A diamond-based nitride semiconductor device and a method for fabricating the same
By depositing an aluminum nitride buffer layer on a diamond substrate using high-temperature radio frequency magnetron sputtering, the lattice mismatch and thermal management problems of GaN devices have been solved, improving the heat dissipation efficiency and power conversion efficiency of the devices and promoting their development in high-power applications.
Patent Information
- Application Number
- CN202210061589.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-05-18
- Filing Date
- 2022-01-19
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-01-19
AI Technical Summary
In the existing technology, silicon-based power transistors have reached their theoretical limit. GaN devices are not competitive at high operating voltages due to high cost and thermal management issues. Furthermore, the growth of gallium nitride on diamond substrates results in lattice mismatch and CTE mismatch, leading to cracks and poor heat dissipation.
Aluminum nitride buffer layer was formed on a diamond substrate using high-temperature radio frequency magnetron sputtering deposition. The deposition temperature and conditions were optimized to grow a nitride semiconductor stack structure, which reduced lattice mismatch and CTE mismatch and improved heat dissipation efficiency.
It improves the power conversion efficiency of gallium nitride-based power electronics, promoting the widespread application of GaN devices in high-power applications, especially in cooling effects in commercial base stations, military radar, and satellite communications.
Smart Images

Figure CN114420563B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor technology, and in particular to a diamond-based nitride semiconductor device and its fabrication method. Background Technology
[0002] Modern human society relies heavily on electricity as its energy source. With the continuous increase in total energy consumption and energy sources, efficient power conversion is crucial. With the development of silicon technology, the efficiency and cost of power management are steadily improving.
[0003] However, the pace of innovation in silicon-based power transistors has slowed significantly as their power conversion efficiency has reached its theoretical limit. GaN, as an emerging candidate in power and radio frequency (RF) electronics, possesses unparalleled advantages in wide bandgap, high electron mobility, and high-temperature stability, resulting in superior high-power processing capabilities. Although research and applications of gallium nitride-based power and RF transistors are still in their early stages, compared to silicon-based power management, gallium nitride-based devices can reduce energy conversion losses with a smaller area.
[0004] However, to date, power conversion based on silicon power transistors remains the dominant technology, while GaN-based power electronics are not competitive beyond limited applications due to high-cost substrates and thermal management issues at high operating voltages.
[0005] Currently commercially available GaN device substrate materials such as sapphire, Si, and SiC have low thermal conductivity (40–400 W·m). -1 ·K -1 Heat dissipation issues severely limit the performance of GaN devices. Meanwhile, in traditional gallium nitride epitaxial layer growth, to prevent wafer cracking and warping caused by large tensile stress in the epitaxial layer after cooling and to reduce through-dislocation density, buffer layers such as AlN, AlGaN, SiC, AlAs, ZnO, and Al2O3 are introduced between the sapphire or silicon substrate and the gallium nitride epitaxial layer to increase the success rate of gallium nitride epitaxial layer growth. However, these methods also suffer from poor heat dissipation.
[0006] To improve the thermal management capabilities of gallium nitride-based power devices, devices with higher thermal conductivity (800–2000 W·m) are used. -1 ·K -1 Using diamond materials as substrates has gradually become a research hotspot.
[0007] In recent years, significant progress has been made in diamond-based GaN HEMT devices, including substrate material growth, diamond-GaN device integration technology, and GaN epitaxy. The performance of diamond-based GaN power devices has been continuously improved. In 2013, DCDumka et al. reported an output power density of 7.9 W·mm² at 10 GHz and a 40 V bias voltage. -1 The power-added efficiency (PAE) exceeds 46%, and the power gain exceeds 11 dB. In 2015, PCChao et al. reported a maximum power density of 11 W·mm² at a 10 GHz operating frequency. -1 The corresponding PAE is 51%.
[0008] Therefore, diamond-based gallium nitride (GaN) devices are highly attractive for high-power applications such as commercial base stations, military radar, satellite communications, and weather radar. These high-power solutions all require the high thermal conductivity of diamond to achieve excellent cooling effects. However, directly growing GaN on diamond is challenging because the growth of Group III nitride semiconductors typically requires substrates with matching lattice and coefficient of thermal expansion (CTE).
[0009] Diamond grown by chemical vapor deposition is typically polycrystalline, making it difficult to grow single-crystal Group III nitride films on it. Gallium nitride (GaN) has a wurtzite crystal structure, while diamond has a cubic phase structure; therefore, a lattice mismatch exists between GaN and polycrystalline diamond, with a mismatch of approximately 11%. Even for single-crystal diamond, the biggest challenges in growing GaN remain lattice mismatch and CTE mismatch. GaN has a higher CTE than diamond, and CTE mismatch can induce significant tensile strain in the GaN epitaxial layer during cooling after growth, leading to cracks and hindering the fabrication of two-dimensional electroluminescent devices.
[0010] To obtain high-quality gallium nitride epitaxial layers, in addition to intermediate layer or buffer layer techniques, there is also lateral epitaxial growth (ELOG) technology. This method introduces SiO2 or Si3N4 mask layers with different shapes on the substrate to promote the lateral epitaxial growth of GaN material. However, with this method, buried cracks and voids may appear in the gallium nitride epitaxial layer.
[0011] To this end, a method for integrating diamond and gallium nitride was disclosed in application number 201911054671.5 on February 25, 2020. The method utilizes the hydrolysis of aluminum nitride to form an aluminum hydroxide bonding layer to bond the gallium nitride epitaxial layer to the diamond substrate. Compared with the conventional method of bonding gallium nitride to the diamond substrate using low thermal conductivity bonding materials, this method reduces the difficulty of the bonding process, reduces the risk of damage to the gallium nitride epitaxial layer, and improves the heat dissipation effect of diamond on gallium nitride semiconductor devices. Summary of the Invention
[0012] To address the issue mentioned in the background section regarding the low thermal conductivity of existing GaN device substrate materials such as sapphire, Si, and SiC, and the lattice mismatch problem between diamond and nitride semiconductors when using diamond as a substrate,
[0013] This invention provides a method for fabricating a diamond-based nitride semiconductor device, the method comprising:
[0014] Provide diamond substrates;
[0015] An aluminum nitride buffer layer is formed on the diamond substrate;
[0016] A nitride semiconductor stack-up structure is formed on the aluminum nitride buffer layer;
[0017] The aluminum nitride buffer layer is formed by high-temperature radio frequency magnetron sputtering deposition, and the deposition temperature used in the high-temperature radio frequency magnetron sputtering deposition method is above 800°C.
[0018] Furthermore, the deposition temperature is preferably above 800°C and below 1000°C.
[0019] Furthermore, the root mean square roughness of the surface of the diamond substrate used to form the aluminum nitride buffer layer is below 1 nm, and the diamond substrate is prepared using the following steps:
[0020] Provide silicon substrates;
[0021] A diamond film was deposited on the silicon substrate using microwave plasma-assisted chemical vapor deposition.
[0022] The diamond film is then planarized.
[0023] Furthermore, in the preparation method, before depositing the diamond film, the silicon substrate is placed in a diamond powder suspension for ultrasonic pretreatment.
[0024] Furthermore, the microwave output power used in the diamond film deposition process is above 3800W and below 4800W, the pressure used in the diamond film deposition process is above 140 Torr and below 160 Torr, the substrate temperature used in the diamond film deposition process is above 800℃ and below 900℃, the total gas flow rate used in the diamond film deposition process is 500 sccm, and the methane concentration used in the diamond film deposition process is above 3% and below 5%.
[0025] Furthermore, the target material for depositing the aluminum nitride buffer layer is an aluminum target, and the gas introduced during the deposition of the aluminum nitride buffer layer is N2 and Ar, wherein the percentage of N2 in the (N2+Ar) gas is 20% to 100%.
[0026] Furthermore, the deposition temperature is above 800°C and below 1000°C, the sputtering gas pressure used in the deposition process of the aluminum nitride buffer layer is above 3 mTorr and below 6 mTorr, and the radio frequency power used in the deposition process of the aluminum nitride buffer layer is above 100W and below 500W.
[0027] Furthermore, the nitride semiconductor stacked structure includes at least a first nitride semiconductor layer and a second nitride semiconductor layer with a composition different from that of the first nitride semiconductor layer;
[0028] A two-dimensional electron gas is generated at the heterojunction between the first nitride semiconductor layer and the second nitride semiconductor layer.
[0029] Furthermore, the first nitride semiconductor layer is a gallium nitride layer, and the second nitride semiconductor layer is an aluminum gallium nitride layer.
[0030] This invention provides a diamond-based nitride semiconductor device, comprising:
[0031] Diamond substrate;
[0032] An aluminum nitride buffer layer is located on the diamond substrate;
[0033] Nitride semiconductor stack-up structure located on the aluminum nitride buffer layer;
[0034] The aluminum nitride buffer layer is formed by high-temperature radio frequency magnetron sputtering deposition, and the deposition temperature used in the high-temperature radio frequency magnetron sputtering deposition method is above 800°C.
[0035] Furthermore, the deposition temperature is preferably above 800°C and below 1000°C.
[0036] Furthermore, the thermal conductivity of the diamond substrate is 2000 W·m. -1 ·K-1 The root mean square roughness of the surface of the diamond substrate used to form the aluminum nitride buffer layer is less than 1 nm, and the thickness of the diamond substrate is more than 50 μm and less than 500 μm.
[0037] Furthermore, the surface roughness of the aluminum nitride buffer layer is above 0.8 nm and below 2 nm, and the thickness of the aluminum nitride buffer layer is above 20 nm and below 2 μm.
[0038] The diamond-based nitride semiconductor device and its fabrication method provided by this invention have the following advantages compared with the prior art:
[0039] By depositing an aluminum nitride buffer layer on a diamond substrate using high-temperature radio frequency magnetron sputtering, a nitride semiconductor stack-up structure can be grown on a diamond substrate with an aluminum nitride buffer layer that can dissipate heat laterally, thereby greatly improving the power conversion efficiency of gallium nitride-based power electronics and accelerating the development of more applications for gallium nitride-based devices.
[0040] Other features and advantages of the invention will be set forth in the following description, and will be apparent in part from the description, or may be learned by practicing the invention. The objects and other advantages of the invention may be realized and obtained by means of the structures and methods particularly pointed out in the description, claims, and drawings. Attached Figure Description
[0041] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0042] Figure 1 A schematic diagram of the structure of a diamond-based nitride semiconductor device provided by the present invention;
[0043] Figure 2 A schematic diagram illustrating the steps of a method for fabricating a diamond-based nitride semiconductor device provided by the present invention;
[0044] Figure 3 The following is a schematic diagram of the diamond film grown by the MPACVD method provided by the present invention: (a) is a macroscopic photograph; (b) is an XRD diffraction pattern; (c) is a Raman spectrum; and (d) is a SEM surface morphology image.
[0045] Figure 4(a) is a SEM image of the diamond film grown by the MPACVD method; (b) is a SEM image of the surface morphology after etching with SF6 (30 sccm, 10 min, 500 W); (c) is a macroscopic photograph of the polished diamond; (d) is an atomic force microscope image of the polished diamond.
[0046] Figure 5(a) shows the ωXRD scan image of the aluminum nitride (002) peak of the sputtered aluminum nitride thin film at a deposition temperature of 1000℃;
[0047] Figure 5(b) shows an atomic force microscope image of an aluminum nitride thin film sputtered at a deposition temperature of 1000℃;
[0048] Figure 6(a) shows the ωXRD scan image of the aluminum nitride (002) peak of the sputtered aluminum nitride thin film at a deposition temperature of 900℃;
[0049] Figure 6(b) shows an atomic force microscope image of an aluminum nitride thin film sputtered at a deposition temperature of 900 °C;
[0050] Figure 7(a) shows the ωXRD scan image of the aluminum nitride (002) peak of the sputtered aluminum nitride thin film at a deposition temperature of 800℃;
[0051] Figure 7(b) shows an atomic force microscope image of an aluminum nitride thin film sputtered at a deposition temperature of 800 °C;
[0052] Figure 8 This is a schematic diagram of another diamond-based nitride semiconductor device provided by the present invention;
[0053] Figure 9 Flowchart for the fabrication of diamond-based gallium nitride heterostructures;
[0054] Figure 10 (a) is a schematic diagram of the GaN 2DEG on sapphire structure; (b) is the output characteristic diagram of AlGaN / GaN HEMTs obtained by applying the gate voltage in 8 steps from -4.0V to 3.0V, starting from the bottom curve; (c) is the transfer curve of HEMTs at a drain voltage of 5V.
[0055] Figure label:
[0056] 10 Diamond substrate 20 Aluminum nitride buffer layer 30 Nitride semiconductor stack
[0057] Structure
[0058] 31 First nitride semiconductor layer 32 Second nitride semiconductor layer Detailed Implementation
[0059] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0060] Diamond-based gallium nitride (GaN) devices are highly attractive for high-power applications, such as commercial base stations, military radar, satellite communications, and weather radar. These high-power solutions all require the use of diamond's high thermal conductivity to achieve excellent cooling performance.
[0061] However, growing gallium nitride directly on diamond is very challenging because the growth of group III nitride semiconductors usually requires a substrate with a matching lattice and coefficient of thermal expansion (CTE), and diamond grown by chemical vapor deposition is usually polycrystalline, so it is not easy to grow single-crystal group III nitride films on it.
[0062] For example, gallium nitride has a wurtzite crystal structure and diamond has a cubic phase structure. Therefore, there is a lattice mismatch of about 11% between gallium nitride and polycrystalline diamond. Even for single-crystal diamond, the biggest challenge in growing gallium nitride on it is still lattice mismatch and CTE mismatch.
[0063] Meanwhile, gallium nitride has a higher CTE than diamond, and CTE mismatch can cause large tensile strain in the gallium nitride epitaxial layer during cooling after growth, resulting in cracks and thus hindering the manufacture of semiconductor devices such as two-dimensional electroluminescent devices.
[0064] Therefore, the growth of gallium nitride on diamond substrate 10 requires a buffer layer structure, such as aluminum nitride. The existing growth method of buffer layer structure widely adopts the bonding of gallium nitride to diamond substrate 10 using low thermal conductivity bonding materials. However, this bonding process is difficult, and the growth of thick buffer layer is time-consuming and complex.
[0065] The various embodiments and comparative examples provided by the present invention will be discussed in detail below. However, it should be understood that many applicable concepts provided by the present invention can be implemented in a variety of specific environments, and the specific embodiments discussed are merely illustrative and do not limit the scope of the present invention.
[0066] Therefore, such as Figure 1 As shown, the present invention provides an embodiment of a diamond-based nitride semiconductor device, comprising:
[0067] Diamond substrate 10;
[0068] An aluminum nitride buffer layer 20 is located on the diamond substrate 10;
[0069] Nitride semiconductor stacked structure 30 formed on the aluminum nitride buffer layer 20;
[0070] The aluminum nitride buffer layer 20 is formed by high-temperature radio frequency magnetron sputtering deposition, and the deposition temperature used in the high-temperature radio frequency magnetron sputtering deposition method is above 800°C;
[0071] Preferably, the deposition temperature is above 800℃ and below 1000℃, such as 850℃, 900℃, 950℃, 1000℃, etc.
[0072] Due to the material parameter mismatch between gallium nitride and diamond, including lattice constant and CTE mismatch, it is difficult to achieve efficient heat dissipation when integrating the gallium nitride HEMT structure with the diamond substrate 10. In order to reduce lattice mismatch and CTE mismatch, an aluminum nitride buffer layer 20 is deposited on the diamond substrate 10 by a high-temperature radio frequency magnetron sputtering system, and then a nitride semiconductor stacked structure 30 is epitaxially grown on the aluminum nitride buffer layer 20. The deposition temperature of the aluminum nitride buffer layer 20 on the diamond substrate 10 is optimized to obtain a high-quality nitride semiconductor device.
[0073] like Figure 2 As shown, the present invention provides a method for fabricating the nitride semiconductor device disclosed in the above embodiments, comprising:
[0074] Step (1): Provide a diamond substrate 10, wherein a high-quality diamond film is deposited on a silicon substrate using microwave plasma-assisted chemical vapor deposition (MPACVD) technology, and the film is planarized.
[0075] In this embodiment, before depositing the diamond film, a 3 mm thick silicon substrate with a diameter of 2 inches is placed in a suspension of diamond powder with a diameter of 50 μm and subjected to ultrasonic bath pretreatment for 30 minutes to improve the nucleation density.
[0076] In other embodiments, the size of the substrate, i.e., the size of the diamond, can be replaced, and is not limited to a diamond film formed on a 2-inch silicon substrate.
[0077] After the silicon substrate pretreatment is completed, the silicon substrate is placed in acetone and deionized water for ultrasonic cleaning for 5 minutes, dried with N2 gas, and finally placed in a molybdenum stage to deposit a diamond film.
[0078] The parameters for growing diamond films using microwave plasma-assisted chemical vapor deposition (MPACVD) technology are as follows: polycrystalline diamond films are grown at a growth rate of approximately 8 μm / hour in a 2.45 GHz (6 kW) microwave plasma-assisted chemical vapor deposition system, with a microwave output power of 4400 W, a pressure of 150 Torr, a substrate temperature of 870 °C, a total gas flow rate of 500 sccm, and a high-purity methane concentration of 3%.
[0079] The morphology and crystallinity of the deposited diamond film were characterized using X-ray diffraction, Raman spectroscopy, and scanning electron microscopy.
[0080] See Figure 3 (a) shows a photograph of a 2-inch, 400-μm thick diamond film obtained on a 3-millimeter thick silicon substrate;
[0081] See Figure 3 (b) shows the XRD spectrum of the sample. The polycrystalline diamond phase is clearly shown by the reflection peaks (111), (220), (311), (400) and (311) shown in the XRD pattern. The strongest peak is at the (111) orientation.
[0082] See Figure 3 (c) shows the Raman spectrum of the diamond film grown by MPACVD. From the figure, it can be clearly seen that at 1333.48 cm⁻¹... -1 There is a sharp and intense diamond peak, no non-diamond peaks, and no obvious sp2 phase carbon impurities;
[0083] See Figure 3 (d) shows the surface morphology of the diamond film sample as measured by scanning electron microscopy (SEM).
[0084] The diamond film prepared using the above-mentioned microwave plasma-assisted chemical vapor deposition (MPACVD) technique has a thermal conductivity of 2000 W·m. -1 ·K -1 The diamond film has an average grain size of 20 μm and a thickness of 402–413 μm, with a thickness deviation within 5%.
[0085] In some other embodiments, the average grain size of the diamond film can be greater than 20 μm and less than 80 μm, and the thickness of the diamond film can be greater than 338 μm and less than 462 μm.
[0086] Furthermore, in order to reduce the surface roughness of the diamond film before epitaxy, the diamond film obtained after deposition is planarized to obtain a diamond substrate 10 with a smoother surface.
[0087] The planarization process can be selected from one or more of the following methods: grinding, mechanical polishing, and plasma etching.
[0088] In this embodiment, the surface smoothing treatment was performed under the following conditions: a pressure of 1250g was applied to the sample, using a water-based diamond slurry containing diamond abrasive grains with a grain size of 40μm, uniformly suspended in the slurry, and a grinding wheel rotation speed of 40r / min; after grinding, the sample was cleaned sequentially with acetone and ethanol in an ultrasonic bath; then, plasma reactive ion etching was applied to further smooth the diamond surface, using an SF6 gas-based etching process, with pressure, time, and plasma power maintained at 1.34Pa, 10min, and 500W, and the total gas flow rate kept constant at 30sccm. Finally, mechanical polishing was performed on a resin-bonded diamond wheel to obtain a smooth diamond surface. During the polishing process, the rotation speed was maintained at 1200r / min, the pressure at 1500g, and the cooling water flow rate maintained at 10ml / min.
[0089] In another preferred embodiment, to obtain an atomically smooth surface, the first step involves using diamond slurry to apply a 2-inch diamond film sample grown on silicon using the MPACVD method. Figure 4 (a) The diamond film sample is ground on an iron disc to prepare a flat diamond film surface. The grinding of the diamond film sample is carried out on a rotating iron disc with a diameter of about 300 mm. The diamond sample is attached to a metal pressure block, which is placed on an iron plate. A certain weight is applied to the sample to apply grinding pressure.
[0090] The parameters for grinding the diamond film sample in this embodiment are as follows: apply a pressure of 1250g to the diamond film sample, use water-based diamond slurry containing diamond abrasive particles, the abrasive particle size is 10μm and is uniformly suspended in the slurry, the grinding wheel speed is 40r / min, the grinding time is within 12h, and after grinding, the diamond film sample is cleaned with acetone and ethanol in an ultrasonic bath in sequence.
[0091] Then, plasma reactive ion etching is applied to further smooth the diamond surface. In this preferred embodiment, a two-step etching process based on SF6 and O2 is used to obtain a smooth diamond film surface. In the SF6-based method, the pressure, time, and plasma power are maintained at 1.34 Pa, 10 min, and 500 W, respectively, and the total gas flow rate is kept constant at 30 sccm. In the O2-based method, a 2.5-minute O2 step is performed first, followed by a 0.5-minute O2 / CF4 plasma step. The first step uses 50 sccm of O2 gas and a fixed plasma power of 800 W, with a pressure of 2 Pa. To improve the etching rate in the O2 plasma etching, a second gas, CF4, is introduced into the process. The second step uses 40 sccm of O2 and 10 sccm of CF4 at 1.6 Pa, with the plasma power becoming 200 W.
[0092] pass Figure 4 (b) The scanning electron microscope image of the chemical vapor deposition diamond surface after plasma etching clearly shows that the sample has no pits and grain boundaries. It can be seen that the smoothness of the diamond film surface after the planarization treatment is further improved, and no obvious etching pits and defects are observed on the entire surface, which further indicates that the grinding process did not damage the chemical vapor deposition diamond surface.
[0093] Finally, mechanical polishing was performed on a resin-bonded diamond wheel to obtain a smooth surface of the diamond substrate 10. Specifically, a resin wheel embedded with diamond abrasive grains was used. The experimental setup included a rotary table, pressure block, sample holder, cooling system, and dressing device. The polishing wheel was placed on the rotary table, and during the mechanical polishing process, the rotation speed was maintained at 1200 r / min, the pressure at 1500 g, and the flow rate of cooling water was maintained at 10 ml / min.
[0094] Figure 4 (c) is a photo of the 2-inch polycrystalline diamond after the mechanical polishing process. Figure 4 (d) shows an atomic force microscope image of a chemical vapor deposition diamond sample after mechanical polishing.
[0095] Roughness was evaluated over an area of 5 μm × 5 μm, with a surface roughness value of 0.278 nm for the polished surface. Electron energy dispersive spectroscopy (EDS) signals confirmed that there was no elemental contamination from the polishing pad on the surface of the chemical vapor deposition diamond sample.
[0096] The diamond substrate 10 obtained after the above planarization treatment has a root mean square roughness of less than 1 nm and a thickness of more than 280 μm and less than 350 μm.
[0097] In some other embodiments, the planarization process includes grinding and polishing, wherein the grinding process preferably removes more than 50 μm and less than 100 μm of the diamond film thickness, and the polishing process preferably removes more than 8 μm and less than 12 μm of the diamond film thickness.
[0098] In other embodiments, the type of abrasive grains, the material and size of the grinding disc, and the etching process can be adjusted according to the different diamond films.
[0099] In this embodiment of the invention, the thickness requirement of the diamond substrate 10 can be set according to different situations. After the diamond film growth is completed, the corresponding matching grinding parameters are selected so that growth and grinding play a complementary role, improving the overall process efficiency and ensuring the quality of the final product. In this way, the silicon substrate can be removed after the planarization process is completed.
[0100] Step (2): Aluminum nitride buffer layer 20 is deposited on the diamond substrate 10 after planarization by high-temperature radio frequency magnetron sputtering deposition, and the temperature of the high-temperature radio frequency magnetron sputtering deposition is 1000℃.
[0101] Due to the material parameter mismatch between gallium nitride and diamond, including lattice constant and CTE mismatch, it is difficult to achieve efficient heat dissipation when integrating the gallium nitride HEMT structure with the diamond substrate 10. In order to reduce lattice mismatch and CTE mismatch, an aluminum nitride buffer layer 20 is deposited on the diamond substrate 10 by a high-temperature radio frequency magnetron sputtering system, and then a nitride semiconductor stacked structure 30 is epitaxially grown on the aluminum nitride buffer layer 20.
[0102] In this embodiment, an aluminum nitride buffer layer 20 is deposited on the surface of the diamond substrate 10 at 1000°C. During deposition, an aluminum target is used. The gas introduced during the deposition of the aluminum nitride buffer layer 20 is N2 and Ar, with a gas volume ratio of 1:1 and a total gas volume of 20 sccm. The aluminum ions and nitrogen plasma form the aluminum nitride buffer layer 20 on the substrate at a working pressure of 5 mTorr. The temperature is set to 1000°C and the radio frequency power is 200 W.
[0103] XPS analysis showed high peak intensity, proving that the aluminum nitride buffer layer 20 was formed on the diamond substrate 10. XRD analysis of the aluminum nitride buffer layer 20 on the diamond substrate 10 by 2θ and ω measurements revealed sharp aluminum nitride peaks. After the 2θ scan, the ω scan of the XRD measurement was performed to obtain the full width at half maximum (FWHM) of the aluminum nitride peak, indicating that a highly oriented crystal structure was formed. According to the atomic force microscopy image, due to the in-situ high temperature conditions during the sputtering deposition process, a smooth aluminum nitride buffer layer 20 was obtained without annealing.
[0104] It can be seen that the aluminum nitride buffer layer 20 obtained by high-temperature radio frequency magnetron sputtering deposition at a deposition temperature of 800℃ or higher, preferably 800℃ or higher and 1000℃ or lower, improves the crystallinity of the aluminum nitride buffer layer 20, so that it can better grow gallium nitride layer.
[0105] The aluminum nitride buffer layer 20 prepared by the above-mentioned high-temperature radio frequency magnetron sputtering deposition technology has a surface roughness of 0.8 nm or more and 2 nm or less, and a thickness of 100 nm or more and 250 nm or less.
[0106] The full width at half maximum (FWHM) of the AlN(002) peak was obtained by XRD measurement of the ω scan. Please refer to [reference needed]. Figure 5(a) , 5(b) The test results shown are for depositing an aluminum nitride buffer layer on a diamond substrate at a deposition temperature of 1000℃, and the surface roughness of the obtained aluminum nitride buffer layer is 0.824 to 1.22 nm.
[0107] Please refer to the test results of the embodiments shown in Figures 6(a) and 6(b), which demonstrate the deposition of an aluminum nitride buffer layer at a deposition temperature of 900°C on a diamond substrate, and the surface roughness of the obtained aluminum nitride buffer layer is between 0.93 and 1.27 nm.
[0108] Please refer to the test results of the embodiments shown in Figures 7(a) and 7(b), which demonstrate the deposition of an aluminum nitride buffer layer at a deposition temperature of 800°C on a diamond substrate, and the surface roughness of the obtained aluminum nitride buffer layer is between 0.976 and 1.49 nm.
[0109] Step (3) A nitride semiconductor stack-up structure 30 is grown on the aluminum nitride buffer layer 20;
[0110] The nitride semiconductor stack-up structure 30 includes at least a first nitride semiconductor layer 31 and a second nitride semiconductor layer 32 with a composition different from that of the first nitride semiconductor layer 31;
[0111] A two-dimensional electron gas 33 is generated at the heterogeneous interface between the first nitride semiconductor layer 31 and the second nitride semiconductor layer 32.
[0112] In this embodiment, see Figure 8 The first nitride semiconductor layer 31 is a gallium nitride layer, and the second nitride semiconductor layer 32 is an aluminum gallium nitride layer. That is, the gallium nitride layer and the aluminum gallium nitride layer are grown sequentially on the aluminum nitride buffer layer 20 by metal-organic chemical vapor deposition, thereby forming an aluminum gallium nitride / gallium nitride heterostructure, and two-dimensional electron gas (2EDG) is generated at the interface by polarization charge.
[0113] See Figure 9 Optionally, the diamond-based nitride semiconductor device may further include the following subsequent implementation steps, such as etching of the epitaxial layer structure, fabrication of each electrode, or specific fabrication of source and drain electrodes, preparation of gate dielectric insertion layer, fabrication of gate electrode, etc., and the above preparation steps can be implemented using methods disclosed in the prior art.
[0114] For example, the etching of the epitaxial layer structure can be achieved by using semiconductor photolithography and / or etching techniques to create device mesa. Semiconductor etching techniques such as inductively coupled plasma (ICP) based on Cl-based gas or reactive ion etching (RIE) are used to etch the surface and achieve mesa isolation. This step is repeated to form grooves in the source and drain regions. The semiconductor photolithography technique includes complete steps such as spin coating, soft baking, exposure, development, and hardening.
[0115] The source and drain electrodes can be fabricated by defining the required areas for the source and drain electrodes using semiconductor photolithography in epitaxial layer etching, and then depositing the source and drain metals of the device using metal deposition techniques such as magnetron sputtering and electron beam evaporation. High-temperature annealing is then used to transform the composite metal structure into an alloy, forming ohmic contacts. Insulating layers can be deposited on the device surface using techniques such as plasma-enhanced chemical vapor deposition (PECVD), low-pressure chemical vapor deposition (LPCVD), magnetron sputtering, or electron beam evaporation.
[0116] It should be noted that the thickness of the diamond substrate 10 and the aluminum nitride buffer layer 20 can be adaptively adjusted according to different nitride semiconductor stack-up structures 30, and is not limited to the aluminum gallium nitride / gallium nitride heterostructure listed in this embodiment. In addition, the diamond-based nitride semiconductor device provided in this invention can be used not only for gallium nitride HEMTs, but also for UCV detectors, gallium nitride-based avalanche photodiodes (APDs), surface acoustic wave filters (SAWs), etc.
[0117] The specific parameters or some commonly used methods in the above embodiments are specific or preferred embodiments under the concept of the present invention, and are not intended to limit it; those skilled in the art can make adaptive adjustments within the concept and protection scope of the present invention.
[0118] See Figure 10As a pair, gallium nitride-based high electron mobility transistors (HEMTs) were fabricated on sapphire substrates and characterized. The 2DEG layer, which accumulates charge carriers in the gallium nitride-based HEMT, enhances the device's conductivity, thereby achieving high current density. Figure 7(a) shows the epitaxial cross-section of the gallium nitride-based HEMT on sapphire. Figure 7(b) shows the current-voltage characteristics of AlGaN / GaN HEMTs, i.e., the output characteristics of AlGaN / GaN HEMTs at different gate voltages, with the gate voltage applied sequentially in eight steps from -4.0V to 3.0V, starting from the bottom curve. Due to the self-heating effect caused by the lack of thermal management, the current in the saturation region decreases slightly at high gate voltages (1.0V-3.0V) and high drain voltages (>10V), as shown in Figure 7(c), which is the transfer curve of HEMTs at a drain voltage of 5V and a threshold voltage of -7V.
[0119] The present invention also provides the following comparative experiment. Compared with the embodiments, when the comparative experiment uses radio frequency magnetron sputtering deposition to deposit aluminum nitride buffer layer 20, if the deposition temperature is lower than 800°C, it will cause aluminum nitride to become amorphous, thus making it impossible to grow gallium nitride layer.
[0120] The comparative experiments described above show that the aluminum nitride buffer layer 20 prepared by the high-temperature radio frequency magnetron sputtering deposition method of the present invention can better improve the defects and dislocation density generated by the growth of the aluminum nitride buffer layer 20 on the diamond substrate 10, while making the deposited aluminum nitride buffer layer 20 have a smoother surface, and overcoming the problems of complex process and high cost caused by bonding method.
[0121] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for fabricating a diamond-based nitride semiconductor device, the method comprising: Provide diamond substrates; The diamond substrate is prepared by the following steps: providing a silicon substrate; A diamond film was deposited on the silicon substrate using microwave plasma-assisted chemical vapor deposition. The diamond film is subjected to a planarization process; An aluminum nitride buffer layer is formed on the diamond substrate; A nitride semiconductor stack-up structure is formed on the aluminum nitride buffer layer; The feature is that the aluminum nitride buffer layer is formed by high-temperature radio frequency magnetron sputtering deposition, and the deposition temperature used in the high-temperature radio frequency magnetron sputtering deposition method is above 800°C and below 1000°C; The sputtering gas pressure used in the deposition process of the aluminum nitride buffer layer is above 3 mTorr and below 6 mTorr, and the radio frequency power used in the deposition process of the aluminum nitride buffer layer is above 100 W and below 500 W. The surface roughness of the aluminum nitride buffer layer (20) is above 0.8 nm and below 2 nm, and the root mean square roughness of the surface of the diamond substrate (10) used to form the aluminum nitride buffer layer (20) is below 1 nm.
2. The method for fabricating a diamond-based nitride semiconductor device according to claim 1, characterized in that, The microwave output power used in the diamond film deposition process is above 3800 W and below 4800 W; the pressure used in the diamond film deposition process is above 140 Torr and below 160 Torr; the substrate temperature used in the diamond film deposition process is above 800 ℃ and below 900 ℃; the total gas flow rate used in the diamond film deposition process is 500 sccm; and the methane concentration used in the diamond film deposition process is above 3% and below 5%.
3. The method for fabricating a diamond-based nitride semiconductor device according to claim 1, characterized in that, The target material for depositing the aluminum nitride buffer layer is an aluminum target, and the gas introduced during the deposition of the aluminum nitride buffer layer is N2 and Ar, with N2 accounting for 20% to 100% of the (N2+Ar) gas.
4. The method for fabricating a diamond-based nitride semiconductor device according to claim 1, characterized in that: The nitride semiconductor stack-up structure includes at least a first nitride semiconductor layer and a second nitride semiconductor layer with a composition different from that of the first nitride semiconductor layer; A two-dimensional electron gas is generated at the heterojunction between the first nitride semiconductor layer and the second nitride semiconductor layer.
5. The method for fabricating a diamond-based nitride semiconductor device according to claim 4, characterized in that, The first nitride semiconductor layer is a gallium nitride layer, and the second nitride semiconductor layer is an aluminum gallium nitride layer.
6. A diamond-based nitride semiconductor device prepared by the method of any one of claims 1-5, comprising: Diamond substrate (10); An aluminum nitride buffer layer (20) is located on the diamond substrate (10). Nitride semiconductor stacked structure (30) located on the aluminum nitride buffer layer (20); The feature is that the aluminum nitride buffer layer (20) is formed by high-temperature radio frequency magnetron sputtering deposition, wherein the deposition temperature of the high-temperature radio frequency magnetron sputtering deposition method is above 800°C and below 1000°C.
7. The diamond-based nitride semiconductor device according to claim 6, characterized in that: The thermal conductivity of the diamond substrate (10) is 2000 W·m. -1 ·K -1 above.
8. The diamond-based nitride semiconductor device according to claim 6, characterized in that: The thickness of the aluminum nitride buffer layer (20) is greater than 20 nm and less than 2 μm.
Citation Information
Patent Citations
Method of integrating diamond and gallium nitride
CN110838438A
LED (light-emitting diode) radiating substrate based on diamond film and manufacturing method thereof
CN102130244A
PVD buffer layers for LED fabrication
CN104246980A