A mud film reinforcing construction method for a shield cutter face and a mud film component
By using the mud film reinforcement construction method, the safety and stability issues of shield cutterhead replacement under complex geological conditions have been solved, enabling safe cutterhead replacement of the shield machine under complex geological conditions, reducing construction risks and costs, and making it widely applicable.
Patent Information
- Application Number
- CN202111451834.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-01
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2041-12-01
AI Technical Summary
Existing methods for changing cutterheads in tunnel boring machines (TBMs) are not effective under complex geological conditions, especially when the ground has poor air tightness at the TBM stop location, the ground lacks reinforcement capabilities, or there is a large amount of water seepage at the tunnel face. In these situations, it is impossible to change cutterheads safely and reliably.
The mud film reinforcement construction method is adopted, which includes forming a mud film grouting zone after the tunnel boring machine stops. Through water-stop rings, shield body and cutterhead protection, filling operation and mud film injection, combined with the use of polyurethane and foaming agent, the soil chamber is stabilized, space is provided for cutter replacement operation, and the shield shell is protected by high temperature gear oil pump and polyurethane injection to prevent the shield body from seizing.
It effectively controls ground settlement, increases the self-stability of the strata, prevents water and sand inrush, ensures the stability and effectiveness of the working face, reduces the risk of cutter replacement, is simple to construct, has low cost, is widely applicable, and reduces environmental impact.
Smart Images

Figure CN114352293B_ABST
Abstract
Description
[0001] Method Domain
[0002] This invention relates to the field of shield tunneling methods, specifically to a mud film reinforcement construction method and mud film composition for the cutterhead replacement face of a shield tunnel.
[0003] Background Method
[0004] Shield tunneling is a fully mechanized construction method for urban rail transit. Its main mechanical equipment is the shield machine, which is divided into two types: earth pressure balance shield machine and slurry balance shield machine, with the earth pressure balance shield machine being more commonly used. During tunnel excavation, the shield machine uses cutters to cut soil and break rocks. After long-distance excavation (especially in hard rock strata or unevenly textured strata), cutter replacement is necessary. However, if the strata where the shield machine stops have poor air tightness, the ground lacks reinforcement capacity, or there is excessive water inflow at the tunnel face, the shield machine cannot be replaced using the methods commonly used in China.
[0005] Currently, the commonly used tool changing methods in China are as follows:
[0006] (1) When the formation has good self-stabilizing ability, the cutterhead is replaced under normal pressure under natural conditions;
[0007] (2) When the strata and the soil chamber are airtight, pressurized cutter replacement is adopted under natural conditions;
[0008] (3) When the formation has poor self-stabilizing ability and the ground has the conditions for reinforcement, the cutter replacement under normal pressure under the formation reinforcement is adopted under natural conditions.
[0009] (4) When the air tightness between the stratum and the soil chamber is poor and the ground has the conditions for reinforcement, the pressurized cutter replacement under the stratum reinforcement is adopted under natural conditions.
[0010] In summary, with the development of rail transit construction, the geological conditions and structural cross-sections of the tunnel sections have become more diverse. This means that the commonly used cutter replacement methods in China are no longer sufficient to meet the current needs, and thus cannot replace the cutterheads of the tunnel boring machine. Summary of the Invention
[0011] The purpose of this invention is to overcome the shortcomings of existing methods and provide a mud film reinforcement construction method and mud film composition for shield tunnel cutterhead replacement face. It is reasonably designed, easy to operate, low in investment cost, high in safety factor and good in use. It can effectively solve the practical problem that existing commonly used cutterhead replacement methods cannot be used when the geological conditions at the shield machine stopping position are complex, fissure water is developed, karst, solution pores and fissures are particularly developed, there are no reinforcement conditions above the cutterhead, and the soil chamber cannot maintain pressure.
[0012] A method for reinforcing the cutterhead face of a tunnel boring machine with mud film includes the following steps:
[0013] Step 1, Tunnel Boring Machine Shutdown Operation: After confirming that the filling chamber atmospheric pressure cutterhead replacement method is adopted, after the tunnel boring machine is shut down, based on the original soil chamber pressure of 1.7 bar, the articulated cylinder is retracted to make the shield body retreat 80mm, leaving a mud film grouting area and providing working space for cutterhead replacement.
[0014] Step 2: Constructing a water-stop ring: To prevent water from flowing into the soil chamber behind the ring-shaped segments and causing filling failure, a water-stop ring needs to be formed by double-liquid grouting around the segments to cut off the water flow behind them. The grouting ring number is selected at the 5th to 10th ring position after the shield tail is removed. Water glass and cement grout are used for double-liquid grouting in a 1:1 ratio, with the cement grout having a water-cement ratio of 1:1.
[0015] Step 3, Shield body and cutterhead protection: (1) Inject the prepared mud film into the shield shell and the back of the 1-3 ring segments that have come off 80mm after the shield machine retreats through the radial holes at the shield tail, filling and wrapping the entire shield machine; (2) After injecting the mud film, open grouting holes in the radial direction at the shield tail, and inject polyurethane into the grouting holes with a high-temperature gear oil pump; (3) Inject grease into the cutterhead sealing system.
[0016] Step 4, filling operation: Inject mud film into the circular area formed by the 1 to 3 ring segments that have come off 80mm backward from the shield machine through the articulated advanced grouting holes, the radial grouting holes of the front shield, and the observation holes of the soil chamber from bottom to top.
[0017] Step 5, Shield tunneling resumption: After the cutterhead is replaced, operate the cutterhead to rotate back and forth to free it from its entrapment, and inject foam agent into the soil chamber to resume tunneling; when resuming tunneling, use a small thrust that increases from zero to push the cutterhead, and tunnel at a low speed, controlling the penetration depth to 1-10 mm / r. When the cutting edge of the cutter is worn out, resume normal tunneling.
[0018] Moreover, in step four, an average of 3m is injected 3 25 kg of sodium carboxymethyl cellulose (CMC) needs to be added to the mud film to prevent segregation of the mud film slurry. When adding sodium carboxymethyl cellulose (CMC) to the mortar tank, it must be sprinkled in layer by layer and the slurry level must be controlled below the highest position of the mixing shaft to ensure uniform mixing.
[0019] Furthermore, after step four is completed, a high-temperature gear oil pump is used to inject polyurethane into each hole of the radial grouting pipe of the front shield in the soil chamber wall, left center, right center, and chamber door, and the cutter head is rotated at a low speed of less than 0.5 r / min. At the same time, the surface settlement is strictly monitored to ensure that the injected polyurethane reacts fully with the excess water in the soil chamber. The pressure is controlled at 4-5 bar during the filling period. After the filling is completed, the soil pressure will decrease and stabilize at 1.8-2.0 bar.
[0020] Moreover, after the earth pressure drops to 1.8-2.0 bar, air is continuously added to the earth chamber through 6 foam agent pipes to increase the pressure until the earth pressure in the earth chamber stabilizes at 2.3-3.0 bar. Then, 400L of water is added to the earth chamber through 14 radial grouting holes until the earth pressure is constant. Finally, single-liquid grout and water glass are alternately injected into the earth chamber.
[0021] The mud membrane used in a mud membrane reinforcement construction method for the cutterhead replacement face of a shield tunneling machine comprises the following components: 840-860 parts bentonite, 360-440 parts fine sand, 150-170 parts cement, and 492-508 parts water.
[0022] The advantages and effects of the present invention are:
[0023] The mud film construction method of this invention can effectively control the settlement of surrounding buildings. In situations where ground reinforcement is not feasible, an innovative process combining filling and grouting is employed, effectively increasing the self-stability of the current stratum, preventing water and sand inrush, and thus preventing settlement of surrounding buildings. A comprehensive displacement monitoring system can be established on the ground and around the buildings, with settlement observation points buried at and around the cutterhead location. Various construction parameters can be adjusted based on the monitoring results.
[0024] The mud film construction method of the present invention can effectively control the stability and safety of the working face and ensure that the working face has the timeliness for operation.
[0025] First, it controls the stability of the tunnel face. By filling the tunnel face with mud film and aerating the tunnel face to form channels, the alternating flow of single-liquid grout and double-liquid grout fills and seals the karst fissures, effectively preventing the instability of the tunnel face, ground subsidence, or even cracking and collapse caused by soil erosion.
[0026] Secondly, it ensures the stability and effectiveness of the working surface. Because this method utilizes the dual protection of cement-bentonite mortar and secondary grouting, several successful cutterhead replacement tests have shown that the working surface has remained stable for more than 10 days, meeting the requirements for cutterhead replacement.
[0027] The mud film construction method of the present invention is simple in construction process, convenient in operation, and low in cost, and effectively prevents the shield from seizing.
[0028] First, the construction is less restricted by conditions. This method is carried out underground, with fewer limitations imposed by surface conditions. It has a wide range of applicable geological conditions and can effectively control water inflow at the cross-section, resulting in good reinforcement of the tunnel face.
[0029] Secondly, it effectively prevents the cutterhead from solidifying during shutdown. This method has minimal impact on the environment and traffic. It has minimal impact on the geological structure and causes minimal surface subsidence; it will not solidify the cutterhead and will not affect the effective advancement of the tunnel boring machine after a long period of shutdown.
[0030] Third, it has high construction efficiency. This method has low construction cost, high construction efficiency, and short construction period, and can achieve the reinforcement effect required for opening the soil in a short time.
[0031] Fourth, reduce the risk of shield cutterhead replacement. The risk of shield cutterhead replacement is extremely high in water-rich strata. By implementing a sophisticated aeration system and strict grouting operation procedures, this risk is reduced, ensuring the safety of personnel and equipment. Attached Figure Description
[0032] Figure 1 This is a flowchart of the construction process of the present invention; Detailed Implementation
[0033] To further understand the content, features, and effects of this invention, the following embodiments are provided, and detailed descriptions are given below in conjunction with the accompanying drawings. It should be noted that these embodiments are descriptive, not limiting, and should not be construed as limiting the scope of protection of this invention.
[0034] like Figure 1 As shown, this construction method is applicable to working conditions where the strata at the tunnel boring machine (TBM) parking location have strongly developed karst, solution pores, and fissures, abundant fissure water, and poor self-stability of the tunnel face under the influence of water and sand inflow. It is particularly suitable for working conditions where the cutterhead is located directly above a major roadway, ground reinforcement is impossible, and the TBM cannot be replaced using the four commonly used methods in China. This method includes the following steps:
[0035] Step 1, Tunnel Boring Machine Shutdown Operation: After confirming the use of the filling chamber atmospheric pressure cutterhead replacement method, after the tunnel boring machine stops, based on the original soil chamber pressure of 1.7 bar, retract the articulated hydraulic cylinder to make the shield body retreat 80mm. The purpose is to ensure that an 80mm mud film protective layer is formed between the face and the cutterhead during the filling process, and to provide working space for cutterhead replacement.
[0036] In actual construction, the tunnel boring machine (TBM) retracts the shield body according to the actual situation, generally by 80-120mm. In this example, the shield body retracted by 80mm under the reaction force of the soil chamber pressure, mainly to ensure the integrity of the mud film protective layer formed between the tunnel face and the cutterhead.
[0037] Step 2: Constructing a Water-Stop Ring: To prevent water from flowing into the soil chamber behind the ring-shaped tunnel segments and causing filling failure, a water-stop ring needs to be formed by double-liquid grouting around the tunnel segments to cut off the water flow. The grouting ring number can be selected at the 5th to 10th ring position after the shield tail exit. Double-liquid grouting using water glass and cement grout is employed, with a cement grout:water glass ratio of 1:1 and a cement grout water-cement ratio of 1:1.
[0038] In actual construction, after the double-liquid grout was injected into the tail of the shield to form a water-stop ring, polyurethane was simultaneously injected into the radial grouting holes at the tail of the shield to provide double protection for the shield body and to block water from the rear.
[0039] Step 3: Protection of the shield and cutterhead
[0040] Injecting cement grout may cause problems such as damage to the synchronous grouting pipe or foam nozzle, cutterhead seal, and shield blockage. To avoid adverse effects of the grout on the shield structure, the following measures should be taken before grouting:
[0041] (1) Prepared cement-bentonite was injected into the shield shell and behind the detached 1-3 ring segments of the tunnel boring machine through the radial holes at the tail of the shield, filling and wrapping the entire tunnel boring machine. A total of 10m³ of cement-bentonite was injected. 3 .
[0042] (2) After injecting cement bentonite, inject two barrels of polyurethane into the four radial holes of the shield tail using a high-temperature gear oil pump to enhance the water-stopping effect at the rear of the shield tail.
[0043] (3) Inject an appropriate amount of grease into the cutter head sealing system to prevent damage to the cutter head main bearing seal.
[0044] In actual construction, the weight ratio of the cement-bentonite slurry prepared through experiments was bentonite:fine sand:cement:water = 850±10:400±40:160±10:500±8. In this case, the weight ratio of the cement-bentonite mortar was bentonite:fine sand:cement:water = 850:400:160:500. To ensure uniform mixing, the commercial concrete plant prepared the slurry according to the ratio, using well-graded fine sand. The specific mix ratio was adjusted according to the actual site conditions.
[0045] Step 4: Filling the warehouse
[0046] (1) Cement-bentonite is injected into the soil chamber from bottom to top through the articulated pre-grouting hole, the radial grouting hole of the front shield, and the soil chamber observation hole. According to calculation (the cutterhead excavation diameter is 6480mm), the theoretical filling volume of the soil chamber is about 40m³. 3 Due to the presence of fissures in the strata, a total of 80m³ was injected three days in advance. 3 Cement bentonite.
[0047] (2) After filling, use a high-temperature gear oil pump to inject two barrels of polyurethane into each hole of the radial grouting pipe of the front shield at the soil chamber wall, left center, right center, and chamber door, while rotating the cutterhead at a low speed (less than 0.5 r / min); at the same time, strictly monitor the surface settlement. Ensure that the injected polyurethane reacts fully with the excess water in the soil chamber. During filling, the pressure is controlled at 4-5 bar. After filling, the soil pressure will decrease and stabilize at 1.8-2.0 bar.
[0048] (3) Continuously pressurize the soil chamber by adding air through 6 foaming agent pipes until the soil pressure inside the chamber stabilizes at 2.3-3.0 bar. Then, add 400L of water through 14 radial grouting holes. After the soil pressure remains unchanged, once the air pressure in the soil chamber stabilizes, alternately inject single-component grout and water glass through the radial grouting holes of the front shield, as follows:
[0049] (4) Check the filling and grouting effect and clear half of the grout.
[0050] During the grouting process, the quality should be checked continuously. Samples should be taken from the manhole wall by opening the ball valve, and the moisture content of the samples should be used to determine the grouting status. When the grouting volume, the grout discharge from the manhole observation hole, and the top pressure all meet the set requirements, the grouting effect should be checked again through the radial grouting holes of the front shield.
[0051] In actual construction, the direction of water flow is determined by observing the opening of the soil chamber door. Grout is injected from bottom to top through the hinged grouting holes of the front shield. 8.3 kg of CMC is added to each cubic meter of injected grout. When adding CMC to the mortar tank, it must be sprinkled layer by layer, and the grout level must be controlled below the highest point of the mixing shaft to ensure uniform mixing. In this example, due to the presence of karst, solution pores, and fissures, with a cutterhead excavation diameter of 6480 mm, the theoretical filling volume of the soil chamber is approximately 40 m³. 3 At that time, 80m was actually injected. 3 The specific injection volume should be adjusted based on the pressure in the soil chamber to ensure the chamber is filled as much as possible and a complete mud film is formed.
[0052] In actual construction, the quality of the specially formulated cement-bentonite grout and secondary grouting is regularly observed through the observation holes of the soil chamber door and radial holes. The chamber door is opened to check the water-stopping effect, whether the conditions for cutter replacement are met, and whether there is water leakage at the working face. In this example, after filling is completed, before injecting the double-liquid grout, 400L of water is injected first to observe the soil pressure. After the pressure is basically stable, single-liquid grout and water glass are injected intermittently, and air is injected simultaneously through the foam system. After the grouting and sealing are completed, the soil is allowed to stand for 3 days. After the conditions for opening the chamber are met, the soil is discharged to the central shaft of the cutterhead using a screw conveyor. The purpose is to provide a working surface for cutter replacement and to expose the central cutter for easy replacement of the central double-edged cutter.
[0053] Step 5: In actual construction, the soil chamber cleaning process: After the filling and grouting are completed, the soil chamber can be cleaned under normal pressure. To ensure safety, when using a high-pressure water gun to wash the cutterhead and tools during soil chamber cleaning, care must be taken to avoid contact with the working face; during the cleaning process, pay attention to ventilation and observe changes in the monitoring data of the working face and ground. If any sudden change occurs, immediately close the chamber door and refill the soil chamber. In this case, ① during the cutter replacement process, the ball valve of the No. 6 articulated pre-grouting pipe was opened to drain water, ensuring that the water level remained below the working face. The cutter replacement was carried out according to the principle of "removing one and installing one". ② During the cleanup and cutter replacement process, a dedicated person must be assigned to monitor the stability of the working face and transmit communication information between the cutter replacement personnel in the soil chamber. If the working face stability is insufficient, personnel should be immediately notified to leave the chamber, close the chamber door, and refill the chamber. ③ When replacing cutters, pay attention to replacing severely damaged cutters first, and adjust the installed cutters according to the degree of wear, such as adjusting a single cutter to a single-blade double-edged cutter. ④ For low-speed rotating cutterheads below the half-chamber that do not have a working face, adjust the cutter position and replace them. ⑤ While replacing cutters, check and clean the integrity of various pipelines and pressure equipment in the soil chamber. ⑥ During the cutter replacement process, attention should be paid to ventilation. Personnel can only enter the chamber if the gas detection is qualified. Ventilation can be achieved by using a small axial flow fan or by injecting air into the bottom of the soil chamber through a foam agent pipe to form air circulation.
[0054] Step Six: Shield Tunneling Resumption: After the cutterhead replacement is completed, a comprehensive inspection of the soil chamber and the area in front of the cutterhead, as well as all pipelines, is conducted to ensure that tools and debris are not left inside the soil chamber. Then, the chamber door is closed. Next, the shield operator repeatedly rotates the cutterhead to free it from obstruction. To prevent the tail shield from locking up, steel plates are welded onto the middle and tail shields if necessary to ensure the overall shield body is freed.
[0055] In actual construction, after the cutterhead replacement is completed, the foam system, cutterhead sealing system, and screw conveyor system must be tested and confirmed to be normal. After confirming normal operation, a certain amount of foaming agent is injected into the soil chamber, and tunneling resumes. When resuming tunneling, a small thrust (increasing from zero) and a low cutterhead speed are used to protect the cutters. Normal tunneling resumes once the cutter edges are worn down. The tunneling parameters are controlled as follows: thrust 1500T-2000T, torque 2000kN.m-2500kN.m, cutterhead speed 1.3r / min-1.5r / min, penetration 1mm / r-10mm / r, and continuous foam injection flow rate of 150L with a foaming rate of 8%.
[0056] Finally, for any aspects of this invention not described herein, mature products and methods from existing technologies are employed.
[0057] It should be understood that those skilled in the art can make improvements or modifications based on the above description, and all such improvements and modifications should fall within the protection scope of the appended claims.
Claims
1. A method for reinforcing the cutterhead face of a tunnel boring machine with mud film, characterized in that, Includes the following steps: Step 1, Tunnel Boring Machine Shutdown Operation: After confirming that the filling chamber atmospheric pressure cutterhead replacement method is adopted, after the tunnel boring machine is shut down, based on the original soil chamber pressure of 1.7 bar, the articulated cylinder is retracted to make the shield body retreat 80mm, leaving a mud film grouting area and providing working space for cutterhead replacement. Step 2: Constructing a water-stop ring: To prevent water from flowing into the soil chamber behind the ring-shaped segments and causing filling failure, a water-stop ring needs to be formed by double-liquid grouting around the segments to cut off the water flow behind them. The grouting ring number is selected at the 5th to 10th ring position after the shield tail is removed. Water glass and cement grout are used for double-liquid grouting in a 1:1 ratio, with the cement grout having a water-cement ratio of 1:
1. Step 3, Shield body and cutterhead protection: (1) Inject the prepared mud film into the shield shell and the back of the 1-3 ring segments that have come off 80mm after the shield machine retreats through the radial holes at the shield tail, filling and wrapping the entire shield machine; (2) After injecting the mud film, open grouting holes in the radial direction at the shield tail, and inject polyurethane into the grouting holes with a high-temperature gear oil pump; (3) Inject grease into the cutterhead sealing system. Step 4, filling operation: Inject mud film into the circular area formed by the 1 to 3 ring segments that have been removed from the shield machine 80mm backward through the articulated advanced grouting holes, the radial grouting holes of the front shield, and the observation holes of the soil chamber from bottom to top. Step 5, Shield tunneling resumption: After the cutterhead is replaced, operate the cutterhead to rotate back and forth to free it from its obstruction, and inject foam agent into the soil chamber to resume tunneling; when resuming tunneling, use a small thrust that increases from zero to push the cutterhead, and tunnel at a low speed, controlling the penetration depth to 1~10mm / r. When the cutting edge of the cutter is worn out, resume normal tunneling. After step four is completed, a high-temperature gear oil pump is used to inject polyurethane into each hole of the radial grouting pipe of the front shield in the soil chamber wall, left center, right center, and chamber door, and the cutter head is rotated at a low speed of less than 0.5 r / min. At the same time, the surface settlement is strictly monitored to ensure that the injected polyurethane reacts fully with the excess water in the soil chamber. The pressure is controlled at 4-5 bar during the filling period. After the filling is completed, the soil pressure will decrease and stabilize at 1.8-2.0 bar. After the earth pressure drops to 1.8-2.0 bar, air is continuously added to the earth chamber through 6 foam agent pipes to increase the pressure until the earth pressure in the earth chamber stabilizes at 2.3-3.0 bar. Then, 400L of water is added to the earth chamber through 14 radial grouting holes until the earth pressure is constant. Finally, single-liquid grout and water glass are alternately injected into the earth chamber. The tunneling parameters of the tunnel boring machine are controlled as follows: thrust 1500T-2000T, torque 2000kN.m-2500kN.m, cutterhead speed 1.3r / min-1.5r / min, penetration 1mm / r-10mm / r, and foam needs to be continuously injected with a flow rate of 150L and a foaming rate of 8%.
2. The method for mud film reinforcement construction at the cutterhead replacement face of a shield tunneling machine according to claim 1, characterized in that: In step four, an average of 3m is injected. 3 25 kg of sodium carboxymethyl cellulose (CMC) needs to be added to the mud film to prevent segregation of the mud film slurry. When adding sodium carboxymethyl cellulose (CMC) to the mortar tank, it must be sprinkled in layer by layer and the slurry level must be controlled below the highest position of the mixing shaft to ensure uniform mixing.
3. The method for mud film reinforcement construction at the cutterhead replacement face of a shield tunneling machine according to claim 1, characterized in that: The mud film comprises the following components: 840-860 parts bentonite, 360-440 parts fine sand, 150-170 parts cement, and 492-508 parts water.
Citation Information
Patent Citations
Tunnel face breast wall filter cake construction process for shield compressed air operations
CN103696779A
High-performance bentonite for shield construction and preparation process of mud film of high-performance bentonite
CN110671119A