Polarizing plate with optical compensation layer and organic el panel using the same
By using the refractive index characteristics of nx > nz > ny and the design of a phase retardation film with flat dispersion in organic EL panels, the problems of high cost and insufficient anti-reflection in the tilt direction of organic EL panels are solved, achieving a low-cost and efficient anti-reflection effect.
Patent Information
- Application Number
- CN202111048359.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-12-02
- Filing Date
- 2021-09-08
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2041-09-08
AI Technical Summary
The existing circular polarizers for organic EL panels are expensive to manufacture and lack sufficient anti-reflective properties in the tilt direction, making it difficult to effectively solve the problems of external light reflection and background reflection.
A polarizer consisting of a polarizer, a first optical compensation layer, and a second optical compensation layer is used. Each layer has a refractive index characteristic of nx > nz > ny. By adjusting the angle between the slow axis and the absorption axis, the in-plane phase difference of each layer is ensured to be equal or substantially parallel, thus forming a phase retardation film with flat dispersion.
It achieves the goal of maintaining excellent anti-reflective properties in the front direction while improving anti-reflective properties in the tilted direction, ensuring hue consistency, and reducing manufacturing costs.
Smart Images

Figure CN114578469B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a polarizer with an optical compensation layer and an organic EL panel using the polarizer with the optical compensation layer. Background Technology
[0002] In recent years, with the popularization of thin-film displays, displays equipped with organic EL panels (organic EL display devices) have been proposed. Organic EL panels have highly reflective metal layers, which easily lead to problems such as external light reflection and background reflection. Therefore, it is known to prevent these problems by placing a circular polarizer on the visual confirmation side. As a common circular polarizer, it is known to be obtained by stacking a retardation film (typically a λ / 4 plate) with its slow axis at an angle of approximately 45° relative to the absorption axis of the polarizer. In addition, in order to further improve the anti-reflection properties, it has been attempted to stack retardation films (optical compensation layers) with various optical properties. For example, a retardation film that satisfies Re(550) > Re(450) is known. Circular polarizers using such retardation films are expected to improve the viewing angle characteristics of organic EL panels. However, such retardation films are expensive, and the cost of manufacturing circular polarizers is high.
[0003] Existing technical documents Patent documents Patent Document 1: Japanese Patent No. 3325560 Summary of the Invention
[0004] The problem that the invention aims to solve The present invention was made to solve the above-mentioned problems. Its main objective is to provide a polarizer with an optical compensation layer that is inexpensive and maintains excellent anti-reflective properties in the front direction while also having excellent anti-reflective properties in the tilt direction, thereby enabling an organic EL panel with a neutral hue in the tilt direction.
[0005] means for solving problems The polarizer with an optical compensation layer of the present invention can be used in organic EL panels. The polarizer with the optical compensation layer sequentially comprises a polarizer, a first optical compensation layer, and a second optical compensation layer. The first and second optical compensation layers exhibit refractive index characteristics of nx > nz > ny, respectively. Furthermore, the Re(450) and Re(550) of the first and second optical compensation layers are substantially equal. In one embodiment, Re(550) is 220 nm to 300 nm, the Nz coefficient is 0.4 to 0.8, and the angle between the absorption axis direction of the polarizer and the slow axis direction of the first optical compensation layer is 5° to 25°. Furthermore, the Re(550) of the second optical compensation layer is 90 nm to 170 nm, the Nz coefficient is 0.4 to 0.8, and the angle between the absorption axis direction of the polarizer and the slow axis direction of the second optical compensation layer is 65° to 85°. Here, Re(450) and Re(550) represent the in-plane phase differences measured with light at 23°C and wavelengths of 450 nm and 550 nm, respectively.
[0006] In one embodiment, the Re(550) of the first optical compensation layer is 280nm to 360nm, the Nz coefficient is 0.5 to 0.9, and the angle between the absorption axis direction of the polarizer and the slow axis direction of the first optical compensation layer is substantially parallel. Furthermore, the Re(550) of the second optical compensation layer is 100nm to 180nm, the Nz coefficient is 0.2 to 0.6, and the angle between the absorption axis direction of the polarizer and the slow axis direction of the second optical compensation layer is 35° to 55°.
[0007] According to other aspects of the invention, an organic EL panel is provided. This organic EL panel includes the aforementioned polarizer with an optical compensation layer.
[0008] Invention Effects According to the present invention, in a polarizer with an optical compensation layer, a first optical compensation layer and a second optical compensation layer are sequentially disposed from the polarizer side. The first optical compensation layer exhibits refractive index characteristics of nx > nz > ny and has a predetermined in-plane phase difference, and the second optical compensation layer exhibits refractive index characteristics of nx > nz > ny and has a predetermined in-plane phase difference. Furthermore, a polarizer with an optical compensation layer is provided in which both the first and second optical compensation layers are composed of a phase difference film with flat dispersion. This allows for the acquisition of a low-cost polarizer with excellent anti-reflective properties in the front direction and excellent anti-reflective properties in the tilt direction, thereby enabling the realization of an organic EL panel with a neutral hue in the tilt direction. Attached Figure Description
[0009] Figure 1 This is a cross-sectional schematic diagram of a polarizer with an optical compensation layer according to one embodiment of the present invention.
[0010] Symbol Explanation 10 polarizers 20 protective layers 30 First optical compensation layer 40 Second optical compensation layer 100 Polarizers with Optical Compensation Layers Detailed Implementation
[0011] The preferred embodiments of the present invention will be described below, but the present invention is not limited to these embodiments.
[0012] (Definitions of terms and symbols) The definitions of terms and symbols used in this specification are as follows.
[0013] (1) Refractive index (nx, ny, nz) “nx” is the refractive index in the direction of maximum in-plane refractive index (i.e., the slow axis direction), “ny” is the refractive index in the direction orthogonal to the slow axis (i.e., the fast axis direction), and “nz” is the refractive index in the thickness direction.
[0014] (2) In-plane phase difference (Re) “Re(λ)” is the in-plane phase difference measured with light at 23°C and a wavelength of λnm. Re(λ) is calculated using the formula: Re=(nx-ny)×d when the thickness of the layer (film) is set to d (nm). For example, “Re(550)” is the in-plane phase difference measured with light at 23°C and a wavelength of 550nm.
[0015] (3) Phase difference in the thickness direction (Rth) “Rth(λ)” is the phase difference in the thickness direction measured with light at 23°C and a wavelength of λnm. Rth(λ) is calculated using the formula: Rth=(nx-nz)×d when the thickness of the layer (film) is set to d (nm). For example, “Rth(550)” is the phase difference in the thickness direction measured with light at 23°C and a wavelength of 550nm.
[0016] (4) Nz coefficient The Nz coefficient is obtained by Nz = Rth / Re.
[0017] (5) In fact, they are orthogonal or parallel The expressions "substantially orthogonal" and "approximately orthogonal" include cases where the angle between the two directions is 90° ± 10°, preferably 90° ± 7°, and more preferably 90° ± 5°. The expressions "substantially parallel" and "approximately parallel" include cases where the angle between the two directions is 0° ± 10°, preferably 0° ± 7°, and more preferably 0° ± 5°. Furthermore, in this specification, the use of "orthogonal" or "parallel" can include states that are substantially orthogonal or substantially parallel.
[0018] A. Overall structure of a polarizer with optical compensation layer Figure 1 This is a cross-sectional schematic diagram of a polarizer with an optical compensation layer according to one embodiment of the present invention. The polarizer 100 with an optical compensation layer of this embodiment sequentially includes a polarizer 10, a first optical compensation layer 30, and a second optical compensation layer 40. In practical terms, a protective layer 20 can be provided on the side of the polarizer 10 opposite to the first optical compensation layer 30, as shown in the example. Alternatively, the polarizer with the optical compensation layer may have another protective layer (also called an inner protective layer) between the polarizer 10 and the first optical compensation layer 30. In the example, the inner protective layer is omitted. In this case, the first optical compensation layer 30 can also function as an inner protective layer. Furthermore, as needed, a conductive layer and a substrate (neither shown) can be sequentially provided on the side of the second optical compensation layer 40 opposite to the first optical compensation layer 30 (i.e., the outer side of the second optical compensation layer 40). The substrate and the conductive layer are tightly laminated. In this specification, "tightly laminated" means that two layers are directly and firmly laminated without being separated by an adhesive layer (e.g., an adhesive layer, bonding agent layer). The conductive layer and substrate can typically be incorporated into the polarizer 100 with an optical compensation layer in the form of a laminate of the substrate and the conductive layer. By further providing the conductive layer and substrate, the polarizer 100 with an optical compensation layer can be applied to an internal touch panel type input display device. Furthermore / or, as needed, the polarizer with an optical compensation layer (essentially the protective layer 20) can be treated to improve visual clarity when visually inspected through polarized sunglasses (typically by imparting (ellipsoidal) polarization or providing an ultra-high phase difference). By implementing such treatment, excellent visual clarity can be achieved even when visually inspecting the display image through polarized lenses such as polarized sunglasses. Therefore, the polarizer with an optical compensation layer can also be applied to image display devices that can be used outdoors.
[0019] The refractive index characteristics of the first optical compensation layer 30 and the second optical compensation layer 40 each exhibit a relationship of nx > nz > ny and have a slow axis. Furthermore, the Re(450) and Re(550) of the first optical compensation layer and the second optical compensation layer are substantially equal. That is, the first optical compensation layer and the second optical compensation layer each have flat dispersion characteristics in which the phase difference value hardly changes with the wavelength of the measured light. In one embodiment, the in-plane phase difference Re(550) of the first optical compensation layer 30 is 220 nm to 300 nm. In this case, the Nz coefficient of the first optical compensation layer is 0.4 to 0.8, and the angle between the slow axis of the first optical compensation layer 30 and the absorption axis of the polarizer 10 is 5° to 25°, preferably 8° to 22°, more preferably 12° to 18°, and even more preferably about 15°.
[0020] Furthermore, the in-plane phase difference Re(550) of the second optical compensation layer 40 is 90 nm to 170 nm. In this case, the Nz coefficient of the second optical compensation layer is 0.4 to 0.8, and the angle between the slow axis of the second optical compensation layer 30 and the absorption axis of the polarizer 10 is 65° to 85°, preferably 68° to 82°, more preferably 72° to 78°, and even more preferably about 75°. In another embodiment, the in-plane phase difference Re(550) of the first optical compensation layer 30 is preferably 280 nm to 360 nm. In this case, the Nz coefficient of the first optical compensation layer is preferably 0.5 to 0.9, and the angle between the slow axis of the first optical compensation layer 30 and the absorption axis of the polarizer 10 is preferably substantially parallel. In addition, the in-plane phase difference Re(550) of the second optical compensation layer 40 is preferably 100 nm to 180 nm. In this case, the Nz coefficient of the second optical compensation layer is preferably 0.2 to 0.6, and the angle between the slow axis of the second optical compensation layer 30 and the absorption axis of the polarizer 10 is preferably 35° to 55°, more preferably 38° to 52°, further preferably 42° to 48°, and particularly preferably about 45°. As described above, a first optical compensation layer exhibiting refractive index characteristics of nx > nz > ny and having a predetermined in-plane phase difference, and a second optical compensation layer exhibiting refractive index characteristics of nx > nz > ny and having a predetermined in-plane phase difference are sequentially arranged from the polarizer side. Furthermore, both the first and second optical compensation layers are composed of a phase retardation film with flat dispersion. This maintains the excellent anti-reflection characteristics in the front direction due to the excellent circular polarization function and prevents light leakage caused by apparent axial offset of the absorption axis of the polarizer when viewed from an oblique direction. As a result, when a polarizer with an optical compensation layer is applied to an organic EL panel, excellent anti-reflective properties can be achieved in the tilt direction, thereby enabling a neutral (i.e., no undesirable hue) color in the tilt direction.
[0021] The following is a detailed description of each layer and optical film that constitute the polarizer with the optical compensation layer.
[0022] A-1. Polarizer As the polarizer 10, any suitable polarizer can be used. For example, the resin film forming the polarizer can be a single-layer resin film or a laminate of two or more layers.
[0023] Specific examples of polarizers composed of single-layer resin films include: polarizers obtained by dyeing and stretching hydrophilic polymer films such as polyvinyl alcohol (PVA) films, partially formalized PVA films, and partially saponified ethylene-vinyl acetate copolymer films using dichroic substances such as iodine and dichroic dyes; and polyene-based oriented films such as dehydrated PVA products and dehydrochlorinated polyvinyl chloride products. From the perspective of superior optical properties, polarizers obtained by dyeing PVA films with iodine and then uniaxially stretching them are preferred.
[0024] The dyeing process using iodine described above is performed, for example, by immersing the PVA membrane in an aqueous iodine solution. The stretching ratio for the uniaxial stretching is preferably 3 to 7 times. Stretching can be performed after dyeing or simultaneously with dyeing. Alternatively, dyeing can be performed after stretching. The PVA membrane can be subjected to swelling treatment, cross-linking treatment, cleaning treatment, drying treatment, etc., as needed. For example, by immersing the PVA membrane in water for washing before dyeing, not only can stains and anti-blocking agents on the surface of the PVA membrane be washed away, but the PVA membrane can also swell to prevent uneven dyeing.
[0025] Specific examples of polarizers obtained using laminates include: polarizers obtained using a resin substrate and a PVA-based resin layer (PVA-based resin film) laminated on the resin substrate, or a resin substrate and a PVA-based resin layer coated on the resin substrate. A polarizer obtained using a resin substrate and a PVA-based resin layer coated on the resin substrate can be manufactured, for example, by coating a PVA-based resin solution onto a resin substrate and drying it to form a PVA-based resin layer on the resin substrate, thereby obtaining a laminate of the resin substrate and the PVA-based resin layer; stretching and dyeing the laminate to form a polarizer from the PVA-based resin layer. In this embodiment, stretching typically includes immersing the laminate in an aqueous boric acid solution for stretching. Furthermore, stretching may, if necessary, further include air stretching of the laminate at a high temperature (e.g., above 95°C) prior to stretching in the aqueous boric acid solution. The resulting resin substrate / polarizer laminate can be used directly (i.e., the resin substrate can be used as a protective layer for the polarizer), or the resin substrate can be peeled off from the resin substrate / polarizer laminate and any suitable protective layer corresponding to the purpose can be laminated on the peeled surface for use. Detailed description of such a polarizer manufacturing method is disclosed, for example, in Japanese Patent Application Publication No. 2012-73580 (Japanese Patent No. 5414738). The entire contents of that publication are incorporated herein by reference.
[0026] The thickness of the polarizer is preferably 25 μm or less, more preferably 1 μm to 12 μm, even more preferably 3 μm to 12 μm, and particularly preferably 3 μm to 8 μm. As long as the thickness of the polarizer is within this range, curling during heating can be well suppressed, and good appearance durability during heating can be obtained.
[0027] The polarizer preferably exhibits absorption dichroism at any wavelength in the range of 380 nm to 780 nm. The transmittance of the polarizer is preferably 42.0% to 46.0%, more preferably 44.5% to 46.0%. The polarization degree of the polarizer is preferably 97.0% or more, more preferably 99.0% or more, and even more preferably 99.9% or more.
[0028] A-2. First optical compensation layer As described above, the refractive index characteristics of the first optical compensation layer 30 exhibit a relationship of nx > nz > ny and have a slow axis. Furthermore, the first optical compensation layer exhibits a flat wavelength dispersion characteristic, where the phase difference value hardly changes with the wavelength of the measured light. Specifically, the Re(450) / Re(550) of the first optical compensation layer is preferably 0.99 to 1.03. A phase retardation film exhibiting flat wavelength dispersion characteristics is less expensive than a phase retardation film exhibiting reverse dispersion characteristics; therefore, by adopting a configuration like that of the embodiment of the present invention, a polarizer with an optical compensation layer that is inexpensive and has excellent optical properties can be obtained.
[0029] The in-plane phase difference Re(550) of the first optical compensation layer 30 is 220nm to 300nm, preferably 230nm to 290nm, and more preferably 250nm to 270nm. As long as the in-plane phase difference of the first optical compensation layer is within this range, by setting the slow axis direction of the first optical compensation layer relative to the absorption axis direction of the polarizer to 5° to 25° (particularly about 15°) as described above, it is possible to prevent a reduction in the anti-reflection function in the tilt direction caused by the apparent axial offset of the absorption axis of the polarizer. Furthermore, in this case, in one embodiment, the Nz coefficient of the first optical compensation layer is 0.4 to 0.8, preferably 0.5 to 0.7, more preferably 0.55 to 0.65, and particularly preferably 0.55 to 0.60. As long as the Nz coefficient is within this range, by adjusting the angle between the slow axis of the first optical compensation layer and the absorption axis of the polarizer to a predetermined angle, superior anti-reflection characteristics in the tilt direction can be achieved.
[0030] In another embodiment, the in-plane phase difference Re(550) of the first optical compensation layer is preferably 280nm to 360nm, more preferably 290nm to 350nm, and even more preferably 310nm to 330nm. As long as the in-plane phase difference of the first optical compensation layer is within such a range, by setting the slow axis direction of the first optical compensation layer to be substantially parallel to the absorption axis direction of the polarizer, it is possible to prevent a reduction in the anti-reflection function in the tilt direction caused by the apparent axial offset of the absorption axis of the polarizer. Furthermore, in this case, in another embodiment, the Nz coefficient is preferably 0.5 to 0.9, more preferably 0.6 to 0.8, even more preferably 0.7 to 0.8, and particularly preferably 0.72 to 0.78. As long as the Nz coefficient is within such a range, by adjusting the angle between the slow axis of the first optical compensation layer and the absorption axis of the polarizer to a predetermined angle, superior anti-reflection characteristics in the tilt direction can be achieved.
[0031] The first optical compensation layer is typically formed of a resin film, which is formed of any suitable resin capable of achieving the aforementioned properties. Examples of resins used to form this resin film include: polycarbonate resins, cyclic olefin resins, cellulose resins, polyester resins, polyvinyl alcohol resins, polyamide resins, polyimide resins, polyether resins, polystyrene resins, acrylic resins, and polyester carbonate resins. Among these, cyclic olefin resins or polycarbonate resins may be suitably used.
[0032] Cyclic olefin resins are a general term for resins polymerized using cyclic olefins as polymerizing units. Examples include resins described in Japanese Patent Application Publication Nos. 1-240517, 3-14882, and 3-122137. Specific examples include: ring-opening (copolymer) polymers of cyclic olefins, addition polymers of cyclic olefins, copolymers of cyclic olefins with α-olefins such as ethylene and propylene (typically random copolymers), and graft-modified products obtained by modifying them with unsaturated carboxylic acids and their derivatives, as well as their hydrides. Specific examples of cyclic olefins include norbornene monomers. Norbornene monomers include monomers described in Japanese Patent Application Publication No. 2015-210459, etc. Various commercially available products are made from the aforementioned cyclic olefin resins. Specific examples include: products manufactured by ZEON Corporation of Japan under the names "ZEONEX" and "ZEONOR", products manufactured by JSR Corporation under the name "Arton", products manufactured by TICNA Corporation under the name "TOPAS", and products manufactured by Mitsui Chemicals Corporation under the name "APEL".
[0033] As a polycarbonate resin, any suitable polycarbonate resin can be used as long as the effects of the present invention are achieved. Preferably, the polycarbonate resin comprises structural units derived from isosorbide-based dihydroxy compounds and structural units derived from at least one dihydroxy compound selected from alicyclic diols, alicyclic diethanols, diethylene glycol, triethylene glycol, or polyethylene glycol, and alkylene glycols or spirodiols. More preferably, the polycarbonate resin comprises structural units derived from isosorbide-based dihydroxy compounds, structural units derived from alicyclic diethanols, and / or structural units derived from diethylene glycol, triethylene glycol, or polyethylene glycol. The polycarbonate resin may, as needed, comprise structural units derived from other dihydroxy compounds. Furthermore, details of the polycarbonate resin and the method for manufacturing the retardation film suitable for use in the present invention are described, for example, in International Publication No. 2011 / 062239, which is incorporated herein by reference.
[0034] The first optical compensation layer can be formed, for example, by coating a coating liquid, in which the aforementioned resin is dissolved or dispersed in any suitable solvent, onto a shrinkable film to form a coating film, and then shrinking the coating film. Typically, regarding the shrinkage of the coating film, the shrinkable film is shrunk by heating the laminate of the shrinkable film and the coating film, thereby shrinking the coating film. The shrinkage rate of the coating film is preferably 0.50 to 0.99, more preferably 0.60 to 0.98, and even more preferably 0.70 to 0.95. The heating temperature is preferably 130°C to 170°C, more preferably 150°C to 160°C. In one embodiment, when shrinking the coating film, the laminate can be stretched along a direction orthogonal to the shrinkage direction. In this case, the stretching ratio of the laminate is preferably 1.01 to 3.0 times, more preferably 1.05 to 2.0 times, and even more preferably 1.10 to 1.50 times. Specific examples of materials constituting a shrinkable film include: polyolefins, polyesters, acrylic resins, polyamides, polycarbonates, norbornene resins, polystyrene, polyvinyl chloride, polyvinylidene chloride, cellulose resins, polyethersulfone, polysulfone, polyimide, polyacrylic acid, acetate resins, polyarylates, polyvinyl alcohol, and liquid crystal polymers. These can be used individually or in combination. A stretchable film formed from these materials is preferred.
[0035] The thickness of the first optical compensation layer is preferably 10 μm to 200 μm, more preferably 20 μm to 150 μm, and even more preferably 20 μm to 60 μm. With such a thickness, the desired in-plane phase difference and Nz coefficient can be obtained.
[0036] A-3. Second optical compensation layer As described above, the refractive index characteristics of the second optical compensation layer 40 exhibit a relationship of nx > nz > ny and have a slow axis. Furthermore, the second optical compensation layer displays a flat wavelength dispersion characteristic, where the phase difference value hardly changes with the wavelength of the measured light. Specifically, the Re(450) / Re(550) ratio of the second optical compensation layer is preferably 0.99 to 1.03. A phase retardation film exhibiting flat wavelength dispersion characteristics is less expensive than a phase retardation film exhibiting reverse dispersion characteristics; therefore, by adopting a configuration like that of the embodiment of the present invention, a polarizer with an optical compensation layer that is inexpensive and possesses excellent optical properties can be obtained.
[0037] As described above, the in-plane phase difference Re(550) of the second optical compensation layer 40 is 90nm to 170nm, preferably 100nm to 160nm, and more preferably 120nm to 140nm. As long as the in-plane phase difference of the second optical compensation layer is within this range, excellent anti-reflection characteristics can be achieved by setting the slow axis direction of the second optical compensation layer at an angle of 65° to 85° (particularly about 75°) relative to the absorption axis direction of the polarizer, as described above. Furthermore, in this case, in one embodiment, the Nz coefficient of the second optical compensation layer is 0.4 to 0.8, preferably 0.5 to 0.7, more preferably 0.55 to 0.65, and particularly preferably 0.57 to 0.63. This allows for the achievement of even better reflective hue.
[0038] In another embodiment, as described above, the in-plane phase difference Re(550) of the second optical compensation layer 40 is preferably 100nm to 180nm, more preferably 110nm to 170nm, and even more preferably 130nm to 150nm. As long as the in-plane phase difference of the second optical compensation layer is within this range, excellent anti-reflection characteristics can be achieved by setting the slow axis direction of the second optical compensation layer at an angle preferably 35° to 55° (particularly preferably about 45°) relative to the absorption axis direction of the polarizer, as described above. Furthermore, in this case, the Nz coefficient is preferably 0.2 to 0.6, more preferably 0.3 to 0.5, even more preferably 0.35 to 0.45, and particularly preferably 0.37 to 0.42. This allows for the achievement of even better reflective hue.
[0039] The material used to form the second optical compensation layer and the method of forming the second optical compensation layer are the same as those used for the first optical compensation layer.
[0040] The thickness of the second optical compensation layer is preferably 10 μm to 150 μm, more preferably 10 μm to 100 μm, and even more preferably 10 μm to 30 μm. With such a thickness, the desired in-plane phase difference and Nz coefficient can be obtained. By combining the first optical compensation layer described in A-2. with the second optical compensation layer described in A-3., it is possible to obtain a polarizer with an optical compensation layer that is inexpensive and maintains excellent anti-reflective properties in the front direction while also exhibiting excellent anti-reflective properties in the tilt direction, thereby enabling an organic EL panel with a neutral hue in the tilt direction.
[0041] A-4. Protective Layer The protective layer 20 is formed of any suitable film that can be used as a protective layer for a polarizer. Specific examples of materials that are the main components of this film include: cellulose resins such as cellulose triacetate (TAC), polyester resins, polyvinyl alcohol resins, polycarbonate resins, polyamide resins, polyimide resins, polyethersulfone resins, polysulfone resins, polystyrene resins, polynorbornene resins, polyolefin resins, (meth)acrylic acid resins, acetate resins, and other transparent resins. Additionally, thermosetting or UV-curing resins such as (meth)acrylic acid resins, urethane resins, (meth)acrylate urethane resins, epoxy resins, and silicone resins can also be used. Furthermore, glassy polymers such as siloxane polymers can also be used. Additionally, the polymer film described in Japanese Patent Application Publication No. 2001-343529 (WO01 / 37007) can also be used. As the material for this membrane, for example, a resin composition containing a thermoplastic resin having substituted or unsubstituted imide groups on the side chains and a thermoplastic resin having substituted or unsubstituted phenyl and nitrile groups on the side chains can be used. Examples include resin compositions having alternating copolymers formed from isobutylene and N-methylmaleimide and acrylonitrile-styrene copolymers. The polymer membrane can be, for example, an extruded product of the above-mentioned resin composition.
[0042] As needed, the protective layer 20 can be subjected to surface treatments such as hard coating, anti-reflective treatment, anti-sticking treatment, and anti-glare treatment.
[0043] The thickness of the protective layer 20 is typically 5 mm or less, preferably 1 mm or less, more preferably 1 μm to 500 μm, and even more preferably 5 μm to 150 μm. Furthermore, when a surface treatment has been performed, the thickness of the protective layer includes the thickness of the surface treatment layer.
[0044] When an inner protective layer is provided between the polarizer 10 and the first optical compensation layer 30, the inner protective layer is preferably optically isotropic. In this specification, "optically isotropic" means that the in-plane phase difference Re(550) is 0 nm to 10 nm and the phase difference Rth(550) in the thickness direction is -10 nm to +10 nm. As long as the inner protective layer is optically isotropic, it can be made of any suitable material. For example, the material can be appropriately selected from the materials described above for the protective layer 20.
[0045] The thickness of the inner protective layer is preferably 5μm to 200μm, more preferably 10μm to 100μm, and even more preferably 15μm to 95μm.
[0046] A-5. Other The layers constituting the polarizer with optical compensation layer are bonded together with any suitable adhesive layer or bonding agent layer.
[0047] Although not shown, an adhesive layer can also be provided on the side of the second optical compensation layer 40 of the polarizer 100 with the optical compensation layer. By pre-providing the adhesive layer, it can be easily bonded to other optical components (such as organic EL panels). Furthermore, it is preferable to attach a release film to the surface of the adhesive layer until it is ready for use. By temporarily attaching the release film, the adhesive layer can be protected and a roll can be formed.
[0048] B. Organic EL Panel The organic EL panel of the present invention includes an organic EL unit and a polarizer with an optical compensation layer as described in item A above, disposed on the visual confirmation side of the organic EL unit. The polarizer with the optical compensation layer is stacked such that the second optical compensation layer is on the organic EL unit side (the polarizer is on the visual confirmation side).
[0049] Example The present invention will be specifically described below through examples, but the present invention is not limited to these examples. Furthermore, the methods for measuring each characteristic are described below.
[0050] (1) Thickness The measurements were performed using a dial indicator (manufactured by PEACOCK, product name "DG-205") and a dial indicator stand (product name "pds-2").
[0051] (2) Phase difference A 50mm × 50mm sample was cut from the phase retardation film of the optical compensation layer of each polarizer constituting the embodiments and comparative examples as a measurement sample, and measurements were performed using an Axoscan manufactured by Axometrics. The measurement wavelengths were 450nm and 550nm, and the measurement temperature was 23°C.
[0052] In addition, the average refractive index was measured using an Abbe refractometer manufactured by Atago, and the refractive indices nx, ny, and nz were calculated from the obtained phase difference values.
[0053] (3) Frontal reflectance An organic EL display device was obtained by bonding a polarizer with an optical compensation layer, obtained from the examples and comparative examples, to the visual confirmation side of the organic EL panel of an organic EL display device (LG Display, product name "55C7P") through an adhesive layer so that the optical compensation layer is on the organic EL side.
[0054] The organic EL was made to display a black image, and the frontal reflectance was measured using a spectrophotometer (product name "CM-2600D") manufactured by Konica Minolta.
[0055] (4) Reflection characteristics in the tilt direction The characteristics of the polarizer with optical compensation layer obtained from the examples and comparative examples were simulated. The tilt direction (polar angle 60°) was evaluated. Shintech's "LCD MASTER Ver. 6.084" was used in the simulation. The reflection characteristics were simulated using the extended functions of LCD Master.
[0056] [Example 1] (i) Fabrication of the first optical compensation layer A commercially available cyclic olefin resin film (manufactured by JSR Corporation, product name "Arton(R5000)") was used as the resin film. It had a thickness of 130 μm and a Tg of 137 °C. A 60 μm thick shrinkable film (manufactured by Toray Industries, product name "TORAYFAN BO2873") was bonded to both sides of the film through an acrylic adhesive layer (15 μm thick), and then unidirectionally stretched at the free end to obtain the retardation film constituting the first optical compensation layer. The stretching temperature was set to 134 °C, and the stretching ratio was set to 1.06 times. The resulting retardation film (i.e., the first optical compensation layer) had a Re(550) of 257 nm, an Nz coefficient of 0.59, and a Re(450) / Re(550) ratio of 1.00.
[0057] (ii) Fabrication of the second optical compensation layer Except that the stretching temperature was set to 135°C and the stretching ratio was set to 1.03, the retardation film constituting the second optical compensation layer was fabricated in the same manner as in (i) the fabrication of the first optical compensation layer. The resulting retardation film (i.e., the second optical compensation layer) had a Re(550) of 130 nm, an Nz coefficient of 0.6, and a Re(450) / Re(550) ratio of 1.00.
[0058] (iii) Fabrication of the polarizer While stretching a 30μm thick polyvinyl alcohol (PVA) resin film (manufactured by Toray, product name "PE3000") unidirectionally to 5.9 times its original thickness using a roller stretching machine, swelling, dyeing, crosslinking, and cleaning processes are simultaneously carried out, and finally drying is performed, thus producing a polarizer with a thickness of 12μm.
[0059] Specifically, for the swelling treatment, the sample was stretched to 2.2 times while being treated with pure water at 20°C. Next, for the dyeing treatment, the sample was stretched to 1.4 times while being treated in an aqueous solution at 30°C with an iodine to potassium iodide weight ratio of 1:7, adjusted to achieve a monomer transmittance of 45.0% for the resulting polarizer. Furthermore, the crosslinking treatment employed a two-stage process. In the first stage, the sample was stretched to 1.2 times while being treated in an aqueous solution containing boric acid and potassium iodide at 40°C. The boric acid content in the first stage crosslinking treatment aqueous solution was set to 5.0% by weight, and the potassium iodide content was set to 3.0% by weight. In the second stage, the sample was stretched to 1.6 times while being treated in an aqueous solution containing boric acid and potassium iodide at 65°C. The boric acid content in the second stage crosslinking treatment aqueous solution was set to 4.3% by weight, and the potassium iodide content was set to 5.0% by weight. Finally, the cleaning treatment was performed in an aqueous solution of potassium iodide at 20°C. The potassium iodide content of the aqueous solution used for cleaning was set at 2.6% by weight. Finally, the polarizer was obtained by drying at 70°C for 5 minutes.
[0060] (iv) Fabrication of polarizers A strip-shaped polarizer with a protective layer / polarizer structure is obtained by bonding an HC-TAC film (thickness: 32 μm, corresponding to the protective layer) with a hard coating (HC) layer (7 μm) formed on one side of the TAC film (25 μm) through a polyvinyl alcohol adhesive and then rolling it together with the polarizer.
[0061] (v) Fabrication of polarizers with optical compensation layers The polarizer, first optical compensation layer, and second optical compensation layer obtained above are cut to a specified size. The polarizer surface of the polarizer and the first optical compensation layer are then bonded together with an acrylic adhesive, and the first and second optical compensation layers are further bonded together with an acrylic adhesive. This results in a polarizer with an optical compensation layer, comprising a protective layer / polarizer / first optical compensation layer / second optical compensation layer. Furthermore, the first optical compensation layer is cut such that the angle between the absorption axis of the polarizer and the slow axis of the first optical compensation layer in the polarizer with the optical compensation layer is 15°. The second optical compensation layer is cut such that the angle between the absorption axis of the polarizer and the slow axis of the second optical compensation layer in the polarizer with the optical compensation layer is 75°. That is, the process of cutting and bonding each layer constituting the polarizer with the optical compensation layer (RtoS) is performed twice.
[0062] The obtained polarizer with optical compensation layer was used for the evaluation described in (3) above. Furthermore, the reflection characteristics described in (4) above were simulated using the properties of the obtained polarizer with optical compensation layer. The results are shown in Table 1.
[0063] [Example 2] Except for the stretching temperature and stretching ratio described in Table 1, the first optical compensation layer and the second optical compensation layer were obtained in the same manner as in Example 1. The obtained first optical compensation layer had a Re(550) of 317 nm, an Nz coefficient of 0.75, and a Re(450) / Re(550) ratio of 1.00. The obtained second optical compensation layer had a Re(550) of 136 nm, an Nz coefficient of 0.41, and a Re(450) / Re(550) ratio of 1.00. The polarizer and the first optical compensation layer were bonded together by roll-to-roll bonding, and the shrinkage film was peeled off to obtain a laminate of protective layer / polarizer / first optical compensation layer. The absorption axis of the polarizer is substantially parallel to the slow axis of the first optical compensation layer. The laminate was cut to a specified size, and the second optical compensation layer was further cut and bonded with the angle between the absorption axis of the polarizer and the slow axis of the second optical compensation layer being 45°, resulting in a polarizer with a protective layer / polarizer / first optical compensation layer / second optical compensation layer. That is, the number of times the process (RtoS) of cutting and bonding each layer constituting the polarizer with optical compensation layer was performed was one. Furthermore, an organic EL panel was fabricated in the same manner as in Example 1, except that the polarizer with optical compensation layer was used. The obtained polarizer with optical compensation layer was evaluated in the same way as in Example 1. The results are shown in Table 1.
[0064] [Comparative Example 1] (i) Fabrication of the first optical compensation layer (i-1) Fabrication of polycarbonate resin film Polymerization was carried out using a batch polymerization apparatus consisting of two vertical reactors equipped with agitators and reflux coolers controlled at 100°C. The molar ratios of 9,9-[4-(2-hydroxyethoxy)phenyl]fluorene (BHEPF), isosorbide (ISB), diethylene glycol (DEG), diphenyl carbonate (DPC), and magnesium acetate tetrahydrate were BHEPF / ISB / DEG / DPC / magnesium acetate = 0.348 / 0.490 / 0.162 / 1.005 / 1.00×10⁻⁶. -5The reactor was fed in the following manner: Nitrogen replacement was performed thoroughly (oxygen concentration 0.0005–0.001% by volume), followed by heating with a heat transfer medium. Stirring was initiated when the internal temperature reached 100°C. After 40 minutes of initial heating, the internal temperature was raised to 220°C and maintained at this temperature. Simultaneously, pressure was reduced, and after reaching 220°C, a pressure of 13.3 kPa was applied for 90 minutes. Phenol vapor, a byproduct of the polymerization reaction, was introduced into a 100°C reflux cooler to return the small amount of monomer components contained in the phenol vapor to the reactor. Uncondensed phenol vapor was recovered by introducing it into a 45°C condenser.
[0065] Nitrogen was introduced into the first reactor to temporarily restore it to atmospheric pressure, and then the oligomerized reaction liquid in the first reactor was transferred to the second reactor. Next, heating and depressurization were initiated in the second reactor, setting the internal temperature to 240°C and the pressure to 0.2 kPa for 50 minutes. Polymerization was then carried out until the specified stirring motive force was reached. At the moment the specified motive force was reached, nitrogen was introduced into the reactor to restore the pressure, and the reaction liquid was extracted in the form of a filament. Granulation was performed using a rotary cutter to obtain a polycarbonate resin with a copolymer composition of BHEPF / ISB / DEG = 34.8 / 49.0 / 16.2 [mol%]. This polycarbonate resin has a specific viscosity of 0.430 dL / g and a glass transition temperature of 128°C.
[0066] (i-2) Fabrication of the first optical compensation layer The obtained polycarbonate resin was vacuum dried at 80°C for 5 hours. Then, a film-forming device equipped with a single-screw extruder (manufactured by Isuzu Chemical Machinery Co., Ltd., screw diameter 25 mm, cylinder set temperature: 220°C), a T-die (width 900 mm, set temperature: 220°C), a cooling roller (set temperature: 125°C), and a winding machine was used to produce a polycarbonate resin film with a thickness of 130 μm. The water absorption rate of the obtained polycarbonate resin film was 1.2%.
[0067] A first optical compensation layer was obtained by obliquely stretching the polycarbonate resin film obtained as described above according to the method of Example 1 of Japanese Patent Application Publication No. 2014-194483. The obtained first optical compensation layer has a Re(550) of 139 nm, an Nz coefficient of 1.10, and a Re(450) / Re(550) ratio of 0.89.
[0068] (ii) Fabrication of the second optical compensation layer A liquid crystal coating solution was prepared by dissolving 20 parts by weight of a side-chain liquid crystal polymer represented by the following chemical formula (II) (where the numbers 65 and 35 represent the molar percentage of monomer units; for convenience, it is represented as a block polymer; the weight-average molecular weight is 5000), 80 parts by weight of a polymerizable liquid crystal displaying a nematic liquid crystal phase (manufactured by BASF: product name Paliocolor LC242), and 5 parts by weight of a photopolymerization initiator (manufactured by Ciba Specialty Chemicals: product name IRGACURE 907) in 200 parts by weight of cyclopentanone. The coating solution was then applied to a substrate film (norbornene resin film: manufactured by ZEON Corporation, Japan, product name "ZEONEX") using a wire-bar coater, and then heated and dried at 80°C for 4 minutes to orient the liquid crystal. The liquid crystal layer was cured by irradiating it with ultraviolet light, forming a liquid crystal fixing layer (thickness: 0.58 μm) on the substrate, which became the second optical compensation layer. The obtained second optical compensation layer has a Re(550) of 0 nm and an Rth(550) of -71 nm.
[0069] Chemical Formula 1 By rolling the polarizer together with the first and second optical compensation layers obtained in (i) and (ii) above, and then peeling off the substrate, a polarizer with an optical compensation layer was obtained, consisting of a protective layer / polarizer / first optical compensation layer / second optical compensation layer. The angle between the absorption axis of the polarizer and the slow axis of the first optical compensation layer is 45°. Furthermore, an organic EL surface was fabricated in the same manner as in Example 1, except that this polarizer with an optical compensation layer was used. The obtained polarizer with an optical compensation layer and the organic EL panel were evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0070] [Comparative Example 2] Except that the thickness of the second optical compensation layer was set to 0.44 μm, a polarizer with an optical compensation layer was obtained in the same manner as Comparative Example 1, consisting of a protective layer / polarizer / first optical compensation layer / second optical compensation layer. The Re(550) of the first optical compensation layer was 139 nm, the Nz coefficient was 1.00, and the Re(450) / Re(550) ratio was 0.89. The Re(550) of the second optical compensation layer was 0 nm, and the Rth(550) was -54. Furthermore, except that this polarizer with an optical compensation layer was used, an organic EL panel was fabricated in the same manner as in Example 1. The obtained polarizer with an optical compensation layer and organic EL panel were evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0071] Table 1
[0072] ※ Indicates the phase difference (Rth) in the thickness direction.
[0073] [evaluate] As shown in Table 1, the polarizer with optical compensation layer in the embodiments of the present invention can maintain excellent anti-reflective properties in the front direction while also exhibiting excellent anti-reflective properties in the tilt direction. Furthermore, according to the embodiments, it was confirmed that the hue in the tilt direction can be set to neutral.
[0074] Industrial availability The polarizer with optical compensation layer of the present invention can be applied to organic EL panels.
Claims
1. A polarizer with an optical compensation layer for use in an organic EL panel, comprising a polarizer, a first optical compensation layer, and a second optical compensation layer in sequence. in, The first optical compensation layer exhibits refractive index characteristics of nx > nz > ny, a Re(550) of 220 nm to 300 nm, and an Nz coefficient of 0.4 to 0.
8. The angle between the absorption axis of the polarizer and the slow axis of the first optical compensation layer is 5° to 25°. The second optical compensation layer exhibits refractive index characteristics of nx > nz > ny, a Re(550) of 90 nm to 170 nm, and an Nz coefficient of 0.4 to 0.
8. The angle between the absorption axis of the polarizer and the slow axis of the second optical compensation layer is 65° to 85°. The Re(450) / Re(550) ratios of the first optical compensation layer and the second optical compensation layer are respectively 0.99~1.
03. Here, Re(450) and Re(550) represent the in-plane phase differences measured with light at 23°C and wavelengths of 450 nm and 550 nm, respectively.
2. A polarizer with an optical compensation layer, used in an organic EL panel, and comprising, in sequence, a polarizer, a first optical compensation layer, and a second optical compensation layer. in, The first optical compensation layer exhibits refractive index characteristics of nx > nz > ny, with Re(550) ranging from 280 nm to 360 nm and Nz coefficients ranging from 0.5 to 0.
9. The angle between the absorption axis of the polarizer and the slow axis of the first optical compensation layer is within the range of 0° ± 10°. The second optical compensation layer exhibits refractive index characteristics of nx > nz > ny, a Re(550) of 100 nm to 180 nm, and an Nz coefficient of 0.2 to 0.
6. The angle between the absorption axis of the polarizer and the slow axis of the second optical compensation layer is 35° to 55°. The Re(450) / Re(550) ratios of the first optical compensation layer and the second optical compensation layer are respectively 0.99~1.
03. Here, Re(450) and Re(550) represent the in-plane phase differences measured with light at 23°C and wavelengths of 450 nm and 550 nm, respectively.
3. An organic EL panel having a polarizer with an optical compensation layer as described in claim 1 or 2.
Citation Information
Patent Citations
Paper transporting roller
JP1979014738A
Production of polymer and precursor thereof
JP1989240517A
Plating composition and plated object
JP1991014882A
Thermoplastic resin molded article
JP1991122137A
Protective film for polarizer and its manufacturing method
JP2001343529A