A method for dispersing oxide nanocrystals in a high-temperature superconducting precursor solution
By dispersing oxide nanocrystals in a high-temperature superconducting precursor solution, using hydrothermal reaction and multiple filtration treatments, the problem of difficulty in controlling the size and distribution of nanocrystals in YBCO films was solved, and the critical current density performance under high magnetic fields was improved. And extend the stable existence time of nanocrystals.
Patent Information
- Application Number
- CN202210285888.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-23
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-03-23
AI Technical Summary
In the existing technology, the size and distribution of non-superconducting nanocrystals in YBCO films are difficult to control, which affects its critical current density performance under high magnetic fields.
By dispersing oxide nanocrystals in a high-temperature superconducting precursor solution, using hydrothermal reaction and multiple filtration treatments, the size and distribution of the nanocrystals are controlled to achieve stable and uniform nanocrystal dispersion in the YBCO film.
The size and distribution of non-superconducting nanocrystals in the YBCO film are effectively controlled, the critical current density performance under high magnetic fields is improved, and the stable existence time of the nanocrystals in the solution is extended.
Smart Images

Figure CN114534528B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of superconducting materials, and in particular to a method for dispersing oxide nanocrystals in a high-temperature superconducting precursor solution. Background Art
[0002] With the development of high-temperature superconductors, there is a need to further develop useful conductors that require low manufacturing costs and critical current density in high magnetic fields; in particular, the use of YBa2Cu3O 7–δ The methanol solution of trifluoroacetate (YBCO) was used to prepare the c =2MAcm -2 –4MAcm -2 ) epitaxial layer can ensure lower manufacturing cost and higher critical current density in high magnetic field; however, during the use stage, with the increase of magnetic field, the critical current density of the epitaxial layer of this type of YBCO film will decrease rapidly. Generally, by artificially introducing non-superconducting defects of the size of flux eddy current cores, the decay rate of critical current density under magnetic field can be effectively reduced; generally, by introducing secondary nanophases in the YBCO matrix to provide non-superconducting defects, YBCO films with excellent performance under high magnetic field can be obtained, and the usual practice is to add metal organic salts of doping elements to the YBCO precursor solution to generate the desired nanosecond phase (for example, Y2O3, BaZrO3, BaHfO3, BaSnO3 and Ba2YTaO6) in the YBCO film.
[0003] Although the introduction of secondary nanophases into the YBCO matrix can prepare an effective nanocomposite superconducting layer, thereby ensuring a higher critical current density of the epitaxial layer in a high magnetic field, this method is extremely dependent on the spontaneous growth of the nanosecond phase, which easily leads to difficulty in controlling the growth of nanocrystals. Therefore, how to control the size and distribution of non-superconducting nanocrystals in YBCO films is a technical problem that urgently needs to be solved. Summary of the invention
[0004] The present application provides a method for dispersing oxide nanocrystals in a high-temperature superconducting precursor solution, so as to solve the technical problem in the prior art that the size and distribution of non-superconducting nanocrystals in YBCO thin films are difficult to control.
[0005] In a first aspect, the present application provides a method for dispersing oxide nanocrystals in a high-temperature superconducting precursor solution, the method comprising:
[0006] obtaining a metal salt and a surfactant;
[0007] The metal salt and the surfactant are dissolved, and then subjected to a hydrothermal reaction and heat preservation at a preset temperature to obtain a mixed slurry;
[0008] Desalting the mixed slurry in a first cross-flow filtration manner to obtain a slurry;
[0009] Adding polycarboxylic acid to the slurry for dilution, and then performing a second cross-flow filtration to obtain an organic phase nanocrystalline dispersion;
[0010] Obtaining a YBCO precursor solution;
[0011] The nanocrystal dispersion is dispersed in the YBCO precursor solution to obtain a high-temperature superconducting precursor solution containing oxide nanocrystals with stable size and uniform distribution.
[0012] Optionally, the molar ratio of the metal salt to the surfactant is 55:1 to 223:1.
[0013] Optionally, the surfactant includes hexadecyltrimethylammonium bromide and / or hexadecyltrimethylammonium chloride;
[0014] The metal salt includes at least one of zirconium oxychloride, hafnium chloride and hafnium oxychloride.
[0015] Optionally, the preset temperature is ≥180°C.
[0016] Optionally, the adding of polycarboxylic acid to the slurry for dilution, followed by a second cross-flow filtration to obtain a nanocrystalline dispersion, specifically comprises:
[0017] Adding polycarboxylic acid to the slurry for dilution, and then performing a second cross-flow filtration to obtain a dehydrated filtrate;
[0018] The dehydrated filtrate is exchanged with an organic solvent to obtain an organic phase nanocrystal dispersion.
[0019] Optionally, the polycarboxylic acid includes citric acid or gluconic acid, and both the citric acid and the gluconic acid contain two or more carboxyl groups in one molecule.
[0020] Optionally, the organic solvent includes methanol or ethanol.
[0021] Optionally, the molar concentration of the YBCO precursor solution is >2 mol / L.
[0022] Optionally, the particle size of the oxide nanocrystals is less than 10 nm.
[0023] Optionally, the storage stability of the high-temperature superconducting precursor solution is greater than 6 months.
[0024] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:
[0025] The embodiment of the present application provides a method for dispersing oxide nanocrystals in a high-temperature superconducting precursor solution. The method comprises the following steps: firstly subjecting a metal salt and a surfactant to a hydrothermal reaction, and then subjecting the metal salt and a surfactant to a first cross-flow filtration desalination treatment, thereby obtaining an aqueous nanocrystal dispersion liquid. Then, by adding a polycarboxylic acid to the aqueous nanocrystal dispersion liquid, and then subjecting the aqueous nanocrystal dispersion liquid to a second cross-flow filtration, the aqueous nanocrystal dispersion liquid is converted into an organic nanocrystal dispersion liquid. Finally, the organic nanocrystal dispersion liquid is dispersed into a YBCO solution. Thus, by utilizing the principle of in-situ reaction, the size of the artificial pinning center of the conductor can be effectively controlled, thereby controlling the size of non-superconducting nanocrystals in the YBCO film. Finally, by means of two cross-flow filtrations, the nanocrystal solution can be effectively dispersed into a YBCO precursor solution with a high ion concentration and acidity, thereby achieving control over the size and distribution of non-superconducting nanocrystals in the YBCO film. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.
[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0028] Figure 1 A schematic diagram of a process for a method provided in an embodiment of the present application;
[0029] Figure 2 Detailed flow chart of the method provided in the embodiment of the present application
[0030] Figure 3 This is a schematic diagram of XRD of oxide nanocrystals in a high-temperature superconducting precursor solution provided in an embodiment of the present application;
[0031] Figure 4 A schematic diagram of TEM results of oxide nanocrystals in a high-temperature superconducting precursor solution provided in an embodiment of the present application;
[0032] Figure 5 A schematic diagram of the particle size distribution of oxide nanocrystals in a high-temperature superconducting precursor solution provided in an embodiment of the present application;
[0033] Figure 6 A schematic diagram showing the results of stable dispersion of oxide nanocrystals of different concentrations in a high-temperature superconducting precursor solution for 120 days provided in an embodiment of the present application;
[0034] Figure 7This is a schematic diagram of TEM results of oxide nanocrystals stably dispersed in a high-temperature superconducting precursor solution provided in an embodiment of the present application after 120 days. DETAILED DESCRIPTION
[0035] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0036] The creative thinking of this application is: when the YBCO superconducting film is used under an external magnetic field, it usually enters a mixed state where the superconducting state and the normal state coexist, and a magnetic flux eddy current center is generated inside. These magnetic flux eddy currents will move under the action of the Lorentz force, causing energy loss and leading to a decrease in the critical current density. Therefore, generally, by artificially introducing non-superconducting defects the size of the magnetic flux eddy current core, the decay rate of the critical current density under a magnetic field can be effectively reduced.
[0037] As for how to control the size and distribution of non-superconducting nanocrystals in YBCO films, it can be done by adding prefabricated nanocrystals (ZrO2, HfO2, etc.) to the YBCO precursor solution, and then generating BaZrO3, BaHfO3, etc. through in-situ reaction, which can serve as effective flux pinning centers. This method can better control the size of the artificial pinning center, and in this method, monodisperse nanocrystals with different sizes and shapes can be prepared by adjusting the synthesis conditions; and achieving monodispersity of nanocrystals in the YBCO precursor solution with high ion concentration and acidity is the key to introducing artificial pinning centers, because only by achieving monodispersity of nanocrystals in the YBCO precursor solution can the size and particle distribution of the doped phase be effectively controlled in the subsequent process links such as solution coating and sintering film formation.
[0038] In one embodiment of the present application, Figure 1 As shown, a method for dispersing oxide nanocrystals in a high-temperature superconducting precursor solution comprises:
[0039] S1. Obtaining a metal salt and a surfactant;
[0040] S2. dissolving the metal salt and the surfactant, and then performing a hydrothermal reaction and heat preservation at a preset temperature to obtain a mixed slurry;
[0041] S3. Desalting the mixed slurry by a first cross-flow filtration method to obtain a slurry;
[0042] S4. Adding a polycarboxylic acid to the slurry for dilution, and then performing a second cross-flow filtration to obtain an organic phase nanocrystalline dispersion;
[0043] S5. Obtaining a YBCO precursor solution;
[0044] S6. Dispersing the nanocrystal dispersion into the YBCO precursor solution to obtain a high-temperature superconducting precursor solution containing oxide nanocrystals of stable size and uniform distribution.
[0045] In some optional embodiments, the molar ratio of the metal salt to the surfactant is 55:1 to 223:1.
[0046] In the present application, the positive effect of the molar ratio of metal salt to surfactant being 55:1 to 223:1 is that within the range of the molar ratio, the metal salt can be uniformly distributed in the solution after being modified by the surfactant, thereby ensuring the stability of the dispersion performance of the metal salt; when the molar ratio is greater than or less than the endpoint value of the range, the adverse effect will be that the content of the metal salt is insufficient or too high, which will lead to waste of raw materials, or the distribution of the metal salt in the solution is uneven, affecting the distribution of the oxide nanocrystals in the later stage.
[0047] In some optional embodiments, the surfactant includes hexadecyltrimethylammonium bromide and / or hexadecyltrimethylammonium chloride;
[0048] The metal salt includes at least one of zirconium oxychloride, hafnium chloride and hafnium oxychloride.
[0049] In the present application, the positive effect of limiting the surfactant to a quaternary ammonium salt is that the ionic properties of the quaternary ammonium salt can be utilized to effectively make the metal salt evenly distributed while ensuring that the particle size of the oxide nanocrystals meets the specifications.
[0050] In some optional embodiments, the preset temperature is ≥ 180°C.
[0051] In the present application, the positive effect of the preset temperature ≥180°C is that within this temperature range, it can effectively promote the effective progress of the hydrothermal reaction, and at the same time ensure that the metal salt can form preliminary crystals in the aqueous solution; when the temperature value is less than the endpoint value of this range, the adverse effect will be that the too low temperature will cause the metal salt to be unable to initially form crystals in the aqueous solution, affecting the subsequent distribution of oxide nanocrystals.
[0052] In some optional embodiments, such as Figure 2 As shown, the polycarboxylic acid is added to the slurry for dilution, and then a second cross-flow filtration is performed to obtain a nanocrystalline dispersion, which specifically includes:
[0053] S41. Adding a polycarboxylic acid to the slurry for dilution, and then performing a second cross-flow filtration to obtain a dehydrated filtrate;
[0054] S42. Exchanging the dehydrated filtrate with an organic solvent to obtain an organic phase nanocrystal dispersion.
[0055] In the present application, by first diluting with a polycarboxylic acid and then performing a second cross-flow filtration, not only can the excess polycarboxylic acid and water be removed, but the characteristics of the cross-flow filtration can also be utilized to disperse the formed oxide nanocrystals into fine particles, and the organic solvent can completely exchange out the oxide nanocrystals to obtain an organic phase nanocrystal dispersion.
[0056] In some optional embodiments, the polycarboxylic acid includes citric acid or gluconic acid, and both the citric acid and the gluconic acid include two or more carboxyl groups in one molecule.
[0057] In the present application, by limiting the types of polycarboxylic acids and limiting the number of carboxyl groups thereof, it is possible to ensure that the initially formed nanocrystals are modified and oxidized, thereby ensuring that oxide nanocrystals are obtained.
[0058] In some optional embodiments, the organic solvent includes methanol or ethanol.
[0059] In the present application, by limiting the organic solvent to common methanol or ethanol, the practicability of the method can be improved, which is conducive to the industrial preparation of oxide nanocrystals and dispersion thereof in the YBCO precursor solution.
[0060] In some optional embodiments, the molar concentration of the YBCO precursor solution is >2 mol / L.
[0061] In the present application, the positive effect of the molar concentration of the YBCO precursor solution being greater than 2 mol / L is that within this molar concentration range, it indicates that the YBCO precursor solution is at a high particle concentration, thereby facilitating the distribution of the oxide nanocrystals after acidification therein.
[0062] In some optional embodiments, the particle size of the oxide nanocrystals is less than 10 nm.
[0063] In some optional embodiments, the storage stability of the high temperature superconducting precursor solution is greater than 6 months.
[0064] Example 1
[0065] like Figure 2 As shown, a method for dispersing oxide nanocrystals in a high-temperature superconducting precursor solution comprises:
[0066] S1. Obtaining a metal salt and a surfactant;
[0067] S2. dissolving the metal salt and the surfactant, and then performing a hydrothermal reaction and heat preservation at a preset temperature to obtain a mixed slurry;
[0068] S3. Desalting the mixed slurry by a first cross-flow filtration method to obtain a slurry;
[0069] S41. Adding polycarboxylic acid to the slurry for dilution, and then performing a second cross-flow filtration to obtain a dehydrated filtrate;
[0070] S42. exchanging the dehydrated filtrate with an organic solvent to obtain an organic phase nanocrystal dispersion;
[0071] S5. Obtaining a YBCO precursor solution;
[0072] S6. Dispersing the nanocrystal dispersion into the YBCO precursor solution to obtain a high-temperature superconducting precursor solution containing oxide nanocrystals of stable size and uniform distribution, wherein the mass ratio of the polycarboxylic acid to the metal salt is 1:10, and n(zirconium):n(yttrium) in the high-temperature superconducting precursor solution is 8.48%.
[0073] The molar ratio of metal salt to surfactant is 223:1.
[0074] The surfactant was hexadecyltrimethylammonium bromide;
[0075] The metal salt is ZrOCl2·8H2O.
[0076] The preset temperature is 180℃
[0077] The polycarboxylic acid is gluconic acid, and gluconic acid contains two or more carboxyl groups in one molecule.
[0078] The organic solvent is methanol.
[0079] The molar concentration of the YBCO precursor solution is >2 mol / L.
[0080] Example 2
[0081] Comparing Example 2 with Example 1, the difference between Example 2 and Example 1 is:
[0082] n(zirconium):n(yttrium)=8.52% in the high-temperature superconducting precursor solution;
[0083] The molar ratio of metal salt to surfactant is 112:1.
[0084] The organic solvent is methanol.
[0085] Example 3
[0086] Comparing Example 3 with Example 1, the difference between Example 3 and Example 1 is:
[0087] The molar ratio of metal salt to surfactant is 75:1.
[0088] The surfactant is hexadecyltrimethylammonium bromide;
[0089] The metal salt is ZrOCl2·8H2O.
[0090] Example 4
[0091] Comparing Example 4 with Example 1, the difference between Example 4 and Example 1 is:
[0092] The molar ratio of metal salt to surfactant was 55:1.
[0093] Example 5
[0094] Comparing Example 5 with Example 1, the difference between Example 5 and Example 1 is:
[0095] The molar ratio of metal salt to surfactant is 223:1.
[0096] The metal salt is HfOCl2·8H2O.
[0097] Example 6
[0098] Comparing Example 6 with Example 1, the difference between Example 6 and Example 1 is:
[0099] The molar ratio of metal salt to surfactant is 223:1.
[0100] The metal salt is HfCl4.
[0101] Related experiments:
[0102] The high temperature superconducting precursor solutions obtained in Examples 1-6 were respectively subjected to performance tests, and the test results are shown in Table 1.
[0103] Test methods for related experiments:
[0104] Particle size of oxide nanocrystals: The oxide nanocrystals in the high-temperature superconducting precursor solution are sampled using a transmission electron microscope, and then observed and tested to obtain the particle size data of the oxide nanocrystals.
[0105] Storage stability of high-temperature superconducting precursor solution: The obtained high-temperature superconducting precursor solution is stored at room temperature, and the time during which the oxide nanocrystals are stably stored is counted.
[0106] Table 1
[0107] Group Particle size of oxide nanocrystals (nm) Storage stability of high-temperature superconducting precursor solutions (d) Example 1 1~10 ≥120 Example 2 3~8 ≥180 Example 3 5~9 ≥180 Example 4 6~10 ≥150 Example 5 6~10 ≥30 Example 6 7~9 ≥30
[0108] Detailed analysis of Table 1:
[0109] The particle size of oxide nanocrystals refers to the particle size of oxide nanocrystals dispersed in the YBCO precursor solution. The particle size of oxide nanocrystals is affected by the ratio of metal salt to surfactant. The narrower the particle size range of oxide nanocrystals, the more uniform the distribution of oxide nanocrystals.
[0110] The storage stability of the high-temperature superconducting precursor solution refers to the length of time that the oxide nanocrystals can stably exist in the YBCO precursor solution. The greater the storage stability of the high-temperature superconducting precursor solution, the more uniform the distribution of the oxide nanocrystals in the YBCO precursor solution.
[0111] From the data of Examples 1-6, it can be seen that:
[0112] According to the method of the present application, a metal salt is treated with a surfactant, and then a first cross-flow filtration desalination treatment is performed to obtain an aqueous nanocrystalline dispersion. Then, a polycarboxylic acid is added to the aqueous nanocrystalline dispersion, and then a second cross-flow filtration is performed to convert the aqueous nanocrystalline dispersion into an organic nanocrystalline dispersion. Finally, the organic nanocrystalline dispersion is dispersed in a YBCO solution, so that the size and distribution of the oxide nanocrystals can be controlled.
[0113] One or more technical solutions in the embodiments of the present application also have at least the following technical effects or advantages:
[0114] (1) The method provided in the embodiment of the present application treats the metal salt with a surfactant, first through a hydrothermal reaction and then through two cross-flow filtrations, thereby achieving the replacement of the aqueous phase and the organic phase of the oxide nanocrystals, and can effectively disperse the nanocrystal solution into the YBCO precursor solution with high ion concentration and acidity, thereby achieving the control of the size and distribution of the non-superconducting nanocrystals in the YBCO film.
[0115] (2) The method provided in the embodiment of the present application preforms nanocrystals through in-situ reaction, thereby ensuring that the nanocrystals are stably dispersed in the YBCO superconducting precursor, solving the problem of monodispersity of oxide nanocrystals in the YBCO precursor solution, and further solving the problem of size control and particle distribution of nano-heterogeneous phases in the YBCO film, so that the nanocrystals form effective flux pinning centers.
[0116] (3) The method provided in the embodiment of the present application can prepare oxide nanocrystals with a size less than 10 nm, and the prepared oxide nanocrystals can be monodispersed in a high concentration YBCO precursor solution with a stability time of more than 120 days.
[0117] Explanation of the attached figure:
[0118] Figure 3 This is a schematic diagram of XRD of oxide nanocrystals in a high-temperature superconducting precursor solution provided in Example 1 of the present application;
[0119] Figure 4 A schematic diagram of TEM results of oxide nanocrystals in a high-temperature superconducting precursor solution provided in Example 1 of the present application;
[0120] Figure 5 A schematic diagram of the particle size distribution of oxide nanocrystals in the high-temperature superconducting precursor solution provided in Example 1 of the present application;
[0121] Depend on Figures 3 to 5 It can be seen that the particle sizes of the oxide nanocrystals obtained in the examples of the present application are all below 10 nm.
[0122] Figure 6 A schematic diagram showing the results of stable dispersion of oxide nanocrystals of different concentrations in a high-temperature superconducting precursor solution for 120 days provided in an embodiment of the present application;
[0123] Depend on Figure 6 It can be seen that organic oxide nanocrystals with different concentrations dispersed in YBCO solution can exist stably for 120 days.
[0124] Figure 7 A schematic diagram of TEM results of oxide nanocrystals stably dispersed in a high-temperature superconducting precursor solution provided in Example 1 of the present application for 120 days;
[0125] Depend on Figure 7 It can be seen that after 120 days of dispersion, the oxide nanocrystals can still exist stably in the YBCO precursor solution.
[0126] It should be noted that, in this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.
[0127] The foregoing is merely a specific embodiment of the present invention, which enables those skilled in the art to understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features claimed herein.
Claims
1. A method for dispersing oxide nanocrystals in a high-temperature superconducting precursor solution, It is characterized in that The method comprises: Obtaining a metal salt and a surfactant, wherein the molar ratio of the metal salt to the surfactant is 55:1 to 223:1; The metal salt and the surfactant are dissolved, and then subjected to a hydrothermal reaction and heat preservation at a preset temperature to obtain a mixed slurry, wherein the preset temperature is ≥180° C.; Desalting the mixed slurry in a first cross-flow filtration manner to obtain a slurry; Adding polycarboxylic acid to the slurry for dilution, and then performing a second cross-flow filtration to obtain a dehydrated filtrate; exchanging the dehydrated filtrate with an organic solvent to obtain an organic phase nanocrystal dispersion; Obtaining a YBCO precursor solution, wherein the molar concentration of the YBCO precursor solution is greater than 2 mol / L; The nanocrystal dispersion is dispersed in the YBCO precursor solution to obtain a high-temperature superconducting precursor solution containing oxide nanocrystals of stable size and uniform distribution. The polycarboxylic acid includes citric acid or gluconic acid. Both the citric acid and the gluconic acid contain more than two carboxyl groups in one molecule. The particle size of the oxide nanocrystals is less than 10 nm. The storage stability of the high-temperature superconducting precursor solution is greater than 6 months.
2. The method according to claim 1, It is characterized in that The surfactant includes hexadecyltrimethylammonium bromide and / or hexadecyltrimethylammonium chloride; The metal salt includes at least one of zirconium oxychloride, hafnium chloride and hafnium oxychloride.
3. The method according to claim 1, It is characterized in that The organic solvent includes methanol or ethanol.
Citation Information
Patent Citations
Second-phase nanoparticle doped YBCO (yttrium barium copper oxide) film and preparation method thereof