A separator and a high voltage battery comprising the same

By coating the surface of inorganic ceramic particles with a modified layer to adsorb metal ions in the battery, the problem of metal precipitation in high-voltage lithium-ion batteries is solved, improving the battery's safety, rate performance, and cycle performance, while maintaining stable internal resistance.

CN114641890BActive Publication Date: 2026-11-24ZHUHAI COSMX BATTERY CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202080077087.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-11-14
Filing Date
2020-11-11
Publication Date
2026-11-24
Estimated Expiration
2040-11-11

AI Technical Summary

Technical Problem

In high-voltage lithium-ion batteries, the deposition of magnetic metal particles or metal ions on the negative electrode surface can cause internal short circuits and affect lithium-ion insertion. Existing adsorption methods can affect electrical performance or increase costs.

Method used

A modified layer is coated on the surface of inorganic ceramic particles. The modified layer is formed by substituted siloxanes or nitrogen-containing heterocyclic compounds, which adsorb metal ions in the battery system, prevent metal precipitation on the negative electrode surface, and improve battery safety and cycle performance.

Benefits of technology

The modified layer effectively adsorbs transition metal ions, improving battery safety, rate performance, and cycle performance, while not affecting battery internal resistance, thus improving battery performance, stabilizing the positive electrode structure, and reducing HF corrosion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114641890B_ABST
    Figure CN114641890B_ABST
Patent Text Reader

Abstract

A separator and a high-voltage battery including the separator are disclosed. By coating the surface of inorganic ceramic particles with a modified layer, the modified layer can adsorb transition metal ions precipitated from the electrode material, thereby preventing the formation of transition metal precipitates on the negative electrode surface and improving the battery's safety, rate performance, and cycle performance. Simultaneously, since the modified layer is coated on the surface of the inorganic ceramic particles, it does not significantly affect the battery's internal resistance, thus not reducing the battery's rate performance, low-temperature performance, and cycle performance. The introduction of the modified material can also achieve the adsorption of trace amounts of HF generated in the battery system. On the one hand, this can inhibit the dissolution of transition metal ions, stabilize the positive electrode surface structure, and improve battery performance; on the other hand, it can reduce the corrosion of the battery outer material by HF, improving battery safety.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of lithium-ion battery technology, specifically relating to a separator suitable for high-voltage battery systems and a battery including the separator. Background Technology

[0002] With the widespread adoption of 3C products and the rise of the electric vehicle market, the demand for lithium-ion rechargeable batteries is increasing. Since some magnetic metal particles or ions inevitably enter the battery system, these particles or ions will precipitate on the surface of the negative electrode during charging and discharging. Additionally, the positive electrode material itself also experiences the dissolution of transition metal ions, which will also precipitate on the surface of the negative electrode. This precipitation is particularly severe in high-voltage battery systems.

[0003] Metal particles deposited on the surface of the negative electrode can cause problems. On the one hand, they can form metal dendrites that can easily pierce the separator and cause a short circuit inside the battery. On the other hand, they can affect the normal insertion of lithium ions and affect the battery's long-term cycle performance.

[0004] Because the precipitated magnetic metal particles or metal ions (including transition metal ions) have the aforementioned problems, existing technologies have reported the adsorption of transition metal ions using porous ceramic particles. However, this method, due to the use of porous ceramic particles, results in high moisture content, which adversely affects electrical performance. Existing technologies have also reported adding a transition metal ion adsorption layer to the surface of the ceramic separator. This method not only increases the manufacturing cost of the separator but also deteriorates ion conductivity due to the added transition metal ion adsorption layer, thus worsening the battery's cycle life and rate discharge performance. Invention Content

[0005] The separator is an essential component in lithium-ion secondary batteries. Its main functions are: firstly, to act as a separator between the positive and negative electrodes, preventing short circuits and ensuring battery safety; and secondly, to act as a channel for lithium ions between the positive and negative electrodes, ensuring normal battery operation. However, after extensive experimental research, the inventors of this application believe that with the continuous pursuit of battery performance, the separator, as one of the key materials of the battery, should play a greater role.

[0006] In order to overcome the shortcomings of the prior art, the purpose of this application is to provide a ceramic particle, as well as a separator and a battery including the ceramic particle.

[0007] like Figure 2As shown, this application involves coating the surface of inorganic ceramic particles with a modified layer. This modified layer can adsorb metal ions present in the battery system (such as transition metal ions precipitated from the positive electrode material, metal ions or metal particles incorporated into the battery system), thereby preventing the formation of metal precipitates on the negative electrode surface and improving the battery's safety, rate capability, and cycle performance. Simultaneously, since the modified layer is coated on the surface of the inorganic ceramic particles, it does not significantly affect the battery's internal resistance, thus not reducing the battery's rate capability, low-temperature performance, or cycle performance.

[0008] The objective of this application is achieved through the following technical solution:

[0009] A type of ceramic particle, wherein, such as Figure 2 As shown, the ceramic particles have a core-shell structure, that is, they include a shell and a core. The material forming the shell includes modified materials, and the material forming the core includes inorganic ceramic materials.

[0010] The modified material is selected from substituted siloxanes, and the substituents are selected from amine compounds containing carboxyl groups or nitrogen-containing heterocyclic compounds.

[0011] According to this application, the amine compound containing a carboxyl group is selected, for example, from polyamine compounds containing at least two carboxyl groups, and further, for example, from one or more of ethylenediaminetetraacetic acid, propylenediaminetetraacetic acid, hydroxyethyl ethylenediaminetriacetic acid, and ethylene glycol diethyl ether diaminetetraacetic acid.

[0012] According to this application, the nitrogen-containing heterocyclic compound is selected, for example, from heterocyclic compounds containing one or two nitrogen atoms, such as from one or more of pyridine and imidazole.

[0013] According to this application, the siloxane is selected from siloxanes containing an amino group; wherein the substituted siloxane is obtained by replacing the amino group in the siloxane with the aforementioned compound. The amino-containing siloxane is, for example, one or more of 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 2-aminoethyltrimethoxysilane, and 2-aminoethyltriethoxysilane.

[0014] According to this application, the ceramic particles can be used in the field of lithium-ion batteries.

[0015] According to this application, the inorganic ceramic material is selected from one or more of alumina, magnesium oxide, boehmite, barium sulfate, barium titanate, zinc oxide, calcium oxide, silicon dioxide, silicon carbide, and nickel oxide.

[0016] According to this application, the shell layer is also referred to as a modified layer.

[0017] According to this application, the thickness of the shell layer is 5nm-1000nm, preferably 50nm-500nm. For example, it is 5nm, 10nm, 50nm, 100nm, 200nm, 500nm or 1000nm.

[0018] According to this application, the average particle size of the inorganic ceramic material is 0.01 μm-20 μm. For example, it is 0.01 μm, 0.05 μm, 0.1 μm, 0.5 μm, 1 μm, 4 μm, 5 μm, 8 μm, 10 μm, 12 μm, 15 μm, 18 μm or 20 μm.

[0019] According to this application, the modified layer (i.e., the shell layer) formed by the modified material coated on the surface of the inorganic ceramic material in the ceramic particles can adsorb transition metal ions precipitated from the positive electrode, thereby preventing transition metal ions from forming transition metal precipitates on the negative electrode surface and improving the safety, rate, and cycle performance of the battery.

[0020] This application also provides a method for preparing the above-mentioned ceramic particles, the method comprising the following steps:

[0021] The ceramic particles are prepared by coating a material comprising a modified material forming a shell onto the surface of a material comprising an inorganic ceramic material forming a core using a silanization process. The ceramic particles have a core-shell structure, comprising a shell and a core. The material forming the shell comprises a modified material, and the material forming the core comprises an inorganic ceramic material.

[0022] For example, the silanization process includes the following steps:

[0023] The material forming the shell is added to a solvent by stirring to form a solution containing the material forming the shell; the material forming the core is added to the aforementioned solution and stirred to mix evenly; the solvent in the mixture is removed by vacuum heating and drying or spray drying to obtain the ceramic particles, wherein the ceramic particles have a core-shell structure, that is, including a shell and a core, the material forming the shell includes modified materials, and the material forming the core includes inorganic ceramic materials.

[0024] The solvent is selected from alcohol-based organic solvents, specifically at least one of methanol, ethanol, propanol, ethylene glycol, propylene glycol, and glycerol. For example, in one embodiment of this application, the preparation of the above-mentioned ceramic particles includes the following steps:

[0025] like Figure 1 As shown, the substituted siloxane (i.e. Figure 1 In the formula, B (where M is a substituent for siloxane) is dissolved in a solvent (ethanol) by stirring to form a mixed solution. Inorganic ceramic material (alumina, i.e.,...) is then added. Figure 1After stirring and mixing evenly, the solvent in the mixture is removed to obtain particles of modified ceramic material coated with the modified material. Figure 1 (C in the middle).

[0026] This application also provides a diaphragm, such as Figure 3 As shown, the diaphragm includes a diaphragm base layer (such as...). Figure 3 The substrate shown) and a coating layer located on at least one side of the diaphragm base layer, the coating layer being obtained by coating at least one side of the diaphragm base layer with a mixture system including the aforementioned ceramic particles (e.g., substrate shown) and a coating layer located on at least one side of the diaphragm base layer. Figure 3 (The coating layer is formed by modified ceramics and binder).

[0027] According to this application, the thickness of the coating layer is 1-10 μm, for example 2-5 μm, such as 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm. The coating layer of the thickness can be obtained by coating once or by coating multiple times.

[0028] According to this application, if the diaphragm includes a diaphragm base layer and coating layers located on both sides of the diaphragm base layer, the thickness of the coating layers on both sides may be the same or different.

[0029] According to this application, the mixture further includes at least one of a polymeric binder and an additive. For example, the mixture further includes a polymeric binder and an additive.

[0030] According to this application, the mass fractions of each component in the mixture system are as follows:

[0031] 50-95 parts by weight of the above-mentioned ceramic particles, 5-40 parts by weight of polymer binder and 0-10 parts by weight of additives.

[0032] For example, the mass fractions of each component in the mixture are shown below:

[0033] 60-95 parts by weight of the above-mentioned ceramic particles, 10-30 parts by weight of polymer binder and 0-5 parts by weight of additives.

[0034] For example, the mass fraction of the ceramic particles is 50, 55, 60, 65, 70, 75, 80, 85, 90 or 95 parts by mass.

[0035] For example, the polymer adhesive is present in parts by weight of 5, 6, 7, 8, 9, 10, 15, 20, 25, 30, 35 or 40 parts by weight.

[0036] For example, the mass fraction of the above-mentioned adjuvant is 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10 parts by mass.

[0037] Specifically, the mass ratio of the shell to the core can generally be (20-100):200.

[0038] According to this application, the mixed system further includes 100-5000 parts by mass of solvent, for example, 500-2000 parts by mass of solvent.

[0039] According to this application, the polymer binder is selected from polytetrafluoroethylene, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyimide, polyacrylonitrile, poly(meth)acrylate, aramid resin, poly(meth)acrylic acid, styrene-butadiene rubber (SBR), polyvinyl alcohol, polyvinyl acetate, carboxymethyl cellulose (CMC), sodium carboxymethyl cellulose (CMC-Na), carboxyethyl cellulose, polyacrylamide, phenolic resin, epoxy resin, waterborne polyurethane, ethylene-vinyl acetate copolymer, multi-component acrylic copolymer, lithium polystyrene sulfonate, waterborne silicone resin, nitrile-polyvinyl chloride blend, styrene-acrylic latex, pure styrene latex, etc., and one or more combinations of blends and copolymers derived from the aforementioned polymer modifications.

[0040] According to this application, the additive is selected from at least one of branched alcohols, triethyl phosphate, polyethylene glycol, fluorinated polyethylene oxide, polyethylene oxide, stearic acid, sodium dodecylbenzene sulfonate, sodium hexadecyl sulfonate, fatty acid glycerides, sorbitan fatty acid esters, and polysorbates.

[0041] According to this application, the solvent is selected from at least one of water, methanol, ethanol, acetone, N-methyl-2-pyrrolidone (NMP), chloroform, xylene, tetrahydrofuran, o-chlorobenzaldehyde, hexafluoroisopropanol, N,N-dimethylformamide, N,N-dimethylacetamide, butanone, and acetonitrile.

[0042] This application also provides a method for preparing the above-mentioned diaphragm, wherein the method includes the following steps:

[0043] (a) The above-mentioned ceramic particles, optionally polymer binder and optionally additives are added to a solvent and mixed to obtain a mixed slurry;

[0044] (b) The mixed slurry from step (a) is coated onto the surface of the diaphragm substrate and dried to obtain the diaphragm.

[0045] According to this application, in step (a), the mass parts of the ceramic particles, optionally the polymer binder, optionally the additives, and the solvent in the mixed slurry are as follows:

[0046] 50-95 parts by weight of the above-mentioned ceramic particles, 5-40 parts by weight of polymer binder, 0-10 parts by weight of additives and 100-5000 parts by weight of solvent.

[0047] For example, the mass fractions of each component in the mixture are shown below:

[0048] 60-95 parts by weight of the above-mentioned ceramic particles, 10-30 parts by weight of polymer binder, 0-5 parts by weight of additives and 500-2000 parts by weight of solvent.

[0049] According to this application, in step (b), the coating method is, for example, spraying, dip coating, gravure printing, extrusion coating, transfer coating, etc.

[0050] According to this application, in step (b), the porosity of the membrane base layer is 20%-80%, the thickness is 5μm-50μm, and the average pore size is D<80nm; the material system of the membrane base layer is selected from at least one of polyethylene, polypropylene, polyethylene terephthalate, polybutylene terephthalate, polystyrene, polynaphthalene system polymers, polyimide, polyamide, aramid, and poly(p-phenylenebenzodiazole).

[0051] This application also provides a lithium-ion battery, which includes the separator described above.

[0052] According to this application, such as Figure 3 As shown, the cell of the lithium-ion battery is composed of a positive electrode, a negative electrode, and the aforementioned separator stacked together; the lithium-ion battery also includes an electrolyte.

[0053] According to this application, the lithium-ion battery is a high-voltage lithium-ion battery.

[0054] The beneficial effects of this application are as follows: This application provides a separator and a high-voltage battery including the separator. This application achieves this by coating the surface of inorganic ceramic particles with a modified layer. This modified layer can adsorb transition metal ions precipitated from the electrode material, thereby preventing the formation of transition metal precipitates on the negative electrode surface and improving the battery's safety, rate performance, and cycle performance. Simultaneously, since the modified layer is coated on the surface of the inorganic ceramic particles, it does not significantly affect the battery's internal resistance, thus not reducing the battery's rate performance, low-temperature performance, and cycle performance. Furthermore, the inventors unexpectedly discovered that the introduction of the modified material can also achieve the adsorption of trace amounts of HF generated in the battery system. On the one hand, this can inhibit the dissolution of transition metal ions, stabilize the positive electrode surface structure, and improve battery performance; on the other hand, it can reduce the corrosion of the battery outer material by HF, improving battery safety performance. Attached Figure Description

[0055] Figure 1 : Schematic diagram of the modification reaction of ceramic particles in this application.

[0056] Figure 2 : Schematic diagram of the adsorption of transition metal ions by ceramic particles in this application.

[0057] Figure 3 : A schematic diagram of the cell structure of the lithium-ion battery of this application.

[0058] Figure 4 : Graph showing the battery cycle test results using the separators of Example 1 and Comparative Example 1.

[0059] Figure 5 Graph showing the battery rate test results using the separators of Example 1 and Comparative Example 1. Detailed Implementation

[0060] The preparation method of this application will be further described in detail below with reference to specific embodiments. It should be understood that the following embodiments are merely illustrative and explanatory of this application and should not be construed as limiting the scope of protection of this application. All technologies implemented based on the above content of this application are covered within the scope of protection intended by this application.

[0061] Unless otherwise specified, the experimental methods used in the following examples are conventional methods; unless otherwise specified, the reagents and materials used in the following examples are commercially available.

[0062] Example 1

[0063] Twenty parts of the modified material were dissolved in ethanol by stirring to form a mixed solution. 200 parts of aluminum oxide were added and stirred until homogeneous. The solvent in the mixture was removed by vacuum heating and drying technology to obtain particles of ceramic material coated with the modified material. The modified material was selected from 3-aminopropyltrimethoxysilane substituted with ethylenediaminetetraacetic acid.

[0064] The prepared ceramic particles have a shell made of a modified material containing 3-aminopropyltrimethoxysilane substituted with ethylenediaminetetraacetic acid, and a core made of aluminum oxide. The mass ratio of the shell to the core is 20:200, the thickness of the shell is 10 nm, and the average particle size of the ceramic particles is about 0.8 μm.

[0065] 80 parts of the ceramic particles prepared above, 20 parts of polyvinylidene fluoride-hexafluoropropylene and 2 parts of polyethylene glycol are added to 900 parts of N,N-dimethylacetamide and mixed evenly to obtain a mixed slurry. The mixed slurry is coated on the surface of the diaphragm base layer by microgravure and dried to obtain the diaphragm.

[0066] The diaphragm is a wet-process substrate diaphragm with a thickness of 9 μm, coated on one side with a coating thickness of 3 μm, and the total areal density of the diaphragm is 10.6 g / m³. 2 .

[0067] The above-mentioned separator is stacked with the positive and negative electrodes or wound to prepare lithium-ion battery cells. After baking, liquid injection, formation and packaging, a high-safety lithium-ion battery is obtained.

[0068] Example 2

[0069] Twenty parts of the modified material were dissolved in ethanol by stirring to form a mixed solution. 200 parts of boehmite were added and stirred until homogeneous. The solvent in the mixture was removed by vacuum heating and drying technology to obtain particles of ceramic material coated with the modified material. The modified material was selected from 3-aminopropyltrimethoxysilane substituted with hydroxyethyl ethylenediamine triacetic acid.

[0070] The prepared ceramic particles have a shell made of a modified material containing 3-aminopropyltrimethoxysilane substituted with hydroxyethyl ethylenediamine triacetic acid, and a core made of boehmite. The mass ratio of the shell to the core is 20:200, the thickness of the shell is 10 nm, and the average particle size of the ceramic particles is about 0.8 μm.

[0071] The preparation methods for the separator and lithium-ion battery are the same as in Example 1, except that the ceramic particles prepared above are used.

[0072] Example 3

[0073] Twenty parts of the modified material were dissolved in ethylene glycol by stirring to form a mixed solution. 200 parts of aluminum oxide were added and stirred until uniform. The solvent in the mixture was removed by vacuum heating and drying technology to obtain particles of ceramic material coated with the modified material. The modified material was selected from pyridine-substituted 3-aminopropyltrimethoxysilane.

[0074] The prepared ceramic particles have a shell made of a modified material containing pyridine-substituted 3-aminopropyltrimethoxysilane and a core made of alumina. The mass ratio of the shell to the core is 20:200, the thickness of the shell is 10 nm, and the average particle size of the ceramic particles is about 0.8 μm.

[0075] The preparation methods for the separator and lithium-ion battery are the same as in Example 1, except that the ceramic particles prepared above are used.

[0076] Example 4

[0077] Twenty parts of the modified material were dissolved in propylene glycol by stirring to form a mixed solution. 200 parts of aluminum oxide were added and stirred until uniform. The solvent in the mixture was removed by vacuum heating and drying technology to obtain particles of ceramic material coated with the modified material. The modified material was selected from imidazole-substituted 3-aminopropyltrimethoxysilane.

[0078] The prepared ceramic particles have a shell made of a modified material containing imidazole-substituted 3-aminopropyltrimethoxysilane and a core made of alumina. The mass ratio of the shell to the core is 50:200, the thickness of the shell is 20 nm, and the average particle size of the ceramic particles is about 0.9 μm.

[0079] The preparation methods for the separator and lithium-ion battery are the same as in Example 1, except that the ceramic particles prepared above are used.

[0080] Example 5

[0081] Twenty parts of the modified material were dissolved in propylene glycol by stirring to form a mixed solution. 200 parts of magnesium oxide were added and stirred until uniform. The solvent in the mixture was removed by vacuum heating and drying technology to obtain particles of ceramic material coated with the modified material. The modified material was selected from imidazole-substituted 3-aminopropyltrimethoxysilane.

[0082] The prepared ceramic particles have a shell made of a modified material containing imidazole-substituted 3-aminopropyltrimethoxysilane and a core made of magnesium oxide. The mass ratio of the shell to the core is 100:200, the thickness of the shell is 40 nm, and the average particle size of the ceramic particles is about 1.0 μm.

[0083] The preparation methods for the separator and lithium-ion battery are the same as in Example 1, except that the ceramic particles prepared above are used.

[0084] Example 6

[0085] The preparation of particles coated with modified ceramic materials is the same as in Example 1.

[0086] 60 parts of the ceramic particles prepared above, 40 parts of poly(meth)acrylate and 4 parts of polyethylene glycol are added to 900 parts of N,N-dimethylacetamide and mixed evenly to obtain a slurry. The slurry is then coated onto the surface of the diaphragm base layer using a microgravure plate and dried to obtain the diaphragm.

[0087] The diaphragm is a wet-process substrate diaphragm with a thickness of 9 μm, coated on one side with a coating thickness of 3 μm, and the total areal density of the diaphragm is 10.6 g / m³. 2 .

[0088] The above-mentioned separator is stacked with the positive and negative electrodes or wound to prepare lithium-ion battery cells. After baking, liquid injection, formation and packaging, a high-safety lithium-ion battery is obtained.

[0089] Example 7

[0090] The preparation of particles coated with modified ceramic materials is the same as in Example 1.

[0091] 95 parts of the ceramic particles prepared above and 5 parts of styrene-butadiene rubber were added to 900 parts of N-methyl-2-pyrrolidone (NMP), and after uniform mixing, a mixed slurry was obtained. The mixed slurry was coated on the surface of the diaphragm base layer by a microgravure plate, and after drying, the diaphragm was obtained.

[0092] The diaphragm is a wet-process substrate diaphragm with a thickness of 9 μm, coated on one side with a coating thickness of 3 μm, and the total areal density of the diaphragm is 10.6 g / m³. 2 .

[0093] The above-mentioned separator is stacked with the positive and negative electrodes or wound to prepare lithium-ion battery cells. After baking, liquid injection, formation and packaging, a high-safety lithium-ion battery is obtained.

[0094] Comparative Example 1

[0095] 80 parts of alumina ceramic particles, 20 parts of polyvinylidene fluoride-hexafluoropropylene and 2 parts of polyethylene glycol were added to 900 parts of N,N-dimethylacetamide and mixed evenly to obtain a slurry. The slurry was then coated onto the surface of the diaphragm substrate using a microgravure plate and dried to obtain the diaphragm.

[0096] The diaphragm is a wet-process substrate diaphragm with a thickness of 9 μm, coated on one side with a coating thickness of 3 μm, and the total areal density of the diaphragm is 10.6 g / m³. 2 .

[0097] The above-mentioned separator is stacked with the positive and negative electrodes or wound to prepare lithium-ion battery cells. After baking, liquid injection, formation and packaging, a high-safety lithium-ion battery is obtained.

[0098] Comparative Example 2

[0099] 20 parts of ceramic particles containing ethylenediaminetetraacetic acid, 80 parts of alumina, 20 parts of polyvinylidene fluoride-hexafluoropropylene, and 2 parts of polyethylene glycol were added to 900 parts of N,N-dimethylacetamide. After uniform mixing, a slurry was obtained. The slurry was coated onto the surface of the membrane substrate using a microgravure plate and dried to obtain the membrane.

[0100] The diaphragm is a wet-process substrate diaphragm with a thickness of 9 μm, coated on one side with a coating thickness of 3 μm, and the total areal density of the diaphragm is 10.6 g / m³. 2 .

[0101] The above-mentioned separator is stacked with the positive and negative electrodes or wound to prepare lithium-ion battery cells. After baking, liquid injection, formation and packaging, a high-safety lithium-ion battery is obtained.

[0102] Test Example 1

[0103] The lithium-ion batteries prepared in Examples 1-7 and Comparative Examples 1-2 were subjected to voltage and internal resistance tests. The test process involved fully charging the lithium-ion batteries prepared in Examples 1-7 and Comparative Examples 1-2 and placing them in an environment of 25°C and 50% humidity. The voltage and internal resistance of the batteries under full charge were tested using a voltage and internal resistance meter (Ampere-Applent, model AT526B). The results are shown in Table 1.

[0104] Table 1. Voltage and internal resistance test results of lithium-ion batteries in Examples 1-7 and Comparative Examples 1-2.

[0105] Sample number Average voltage of lithium battery Internal resistance of lithium-ion batteries Example 1 4.2016V 12.18mΩ Example 2 4.2011V 12.32mΩ Example 3 4.2012V 11.98mΩ Example 4 4.2008V 12.21mΩ Example 5 4.2011V 11.97mΩ Example 6 4.2009V 11.87mΩ Example 7 4.2003V 12.05mΩ Comparative Example 1 4.2010V 12.36mΩ Comparative Example 2 4.2017V 18.35mΩ

[0106] Examples 1-7 involve applying modified ceramic material particles to separators and assembling them into lithium-ion batteries. According to the data in Table 1, the lithium-ion batteries prepared in Examples 1-7 and Comparative Examples 1-2 have normal voltages after sorting, but the internal resistance of Comparative Example 2 increases significantly. This is mainly because adding modified materials directly to the slurry affects the permeability of lithium ions.

[0107] The lithium-ion batteries prepared in Example 1 and Comparative Example 1 were subjected to charge-discharge cycle and rate performance tests. The charge-discharge cycle tests were conducted using a 1C charge / 1C discharge regime; the rate performance tests were conducted using a 0.2C charge / 0.2C, 0.5C, 1C, 3C, and 5C discharge regime. The results are as follows: Figure 4 and Figure 5 As shown, from Figure 4 and Figure 5 As can be seen, the battery of Example 1 not only maintains a good capacity retention rate in the later stage of cycling, but also maintains a good capacity retention rate under high-rate discharge.

[0108] By comparing the experimental results of Examples 1-7 and Comparative Examples 1-2, the following conclusions are drawn:

[0109] 1. Directly adding modified materials to the coating and applying them to lithium-ion battery separators will affect the permeability of lithium ions in the lithium-ion battery, leading to an increase in the internal resistance of the lithium-ion battery.

[0110] 2. The modified materials used in Examples 1-7 to coat ceramic particles and apply them to lithium-ion battery separators do not affect the internal resistance, voltage, or charge / discharge cycle of the lithium-ion battery, thus meeting application requirements.

[0111] Test Example 2

[0112] The lithium-ion battery separators prepared in Examples 1-7 and Comparative Examples 1-2 were subjected to metal ion testing. The testing process is as follows:

[0113] Take 100mm*100mm diaphragm sheets prepared in Examples 1-7 and Comparative Examples 1-2, place them in beakers containing 100mL of 0.1wt% CoCl2 aqueous solution, place the beakers on a heating plate at 150℃ for 30min, and after cooling, remove the diaphragms and perform ICP test analysis.

[0114] The ICP test results are as follows:

[0115] Sample number Co content (PPM) Example 1 177 Example 2 181 Example 3 183 Example 4 205 Example 5 227 Example 6 178 Example 7 182 Comparative Example 1 126 Comparative Example 2 183

[0116] The data above shows that the membrane with modified ceramic particles has a significantly improved adsorption capacity for metal ions.

[0117] Test Example 3

[0118] The lithium-ion batteries prepared in Example 1 and Comparative Example 1 were disassembled after cycling, and their separators and negative electrodes were subjected to ICP testing. The test results are as follows:

[0119] Sample number Diaphragm (ppm) Negative electrode (ppm) Example 1 1275 336 Comparative Example 1 267 1130

[0120] The data above shows that the membrane with modified ceramic particles has a significantly improved ability to adsorb metal ions, thus ensuring the cycle performance of the battery.

[0121] The embodiments of this application have been described above. However, this application is not limited to the above embodiments. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the protection scope of this application.

Claims

1. A separator for lithium-ion batteries, wherein, The diaphragm includes a diaphragm base layer and a coating layer located on at least one side surface of the diaphragm base layer, the coating layer being obtained by coating at least one side surface of the diaphragm base layer with a mixture system including ceramic particles; The material system of the diaphragm base layer is selected from at least one of polyethylene, polypropylene, polyethylene terephthalate, polybutylene terephthalate, polystyrene, polynaphthalene system polymers, polyimide, polyamide, aramid, and poly(p-phenylenebenzodiazole); The ceramic particles have a core-shell structure, that is, they include a shell and a core. The material forming the shell includes modified materials, and the material forming the core includes inorganic ceramic materials. The modified material is selected from substituted siloxanes, and the compound forming the substituent is selected from polyamine compounds containing at least two carboxyl groups, or from heterocyclic compounds containing one or two nitrogen atoms. The siloxane is selected from siloxanes containing an amino group, and the amino group is substituted by the substituent to obtain the substituted siloxane; The polyamine compound containing at least two carboxyl groups is selected from one or more of ethylenediaminetetraacetic acid, propylenediaminetetraacetic acid, hydroxyethyl ethylenediaminetriacetic acid, and ethylene glycol diethyl ether diaminetetraacetic acid; The heterocyclic compound containing one or two nitrogen atoms is selected from one or more of pyridine and imidazole.

2. The separator for lithium-ion batteries according to claim 1, wherein, The amino-containing siloxane is selected from one or more of 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 2-aminoethyltrimethoxysilane, and 2-aminoethyltriethoxysilane.

3. The separator for lithium-ion batteries according to claim 1 or 2, wherein, The inorganic ceramic material is selected from one or more of the following: alumina, magnesium oxide, boehmite, barium sulfate, barium titanate, zinc oxide, calcium oxide, silicon dioxide, silicon carbide, and nickel oxide. And / or, the shell is also referred to as a modified layer; And / or, the thickness of the shell layer is 5nm-1000nm; And / or, the average particle size of the inorganic ceramic material is 0.01μm-20μm.

4. The separator for lithium-ion batteries according to claim 1, wherein, The thickness of the coating layer is 1-10 μm; the coating layer of this thickness can be obtained by a single coating or by multiple coatings. When the diaphragm includes a diaphragm base layer and coating layers located on both sides of the diaphragm base layer, the thickness of the coating layers on both sides may be the same or different.

5. The separator for lithium-ion batteries according to claim 1 or 4, wherein, The mixture system also includes at least one of a polymer binder and an additive; The mass fractions of each component in the mixture are shown below: 50-95 parts by weight of inorganic ceramic particles, 5-40 parts by weight of polymer binder and 0-10 parts by weight of additives.

6. The separator for lithium-ion batteries according to claim 5, wherein, The mass fractions of each component in the mixture are shown below: 60-95 parts by weight of inorganic ceramic particles, 10-30 parts by weight of polymer binder and 0-5 parts by weight of additives; The mixture also includes 100-5000 parts by mass of solvent.

7. The method for preparing a separator for a lithium-ion battery according to any one of claims 1-6, wherein, The method includes the following steps: (a) The ceramic particles, optionally a polymer binder, and optionally an additive are added to a solvent and mixed to obtain a mixed slurry; (b) The mixed slurry from step (a) is coated onto the surface of the diaphragm substrate and dried to obtain the diaphragm.

8. The preparation method according to claim 7, wherein, In step (a), the mass parts of the inorganic ceramic particles, the optionally polymeric binder, the optionally additives, and the solvent in the mixed slurry are as follows: 50-95 parts by weight of inorganic ceramic particles, 5-40 parts by weight of polymer binder, 0-10 parts by weight of additives and 100-5000 parts by weight of solvent.

9. The preparation method according to claim 8, characterized in that, The mass fractions of each component in the mixture are shown below: 60-95 parts by weight of inorganic ceramic particles, 10-30 parts by weight of polymer binder, 0-5 parts by weight of additives and 500-2000 parts by weight of solvent.

10. A lithium-ion battery, the lithium-ion battery comprising the separator for a lithium-ion battery as described in any one of claims 1-6; The lithium-ion battery also includes a positive electrode, a negative electrode, and an electrolyte.

Citation Information

Patent Citations

  • Method for coating inorganic particles on lithium secondary battery substrate, and lithium secondary battery including substrate coated by the method

    CN104054195A

  • Anti-flaming ceramic modified size and lithium ion battery membrane coated with same

    CN106519742A

  • A preparation method of a coating modified ceramic separator for lithium ion battery

    CN109192903A