An aluminum material antioxidant composition, a preparation method and application thereof

By forming an anti-oxidation film on the surface of aluminum, the problems of easy corrosion and poor lubricity of aluminum are solved, achieving efficient cleaning and lubrication effects, and improving the corrosion resistance and surface finish of aluminum.

CN114644957BActive Publication Date: 2026-11-24HUNAN HENG JIA NEW MATERIALS TECHNOLOGY CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202210412851.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-04-19
Publication Date
2026-11-24
Estimated Expiration
2042-04-19

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

This invention relates to an anti-oxidation composition for aluminum materials, which, by mass concentration percentage, comprises the following components: 35-45% aluminum corrosion inhibitor; 5-8% synthetic ester; 12-17% emulsifier; 3-5% stabilizer; 8-12% cleaning agent; 0.5-1.5% mildew and corrosion inhibitor; 2-3% defoamer; and the balance being deionized water. This anti-oxidation composition can be used for online treatment of aluminum materials (including but not limited to aluminum or aluminum alloy rods, tubes, bars, and plates), forming an effective thin protective film on the aluminum surface. This not only improves the corrosion resistance of the aluminum but also enhances its surface lubrication, preventing problems such as adhesion of the tubes in subsequent processes. The anti-oxidation composition also has excellent cleaning properties, removing impurities or oil residues remaining on the aluminum surface from previous processing steps. It can be used as a cleaning solution during the winding of aluminum rods in continuous casting and rolling production, providing effective cleaning, lubrication, and anti-corrosion effects, and improving the surface smoothness and gloss of the aluminum rods.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of materials preparation technology, specifically relating to an anti-oxidation composition for aluminum materials, its preparation method, and its application. Background Technology

[0002] Due to its light weight and corrosion resistance, aluminum and aluminum alloys are among the most widely used and economical materials. Aluminum is a reactive metal, so an oxide film forms on its surface in the air to prevent corrosion. However, because this naturally formed oxide film is thin and not dense, long-term exposure to corrosive media or environments makes the aluminum surface highly susceptible to pitting corrosion. Therefore, anti-corrosion treatment of the aluminum surface is an important way to improve its corrosion resistance. Patent CN101775596B proposes a simple and rapid chromium-free passivation solution formula and process. This method can indeed improve the corrosion resistance of aluminum tubes. However, this passivation solution only improves the corrosion resistance of the aluminum surface; it cannot clean the aluminum surface during production to remove impurities or oil residues from previous processing steps, nor can it increase the lubrication of the aluminum during processing. Only tubes with good lubricity will not stick during subsequent processing or feeding, which is beneficial for smooth process operation. Summary of the Invention

[0003] (a) Technical problems to be solved

[0004] In view of the above-mentioned technical problems, the technical objective of the present invention is to provide an anti-oxidation composition for aluminum materials. After aluminum materials are treated with this composition, they can obtain excellent corrosion resistance while also having a good cleaning effect on the surface of the aluminum materials and giving the cleaned aluminum materials excellent lubricity.

[0005] (II) Technical Solution

[0006] To achieve the above objectives, the main technical solutions adopted by the present invention include:

[0007] In a first aspect, the present invention provides an anti-oxidation composition for aluminum materials, comprising, by mass concentration percentage: 35-45% aluminum corrosion inhibitor; 5-8% synthetic ester; 12-17% emulsifier; 3-5% stabilizer; 8-12% cleaning agent; 0.5-1.5% mildew and corrosion inhibitor; 2-3% defoamer; and the balance being deionized water.

[0008] Preferably, the aluminum corrosion inhibitor is DX5830 aluminum corrosion inhibitor.

[0009] Preferably, the synthetic ester is one or more of polyol esters, diesters, and monoesters.

[0010] Preferably, the emulsifier is a nonionic emulsifier.

[0011] Preferably, the stabilizer is a metal soap stabilizer.

[0012] Preferably, the defoamer is an organosiloxane defoamer.

[0013] Secondly, the present invention provides a method for preparing an anti-oxidation composition for aluminum materials, the method comprising: mixing an aluminum corrosion inhibitor, a synthetic ester, an emulsifier, a stabilizer, a cleaning agent, a mildew and corrosion inhibitor, a defoamer, and deionized water in a specified amount to obtain the anti-oxidation composition for aluminum materials.

[0014] Thirdly, the present invention provides a lubricating and cooling process fluid for aluminum materials, wherein 1 part by weight of the antioxidant composition is diluted with 10-25 parts by weight of water to form a diluent.

[0015] Fourthly, the present invention also provides an aluminum processing method, wherein after the aluminum material is formed, the temperature of the lubricating and cooling process liquid is controlled at 40-55°C, and the aluminum material is passed through the lubricating and cooling process liquid at a speed of 70-90 m / min. A temperature of 40-55°C is beneficial for improving the emulsification effect of the antioxidant composition, increasing the adhesion of the antioxidant film, and shortening the film drying time.

[0016] Preferably, the aluminum material is immersed in the lubricating and cooling process liquid for 0.2-0.3 seconds, and is first scraped with a rubber scraper and then blown dry to form an anti-oxidation film with a thickness of 5-10 micrometers on the surface of the aluminum material.

[0017] The longer the dwell time, the thicker the oxide film on the aluminum surface, and the better its corrosion resistance. However, this needs to be matched with the equipment and the output speed of the aluminum production line. Since the anti-oxidation treatment of aluminum is done online, the output speed of the aluminum is almost fixed. Conventional anti-oxidation compositions are difficult to achieve good anti-oxidation treatment effects within 0.2-0.3 seconds. However, this invention fully meets this requirement. It can ensure that the oxide film on the aluminum surface has sufficient corrosion resistance thickness and corrosion resistance. The shorter the treatment time, the better the technical effect of the anti-oxidation composition.

[0018] The use of a rubber scraper with a certain degree of elasticity is mainly to ensure that the thickness of the antioxidant film on the aluminum surface is uniform, and then it can be dried with heated air.

[0019] (III) Beneficial Effects

[0020] This invention provides an anti-oxidation composition for aluminum materials, the main components of which are aluminum corrosion inhibitors, synthetic esters, and emulsifiers. It also includes various additives such as stabilizers, cleaning agents, mildew and corrosion inhibitors, and defoamers. The uses of this anti-oxidation composition include: First, improving the corrosion resistance of aluminum materials. Experiments have shown that aluminum materials treated with this anti-oxidation composition form a protective film on their surface during processing, making their corrosion resistance more than three times that of ordinary aluminum materials. Second, improving the surface lubrication properties of aluminum materials, while also cleaning away impurities or oil stains remaining on the surface of the aluminum materials from previous processing steps. Aluminum tubes treated with this anti-oxidation composition do not slip or stick together, preventing adhesion between tubes during automatic feeding. This anti-oxidation composition exhibits good stability, maintaining its properties and performance stability and effectiveness even after long-term use. It is not prone to odor, deterioration, or stratification, and is suitable for long-term transportation and storage at room temperature, offering good economic benefits.

[0021] This invention relates to an anti-oxidation composition for aluminum materials, primarily used for: ① cleaning solutions during the winding of aluminum rods in continuous casting and rolling processes, providing effective cleaning, lubrication, and corrosion resistance, significantly improving the surface finish and gloss of the aluminum rods. ② Surface wetting or spraying before winding extruded aluminum tubes, forming an effective protective film on the aluminum tube surface, effectively improving the surface quality of the aluminum tube, and facilitating the subsequent winding process. ③ Surface cleaning and corrosion resistance for aluminum rods or plates.

[0022] The aluminum materials used in this application include, but are not limited to, aluminum or aluminum alloy rods, tubes, bars, and plates. Detailed Implementation

[0023] To better explain and facilitate understanding of the present invention, the present invention will be described in detail below with reference to specific embodiments.

[0024] This invention provides an anti-oxidation composition for aluminum materials, which, by mass concentration percentage, comprises the following components: 35-45% aluminum corrosion inhibitor; 5-8% synthetic ester; 12-17% emulsifier; 3-5% stabilizer; 8-12% cleaning agent; 0.5-1.5% mildew and corrosion inhibitor; 2-3% defoamer; and the balance being deionized water.

[0025] In improving the corrosion resistance of aluminum or aluminum alloys, the invention primarily works by forming a 5-10 micrometer-thick anti-oxidation film on the aluminum surface through the combined action of aluminum corrosion inhibitors, anti-mold and anti-corrosion agents, and stabilizers. Regarding improving the lubrication performance of aluminum surfaces, the invention mainly utilizes synthetic greases and emulsifiers to form an anti-oxidation film on the aluminum surface, enhancing corrosion resistance while also improving lubrication. In terms of cleaning performance, the invention primarily relies on the combined action of cleaning agents, defoamers, and anti-mold and anti-corrosion agents.

[0026] The aluminum corrosion inhibitor mentioned is DX5830. DX5830 is a novel, environmentally friendly aluminum alloy corrosion inhibitor that is free of phosphorus, silicon, nitrogen, and boron, and is a multi-acid type. It is easily soluble in water, and its aqueous solution is alkaline. It has a good corrosion inhibition effect on aluminum alloys in both weak acid and strong alkali systems. It can be used as an aluminum alloy corrosion inhibitor additive in metalworking fluids and water-based cleaning agent systems to prevent problems such as blackening, graying, loss of gloss, and discoloration of aluminum under alkaline conditions. In the antioxidant composition, the aluminum corrosion inhibitor component content is 35-45%. Excessive concentration will affect the emulsification effect and increase the difficulty of cleaning. Furthermore, excessively increasing the amount of aluminum corrosion inhibitor will not increase the corrosion resistance of the aluminum, while insufficient concentration will result in insufficient oxide film thickness, thus reducing the corrosion resistance of the aluminum.

[0027] Synthetic esters are produced by the esterification and dehydration of fatty acids and fatty alcohols under the action of a catalyst. Depending on the types of fatty acids and fatty alcohols involved, synthetic esters can be classified as polyol esters, diesters, monoesters, etc. Generally, synthetic esters possess the following superior properties: high viscosity index, high flash point, low pour point, good low-temperature fluidity, wider operating temperature range, low evaporation loss, good high-temperature stability, good oxidation stability, low carbon residue, excellent lubrication performance, extremely low toxicity, and good environmental and biodegradability. Synthetic esters can be prepared by mixing monoesters, diesters, and polyol esters in a 1:1:1 mass ratio. Synthetic esters are a superior component of crude oil. Through chemical reactions and controlled manipulation, they achieve a desired molecular structure with a well-organized molecular arrangement, exhibiting strong resistance to external variables. Their thermal stability, antioxidant properties, and viscosity resistance are superior to mineral oils. Preferably, the synthetic ester is one or more of trihydroxypropane oleate, pentaerythritol oleate, and tetrameric castor oil oleate.

[0028] The emulsifier is a nonionic emulsifier, which does not generate ions in aqueous solution and has a certain degree of resistance to hard water. Most nonionic emulsifiers are in liquid or slurry state, and their solubility in water decreases with increasing temperature. They possess excellent washing, dispersing, emulsifying, wetting, solubilizing, leveling, and anti-corrosion properties. In the antioxidant composition, the emulsifier content is 12-17%. Excessive emulsifier concentration will accelerate the volatilization of the antioxidant composition, causing a rapid decrease in concentration, thus shortening the solution's lifespan and increasing production costs. Conversely, insufficient concentration will result in poor emulsification, affecting the formation and uniformity of the antioxidant film. The nonionic emulsifier is at least one of the following: sorbitan monooleate (Span-80), polyoxyethylene sorbitan monostearate (Tween-61), polyoxyethylene dehydrated sorbitan monooleate (Tween-80), fatty alcohol polyoxyethylene ether (AEO-9), isomeric tridecyl alcohol polyoxyethylene ether, and polyoxyethylene monooleate (PEG400).

[0029] The stabilizer is a metal soap stabilizer, which slows down the reaction, maintains chemical equilibrium, reduces surface tension, and prevents photo-, thermal, or oxidative decomposition. In the antioxidant composition, the stabilizer content is 3-5%, primarily to ensure the stability of the solution concentration and the stability of the formed antioxidant film. Preferably, the metal soap stabilizer is at least one of barium stearate, barium laurate, calcium stearate, calcium laurate, zinc stearate, and zinc laurate. Metal soap stabilizers also possess lubricating properties. The metal soap can be a metal (lead, barium, cadmium, zinc, calcium, etc.) salt of fatty acids (lauric acid, stearic acid, naphthenic acid, etc.), with stearates being the most commonly used. Preferably, non-toxic and non-polluting stabilizers such as calcium stearate, calcium laurate, zinc stearate, or zinc laurate are preferred.

[0030] The main function of the cleaning agent is to reduce the surface tension of water and improve the cleaning effect. In the antioxidant composition, the cleaning agent dosage is 8-12%; too high a concentration increases production costs and makes waste liquid treatment more difficult, while too low a concentration will affect the cleaning effect on the aluminum surface, thus reducing the adhesion of the antioxidant film. The cleaning agent can be water-based, semi-aqueous, or non-aqueous. Various commercially available brands of metal dirt cleaners or metal surface cleaners are available, such as Hill, Rockwell, Guangdong Haoyang, Shanghai Lanfei, etc.

[0031] The main function of antifungal and preservative agents is to inhibit the growth and reproduction of microorganisms, thereby extending the shelf life of goods. In antioxidant compositions, the optimal concentration of antifungal and preservative agents is 0.5-1.5%; too low a concentration will reduce the shelf life and service life of the solution. Antifungal and preservative agents can be inorganic or organic. Inorganic antifungal agents can be antibacterial agents containing metal ions such as silver, copper, and zinc, and metal oxides (such as titanium dioxide and zinc oxide). Organic antifungal agents mainly include phenolic compounds (substituted aromatic hydrocarbons), organometallic compounds, nitrogen-containing organic compounds, halogenated organic compounds, and sulfur-containing organic compounds.

[0032] The defoamer is an organosiloxane defoamer, whose main function is to eliminate bubbles in the composition. It reduces the surface tension of water, solutions, suspensions, etc., preventing foam formation, or reducing or eliminating existing foam, ensuring uniform contact and distribution of the composition with the aluminum surface. In the antioxidant composition, the dosage of defoamer is 2-3%. Excessive dosage will accelerate the evaporation of the solution, thus affecting the lubricity of the aluminum surface; insufficient concentration will reduce the fluidity of the solution, resulting in uneven thickness of the formed antioxidant film.

[0033] To further clarify the present invention and its technological advancements, the following description is provided in conjunction with specific embodiments and technical effects.

[0034] Example 1

[0035] This embodiment provides an aluminum anti-oxidation composition, which, by mass percentage concentration, comprises: 40% aluminum corrosion inhibitor DX5830, 6% trihydroxypropane oleate, 14% Tween-80, 4% calcium stearate, 10% cleaning agent, 1% organic mildew inhibitor, 3% organosiloxane defoamer, and the balance being deionized water.

[0036] Take 1 part by weight of the antioxidant composition and dilute it with 15 parts by weight of deionized water to prepare a lubricating and cooling process fluid. This fluid is then placed in a chute (300m in length) and the temperature is controlled at 40-55℃. During the process, aluminum material passes through the chute at a speed of 70-90 m / min. The aluminum material is immersed in the lubricating and cooling process fluid for 0.2-0.3 seconds. A 1mm thick elastic rubber is used to scrape the surface, followed by hot air drying, forming a 5-10 micrometer thick antioxidant film on the aluminum material's surface.

[0037] The effects of this antioxidant composition on aluminum materials are as follows:

[0038] (1) Corrosion resistance: Aluminum materials treated with the antioxidant composition of Example 1 and untreated aluminum materials were subjected to an artificial atmosphere corrosion test, i.e., a salt spray test, according to the national standard GB / T10125. The results showed that the time for corrosion spots to appear on the surface of untreated aluminum materials in the salt spray test was 240 hours, while the time for corrosion spots to appear on the surface of aluminum materials treated with the antioxidant composition was no less than 720 hours. Therefore, the corrosion resistance of aluminum materials treated with the antioxidant composition is more than three times that of ordinary aluminum materials.

[0039] (2) Lubrication performance: By touch and visual observation, the aluminum material treated with the antioxidant composition of Example 1 can be felt to have a thin oil film on the surface of the aluminum material. It can be observed by the naked eye that the aluminum tubes slip and do not stick together during the production line process, and the aluminum material does not stick together with each other during the automatic feeding process.

[0040] (3) Cleaning performance: By visual inspection, the aluminum materials treated with the antioxidant composition of Example 1 have a clean, smooth and shiny surface, without any impurities or oil stains left over from the previous processing steps.

[0041] Examples 2-6

[0042] Examples 2-6 each provide an anti-oxidation composition for aluminum materials, the ingredients of which are shown in the table below (any fraction less than 100% is made up with water):

[0043]

[0044] To further illustrate the technical effects of the present invention, the following comparative examples are also provided.

[0045] Comparative Example 1

[0046] This comparative example is based on Example 1, without the addition of synthetic esters, and the corresponding percentages are replaced with an equal amount of water.

[0047] Comparative Example 2

[0048] This comparative example is based on Example 1, without the addition of emulsifier, and the corresponding percentages are replaced with an equal amount of water.

[0049] Comparative Example 3

[0050] This comparative example is based on Example 1, without the addition of stabilizers, and the corresponding percentages are replaced with an equal amount of water.

[0051] Comparative Example 4

[0052] This comparative example is based on Example 1, but the proportion of aluminum corrosion inhibitor DX5830 is increased to 50%.

[0053] Following the same method as in Example 1, 1 part by weight of the antioxidant composition was diluted with 15 parts by weight of deionized water to prepare a lubricating and cooling process fluid, which was then used to process the formed aluminum material online.

[0054] The performance of the antioxidant compositions of Examples 2-6 and Comparative Examples 1-4 is compared as follows:

[0055]

[0056] In summary, Examples 1-6 of this invention can enhance the corrosion resistance and surface lubrication properties of aluminum materials, while also removing impurities or oil residues remaining on the aluminum surface from previous processing steps. Aluminum tubes treated with the anti-oxidation composition of this invention slip against each other without sticking, preventing adhesion between tubes during automatic feeding. Furthermore, the anti-oxidation compositions prepared in Examples 1-6 exhibit good stability, maintaining their properties and performance stability and effectiveness even after prolonged use. They are not prone to odor, deterioration, or stratification, and are suitable for long-term transportation and storage at room temperature, offering good economic benefits.

[0057] However, Comparative Examples 1-3 exhibited problems such as poor lubrication performance and poor storage stability due to the lack of synthetic esters, emulsifiers, and stabilizers. Furthermore, the lack of emulsifiers and stabilizers weakened the effect of the antioxidant composition on enhancing the corrosion resistance of the aluminum; simultaneously, the storage performance of the antioxidant composition lacking emulsifiers and stabilizers also deteriorated. In Comparative Example 4, the excessively high proportion of DX5830 increased the difficulty of cleaning, leaving a heavy hazy residue after cleaning, making it difficult to thoroughly clean and resulting in a dull aluminum surface.

[0058] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A lubricating and cooling process fluid for aluminum materials, characterized in that, This product is prepared by mixing 1 part by weight of an aluminum anti-oxidation composition with 10-25 parts by weight of water. The aluminum anti-oxidation composition, by mass concentration percentage, comprises the following components: DX5830 aluminum corrosion inhibitor 35-45%; synthetic ester 5-8%; emulsifier 12-17%; stabilizer 3-5%; cleaning agent 8-12%; mildew and corrosion inhibitor 0.5-1.5%; defoamer 2-3%; and the balance being deionized water. The synthetic ester is one or more of trihydroxypropane oleate, pentaerythritol ester, and tetrameric castor oil oleate. The emulsifier is a nonionic emulsifier. The stabilizer is a metal soap stabilizer. The defoamer is an organosiloxane defoamer. The lubricating and cooling process liquid is used to immerse aluminum material at 40-55℃ for 0.2-0.3 seconds. After immersion, the material is first scraped with a rubber and then dried with hot air, which can form an anti-oxidation film with a thickness of 5-10 micrometers on the surface of the aluminum material.

2. A method for anti-oxidation processing of aluminum materials, characterized in that, include: The temperature of the lubricating and cooling process fluid as described in claim 1 is controlled at 40-55℃. The aluminum material is passed through the lubricating and cooling process fluid at a speed of 70-90m / min, so that the immersion time of the aluminum material in the lubricating and cooling process fluid is 0.2-0.3 seconds. After the aluminum material is removed, it is first scraped with a rubber and then dried with hot air to form an anti-oxidation film with a thickness of 5-10 micrometers on the surface of the aluminum material. The aluminum material is a rod, tube, bar or plate of aluminum or aluminum alloy.

Citation Information

Patent Citations

  • Chromium-free passivation method of aluminum pipe for evaporator of refrigerator or freezer and passivation solution thereof

    CN101775596B

  • Chromium-free passivation method of aluminum pipe for evaporator of refrigerator or freezer and passivation solution thereof

    CN101775596A

  • Environmental-friendly water-based cutting fluid

    CN103361164A

  • Aluminum alloy aqueous environment-friendly cleaning agent and preparation method of same

    CN104818492A

  • Diester-type semisynthetic cutting fluid with high lubrication and high hard water resistance and preparation method thereof

    CN105647633A