm, or 230μm, or 240μm, or 250μm, or 260μm, or 270μm, or 280μm, or 290μm, or 300μm.

[0201] In one embodiment, the ceramic shell body 110 comprises ceramic, and the colorimetric substance comprises metal cations. The thickness d1 of the ceramic shell body 110 satisfies: 0.4 mm ≤ d1 ≤ 0.5 mm. To distinguish the minimum dispersion thickness d2 of the colorimetric substance (labeled d2' for ease of illustration in the figure), it satisfies: 1 μm ≤ d2' ≤ 2 μm; the maximum dispersion thickness d2 of the colorimetric substance satisfies: 100 μm ≤ d2 ≤ 200 μm.

[0202] In one embodiment, the ceramic material includes one of zirconia ceramic and alumina ceramic; the metal cation includes at least one or more of iron ions, cobalt ions, and nickel ions.

[0203] In one implementation, please refer to the following: Figure 18 , Figure 18 This is a schematic diagram of a housing provided for another embodiment of this application. The first pattern 130 has a first color, and the housing 10 also has a second pattern 140, which has a second color.

[0204] The first pattern 130 has a first color, and the grayscale of the first color in different parts of the first pattern 130 may be the same or different, which is not limited in this embodiment. The second pattern 140 has a second color, and the grayscale of the second color in different parts of the second pattern 140 may be the same or different, which is not limited in this embodiment.

[0205] In this embodiment of the application, the housing 10 has a first pattern 130 and a second pattern 140, thereby giving the housing 10 a richer appearance.

[0206] This application also provides an electronic device 1, which includes the housing described in any of the foregoing embodiments. The electronic device 1 provided in this application will now be described in detail with reference to the accompanying drawings. Please refer to them together. Figure 19 and Figure 20 , Figure 19 A perspective view of an electronic device provided according to an embodiment of this application; Figure 20 for Figure 19 The diagram shows an exploded view of the electronic device. The electronic device 1 can be, but is not limited to, a mobile phone, tablet computer, or other device with a housing 10. The housing 10 is described previously and will not be repeated here. In this embodiment, the predetermined surface 110 of the housing 10 constitutes part of the exterior surface of the electronic device 1.

[0207] In this embodiment, the electronic device 1 includes a housing 10, a display screen 30, a mid-frame 70, a circuit board 40, and a camera module 50. The housing 10 and the display screen 30 are respectively disposed on opposite sides of the mid-frame 70. The mid-frame 70 supports the display screen 30, and the sides of the mid-frame 70 are exposed above the housing 10 and the display screen 30. The housing 10 and the mid-frame 70 form a receiving space for accommodating the circuit board 40 and the camera module 50. The housing 10 has a light-transmitting portion 10a, through which the camera module 50 can capture images; that is, in this embodiment, the camera module 50 is a rear-facing camera module. It can be understood that in other embodiments, the light-transmitting portion 10a may be disposed on the display screen 30, i.e., the camera module 50 is a front-facing camera module. In the schematic diagram of this embodiment, the light-transmitting part 10a is shown as an opening. In other embodiments, the light-transmitting part 10a may not be an opening, but may be made of a light-transmitting material, such as plastic or glass.

[0208] It is understood that the electronic device 1 described in this embodiment is merely one form of the electronic device 1 used in the housing 10, and should not be construed as a limitation on the electronic device 1 provided in this application, nor should it be construed as a limitation on the housing 10 provided in various embodiments of this application.

[0209] Although embodiments of this application have been shown and described above, it is understood that the above embodiments are exemplary and should not be construed as limiting this application. Those skilled in the art can make changes, modifications, substitutions and variations to the above embodiments within the scope of this application, and such improvements and refinements are also considered to be within the protection scope of this application.

Claims

1. A method for preparing a shell, characterized in that, The shell preparation method includes: A ceramic housing body is provided, the ceramic housing body having a first surface and a second surface disposed opposite to each other, the first surface being the outer surface of the prepared housing; A first glaze layer is formed on at least a portion of the surface of the ceramic housing body, the first glaze layer being formed from a first glaze slurry, wherein the surface is the first surface; and The first glaze layer is patterned to form a first patterned layer; A ceramic shell body with a first patterned layer is sintered at a first sintering temperature of 950°C to 1200°C for a sintering time of 2 hours to 3 hours to obtain a shell with a first pattern. The first patterned layer includes a coloring substance, the first pattern has a first color, and the coloring substance includes metal cations. The metal cations penetrate into the ceramic shell body and are located in at least a portion of the ceramic shell body, so that the shell has the first pattern. The coloring substance is disposed in the ceramic shell body adjacent to the first surface and distributed in the portion where the outer surface is located. The thickness of the shell is 0.2 mm to 1.0 mm, and the thickness of the portion of the shell infiltrated by the metal cations is 1 μm to 300 μm. A second glaze layer is provided on at least a portion of the surface of the housing, the second glaze layer being formed from a second glaze slurry; The second glaze layer is patterned to form a second patterned layer; The shell with the second patterned layer is sintered at a second sintering temperature to obtain a shell with a second pattern, wherein the second sintering temperature is different from the first sintering temperature, and the second pattern has a second color.

2. The shell preparation method according to claim 1, characterized in that, The ceramic housing body includes: Ceramic granules are shaped to obtain a shell green body; The shell blank is debonded and sintered to obtain the shell blank; and The shell blank is processed and polished to obtain the ceramic shell body.

3. The shell preparation method according to claim 2, characterized in that, The process of molding ceramic granules to obtain a shell green body includes: ceramic powder and a binder are mixed and granulated to obtain ceramic granules, wherein the ceramic powder has a particle size range of 0.2 μm to 0.8 μm, the ceramic granules have a mesh range of 40 mesh to 100 mesh, the BET specific surface area of the granules is 6 m 2 / g to 10 m 2 / g, the binder is at least one of an epoxy-based binder, a polyether-based binder, and the weight percentage of the binder in the ceramic granules ranges from 3% to 5%; and The ceramic particles are shaped to obtain a shell green body.

4. The shell preparation method according to claim 3, characterized in that, The forming process includes compression molding or injection molding; when the forming process is compression molding, the step of forming the ceramic particles to obtain a shell green body includes: The molding pressure ranges from 10MPa to 15MPa, and the pressure is held for 10s to 20s to form the ceramic particles to obtain a shell green body.

5. The shell preparation method according to claim 2, characterized in that, The process of debinding and sintering the shell blank to obtain the shell blank includes: The shell blank is gradually heated to 800°C to 950°C to remove the adhesive, and the adhesive removal time is between 2 hours and 3 hours, so as to remove the adhesive from the shell blank. The temperature is gradually increased to 1350℃ to 1500℃ for sintering, and the sintering time ranges from 8 hours to 10 hours; and The shell blank is obtained by cooling it to room temperature.

6. The shell preparation method according to claim 2, characterized in that, The process of machining and polishing the shell blank to obtain the ceramic shell body includes: The shell blank is processed to obtain a shell blank of a preset size; and The ceramic shell body is obtained by grinding and polishing a shell blank of a preset size, wherein the surface gloss of the ceramic shell body is 130Gu to 160Gu.

7. The shell preparation method according to claim 1, characterized in that, The first glaze slurry includes a glaze solution and a thickener, wherein the mass ratio of the glaze solution to the thickener ranges from 1:1 to 3:1; the glaze solution includes a metal cation salt and a solvent, wherein the weight percentage of the metal cation salt to the solvent is 50% to 75%.

8. The shell preparation method according to claim 1, characterized in that, The formation of a first glaze layer on at least a portion of the surface of the ceramic shell body, the first glaze layer being formed from a first glaze slurry, includes: A first glaze slurry is formed in at least a portion of the ceramic shell body, the thickness of the first glaze slurry being less than or equal to 20 μm; The first glaze slurry is dried by baking at 80°C to 150°C for 20 to 50 minutes to form the first glaze layer on the ceramic shell body.

9. The shell preparation method according to claim 1, characterized in that, The step of patterning the first glaze layer to form a first patterned layer includes: Output the preset pattern to the laser engraving device; The power of the laser output by the laser engraving device is controlled according to the preset pattern. Different gray levels in the preset pattern correspond to different laser powers, wherein areas with higher gray levels correspond to lower laser powers. The first glaze layer is irradiated with the laser to remove part of the glaze in the first glaze layer to form the first patterned layer.

10. A ceramic shell, characterized in that, The housing includes: A ceramic housing body, the ceramic housing body having a first surface and a second surface disposed opposite to each other, the first surface being the outer surface of the housing; and A color-developing substance comprising a metal cation, the metal cation permeating into a ceramic shell body and located in at least a portion of the ceramic shell body to give the shell a first pattern, wherein the color-developing substance is disposed in the ceramic shell body adjacent to the first surface and distributed in the portion where the outer surface is located, the shell thickness is 0.2 mm to 1.0 mm, the thickness of the portion of the shell infiltrated by the metal cation is 1 μm to 300 μm, the first pattern has a first color, and the shell also has a second pattern having a second color, wherein the sintering temperature for forming the first pattern is a first sintering temperature, the temperature for forming the second pattern is a second sintering temperature, and the second sintering temperature is different from the first sintering temperature.

11. The housing as claimed in claim 10, characterized in that, The gloss of the first surface is greater than that of the second surface.

12. The housing as claimed in claim 10, characterized in that, The thickness d1 of the ceramic shell body satisfies: 0.2mm≤d1≤1.0mm; the dispersion thickness d2 of the colorimetric substance satisfies: 1μm≤d2≤300μm.

13. The housing as claimed in claim 12, characterized in that, The ceramic shell body comprises ceramic, and the thickness d1 of the ceramic shell body satisfies: 0.4mm ≤ d1 ≤ 0.5mm; the minimum dispersion thickness d2 of the colorimetric substance satisfies: 1μm ≤ d2 ≤ 2μm; the maximum dispersion thickness d2 of the colorimetric substance satisfies: 100μm ≤ d2 ≤ 200μm.

14. The housing as claimed in claim 13, characterized in that, The ceramic material includes one of zirconia ceramic and alumina ceramic; the metal cation includes at least one or more of iron ion, cobalt ion, and nickel ion.

15. The housing as claimed in claim 10, characterized in that, The first pattern includes at least one of a texture pattern and a gradient pattern.

16. An electronic device, characterized in that, The electronic device includes a housing as described in any one of claims 11-15.

Citation Information

Patent Citations

  • Casing and production method thereof

    CN108527622A

  • Surface treatment method for ceramic material piece, housing assembly and electronic device

    CN109050139A

  • Ceramic shell, method for processing surface thereof, and electronic equipment

    CN111031158A

  • Preparation method of shell and electronic equipment

    CN112872603A

  • Covers for electronic devices

    US20220071036A1