Synthesis method of polyether polyols coated with polyurethane for preparing slow-release fertilizers at room temperature

By polymerizing polyols and epoxy compounds at room temperature under the action of a catalyst, and designing the content and polymerization method of the polymerized monomers propylene oxide and ethylene oxide, the high-temperature problem of thermoplastic and thermosetting resin coating materials is solved, and the product is made Low-cost, degradable slow-release fertilizer coating material achieves stable fertilizer release and high-performance coating properties.

CN114539517BActive Publication Date: 2024-10-01SHANDONG BLUSR DONGDA CHEM
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011328166.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-11-24
Publication Date
2024-10-01
Estimated Expiration
2040-11-24

Smart Images

  • Figure HDA0002794980820000011
    Figure HDA0002794980820000011
Patent Text Reader

Abstract

The present invention belongs to the technical field of polyether polyol synthesis, and specifically relates to a method for synthesizing polyether polyol for preparing polyurethane coating of slow-release fertilizer at room temperature. The synthesis method is prepared by using polyol compounds as initiators, catalyzed by catalysts, and polymerizing with epoxy compounds; wherein the polyol compounds are one or more of glycerol, propylene glycol, diethylene glycol, ethylene glycol, pentaerythritol, castor oil, palm oil, corn oil, rapeseed oil, soybean oil or sunflower oil; the epoxy compound is a mixture of ethylene oxide and propylene oxide, and the mass of ethylene oxide accounts for more than 20% of the total mass of the epoxy compound. The polyether polyol can be applied to slow-release fertilizer coating, and has the characteristics of low cost, room temperature coating, degradability, environmental friendliness, etc., and it has a good slow-release effect when used as a slow-release fertilizer coating material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polyether polyol synthesis, and particularly relates to a method for preparing a polyether polyol for preparing a polyurethane-coated slow-release fertilizer at room temperature. Background Art

[0002] How to improve the utilization rate of fertilizers and extend the effective period of fertilizers has become a research hotspot in the fertilizer field. Slow-release fertilizers are an effective means to improve utilization. Controlled-release fertilizer coating materials are divided into two categories: one is thermoplastic resin, which is mainly polyolefins, including polyethylene, polypropylene, polystyrene, etc. The coating process of these materials must be solvent-based, and the solvents are generally tetrachloroethylene, rosin, etc. In addition to the high coating cost, environmental pollution, production speed, and poor degradation of solvent-based technology, there is also a very fatal defect that the release of fertilizers is very unstable. The main feature is that the initial release is very fast (mainly caused by surface defects), and the later release is very slow, resulting in a curve that is fast at first and then slow, which is exactly the opposite of the S curve that plants like. One is thermosetting resin. Most thermosetting resin coatings are solvent-free. Compared with thermoplastics, they have the advantages of low production cost and environmental protection. Thermosetting resins mainly include polyurethane resin, epoxy resin, alkyd resin, unsaturated polyester resin, phenolic resin, acrylic resin, urea resin, melamine resin, silicone resin, etc. Among them, alkyd resin, polyurethane and epoxy resin are the most common coating materials.

[0003] The processing technology of polyurethane coating is mostly at 60-80℃. Higher coating temperature will definitely increase equipment investment cost and energy consumption cost. Higher coating temperature will also accelerate the solvent rate and membrane penetration rate of fertilizer, shortening the effective time of the prepared slow-release fertilizer. Existing polyether polyols have problems such as reaction activity. If they are directly used for coating at low temperature, the surface of the coating will become sticky due to insufficient reaction maturation, and significant adhesion will occur between the coatings. Summary of the invention

[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a method for synthesizing polyether polyols coated with polyurethane for preparing slow-release fertilizers at room temperature. The polyether has the characteristics of low cost, room temperature coating, biodegradability, and environmental friendliness. Using it as a slow-release fertilizer coating material has a good slow-release effect.

[0005] The method for synthesizing polyether polyol coated with polyurethane for preparing slow-release fertilizer at room temperature of the present invention is to use polyol compound as initiator, catalyze by catalyst, and polymerize with epoxy compound to obtain the polyether polyol;

[0006] Wherein, the polyol compound is one or more of glycerol, propylene glycol, diethylene glycol, ethylene glycol, pentaerythritol, castor oil, palm oil, corn oil, rapeseed oil, soybean oil or sunflower oil; the epoxy compound is a mixture of ethylene oxide and propylene oxide, and the mass of ethylene oxide accounts for more than 20% of the total mass of the epoxy compound.

[0007] Preferably, the polyol compound is castor oil.

[0008] The catalyst is one of an alkali metal catalyst or a bimetallic catalyst, wherein the alkali metal catalyst is one of potassium hydroxide, sodium hydroxide, potassium methoxide or sodium methoxide.

[0009] The polyether polyol has a functionality of 2-4 and a number average molecular weight of 400-5000 g / mol.

[0010] The polymerization reaction is carried out in one of the following ways:

[0011] Method (1), the initiator is mixed with a mixture of propylene oxide and ethylene oxide;

[0012] Method (2), the initiator is first co-polymerized with a mixture of propylene oxide and ethylene oxide, and then capped with ethylene oxide;

[0013] Method (3), the initiator is first polymerized with propylene oxide and then capped with ethylene oxide;

[0014] Method (4) is that the initiator is first polymerized with ethylene oxide, then polymerized with propylene oxide, and finally capped with ethylene oxide.

[0015] The polymerization reaction has a reaction temperature of 90-130° C. and a reaction pressure of 0.1-0.4 MPa.

[0016] After the polymerization reaction, post-treatment is performed, and the post-treatment is performed using water, acid and an auxiliary agent. The acid is one or more of phosphoric acid, sulfuric acid, hydrochloric acid, oxalic acid, lactic acid or acetic acid; and the auxiliary agent is one or more of aluminum silicate, magnesium silicate or magnesium aluminum silicate.

[0017] Compared with the prior art, the present invention has the following beneficial effects:

[0018] 1. The present invention accelerates the coating maturation rate by designing the content and polymerization mode of the polymerization monomers propylene oxide and ethylene oxide in the polyether polyol, controls the heating temperature at room temperature, relaxes the processing environment of the slow-release fertilizer, and reduces equipment investment and energy consumption.

[0019] 2. The higher content of ethylene oxide and its distribution effectively solve the defect of uneven mixing of isocyanate component and polyether polyol component on the fertilizer particles.

[0020] 3. The polyether polyol produced by the present invention can meet the requirements of high-performance polyurethane materials and is used as a coating material for slow-release fertilizers. It has the characteristics of foamability, high elasticity, wear resistance, solvent resistance, and excellent electrical insulation. The combination of soft segments and hard segments and the existence of physical and chemical crosslinking in its structure determine that it has a good slow-release effect as a coating material for slow-release fertilizers. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The figures are the envelopes prepared by the polyethers of the examples and comparative examples, wherein, on the left: the example of the example, the particles are intact; on the right: the comparative example, the surface is sticky, and the particles are adhered to each other. DETAILED DESCRIPTION

[0022] The present invention is further described below with reference to the embodiments.

[0023] Example 1

[0024] In a 5L stainless steel reactor, add 630g castor oil, 0.041g bimetallic catalyst and 19ppm sulfuric acid. Nitrogen replacement until the oxygen content in the reactor is less than 80ppm. Heat to 130-135℃ and decompress and dehydrate, and the H2O content is not higher than 0.05%. 362.96g of propylene oxide and ethylene oxide are mixed and fed, and pre-dripped after heating to 140℃. After the reaction is initiated, the reaction temperature is controlled at 135±2℃, and the feed flow rate is 700g / h. After the feeding is completed, the internal pressure reaction is carried out for 0.5 hours, and the temperature is controlled at 130±2℃, the pressure is 0.05-0.1MPa, and the temperature is lowered to 90℃. Antioxidant 1076 is added, and samples are taken to detect physical and chemical indicators, and it is named polyether polyol A. The analytical indicators are as follows: hydroxyl value: 75.73 mgKOH / g; acid value: 0.03 mgKOH / g; unsaturation value: 0.02 mol / kg; moisture: 0.01%; pH value: 6.95. The functionality of the polyether polyol is 2.7 and the molecular weight is 2000 g / mol.

[0025] Example 2

[0026] 400g of castor oil and 9.06g of solid KOH were added to a 5L stainless steel reactor. After nitrogen replacement, the oxygen content in the reactor was measured to be less than 80ppm, the temperature was raised to 120-125℃ for decompression and dehydration, and the time was 1 hour. The H2O content was not higher than 0.05%. 1722.01g of propylene oxide was added, and the reaction temperature was controlled to be 125±2℃, the flow rate was 300g / hour, and the pressure was not higher than 0.4MPa. After the feeding was completed, the internal pressure reaction was carried out for 1 hour, and the monomer removal was carried out for 0.5 hour. Nitrogen pressurization was carried out, and the nitrogen was charged to 0.18MPa. The temperature was controlled at 115℃, and 430.50g of ethylene oxide was added, and the feed flow rate was 250g / h. After the addition, the internal pressure reaction was carried out for 2 hours, and the monomer removal was carried out. The temperature was lowered to 80℃, and pure water, phosphoric acid, and an auxiliary agent (aluminum silicate) were added. The reaction was vacuum dried, filtered and circulated, and the sampling and detection indicators were taken. The polyether polyol B was named. The analytical indicators are as follows: hydroxyl value: 30.29 mgKOH / g; acid value: 0.036 mgKOH / g; unsaturation value: 0.07 mol / kg; moisture: 0.02%; pH value: 6.44, potassium ion: 0 ppm. The functionality of the polyether polyol is 2.7 and the molecular weight is 5000 g / mol.

[0027] Example 3

[0028] To a 5L stainless steel reactor, 223.24g of glycerol and 100g of pentaerythritol were added, and 10.5g of potassium methoxide was vacuum-drawn for nitrogen replacement. After the oxygen content in the reactor was measured to be less than 80ppm, the temperature was increased and the reduced pressure was reduced for dehydration. The H2O content was not higher than 0.05%. The temperature was increased to 115°C, and feeding was started. 783.14g of propylene oxide was added. During the reaction, the pressure was not higher than 0.4MPa and the temperature was controlled at 115±2°C. After the addition was completed, the internal pressure was reacted for 1 hour and the monomer removal was performed for 0.5 hour. Nitrogen pressure was increased to 0.18MPa, the temperature was controlled at 115°C, ethylene oxide 474.16 was added, the internal pressure was reacted for 30 minutes, the monomer was removed for 0.5 hours, the temperature was lowered to 80°C, pure water, acetic acid, and auxiliary agent (magnesium silicate) were added, vacuum dried, filtered and circulated, and the test indicators were: hydroxyl value: 362.41mgKOH / g; potassium ion: 1ppm; moisture: 0.01%; acid value: 0.022mgKOH / g. The polyether polyol was named polyether polyol C, with a functionality of 3.2 and a molecular weight of 500g / mol.

[0029] Example 4

[0030] Using polyether polyol C as the oligomer, add 300g of polyether polyol C to a 5L stainless steel reactor, add 0.06g of bimetallic catalyst and 19ppm sulfuric acid at a temperature of 60-70℃ and a pressure of 0.02-0.06MPa. After nitrogen replacement and measuring that the oxygen content in the reactor is less than 80ppm, heat it to 130-135℃ and decompress it to dehydrate, and the H2O content is not higher than 0.05%. Pre-drip 30g of ethylene oxide and 30g of propylene oxide mixture into the reactor to initiate the reaction. After initiation, add a mixture of 728.45g of ethylene oxide and 728.45g of propylene oxide into the reactor, control the reaction temperature to 130℃, and the reaction pressure does not exceed 0.2MPa. After the feeding is completed, react under internal pressure for 0.5 hours, cool to 90℃, add antioxidant 1076, take samples to test indicators, and name it polyether polyol D. The analytical indicators are as follows: hydroxyl value: 59.84 mgKOH / g; acid value: 0.026 mgKOH / g; unsaturation value: 0.008 mol / kg; moisture: 0.01%; pH value: 6.88. The functionality of the polyether polyol is 3.2 and the molecular weight is 3000 g / mol.

[0031] Add 200g of weighed polyether polyol, 5g of cross-linking agent, 8g of silicone oil, 1g of catalyst, 1g of foaming agent, 450g of light calcium carbonate and 60g of xylene into a 2000ml three-necked flask in turn, stir at room temperature for 40 minutes, which is called white material. Heat to 50°C, add 80g of black material. The black material is modified MDI and polymethylene polyphenyl polyisocyanate (PAPI) in a ratio of 2:1. React for 2.5 hours. The ratio of the amount of isocyanate group to the amount of hydroxyl substance is 1.2:1.

[0032] Weigh large-particle compound fertilizer with a particle size of 3 mm, place it in a rotating drum, turn on the switch, mix the black material with the white material, add the curing agent E300, and the film-aiding agent without preheating before spraying. The nozzle atomization pressure during spraying is 0.65MPa. Place it in the rotating drum and spray for 3 minutes. After reacting for 8 minutes, the coated controlled-release fertilizer is obtained. The controlled-release performance is measured by water immersion method, see Table 1 for details.

[0033] Comparative Example

[0034] Add 630g of castor oil to a 5L stainless steel reactor, vacuum draw in 10.5g of potassium methylate, replace with nitrogen, measure the oxygen content in the reactor to be less than 80ppm, heat up and decompress to dehydrate, the H2O content is not higher than 0.05%, heat up to 115℃, start feeding, add 725.92g of propylene oxide, the pressure is not higher than 0.4MPa during the reaction, the temperature is controlled at 115±2℃, after adding, react under internal pressure for 1 hour, and remove monomers for 0.5 hour. Add pure water, acetic acid, add auxiliary agent (aluminum silicate), vacuum dry, filter and cycle, test indicators: hydroxyl value: 75.73mgKOH / g; potassium ion: 1ppm; moisture: 0.01%; acid value: 0.022mgKOH / g. The polyether polyol is named polyether polyol E, with a functionality of 2.7 and a molecular weight of 2000mol / g.

[0035] from Figure 1 It can be seen that the polyether polyols in the examples can be used to prepare a good coating at room temperature, while the coatings prepared by conventional polyether products are not sufficiently matured, have a sticky surface, and adhesion occurs between the coatings, which does not meet the requirements.

[0036] According to the slow-release fertilizer industry standard (HG / T3931-2007) and the controlled-release fertilizer evaluation standard recommended by the European Committee for Standardization (CEN), it can be seen from Table 1 that the dissolution of the slow-release fertilizer prepared by the polyether product of the embodiment meets the standard requirements.

[0037] Table 1 Evaluation results of the application of different polyether polyols in making coating materials

[0038] Brand Initial dissolution rate% Controlled release period% 12-month degradation rate % Polyether polyol A to make coating material 1.0 88 8.4 Polyether polyol B to make coating material 0.7 92 9.3 Polyether polyol C to make coating material 1.1 87 8.2 Polyether polyol D to make coating material 0.9 96 7.8

Claims

1. An application of a polyether polyol, characterized in that: Used for preparing slow-release fertilizer polyurethane coating at room temperature; the polyether polyol is prepared by using polyol compounds as initiators, catalyzed by catalysts, and polymerizing with epoxy compounds; Wherein, the polyol compound is one or more of glycerol, pentaerythritol, and castor oil; the epoxy compound is a mixture of ethylene oxide and propylene oxide, and the mass of ethylene oxide accounts for more than 20% of the total mass of the epoxy compound; The polyether polyol has a functionality of 2-4 and a number average molecular weight of 400-5000 g / mol; The polymerization reaction is carried out in one of the following ways: Method (1), the initiator is mixed with a mixture of propylene oxide and ethylene oxide; Method (2), the initiator is first co-polymerized with a mixture of propylene oxide and ethylene oxide, and then capped with ethylene oxide; Method (3), the initiator is first polymerized with propylene oxide and then capped with ethylene oxide; Method (4) is that the initiator is first polymerized with ethylene oxide, then polymerized with propylene oxide, and finally capped with ethylene oxide.

2. The use of the polyether polyol according to claim 1, characterized in that: The polyol compound is castor oil.

3. The use of the polyether polyol according to claim 1, characterized in that: The catalyst is an alkali metal catalyst or a bimetallic catalyst.

4. The use of the polyether polyol according to claim 3, characterized in that: The alkali metal catalyst is one of potassium hydroxide, sodium hydroxide, potassium methoxide or sodium methoxide.

5. The use of the polyether polyol according to claim 1, characterized in that: The polymerization reaction has a reaction temperature of 90-130° C. and a reaction pressure of 0.1-0.4 MPa.

6. The use of the polyether polyol according to claim 1, characterized in that: After the polymerization reaction, post-treatment is performed, wherein the post-treatment is performed using water, acid and an auxiliary agent.

7. The use of the polyether polyol according to claim 6, characterized in that: The acid is one or more of phosphoric acid, sulfuric acid, hydrochloric acid, oxalic acid, lactic acid or acetic acid.

8. The use of the polyether polyol according to claim 6, characterized in that: The auxiliary agent is one or more of aluminum silicate, magnesium silicate or magnesium aluminum silicate.