Electronic assemblies and methods of manufacturing electronic assemblies
By using a combination of microporous inner and outer sealing films in multilayer ceramic capacitors, the problem of fluid permeation path is solved, effectively blocking fluid and improving the reliability and performance of electronic components.
Patent Information
- Application Number
- CN202111484827.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-12-18
- Filing Date
- 2021-12-07
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2041-12-07
AI Technical Summary
In the manufacturing process of existing multilayer ceramic capacitors, it is difficult to effectively block fluid penetration paths, leading to performance degradation and reliability issues in electronic components.
A combination structure of microporous inner sealing film and outer sealing film is adopted. A sealing film is formed on the surface and inside of the micro-substrate through a vapor phase deposition process to seal the micropores and prevent fluid penetration.
It effectively blocks fluid penetration, improves the reliability and performance stability of electronic components, prevents fluid from corroding and reacting with the dielectric layer, internal electrodes and external electrodes, and extends service life.
Smart Images

Figure CN114649145B_ABST
Abstract
Description
[0001] This application claims the benefit of priority to Korean Patent Application No. 10-2020-0178556, filed on December 18, 2020, with the Korean Intellectual Property Office, the disclosure of which is incorporated herein by reference in its entirety. Technical Field
[0002] This disclosure relates to an electronic component and a method for manufacturing the electronic component. Background Technology
[0003] In electronic components, multilayer ceramic capacitors (MLCCs) can be chip capacitors mounted on printed circuit boards of various electronic products (such as imaging devices (including liquid crystal displays (LCDs)), computers, smartphones, and mobile phones) for charging or discharging.
[0004] Multilayer capacitors are used as components in a variety of electronic devices because they offer small size, high capacitance, and ease of installation. Recently, as electronic device components have become increasingly miniaturized, the demand for miniaturized and high-capacitance multilayer capacitors has increased.
[0005] A multilayer capacitor may include: a plurality of dielectric layers and a plurality of inner electrodes arranged alternately, with the dielectric layers situated between the inner electrodes; and an outer electrode connected to the inner electrodes. The dielectric layers, inner electrodes, and outer electrodes are preferably tightly bonded to each other, but defects may occur in some cases. Such defects may become pathways for fluid permeation. Summary of the Invention
[0006] One aspect of this disclosure is to provide an electronic component in which the path of fluid permeation into the electronic component is blocked.
[0007] One aspect of this disclosure is to provide a method for manufacturing an electronic component, wherein the path of fluid permeation into the electronic component is blocked.
[0008] According to one aspect of this disclosure, an electronic component includes: a microbody comprising a body and an electrode layer, the body including a plurality of dielectric layers and a plurality of internal electrodes, the plurality of internal electrodes being disposed with a respective dielectric layer between the plurality of internal electrodes, the electrode layer being disposed on an outer surface of the body and connected to a portion of the plurality of internal electrodes; and a sealing film. The microbody includes a first micropore extending through a surface of the microbody in at least a portion of the dielectric layers, the internal electrodes, and the electrode layers. The sealing film includes an inner sealing film disposed in at least a portion of the internal space of the first micropore to seal the first micropore.
[0009] According to another aspect of this disclosure, an electronic component includes: a body including a plurality of dielectric layers and a plurality of internal electrodes, the plurality of internal electrodes being disposed with a respective dielectric layer between the plurality of internal electrodes; an external electrode including an electrode layer and a plating layer, the electrode layer being disposed on the body and connected to a respective internal electrode, the plating layer being disposed on the electrode layer; and an external sealing film disposed on an interface surface between an end of the electrode layer and the body.
[0010] According to another aspect of this disclosure, a method of manufacturing an electronic component includes: providing a microbody comprising a body and an electrode layer, the body comprising a plurality of dielectric layers and a plurality of internal electrodes, the plurality of internal electrodes being configured such that a respective dielectric layer is disposed between the plurality of internal electrodes, the electrode layers being disposed on an outer surface of the body and connected to a portion of the plurality of internal electrodes; forming a sealing film on the microbody by a vapor deposition process; and removing at least a portion of the sealing film. Attached Figure Description
[0011] The above and other aspects, features and advantages of this disclosure will be more clearly understood by taking into account the accompanying drawings and the following detailed description, in which:
[0012] Figure 1 This is a perspective view showing an electronic component according to an example embodiment;
[0013] Figure 2 It is shown Figure 1 An exploded 3D view of the electronic components in the image;
[0014] Figure 3 It is shown Figure 1 An exploded perspective view of the main body of the electronic components;
[0015] Figure 4 It is along Figure 1 A cross-sectional view taken from line IV-IV′ in the diagram;
[0016] Figure 5 This is a cross-sectional view showing a portion of the microbody prior to the formation of the sealing film according to an example embodiment;
[0017] Figure 6 It is a diagram showing the state of a micro-matrix, including open micropores, exposed to fluid;
[0018] Figure 7 It is a diagram showing the state of a micro-matrix, including closed micropores, exposed to fluid;
[0019] Figure 8 This is a cross-sectional view showing a portion of the structure in which a sealing film is formed on the microbody;
[0020] Figure 9 This is a diagram showing a microbody exposed to fluid, in which a sealing film is formed in an open micropore;
[0021] Figures 10 to 16 This is a cross-sectional view illustrating the process of manufacturing an electronic component according to an example embodiment, wherein, Figure 12 This is a diagram illustrating the process of forming a sealing film for an electronic component according to an example embodiment. Figure 14 This is a cross-sectional view showing the growth direction of the sealing film;
[0022] Figure 17 This is a cross-sectional view showing the inner sealing film of an electronic component according to an example embodiment;
[0023] Figure 18 This is a cross-sectional view illustrating a method for forming a coating in open micropores using a wet process; and
[0024] Figure 19 This is a cross-sectional view showing an electronic component according to another example embodiment. Detailed Implementation
[0025] In the following description, embodiments of the present disclosure will be described with reference to the accompanying drawings.
[0026] However, this disclosure may be exemplified in many different forms and should not be construed as being limited to the specific embodiments set forth herein. Rather, these embodiments are provided so that this disclosure will be thorough and complete, and will fully convey the scope of this disclosure to those skilled in the art. Accordingly, for clarity of description, the shape and size of the elements in the drawings may be exaggerated, and in the drawings, elements indicated by the same reference numerals are the same elements.
[0027] A construction in which an element or layer is described as being disposed "on" another element or layer can include the following constructions: a construction in which other layers or other elements are located between the element or layer and the other element or layer, and a construction in which the element or layer is disposed directly on the other element or layer. A construction in which an element is described as being "directly on" indicates that no other elements or other layers are located between the element or layer and the other element or layer.
[0028] The spatial relative terms "below," "below," "lower," "above," and "upper" can be used to easily describe the relationship between elements. In addition to including the orientation shown in the figures, spatial relative terms can also include different orientations of the elements during use or operation. For example, when the elements shown in the figures are inverted, an element described as "below" or "below" another element can be placed "above" another element. Therefore, the example term "below" can include both "below" and "above" orientations. Elements can be oriented in other directions, and thus spatial relative terms can be interpreted according to orientation.
[0029] The terms “first,” “second,” etc., may be used to describe various elements and / or parts, but the elements and / or parts are not limited by these terms. These terms are used only to distinguish one element or part from another. Therefore, in the example embodiment, the first element or first part mentioned below may be a second element or second part.
[0030] Figure 1 This is a perspective view showing an electronic component according to an example embodiment. Figure 2 It is shown Figure 1 An exploded 3D view of the electronic components. Figure 3 It is shown Figure 1 An exploded 3D view of the main body of the electronic components. Figure 4 It is along Figure 1 The cross-sectional view taken from line IV-IV′ in the diagram.
[0031] Reference Figures 1 to 4 The electronic component 100 may include a first internal electrode and a second internal electrode separated from each other, and a dielectric layer between the first internal electrode and the second internal electrode. A plurality of first internal electrodes and a plurality of second internal electrodes may be provided, and the plurality of first internal electrodes and the plurality of second internal electrodes may be stacked alternately on top of each other. The dielectric layer may be disposed between the internal electrodes. The plurality of first internal electrodes, the plurality of second internal electrodes, and the dielectric layer may form a multilayer capacitor. The construction of the electronic component 100 will be described in more detail in the following description.
[0032] The electronic component 100 may include a main body 110, a first external electrode 161, and a second external electrode 162.
[0033] The main body 110 may have, for example, a hexahedral shape. For example, as... Figure 2As shown, the body 110 may include six surfaces M1, M2, F1, F2, C1, and C2. The first surface M1 and the second surface M2 may be opposite each other in a third direction T (or in the thickness direction of the body 110 or the electronic component 100). When the electronic component 100 is mounted on a substrate, the first surface M1 or the second surface M2 may be a surface mounted on the substrate (mounting surface). The third surface F1 and the fourth surface F2 may be opposite each other in a second direction W (or in the width direction of the body 110 or the electronic component 100). The third surface F1 and the fourth surface F2 may be connected to the first surface M1 and the second surface M2. The fifth surface C1 and the sixth surface C2 may be opposite each other in a first direction L (or in the length direction of the body 110 or the electronic component 100). The fifth surface C1 and the sixth surface C2 may be connected to the first surface M1, the second surface M2, the third surface F1, and the fourth surface F2.
[0034] like Figure 3 As shown, the main body 110 may include a plurality of dielectric layers 111, a plurality of first internal electrodes 121, and a plurality of second internal electrodes 122. In other words, the plurality of dielectric layers 111 may be stacked, and the plurality of first internal electrodes 121 and the plurality of second internal electrodes 122 may be alternately arranged with the dielectric layer 111 located between the first internal electrodes 121 and the second internal electrodes 122.
[0035] Multiple dielectric layers 111 can be in a sintered state and can be integrated, making the boundaries between adjacent layers difficult to identify.
[0036] The dielectric layer 111 may comprise a ceramic material having a high dielectric constant, and may include, for example, barium titanate (BaTiO3) powder or strontium titanate (SrTiO3) powder, but exemplary embodiments are not limited thereto. In other words, any material that can achieve sufficient electrostatic capacitance can be used as the material of the dielectric layer 111. Furthermore, ceramic additives, organic solvents, plasticizers, binders (e.g., organic binders), and dispersants may be selectively added to the dielectric layer 111 along with the ceramic powder. Ceramic additives may include transition metal oxides or transition metal carbides, rare earth elements, magnesium (Mg), or aluminum (Al), but examples of ceramic additives are not limited thereto.
[0037] Multiple first internal electrodes 121 may be stacked with multiple second internal electrodes 122 in a third direction T (or in the thickness direction of the body 110), and the stacked area may be related to the formation of the capacitance of the capacitor.
[0038] The first internal electrode 121 and the second internal electrode 122 may include nickel (Ni). The first internal electrode 121 and the second internal electrode 122 include nickel as the main component and may also include additives. For example, at least one material selected from the group consisting of Li, Na, and K may be used as an additive to improve the conductivity of the internal electrodes 121 and 122 by reducing the formation of nickel oxide (NiO). Furthermore, to improve the reliability of the internal electrodes 121 and 122, at least one material selected from the group consisting of Sn, Cu, Ag, Pt, Rh, Ir, Ru, Os, In, Ga, Zn, Bi, and Pb may be used as an additive. Additionally, to uniformly form the composition at the interface surfaces of the internal electrodes 121 and 122, at least one material selected from the group consisting of Ba, Mg, Dy, and Ti may be used as an additive.
[0039] like Figure 4 As shown, a plurality of first inner electrodes 121 may be exposed on (or in contact with or extending from) the fifth surface C1, and may be electrically connected to the first outer electrode 161. A plurality of second inner electrodes 122 may be exposed on (or in contact with or extending from) the sixth surface C2, and may be electrically connected to the second outer electrode 162. When a voltage is applied to the first outer electrode 161 and the second outer electrode 162, charge may accumulate between the opposing first inner electrodes 121 and the second inner electrode 122.
[0040] The main body 110 may further include a lower cover layer 111L, which is disposed below the lowermost inner electrode among the plurality of first inner electrodes 121 and the plurality of second inner electrodes 122. Furthermore, the main body 110 may also include an upper cover layer 111H, which is disposed above the uppermost inner electrode among the plurality of first inner electrodes 121 and the plurality of second inner electrodes 122. The lower cover layer 111L and the upper cover layer 111H may be sintered together with the plurality of dielectric layers 111 and may be integrated, making the boundaries between adjacent layers difficult to identify.
[0041] The lower cover layer 111L and the upper cover layer 111H can be formed by laminating a single dielectric layer 112 / 113 or two or more dielectric layers 112 / 113 in a third direction T (e.g., in the thickness direction of the body 110). The lower cover layer 111L and the upper cover layer 111H prevent physical / chemical stress from damaging the first inner electrode 121 and the second inner electrode 122. Furthermore, to eliminate mounting orientation, the thickness TL of the lower cover layer 111L and the thickness TH of the upper cover layer 111H can be configured to be the same, but exemplary embodiments are not limited thereto. The lower cover layer 111L or the upper cover layer 111H can have the same material and construction as the dielectric layer 111, but exemplary embodiments are not limited thereto.
[0042] In the example embodiment, the shape and size of the body 110, the number of stacked dielectric layers 111, the number of stacked first inner electrodes 121 / the number of stacked second inner electrodes 122, and the thickness TL of the lower cover layer 111L / the thickness TH of the upper cover layer 111H can be varied and are not limited to the example shown.
[0043] The first external electrode 161 may include a first connecting portion 161a, a first mounting portion 161b, and a first side portion 161c.
[0044] The first connecting portion 161a may be disposed on the fifth surface C1 of the body 110 and may be connected to a plurality of first internal electrodes 121 exposed on the fifth surface C1. The first connecting portion 161a may cover the entire fifth surface C1 of the body 110.
[0045] The first mounting portion 161b extends from the first connecting portion 161a to the first surface M1 and the second surface M2 of the body 110. The first mounting portion 161b partially covers the first surface M1 and the second surface M2 of the body 110.
[0046] The first side portion 161c may extend from the first connecting portion 161a to the third surface F1 and the fourth surface F2 of the body 110. The first side portion 161c may partially cover the third surface F1 and the fourth surface F2 of the body 110.
[0047] The first mounting portion 161b may be parallel to the plane formed by the first inner electrode 121, and the first side portion 161c may be perpendicular to the plane formed by the first inner electrode 121.
[0048] The first mounting portion 161b disposed on the first surface M1 of the main body 110 and the first mounting portion 161b disposed on the second surface M2 of the main body 110 may be symmetrical to each other in a third direction T with respect to the main body 110. For example, the length of the first mounting portion 161b disposed on the first surface M1 of the main body 110 in the first direction L (or the second direction W) may be the same as the length of the first mounting portion 161b disposed on the second surface M2 of the main body 110 in the first direction L (or the second direction W).
[0049] Similarly, the first side portion 161c provided on the third surface F1 of the body 110 and the first side portion 161c provided on the fourth surface F2 of the body 110 can be symmetrical to each other with respect to the body 110 in the second direction W. In other words, the length of the first side portion 161c provided on the third surface F1 of the body 110 in the first direction L (or the third direction T) can be the same as the length of the first side portion 161c provided on the fourth surface F2 of the body 110 in the first direction L (or the third direction T).
[0050] Similar to the first external electrode 161, the second external electrode 162 may include a second connecting portion 162a, a second mounting portion 162b, and a second side portion 162c.
[0051] The second connecting portion 162a may be disposed on the sixth surface C2 of the body 110 and may be connected to a plurality of second internal electrodes 122 exposed on the sixth surface C2. The second connecting portion 162a may cover the entire sixth surface C2 of the body 110.
[0052] The second mounting portion 162b extends from the second connecting portion 162a to the first surface M1 and the second surface M2 of the body 110. The second mounting portion 162b partially covers the first surface M1 and the second surface M2 of the body 110.
[0053] The second side portion 162c can extend from the second connecting portion 162a to the third surface F1 and the fourth surface F2 of the body 110. The second side portion 162c can partially cover the third surface F1 and the fourth surface F2 of the body 110.
[0054] The second mounting portion 162b may be parallel to the plane formed by the second inner electrode 122, and the second side portion 162c may be perpendicular to the plane formed by the second inner electrode 122.
[0055] The second mounting portion 162b disposed on the first surface M1 and the second mounting portion 162b disposed on the second surface M2 of the main body 110 are symmetrical to each other with respect to the main body 110 in the third direction T. The second side portion 162c disposed on the third surface F1 and the second side portion 162c disposed on the fourth surface F2 of the main body 110 are symmetrical to each other with respect to the main body 110 in the second direction W.
[0056] As described above, the first mounting portion 161b / second mounting portion 162b formed on the first surface M1 of the body 110 and the first mounting portion 161b / second mounting portion 162b formed on the second surface M2 of the body 110 can be symmetrical to each other, and the thickness TL of the lower cover layer 111L can be configured to be the same as the thickness TH of the upper cover layer 111H. Therefore, when the electronic component 100 is mounted on the substrate, mounting orientation can be eliminated. In other words, the electronic component 100 can be mounted such that the first surface M1 of the body 110 is opposite to the substrate, or such that the second surface M2 of the body 110 is opposite to the substrate.
[0057] One side of the main body 110 may be disposed in the first internal space IS1, and the other side of the main body 110 may be disposed in the second internal space IS2.
[0058] The first external electrode 161 may define a first internal space IS1. The first internal space IS1 may be defined by a first connecting portion 161a and a first mounting portion 161b and a first side portion 161c that bend from the first connecting portion 161a. The space surrounded by the first connecting portion 161a, the first mounting portion 161b and the first side portion 161c can be the first internal space IS1. Specifically, the first connecting portion 161a may have a rectangular shape, and the first mounting portion 161b / first side portion 161c may be bent vertically from each side of the first connecting portion 161a and may extend toward the second external electrode 162.
[0059] The second external electrode 162 may define a second internal space IS2. The second internal space IS2 may be defined by the second connecting portion 162a, the second mounting portion 162b bent from the second connecting portion 162a, and the second side portion 162c. The space surrounded by the second connecting portion 162a, the second mounting portion 162b, and the second side portion 162c can be the second internal space IS2. Specifically, the second connecting portion 162a may have a rectangular shape, and the second mounting portion 162b / second side portion 162c may be bent vertically from each side of the second connecting portion 162a and may extend toward the first external electrode 161.
[0060] Furthermore, the first external electrode 161 and the second external electrode 162 may be symmetrical with respect to the central portion of the main body 110.
[0061] For example, the first mounting portion 161b of the first external electrode 161 disposed on the first surface M1 of the main body 110 and the second mounting portion 162b of the second external electrode 162 disposed on the first surface M1 of the main body 110 are symmetrical to each other with respect to the main body 110 in the first direction L. Furthermore, the first side portion 161c of the first external electrode 161 disposed on the third surface F1 of the main body 110 and the second side portion 162c of the second external electrode 162 disposed on the third surface F1 of the main body 110 are symmetrical to each other with respect to the main body 110 in the first direction L. Furthermore, the first connecting portion 161a of the first external electrode 161 disposed on the fifth surface C1 of the main body 110 and the second connecting portion 162a of the second external electrode 162 disposed on the sixth surface C2 of the main body 110 are symmetrical to each other with respect to the main body 110 in the first direction L.
[0062] The fifth surface C1 and the sixth surface C2 of the main body 110 can be completely covered by the first external electrode 161 and the second external electrode 162, respectively, while the first surface M1, the second surface M2, the third surface F1 and the fourth surface F2 of the main body 110 can be partially exposed.
[0063] Each of the first external electrode 161 and the second external electrode 162 may include an electrode layer and a plating layer stacked sequentially.
[0064] The electrode layer 131 of the first external electrode 161 may be disposed on the entire fifth surface C1 of the body 110, and partially disposed on the first surface M1, second surface M2, third surface F1, and fourth surface F2 of the body 110. The electrode layer 132 of the second external electrode 162 may be disposed on the entire sixth surface C2 of the body 110, and partially disposed on the first surface M1, second surface M2, third surface F1, and fourth surface F2 of the body 110. The electrode layers 131 of the first external electrode 161 and 132 of the second external electrode 162 may be formed using substantially the same material and may have the same structure. Electrode layers 131 and 132 may include at least one conductive metal, such as copper (Cu), nickel, gold, silver, platinum, palladium, and alloys thereof, but exemplary embodiments thereof are not limited thereto. In addition, electrode layers 131 and 132 may also include glass as an auxiliary material. The conductive metal ensures the sealing properties of the sheet and the electrical connection between the sheets, and the glass can fill the empty space when the conductive metal is calcined and reduced, and can also provide the bonding force between the first external electrode 161 and the body 110.
[0065] A plating layer 151 may be disposed on the electrode layer 131 of the first external electrode 161, and a plating layer 152 may be disposed on the electrode layer 132 of the second external electrode 162. The plating layers 151 and 152 may be formed by electroplating based on the electrode layers 131 and 132 disposed below the plating layers 151 and 152. Therefore, the plating layers 151 and 152 may have a pattern shape that is substantially the same as the pattern shape of the electrode layers 131 and 132 disposed below the plating layers 151 and 152.
[0066] The plating 151 of the first external electrode 161 and the plating 152 of the second external electrode 162 may be formed using substantially the same material and may have the same structure. Platings 151 and 152 may include nickel (Ni) plating and / or tin (Sn) plating. Platings 151 and 152 may include a nickel / tin alloy. In an example embodiment, platings 151 and 152 may include two or more layers. For example, platings 151 and 152 may include a first plating layer formed on electrode layers 131 and 132 and comprising nickel, and a second plating layer formed on the first plating layer and comprising tin.
[0067] Electronic component 100 may include sealing films ST (inner sealing film ST_I and outer sealing film ST_O). The sealing film ST may be disposed on the surface of or within the structure including the body 110 and electrode layers 131 and 132, and may prevent fluid penetration into the structure. When the structure in which electrode layers 131 and 132 are formed on the body 110 (that is, the structure in electronic component 100 other than plating layers 151 and 152) is defined as a micro-body, the sealing film ST may be disposed on the surface and / or within the micro-body. The sealing film ST may include an outer sealing film ST_O disposed on the surface of the micro-body and an inner sealing film ST_I disposed within the micro-body.
[0068] An external sealing film ST_O may be disposed on a stepped portion STP formed by the body 110 and the ends of electrode layers 131 and 132 disposed on the body 110. The external sealing film ST_O may be disposed on the interface surface between the ends of electrode layers 131 and 132 and the body 110, and may cover this interface surface. The external sealing film ST_O may be disposed on a first surface M1, a third surface F1, a second surface M2, and a fourth surface F2 of the body 110 where the ends of electrode layers 131 and 132 are disposed. The external sealing film ST_O may be disposed continuously to completely surround the interface surface between the ends of electrode layers 131 and 132 and the body 110, but exemplary embodiments are not limited thereto. The external sealing film ST_O may be disposed intermittently. The thickness of the external sealing film ST_O (the maximum height measured vertically from the interface surface with the ends of electrode layers 131 and 132 or the body 110) may be from 20 nm to 200 nm, but exemplary embodiments are not limited thereto.
[0069] When the microbody includes micropores OP (open micropores OP_H and closed micropores OP_C) disposed within the microbody, an inner sealing film ST_I may be disposed within the micropores OP. The sealing film ST and the micropores OP of the microbody will be described in more detail below.
[0070] Figure 5 This is a cross-sectional view showing a portion of the microbody prior to the formation of a sealing film according to an example embodiment. Figure 5 In this context, the size and arrangement of microporous ops can be exaggerated. Furthermore, Figure 5 A portion of a first external electrode 161 in which an electrode layer 131 is disposed is shown, and the example shape shown can also be applied to a portion or other portion of a second external electrode 162 in which an electrode layer 132 is disposed.
[0071] Reference Figure 4 and Figure 5The microbody of the electronic component 100 may include micropores OP disposed within the microbody. In one example, OP may uniformly refer to the structures represented by OP_C and / or OP_H as shown in the accompanying drawings. The micropore OP may be defined as a space formed where adjacent materials are not fully bonded. The materials included in the microbody may be separated from each other based on the micropore OP. In other words, the micropore OP may form discontinuous portions of the material.
[0072] Microporous operating systems (OPs) can be empty spaces not occupied by solid material, providing space for fluids to reside or move. For example, a portion of an OP can be large enough to allow liquids (such as plating solutions) to pass through. Other portions of an OP can be relatively small enough that liquids cannot pass through while gases can.
[0073] Microporous OPs can be formed during the manufacturing process of micro-substrate. Microporous OPs can be formed intentionally for a specific purpose or unintentionally. For example, in manufacturing processes (such as sintering and calcination), it is desirable for the material forming the layer or electrode to completely fill the space and solidify or harden; however, due to various variables in the process conditions or limitations of the adopted process conditions, defects may exist where the material cannot fill local spaces. This defect can be present in the electronic assembly 100 in the form of microporous OPs. Furthermore, microporous OPs can be formed by cracks generated during the manufacturing or processing of the micro-substrate, or by cracks caused by external impacts.
[0074] Microporous operating surfaces (OPs) can have various shapes. For example, they can take the form of gaps, tunnels, pores, or pits with uniform or non-uniform widths, and can be raised between interfacial surfaces. Furthermore, microporous OPs can have island-like shapes (such as spherical, elliptical, and amorphous shapes) and connected linear shapes (such as straight lines, curves, forked shapes, or road shapes). Microporous OPs can be observed using field emission scanning electron microscopy (FE-SEM) images.
[0075] Microporous OPs can be placed at various locations within a microbody.
[0076] For example, microporous OPs can be disposed in specific components (such as electrode layer 131 or dielectric layer 111 or inner electrodes 121 and 122 of body 110). Specifically, components such as dielectric layer 111, inner electrodes 121 and 122, and electrode layer 131 can be disposed in a paste state and can be solidified or cured by sintering and / or calcination. The paste can be bonded and integrated in most areas by sintering and / or calcination, but in some cases, bonding may not occur in some areas, or the paste may bond and then re-separate. Unbonded areas can form microporous OPs.
[0077] As another example, micropores (OPs) can also be disposed on the interface surfaces between different components, such as the interface surface between dielectric layer 111 and inner electrodes 121 and 122, the interface surface between dielectric layer 111 and electrode layer 131, and the interface surface between inner electrode 121 and electrode layer 131. Furthermore, micropores (OPs) can be disposed on the interface surfaces of the same component, such as the interface surface between adjacent dielectric layers 111 formed of ceramic sheets. In the process of manufacturing micro-body components, different components can solidify in close contact. Materials can bond to each other on most interface surfaces, and no empty spaces can be created between materials. However, when materials are not bonded to each other on a portion of the interface surface (i.e., when a particular layer bulges from another layer), the corresponding spaces can form micropores (OPs).
[0078] The microvia OP of the electronic component 100 can be disposed at one or more locations selected from the various locations listed above. Furthermore, a continuously formed single microvia OP can be disposed at two or more locations listed above. For example, a portion of the microvia OP can extend through the dielectric layer 111 from the interface surface between the dielectric layer 111 and the inner electrodes 121 and 122 to the interface surface between the dielectric layer 111 and the electrode layer 131, and can extend through the electrode layer 131 and be open on the outer surface of the electrode layer 131.
[0079] Micro-orifice OPs can be classified according to whether they are open to the surface of the micro-substrate. The surface of the micro-substrate may include the surface of the electrode layer 131 and the surface of the subject 110, and in the area of the surface of the subject 110 covered by the electrode layer 131, the surface of the electrode layer 131 may become the surface of the micro-substrate.
[0080] Microvias OP can include: open microvias OP_H, in which a single microvia OP formed continuously in space is open to the surface of the microbody; and closed microvias OP_C, in which a single microvia OP formed continuously in space is not open to the surface of the microbody, and its entire space is closed. The distinction between closed and open types can be based on the microvia OP defined by the microbody. In other words, a microvia OP can be defined by at least a portion of the material of the body 110 (such as dielectric layer 111 or inner electrodes 121 and 122) and the material of the electrode layer 131. For example, when a microvia OP formed using components such as dielectric layer 111, inner electrodes 121 and 122, and electrode layer 131 is open from the surface of the body 110 or electrode layer 131, the opening can be a surface opening EN in relation to the microvia OP, even if the opening is blocked by a thin film or coating material, and therefore the microvia OP can be referred to as an open microvia OP_H.
[0081] Figure 6 It is a diagram showing the state of a micro-matrix, including open micropores, exposed to fluid. Figure 7 It is a diagram showing the state of a micro-matrix, including closed micropores, exposed to fluid.
[0082] Reference Figure 6 and Figure 7 The intermediate structure (e.g., micro-substrate) of electronic component 100 during the manufacturing process, or the surface of the manufactured electronic component 100, may be exposed to fluids. For example, the plating 151 of electronic component 100 may be formed by electroplating, but not limited to, immersing the electrode layer 131 in a plating solution, after forming the electrode layer 131 on the body 110. In this case, the micro-substrate (the intermediate structure of electronic component 100) may be exposed to the liquid plating solution. In addition to actively immersing the layer in a liquid as described above, electronic component 100 or its micro-substrate may be exposed to moisture or other gases in the atmosphere.
[0083] Because the closed micropore OP_C is not spatially connected to the surface of the micro-substrate (e.g. Figure 7 As shown), this prevents fluid from penetrating into the closed micropores OP_C. For open micropores OP_H, fluid can penetrate into the open micropores OP_H through the surface openings EN (e.g., Figure 6 (As shown). Fluid permeating into the microporous OP can enter the microbody along the extension direction of the microporous OP. The permeated fluid can contact the dielectric layer 111, internal electrodes 121 and 122 and / or electrode layer 131 surrounding the microporous OP, and can affect the contacted components. For example, when the permeating fluid is a plating solution, the plating solution can undergo electrochemical reactions with the internal electrodes 121 and 122 or electrode layer 131, and can change the characteristics of the electrodes. In addition, byproducts generated by the reaction (such as hydrogen gas) may expand in volume and may generate cracks in the microbody. Furthermore, the permeating fluid can react with the dielectric and can reduce the dielectric constant or generate byproducts. As described above, when the fluid comes into contact with components in the microbody, defects such as degradation of the characteristics of the electronic component 100 (e.g., breakdown voltage) or cracks may occur. Such defects may be caused by the plating solution or by moisture (e.g., water vapor or humidity) or other gases permeating into the microporous OP.
[0084] By using a sealing film ST to fill the open micropores OP_H to block the flow path of the fluid, fluid can be effectively prevented from penetrating through the open micropores OP_H.
[0085] Figure 8 This is a cross-sectional view showing a portion of the structure in which a sealing film is formed on the microbody. Figure 9 This is a diagram showing a microbody exposed to a fluid, in which a sealing film is formed in an open micropore.
[0086] Reference Figure 8 The electronic component 100 may include an inner sealing film ST_I and / or an outer sealing film ST_O. Figure 8 An example of forming both an inner sealing film ST_I and an outer sealing film ST_O is shown, but only the inner sealing film ST_I or only the outer sealing film ST_O may be included as the sealing film ST. Whether the inner sealing film ST_I is formed in the electronic component 100 that has undergone the process of forming the sealing film ST can be determined by whether the microbody includes an open micropore OP_H. Whether the outer sealing film ST_O is retained and the thickness of the outer sealing film ST_O can be determined based on the deposition thickness of the sealing film ST and the variables of the surface removal process. In one example, ST may uniformly refer to the structure represented by ST_O, ST_I, and / or ST_W shown in the figures.
[0087] An inner sealing membrane ST_I can be disposed within an open microorifice OP_H within a microorifice OP. The inner sealing membrane ST_I can at least partially fill the internal space of the open microorifice OP_H. For example, the inner sealing membrane ST_I can completely fill the internal space of the open microorifice OP_H. When the inner sealing membrane ST_I completely fills the internal space of the open microorifice OP_H, the empty space disappears, thus blocking the flow path of the fluid.
[0088] The inner sealing membrane ST_I can fill only a portion of the internal space of the open micropore OP_H. For example... Figure 9 As shown, the inner sealing film ST_I may not completely fill the internal space of the open micropore OP_H, and may define a void, which may be an empty space RM. By closing the opening of the open micropore OP_H adjacent to the surface to prevent fluid movement, the open micropore OP_H may be in the same state as the closed micropore OP_C in terms of fluid flow channels, thus preventing fluid from entering the open micropore OP_H from the surface.
[0089] An outer sealing film ST_O can be disposed on the interface surface between the end of electrode layer 131 and the body 110. The outer sealing film ST_O seals the interface surface between the end of electrode layer 131 and the body 110 and blocks the fluid flow path. When the open micropore OP_H extends to the interface surface between the body 110 and the electrode layer 131, the sealing film ST can grow into the open micropore OP_H. In this case, the outer sealing film ST_O and the inner sealing film ST_I can be connected to each other.
[0090] The sealing film ST can be deposited on the surrounding components (dielectric layer 111, inner electrodes 121 and 122, electrode layer 131) via a vapor deposition process and can be at least partially bonded to the surrounding components. Bonding may include chemical bonding. Compared to organic coatings formed through coating and curing processes, chemical bonding provides stronger adhesion to the surrounding components.
[0091] The sealing film ST can have crystallinity. Specifically, the sealing film ST can be fully or at least partially crystallized through a deposition process. Crystallized sealing film ST can form a mechanically stronger film than organic coatings formed by coating and curing processes, and can have better sealing properties, thereby effectively preventing fluid penetration.
[0092] The sealing film ST may include a waterproof material. The contact angle of the sealing film ST may be, for example, 90° to 110°, but its exemplary embodiments are not limited thereto. When the sealing film ST is waterproof, it effectively prevents fluids (such as plating solutions or moisture) from penetrating into the micro-body.
[0093] In an example embodiment, the sealing film ST may include fluorine. Specifically, the sealing film ST may include fluorine-based organic materials (such as, C...). x F y The average thickness of the sealing film ST can vary depending on the location of the sealing film ST, but the maximum thickness of the sealing film ST can be adjusted in the range of 20 nm to 200 nm. The maximum thickness can be measured by, for example, an optical microscope or a scanning electron microscope (SEM). Other methods and / or tools that are understood by those skilled in the art may be used, even if not described in this disclosure.
[0094] In the following description, the sealing film ST will be described in more detail while describing the method of manufacturing electronic component 100.
[0095] Figures 10 to 16 This is a cross-sectional view illustrating the process of manufacturing an electronic component according to an example embodiment.
[0096] Reference Figure 10 A micro-substrate comprising a body 110 and electrode layers 131 and 132 may be provided. The micro-substrate may be manufactured by forming the body 110 and forming electrode layers 131 and 132 on the body 110.
[0097] The body 110 can be formed using commonly used methods. For example, multiple ceramic green sheets can be prepared, and conductive paste can be applied to each ceramic green sheet using a printing method (such as screen printing or gravure printing). Multiple ceramic green sheets can be stacked, and the stacked ceramic green sheets and the conductive paste for the internal electrodes 121 and 122 can be compressed against each other by compression in the stacking direction. The compressed stack can be cut for each region corresponding to the body 110 of a single multilayer capacitor, thereby completing an unsintered body. Subsequently, a sintered and / or calcined body 110 can be obtained by heat-treating the body to burn off the binder and performing calcination in a reducing atmosphere.
[0098] Subsequently, electrode layers 131 and 132 may be formed on the body 110. Electrode layers 131 and 132 may be formed to provide electrical properties by applying a conductive paste or conductive epoxy resin to the body 110 and calcining it by performing a heat treatment, wherein the conductive paste or conductive epoxy resin comprises conductive material powder (such as at least one of copper (Cu), nickel, gold, silver, platinum, palladium, and alloys thereof) and glass powder.
[0099] As described above, the micro-substrate following the sintering and / or calcination of the body 110 and the electrode layers 131 and 132 may include micropores OP located within the micro-substrate. When multiple micro-substrates are manufactured, some micro-substrates may include micropores OP, and others may not include micropores OP. Some micro-substrates including micropores OP may include only closed micropores OP_C and not open micropores OP_H, and others may include only open micropores OP_H and not closed micropores OP_C. Still others of the micro-substrate including micropores OP may include both open micropores OP_H and closed micropores OP_C.
[0100] For microsubstrates without micropores OP or consisting only of closed micropores OP_C without open micropores OP_H, even when immersed in the plating solution during subsequent plating processes, plating solution penetration into the microsubstrates will not occur, thus eliminating the need for a process to form a sealing film ST to prevent fluid penetration. For microsubstrates including open micropores OP_H, a process to form a sealing film ST to prevent fluid penetration is preferred.
[0101] After fabricating the micro-substrate, if the presence of open micro-vias (OP_H) is identified through a process inspection, it would be efficient to perform the sealing film (ST) formation process only on micro-substrate containing open micro-vias (OP_H). However, due to the small size of the micro-substrate, it may be difficult to inspect for the presence of open micro-vias (OP_H), and the process cost may also be high. Furthermore, even when micro-substrate containing open micro-vias (OP_H) is identified, selectively selecting micro-substrate from a variety of micro-substrate is inefficient in terms of process. More precisely, by performing the sealing film (ST) formation process on all fabricated micro-substrate, without inspecting and selecting open micro-vias (OP_H), the overall process defect rate can be reduced, and efficiency can be improved. When a sealing film ST is formed on a microbody that does not include open micropores OP_H, only an outer sealing film ST_O can be formed without forming an inner sealing film ST_I. Since the outer sealing film ST_O can perform the function of preventing fluid from penetrating between the body 110 and the electrode layers 131 and 132 in the finished electronic component 100 and the plating process, the reliability of the electronic component 100 can be improved without any negative effects.
[0102] Therefore, the method of manufacturing electronic component 100 according to the example embodiment may include a process of forming a sealing film ST without performing a process of checking whether open micropores OP_H exist on the micro-substrate that has already undergone baking.
[0103] Reference Figure 11 The process for forming a sealing film (ST) can be performed using vapor deposition processes such as CVD, PECVD (or plasma deposition), PVD, ALD, etc. As an example, the process for forming a sealing film ST can be performed using PECVD, where the micro-substrate can be placed within a PECVD apparatus. For example, C... x F y Gases (such as C3F6) are used as source gases. When the deposition process is performed by forming plasma in a PECVD apparatus, C... x F y The material can be deposited on the surface of the micro-matrix.
[0104] The thickness of the sealing film ST can be related to the deposition direction. Generally, the thickness of the sealing film ST can be increased when the surface to be deposited is opposite to the electric field direction of the nozzle of the PECVD equipment and plasma generation apparatus. The microbody can have a cuboid shape. For example, when the second side of the microbody (the side corresponding to the second surface M2 of the microbody) is opposite to the nozzle of the PECVD equipment and the first side of the microbody (the side corresponding to the first surface M1 of the microbody) (the opposite side) is opposite to the ground, a sealing film ST of sufficient thickness can be formed on the second side, while a sealing film ST of smaller thickness can be formed on the surfaces of the microbody perpendicular to the second side, corresponding to the third surface F1, fourth surface F2, fifth surface C1, and sixth surface C2 of the microbody. When the first side of the microbody is in contact with components of the PECVD equipment, such as supports or seats, the sealing film ST may be formed very little on the first side.
[0105] While it is not determined on which surface of the microbody the open micropore OP_H will be open, preferably, a film of uniform thickness can be formed on all surfaces of the microbody to reliably seal the open micropore OP_H. One method for forming a uniform film is to perform the deposition process while changing the position of each surface (rather than fixing the relative surfaces of the microbody to the nozzle-facing position).
[0106] Figure 12 An example method for altering the surface to be deposited is shown in the figure. Figure 12 This is a diagram illustrating the process of forming a sealing film for an electronic component according to an example embodiment. Figure 12 A spin deposition process is illustrated, in which the deposition process is performed simultaneously while multiple micro-substrates rotate within a drum-type PECVD apparatus 200. (See diagram below.) Figure 12 As shown, when a micro-substrate is placed in a drum and a deposition process is performed while the drum is rotating, each surface of the micro-substrate can rotate regularly or randomly, thereby allowing deposition to be performed uniformly on all surfaces of the micro-substrate.
[0107] Reference Figure 13 C, the deposition material in the PECVD equipment x F yIt can be deposited on the microbody, can be bonded, can be grown in the thickness direction, and can be formed as a sealing film ST_W. The sealing film ST_W can be formed on the entire surface of the microbody, externally speaking. In other words, the sealing film ST_W can be formed on the electrode layers 131 and 132 and the exposed portions of the body 110 not covered by the electrode layers 131 and 132. The sealing film ST_W can be formed to cover the exposed surface (outer surface) of the body 110 and the entire surface (outer surface) of the exposed electrode layers 131 and 132. A step portion STP corresponding to the thickness of the electrode layers 131 and 132 can be defined between the ends of the electrode layers 131 and 132 and the body 110, and the sealing film ST_W can be conformally formed along the step portion STP.
[0108] The sealing film ST_W can have a uniform thickness across the entire surface of the micro-substrate. The thickness of the deposited sealing film ST_W can be adjusted by process time or condition control. The average thickness of the sealing film ST_W deposited on the micro-substrate can be determined within a range sufficient to fully seal the opening of the open micro-orifice OP_H. The thickness of the sealing film ST_W satisfying the above conditions can vary depending on the size of the open micro-orifice OP_H. However, based on experiments with multiple micro-substrates formed under general process conditions, when the average thickness of the sealing film ST_W is determined to be in the range of 20 nm to 200 nm, the degradation of the electronic component 100 caused by fluid permeation is reduced.
[0109] Figure 14 This is a cross-sectional view showing the growth direction of the sealing film. (Refer to...) Figure 14 In a PECVD apparatus, micromasses can be exposed to a vapor-deposited material. When the deposited material encounters the surface of the micromass, it can bond to the surface. The vapor-deposited material can contact and bond to the exposed outer surface of the micromass. Furthermore, since the vapor-deposited material can penetrate into the open micropores OP_H, it can contact and bond to the inner walls of the open micropores OP_H.
[0110] As the deposition process continues, the vapor-deposited material can contact and bond with the previously deposited material bound to the micromatrix. Through this process, a sealing film (ST) can be grown. For example... Figure 14 As shown, typically, the main growth direction of the sealing film ST can be perpendicular to the surface to be deposited.
[0111] On the outer surface of the micro-matrix, the sealing film ST_W can grow in an outward direction. Since there are no structures on the outer surface of the micro-matrix that could hinder growth, the sealing film ST_W can grow to a thickness corresponding to a predetermined thickness.
[0112] For open micropores OP_H, the sealing film ST_W can grow vertically from the inner wall. The sealing film ST_W can grow from the entire inner circumference of the inner wall of the open micropore OP_H towards the center of the open micropore OP_H.
[0113] As the sealed film ST_W grows in the open micropores OP_H, the empty space RM in the open micropores OP_H can be gradually reduced. Even as the size of the empty space RM decreases, as long as the space is retained, the vapor-deposited material can communicate with the interior and exterior of the open micropores OP_H through the empty space RM. Therefore, a separate film can be formed in the interior space of the region where the film is formed.
[0114] As the sealing film ST_W grows further within the open micropore OP_H, additional films can contact the relatively growing sealing film ST_W. During the deposition process, the conditions under which the sealing films ST_W growing in different directions on the inner wall of the open micropore OP_H can contact each other are related to the defined thickness of the films (relative to the thickness of the outer surface) and the minimum inner diameter of the open micropore OP_H. For example, assuming the film formation rate on the outer surface of the microbody is the same as the film formation rate in the open micropore OP_H, and the inner diameter of the open micropore OP_H is less than or equal to twice the defined thickness of the film, the sealing films ST_W growing in different directions on the inner wall of the micropore OP_H can contact each other. When the film formation rate in the open micropore OP_H is half the film formation rate on the outer surface, the condition that the inner diameter of the open micropore OP_H is less than the defined thickness of the film can be a necessary condition for the sealing film ST_W in the open micropore OP_H to contact the central portion. In other words, taking into account at least the size of the open micropore OP_H and the film formation rate in the open micropore OP_H, the thickness of the sealing film ST_W can be determined such that the open micropore OP_H can be sealed by the deposition process.
[0115] The sealing films ST_W that are in contact with each other can bond together at the joint. When the sealing films ST_W that grow opposite each other are completely bonded without any gaps, the space in the region can be sealed off. Therefore, even if vapor-deposited material subsequently enters the sealed region, no further film formation is required. When the empty space RM is retained in the sealed region during sealing, the internal empty space RM remains unchanged even when the deposition process continues thereafter. When the empty space RM connected to the opening of the open micropore OP_H is retained outside the sealed region during sealing, film formation can continue unless another opening is sealed.
[0116] Reference Figure 15After the process of forming the sealing film ST_W, a process for removing the sealing film ST_W can be performed. The process for removing the sealing film ST_W can be a process that at least partially removes the sealing film ST_W. The process for removing the sealing film ST_W can be performed to remove the sealing film ST_W disposed on electrode layers 131 and 132. Plating layers 151 and 152 can be formed on electrode layers 131 and 132, and when electrode layers 131 and 132 are covered by the sealing film ST_W, it may be difficult to perform the plating process smoothly. Furthermore, when the sealing film ST_W remains on electrode layers 131 and 132, the resistance between electrode layers 131 and 132 and the plating layers 151 and 152 disposed thereon may increase. Therefore, by removing the sealing film ST_W covering electrode layers 131 and 132 by this process, the subsequent plating process can be performed smoothly, and the increase in resistance between electrode layers 131 and 132 and plating layers 151 and 152 can be prevented.
[0117] The process of removing the sealing film ST_W can be performed while retaining the sealing film ST_W formed in the open micropore OP_H. However, if the sealing film ST_W formed in the open micropore OP_H is also removed, it may not prevent the plating solution from penetrating in subsequent plating processes. Therefore, a removal process can be selected that removes the sealing film ST_W formed on the outer surface of the microbody while simultaneously retaining the sealing film ST_W formed in the open micropore OP_H.
[0118] Dry polishing can be an example of a process for removing the sealing film ST_W that meets the above conditions. Mechanical (or physical) polishing can be an example of dry polishing. Mechanical polishing can be performed by physically separating the sealing film ST_W by colliding abrasive particles (ABR) with the micro-matrix on which the sealing film ST_W is formed.
[0119] Mechanical polishing can be performed in a drum. In other words, multiple micro-subjects with a sealing film ST formed on them can be placed in a drum, and abrasive particles ABR (or abrasive compound) can collide with the micro-subjects as the drum rotates. For drum polishing, the entire surface of the micro-subjects can be polished uniformly, and multiple micro-subjects can be polished simultaneously, thereby improving process efficiency. Besides drum polishing, various mechanical polishing processes commonly used in various fields (such as sandblasting) can be applied to the process of partially removing the sealing film ST_W.
[0120] Abrasive particle ABRs can be formed using inorganic materials (such as sand, glass, metal, or resins such as silicone), but exemplary embodiments are not limited thereto, and abrasive particle ABRs of various materials for mechanical polishing can be applied.
[0121] The shape of the abrasive particles ABR can be spherical, elliptical, etc., but its example embodiments are not limited to this, and various shapes such as amorphous shapes can be suitable as the shape of the abrasive particles ABR.
[0122] The size of the abrasive particles (ABR) can be 1 mm or smaller, but is not limited to this. In example embodiments, the diameter of the abrasive particles (ABR) can range from 0.5 mm to 0.8 mm. For example, in mechanical polishing processes, abrasive particles (ABR) with an average diameter of 0.7 mm or 0.6 mm can be used.
[0123] Polishing conditions, including polishing time, can be defined as conditions in which the entire sealing film ST_W formed on electrode layers 131 and 132 is removed and electrode layers 131 and 132 are exposed.
[0124] Figure 16 This is a cross-sectional view of a micro-substance that has undergone a process of partially removing the sealing film.
[0125] Reference Figure 16 Most of the sealing film formed on the outer surface of the microbody can be removed by a process that removes the sealing film, thus exposing the outer surface of the microbody. Since the abrasive particles ABR have no direct effect on the sealing film formed in the open micropores OP_H, the sealing film can be retained instead of being removed. The sealing film retained in the open micropores OP_H can become the aforementioned inner sealing film ST_I.
[0126] In the stepped portion STP between the ends of electrode layers 131 and 132 and the body 110, the side surfaces of electrode layers 131 and 132 can act as shields against abrasive particles (ABR). Furthermore, since the abrasive particles (ABR) have a predetermined size, the inner edge portion of the stepped portion STP, which has a relatively narrow width, is protected from physical impact by the abrasive particles (ABR). Therefore, despite mechanical polishing, the sealing film provided on the interface surface between the ends of electrode layers 131 and 132 and the body 110 does not need to be removed, and at least a portion of this sealing film can be retained. The sealing film ST_W retained on the interface surface between the ends of electrode layers 131 and 132 and the body 110 can become the aforementioned outer sealing film ST_O. The maximum thickness of the outer sealing film ST_O can be substantially the same as the formation thickness of the sealing film ST_W.
[0127] After the process of removing the sealing film, plating layers 151 and 152 can be formed on electrode layers 131 and 132, thereby forming a structure as shown in the figure. Figure 4The electronic component 100 shown. Coatings 151 and 152 can be formed by a plating process of immersing the micro-substrate in a plating solution. A process for removing the sealing film removes the sealing film from the outer surfaces of the electrode layers 131 and 132, exposing the outer surfaces of the electrode layers 131 and 132, allowing for the smooth formation of coatings 151 and 152. Furthermore, since the open micropores OP_H of the micro-substrate are sealed by the inner sealing film ST_I, plating solution is prevented from entering the micro-substrate through the open micropores OP_H. Additionally, since the outer sealing film ST_O is formed on the interface surface between the ends of the electrode layers 131 and 132 and the body 110, inward penetration of plating solution through the interface surface is prevented.
[0128] Depending on the shape and size of the open micropore OP_H and the process conditions used to form the sealing film, the aforementioned inner sealing film ST_I can be arranged in various forms within the open micropore OP_H. Figure 17 Several examples of the inner sealing film ST_I are shown.
[0129] Figure 17 This is a cross-sectional view showing the inner sealing film of an electronic component according to an example embodiment.
[0130] Figure 17 (a) shows the form in which the inner sealing film ST_I is completely filled in the open micropores OP_H. In the process of forming the sealing film ST, when the deposited material is uniformly diffused into the open micropores OP_H and grows sequentially from the inside, a form such as... Figure 17 The form shown in (a) above. When the inner sealing film ST_I completely fills the open micropores OP_H as described above, the inner sealing film ST_I can have high mechanical strength.
[0131] Figure 17 (b) illustrates an example where a predetermined portion, beginning with the surface opening EN of the open micropore OP_H, can be filled with an inner sealing film ST_I, thereby defining a closed region, while voids (empty spaces RM) can remain inside the closed region. When the opening is closed before the deposited material completely fills the internal space of the open micropore OP_H, a result such as... Figure 17 The inner sealing film ST_I is shown in (b) of the diagram.
[0132] Figure 17 (c) illustrates an example where two or more closed regions are formed such that two or more separate empty spaces RM remain within an open micropore OP_H. When the first closure is performed at a relatively deep location, and the second and third closures are performed sequentially at shallower locations, a result can be formed as shown in the example. Figure 17 The inner sealing film ST_I is shown in (c) of the diagram.
[0133] In such Figure 17 In the example shown in (a), the open micropore OP_H is completely filled by the inner sealing film ST_I, and in the example shown in (a), the open micropore OP_H is completely filled by the inner sealing film ST_I. Figure 17 In the examples shown in (b) and (c) where voids (empty spaces RM) are formed in the open micropores OP_H, the penetration of fluids (such as plating solutions) is prevented because the openings of the open micropores OP_H are closed. Furthermore, Figure 17 The voids included in (b) and (c) along with the closed micropores OP_C can alleviate the stress exerted by external impacts or expansion of the electronic component 100.
[0134] Since vapor deposition is used to form the inner sealing film ST_I in the above example embodiment, fluid permeation can be blocked by effectively sealing the openings of the open micropores OP_H. Compared with methods of forming coatings by wet methods, vapor deposition has advantages in terms of the reliability of blocking the openings of the open micropores OP_H, which will be described in more detail below.
[0135] Figure 18 This is a cross-sectional view illustrating a method for forming a coating in open micropores using a wet process. The method for forming a coating using a wet process may include the following steps: filling the open micropores OP_H (see [reference]) with an organic composition ORL as a coating composition. Figure 18 (a) in the text, and the drying and / or curing organic composition ORL (see also...). Figure 18 (b) in the middle.
[0136] Organic composition ORL can be provided in liquid form. The process of filling the organic composition ORL into open micropores OP_H can be performed by immersing the micro-mass in the liquid organic composition ORL. A drying and / or curing process is necessary to retain the organic composition ORL as an organic coating ORC. The liquid component of the organic composition ORL can be evaporated or volatilized through the drying and / or curing process, while the solid component can be retained, thereby forming the coating ORC. With the above process, the volume of the organic composition ORL can be reduced. Figure 18 As shown in (b), solid components may not remain in the openings of the open micropores OP_H, which can become channels for the evaporation of liquid components. In this case, although the deeper interior of the open micropores OP_H can be filled by the coating ORC, the surface openings EN can still remain open. Therefore, even after the formation of the coating ORC, the fluid permeation channels in the microbody may not be completely blocked.
[0137] exist Figure 17In the case of the internal sealing film ST_I shown, although an empty space RM is formed in the open micropore OP_H, at least the surface opening EN of the open micropore OP_H can be firmly closed. Therefore, improved sealing reliability can be obtained.
[0138] Figure 19 This is a cross-sectional view illustrating an electronic component according to another example embodiment. In the following description, the description of the electrode layer 131 and / or plating layer 151 of the first external electrode 161 also applies to the electrode layer 132 and / or plating layer 152 of the second external electrode 162.
[0139] Reference Figure 19 In the example embodiment, electronic component 101 and Figure 4 The difference in the example embodiment may be that the outer sealing film ST_O is not included, and the inner sealing film ST_I may be retreated a predetermined distance from the surface opening EN of the open micropore OP_H. The end of the inner sealing film ST_I may be located at a predetermined depth from the surface opening EN of the open micropore OP_H, and may form a closed portion at least in the located area. Therefore, fluid may penetrate into the recess defined by the open micropore OP_H and the inner sealing film ST_I, but further penetration into its internal space is prevented. The distance by which the inner sealing film ST_I retreats from the surface opening EN of the open micropore OP_H may be 100 nm or less, but the example embodiment is not limited to this. When the surface opening EN of the open micropore OP_H is located in the electrode layer 131, the coating 151 may fill the space retracted by the inner sealing film ST_I.
[0140] Figure 19 The electronic component 101 shown can be manufactured using the same method as in the example embodiments described above, but dry etching or wet etching can be used instead of the process of removing the sealing film (instead of dry polishing).
[0141] As an example of wet etching process, when... Figure 13 When the resulting product is immersed in an etching solution or sprayed with an etching solution, the sealing film ST_W can be etched across the entire surface of the micro-substrate. The thickness of the etched sealing film ST_W can be substantially proportional to the duration of exposure of the film to the etching solution (i.e., the etching time). The etching time can be determined to remove all of the sealing film ST_W on the electrode layer 131. When removing all of the sealing film ST_W on the electrode layer 131, a sealing film ST_W of similar thickness disposed on another surface of the micro-substrate can also be removed. The sealing film ST_W disposed on the step portion STP between the end of the electrode layer 131 and the body 110 can also be removed by the etching solution.
[0142] Even in the region forming the open microvia OP_H, the sealing film ST can be stacked on the outer surface with a uniform thickness, so that the end of the inner sealing film ST_I can be exposed when the sealing film ST_W on the electrode layer 131 is removed. When the etching process is stopped at this point, as... Figure 16 As in the example embodiment, the inner sealing film ST_I can be retained without retracting from the surface opening EN of the open micropore OP_H.
[0143] To ensure complete removal of the sealing film ST_W on electrode layer 131, an over-etching process with a predetermined additional time can be performed. In this case, the inner sealing film ST_I can be exposed to the etching solution during the over-etching and can be further etched. Therefore, as Figure 19 As shown, the inner sealing film ST_I can be retained in a form that is set to retract to a predetermined depth from the surface opening EN of the open micropore OP_H.
[0144] When over-etching is performed for an excessively long time, the entire inner sealing film ST_I may be over-etched and removed, or the opening of the open microvia OP_H may not be sealed (e.g. Figure 18 (as shown in (b)). Therefore, the over-etching time can be adjusted so that the inner sealing film ST_I can have a suitable retraction distance range (e.g., 100 nm or less).
[0145] The exemplary embodiments will be described in more detail below with reference to manufacturing examples and test examples.
[0146] <Manufacturing Example 1>
[0147] By reference Figure 10 The described method fabricates micro-substrate comprising a host and an electrode layer. The micro-substrate sample is observed using scanning focused ion beam (FIB).
[0148] <Manufacturing Example 2>
[0149] By reference Figure 10 , Figure 11 , Figure 13 , Figure 15 and Figure 16 The described method manufactures electronic components. A sealing film formation process is performed using C3F6 as the source gas in a roller-type PECVD apparatus. Process conditions are determined such that the average deposition thickness of the material is 100 nm. A sealing film removal process is then performed in a roller-type mechanical polishing apparatus. The average size of the abrasive particles used is 0.7 mm. After the sealing film removal process, a coating is formed, thus completing the electronic component.
[0150] The electronic component sample was observed using a scanning focused ion beam (FIB).
[0151] <Manufacturing Examples 3 to 5>
[0152] The electronic components were manufactured using the same method as in Manufacturing Example 2, except that the average deposition thickness of the deposited material was changed to 15 nm (manufacturing example 3), 60 nm (manufacturing example 4), and 300 nm (manufacturing example 5).
[0153] <Manufacturing Example 6>
[0154] Electronic components are manufactured by directly forming a coating on a micro-substrate without forming a sealing film or removing the sealing film.
[0155] <Experimental Example>
[0156] The breakdown voltage (BDV) of several samples according to manufacturing examples 1 to 6 was studied, and the results are listed in Table 1 below.
[0157] [Table 1]
[0158]
[0159] In Table 1, “min” represents the minimum BDV measured in the manufacturing examples, and “avg” represents the average BDV of the manufacturing examples. Referring to Table 1, manufacturing example 1, which was not exposed to the plating process, has a relatively high minimum BDV compared to manufacturing examples 2 to 6, which underwent the plating process. “Occupancy rate of 38V or less” in Table 1 indicates the proportion of samples exhibiting BDV characteristics less than or equal to 38V in each manufacturing example, where 38V is the minimum BDV of manufacturing example 1. This indicates that the smaller the “occupancy rate of 38V or less”, the better the BDV characteristics. Referring to Table 1, among the manufacturing examples that underwent the plating process, manufacturing example 6, which did not perform the process of forming a sealing film, or manufacturing example 3, whose average deposition thickness of the sealing film is less than 20 nm, exhibited a relatively high “occupancy rate of 38V or less”, approximately 24,000 ppm. Manufacturing examples 2, 4, and 5, with an average deposition thickness of 20 nm or greater for the sealing film, exhibited relatively small “occupancy rates of 38V or less”, thus demonstrating improved BDV characteristics. Although the process time of manufacturing example 5, with an average deposition thickness of 300 nm, is three times or more than that of manufacturing example 2, with an average deposition thickness of 100 nm, manufacturing example 5 exhibits a similar "38V or less occupancy" to manufacturing example 2.
[0160] Using the electronic components and manufacturing method thereof according to the foregoing example embodiments, fluid penetration into the electronic components can be prevented. Therefore, defects caused by the exposure of internal components of electronic products to fluid can be prevented.
[0161] While exemplary embodiments have been shown and described above, it will be readily understood by those skilled in the art that modifications and variations may be made without departing from the scope of the invention as defined by the appended claims.
Claims
1. An electronic component, comprising: A micro-subject includes a body and an electrode layer. The body includes multiple dielectric layers and multiple internal electrodes. The multiple internal electrodes are configured such that a corresponding dielectric layer is located between the multiple internal electrodes. The electrode layers are disposed on an outer surface of the body and connected to a portion of the multiple internal electrodes. as well as Sealing film, The micro-matrix includes a first micropore that extends through the surface of the micro-matrix and into at least a portion of the dielectric layer, the inner electrode, and the electrode layer. The sealing film includes an inner sealing film, which is disposed in at least a portion of the internal space of the first micropore to seal the first micropore. The first micropore includes an open micropore that opens from the surface of the electrode layer, and the open micropore is sealed by the inner sealing film.
2. The electronic component according to claim 1, wherein, The entire internal space of the first micropore is filled with the inner sealing film.
3. The electronic component according to claim 1, wherein, At least one of the first micropores includes a region sealed by the inner sealing film and an empty space not filled by the inner sealing film, and the empty space is disposed inside the region.
4. The electronic component according to claim 1, wherein, The micro-substrate further includes a second micropore, which is disposed in at least a portion of the dielectric layer, the inner electrode, and the electrode layer and spaced apart from the surface of the micro-substrate.
5. The electronic component according to claim 4, wherein, Of the first micropore and the second micropore, the inner sealing film is disposed only in the first micropore.
6. The electronic component according to claim 1, wherein, The sealing film also includes an outer sealing film, which is disposed on the interface surface between the end of the electrode layer and the body.
7. The electronic component according to claim 6, wherein, The outer sealing film comprises the same material as the inner sealing film.
8. The electronic component according to claim 1, wherein, The inner sealing film includes fluorine.
9. The electronic component according to claim 1, wherein, The inner sealing film has crystallinity.
10. The electronic component according to claim 1, further comprising: A plating layer is disposed on the electrode layer. The sealing film is not disposed between the electrode layer and the coating layer.
11. The electronic component according to claim 1, wherein, The inner sealing film is configured to retract in the depth direction from the opening of the first micropore.
12. The electronic component according to claim 11, wherein, The sealing film is not disposed on the outer surface of the microbody.
13. An electronic component, comprising: The main body includes multiple dielectric layers and multiple internal electrodes, wherein the multiple internal electrodes are configured such that a corresponding dielectric layer is located between the multiple internal electrodes; An external electrode includes an electrode layer and a plating layer. The electrode layer is disposed on the body and connected to a corresponding internal electrode. The plating layer is disposed on the electrode layer. The electrode layer includes micropores that open from the surface of the electrode layer. An outer sealing film is disposed on the interface surface between the end of the electrode layer and the body; and An inner sealing film is disposed in at least a portion of the internal space of the micropores to seal the micropores.
14. The electronic component according to claim 13, wherein, The outer sealing film includes fluorine.
15. The electronic component according to claim 13, wherein, The outer sealing film has crystallinity.
16. The electronic component according to claim 13, wherein, The maximum thickness of the outer sealing film is 20 nm to 200 nm.
17. A method for manufacturing an electronic component, the method comprising: A microbody is provided, the microbody including a body and an electrode layer, the body including a plurality of dielectric layers and a plurality of internal electrodes, the plurality of internal electrodes being configured such that a corresponding dielectric layer is disposed between the plurality of internal electrodes, the electrode layer being disposed on an outer surface of the body and connected to a portion of the plurality of internal electrodes, wherein the electrode layer includes open micropores opening from the surface of the electrode layer; A sealing film is formed on the micro-substrate using a vapor phase deposition process; and Remove at least a portion of the sealing film. In this step, after removing at least a portion of the sealing film, the open micropores are sealed by the retained portion of the sealing film.
18. The method according to claim 17, wherein, Using C x F y The step of forming a sealing film is performed in a plasma deposition apparatus using a source gas.
19. The method according to claim 17, wherein, The step of removing at least a portion of the sealing film includes a dry polishing process.
20. The method of claim 17, further comprising: After removing at least a portion of the sealing film, a plating layer is formed on the electrode layer.
21. The method according to claim 17, wherein, The microbody includes micropores that extend through the surface of the microbody in at least a portion of the dielectric layer, the inner electrode, and the electrode layer, and the micropores include open micropores, wherein the micropores are sealed by a retained portion of the sealing film after the step of removing at least a portion of the sealing film.
22. The method according to claim 17, wherein, The step of removing at least a portion of the sealing film includes an etching process, after which the sealing film is retained in a form that retracts in the depth direction from the opening of the open micropore.
23. The method according to claim 17, wherein, The step of forming the sealing film is performed using a spin deposition process.
24. The method according to claim 23, wherein, In the step of performing the rotary deposition process, a plurality of the micro-substrate are placed in a drum-type deposition apparatus, and the deposition process is performed while the drum-type deposition apparatus is rotated.
25. An electronic component, comprising: A micro-subject includes a body and an electrode layer. The body includes multiple dielectric layers and multiple internal electrodes. The multiple internal electrodes are configured such that a corresponding dielectric layer is located between the multiple internal electrodes. The electrode layers are disposed on an outer surface of the body and connected to a portion of the multiple internal electrodes. as well as Sealing film, The micro-matrix includes micropores that extend through the surface of the micro-matrix and within at least a portion of the dielectric layer, the inner electrode, and the electrode layer. The sealing film includes an inner sealing film, which is disposed in at least a portion of the internal space of the micropore to seal the micropore. Wherein, at least one of the micropores includes a region sealed by the inner sealing film and an empty space not filled by the inner sealing film, and the empty space is disposed inside the region.
26. An electronic component, comprising: A micro-subject includes a body and an electrode layer. The body includes multiple dielectric layers and multiple internal electrodes. The multiple internal electrodes are configured such that a corresponding dielectric layer is located between the multiple internal electrodes. The electrode layers are disposed on an outer surface of the body and connected to a portion of the multiple internal electrodes. as well as Sealing film, The micro-matrix includes micropores that extend through the surface of the micro-matrix into at least a portion of the dielectric layer, the inner electrode, and the electrode layer. The sealing film includes an inner sealing film, which is disposed in at least a portion of the internal space of the micropore to seal the micropore. In the electrode layer, the inner sealing film is flush with or recessed relative to the outer surface of the electrode layer.
Citation Information
Patent Citations
Method for producing electronic component
CN109313981A
Ceramic electronic component