Selective deposition of passivation films
Through anchor reactants and cyclic deposition technology, the challenge of selective deposition of passivation films in the semiconductor industry is solved, and high selectivity and stable ALD film growth is achieved, mushroom-like growth effect is avoided, and the manufacturing of nano-scale structures is improved. Efficiency and device miniaturization capability.
Patent Information
- Application Number
- CN202180003885.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-26
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2041-10-26
Smart Images

Figure CN114761613B_ABST
Abstract
Description
Technical Field
[0001] Various embodiments of the present disclosure relate to methods for selectively depositing a passivation film. In particular, various embodiments of the present disclosure relate to methods for selectively depositing a passivation film on a metal surface or a dielectric surface. Background Art
[0002] The semiconductor industry faces many challenges in the pursuit of device miniaturization involving rapid scaling of nanoscale structures. These issues include the introduction of complex manufacturing steps, such as multiple photolithography steps and the integration of high-performance materials. To maintain the pace of device miniaturization, selective deposition shows promise because it has the potential to eliminate expensive photolithography steps by simplifying the integration scheme.
[0003] Selective deposition of materials can be achieved in a variety of ways. Chemical precursors can react selectively with one surface relative to another surface (metal or dielectric). Process parameters such as pressure, substrate temperature, precursor partial pressure and / or gas flow can be adjusted to adjust the chemical kinetics of a particular surface reaction. Another possible approach involves surface pretreatment, which can be used to activate or passivate the target surface for the introduced thin film deposition precursors.
[0004] Area-selective atomic layer deposition (AS-ALD) can be used for the selective deposition of materials. During AS-ALD, when the deposited ALD film becomes thicker than the self-assembled monolayer (SAM) used to passivate the non-growth surface, the ALD film may grow laterally (this may be referred to as mushrooming), thereby reducing selectivity. Direct formation of a thicker protective SAM is not feasible because the precursors cannot be delivered in the vapor phase. There is a continuing need in the art for methods to improve deposition selectivity and avoid problems that occur during AS-ALD. Summary of the invention
[0005] One embodiment of the present disclosure relates to a method for selectively depositing a passivation film on a substrate, comprising: exposing a substrate comprising a first surface and a second surface to an anchoring reactant; and selectively depositing the anchoring reactant on the first surface as a seed layer, wherein the anchoring reactant comprises an ethynyl derivative having a head group selectively targeted to the first surface.
[0006] Another embodiment relates to a method of depositing an ALD film having a high aspect ratio, comprising: (a) exposing a substrate comprising a first surface and a second surface to an anchor reactant, wherein the anchor reactant is a 4-ethynylbenzene derivative having a head group that selectively targets the first surface and forms a seed layer; (b) forming a passivation film, wherein the seed layer is exposed to a first monomer to form a passivation film having a thickness; (c) increasing the thickness of the passivation film, wherein the passivation film reacts with a second monomer; (d) performing atomic layer deposition to deposit an ALD film having a thickness, wherein the thickness of the ALD film remains equal to or less than the thickness of the passivation film; (e) sequentially repeating steps (b), (c) and (d) at least once, wherein with each repetition of (b) and (c), the passivation film increases in thickness in a range from 1 nm to 50 nm; and (f) removing the passivation film by exposure to O2 or O2 plasma.
[0007] Another aspect relates to a non-transitory computer-readable medium comprising instructions that, when executed by a controller of a substrate processing chamber, cause the substrate processing chamber to expose a substrate to an anchor reactant, a first monomer, a second monomer, to form a passivation layer having a thickness and an ALD reactant in a predetermined order, such that the thickness of the resulting ALD film remains less than or equal to the thickness of the passivation layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0008] In order to understand the above-mentioned characteristic structure of the present disclosure in detail, a more specific description of the present disclosure briefly summarized above can be obtained by referring to multiple embodiments (some of which are depicted in the accompanying drawings). However, it should be noted that the accompanying drawings only show multiple typical embodiments of the present disclosure and should not be considered as limiting the scope of the present disclosure, because the present disclosure may allow for other multiple equally effective embodiments.
[0009] Figure 1 A schematic diagram of a reaction for selectively depositing an ALD film on a substrate according to one or more embodiments is shown;
[0010] Figure 2 A reaction diagram illustrating a method for selectively depositing a seed layer and a subsequent passivation film according to one or more embodiments; and
[0011] Figure 3 is a flow chart of a method according to one or more implementations. DETAILED DESCRIPTION
[0012] Before describing several exemplary embodiments of the present invention, it should be understood that the present invention is not limited to the details of construction or process steps set forth in the following description. The present invention is capable of other numerous embodiments and can be practiced or carried out in various ways.
[0013] As used herein, "substrate" or "substrate surface" refers to any portion of the substrate or the portion of the surface of the material formed on the substrate on which film treatment is performed. For example, the substrate surface that can be treated on the substrate surface includes materials such as silicon, silicon oxide, silicon nitride, doped silicon, germanium, gallium arsenide, glass, sapphire, and any other materials such as metals, metal nitrides, metal alloys, and other conductive materials, depending on the application. Substrates include, but are not limited to, semiconductor wafers. The substrate may be exposed to a pretreatment process to polish, etch, reduce, oxidize, hydroxylate, anneal, UV cure, electron beam cure, and / or bake the substrate surface. In addition to performing film treatment directly on the surface of the substrate itself, in the present disclosure, any film treatment step disclosed may also be performed on a bottom layer formed on the substrate as disclosed in more detail below, and the term "substrate surface" is intended to include the bottom layer indicated by the context. Thus, for example, when a film / layer or a portion of a film / layer has been deposited on the substrate surface, the exposed surface of the newly deposited film / layer becomes the substrate. The substrate may have various sizes, such as a wafer with a diameter of 200 mm or 300 mm, and a rectangular or square window pane. In some embodiments, the substrate comprises a rigid discrete material.
[0014] As used herein, "atomic layer deposition" or "cyclic deposition" refers to a process that includes sequential exposure of two or more reactive compounds to deposit a layer of material on a substrate.
[0015] As used in this specification and the appended claims, the terms "reactive compound," "reactive gas," "reactive species," "precursor," "processing gas," and the like are used interchangeably and refer to a substance having a species capable of reacting with a substrate or a material on the substrate in a surface reaction (e.g., chemisorption, oxidation, reduction, cycloaddition). The substrate or a portion of the substrate is sequentially exposed to two or more reactive compounds introduced into a reaction zone of a processing chamber.
[0016] As used herein, "metal" refers to metals, metal alloys, metal oxides, metal nitrides, or combinations thereof, including, for example, copper, cobalt, nickel, tungsten, ruthenium, chromium, iron, platinum, gold, silver, molybdenum, gallium, indium, indium tin oxide, fluorine-doped tin oxide, and aluminum-doped zinc oxide. In one or more embodiments, the metal oxide does not include a dielectric oxide.
[0017] As used herein, "metal surface" refers to any portion of a substrate or portion of a material surface formed from metal. The metal surface may be exposed to a pretreatment process to polish, coat, dope, etch, reduce, oxidize, hydroxylate, anneal, UV cure, electron beam cure, and / or bake the substrate. In addition to pretreatment directly on the metal surface itself, in the present disclosure, any metal surface treatment disclosed may also be performed on the underlying metal surface as disclosed in more detail below, and the term "metal surface" is intended to include the underlying layer as indicated by the context. Thus, for example, when a film / layer or portion of a film / layer has been deposited onto a metal surface, the exposed surface of the newly deposited film / layer becomes the metal surface.
[0018] As used herein, "dielectric surface" refers to any portion of a substrate or portion of a material surface formed from a dielectric material. Non-limiting examples of dielectric materials include SiO x 、Si x N y 、Si、SiON、AlO x 、Al2O3、HfO x 、ZrO2、TiO x 、TiN、Ta x O5, Ta2O5, Y2O3, La2O3, AlN, MgO, CaF2, LiF, SrO, SiC, BaO, HfSiO4, LaAlO3, Nb2O5, BaTiO3, SrTiO3, Bi4Ti3O 12 、Pb(Zr,Ti)O3、CaCu3Ti4O 12 , LiNbO3, BaTiO3, LiNbO3, and KNbO3. The dielectric surface can be exposed to a pretreatment process to polish, coat, dope, etch, reduce, oxidize, hydroxylate, anneal, UV cure, electron beam cure, and / or bake the substrate. In addition to pretreatment directly on the dielectric surface itself, in the present disclosure, any dielectric surface treatment disclosed may also be performed on the underlying metal surface as disclosed in more detail below, and the term "dielectric surface" is intended to include the underlying layer as indicated by the context. Thus, for example, when a film / layer or portion of a film / layer has been deposited onto a dielectric surface, the exposed surface of the newly deposited film / layer becomes the dielectric surface.
[0019] As used in this specification and the appended claims, the phrase "selectively deposits" or similar phrases means that the material of the indicator is deposited on the surface to a greater extent than on another surface. In some embodiments, "selectively" means that the material of the indicator is formed on the selective surface at a rate greater than or equal to about 10x, 15x, 20x, 25x, 30x, 35x, 40x, 45x, or 50x the rate of formation on the non-selective surface.
[0020] Various embodiments of the present disclosure advantageously provide a method for pre-treating a substrate. The substrate includes a first surface and a second surface. The pre-treating selectively blocks the first surface and allows subsequent deposition of a metal or dielectric material on the second surface.
[0021] Multiple embodiments provide methods that allow the growth of thicker AS-ALD films and avoid the mushroom growth effect by simultaneously growing a protective film. In one or more embodiments, molecular precursors are selected to form rigid linear structures and minimize the reactivity of the polymer during the ALD process. This allows adjustment of the height of the polymer layer during the ALD process, limiting the mushroom growth effect, thereby enabling the deposition of high aspect ratio (AR) structures. In some embodiments, the protective film is grown in situ, made of rigid chains to prevent folding, the precursor is a small molecule, and the thickness of the protective film can be gradually increased during the ALD process. According to one or more embodiments, mushroom growth of the ALD film is avoided. In some embodiments, the method allows the growth of high aspect ratio films. In some embodiments, the use of small molecule precursors that are easier to deliver provides an adjustable film thickness.
[0022] Various embodiments utilize the inverse electron demand Diels-Alder reaction between tetrazines and alkynes. 1,4-diethynylbenzene and 1,2,4,5-tetrazine serve as bifunctional reagents and can react sequentially to form polyphenylene polymers. In various embodiments, there is deposition of a seed SAM layer in the non-growth region. The seed layer consists of a 4-ethynylbenzene derivative with an anchoring group. The anchoring group can be designed to be selective for the non-growth region. After formation of the seed SAM, the two reagents are sequentially pulsed in the ALD tool, resulting in ring-by-ring growth of the polymer. The resulting polyphenylene polymer should be inert to most ALD processes. Both monomers can interact with metal surfaces, but due to their low molecular weight, should favor desorption during the purge step of the cycle. The growth of the polymer layer can alternate with the growth of the ALD film, forming a super cycle.
[0023] In various embodiments, a thin polymer film is deposited first, followed by the desired ALD film. When the thickness of the two films are comparable, more polymer can be grown and the sequence repeated. Keeping the polymer passivation film thicker than the other ALD films limits the lateral growth of the ALD film (mushroom-like growth effect). Growing both films simultaneously gradually reduces the chances of polymer chains folding and collapsing at the edges.
[0024] For sealing, the substrate is pretreated with an anchoring reactant. The anchoring reactant selectively reacts with and binds to a metal surface or a dielectric surface to form a seed layer. In some embodiments, the anchoring reactant comprises an ethynyl derivative having a head group that selectively targets a first surface. In some embodiments, the ethynyl derivative comprises a 4-ethynylbenzene derivative.
[0025] In some embodiments, non-limiting examples of anchor reactants have structures according to Formula (I), Formula (II), Formula (III), or Formula (IV):
[0026]
[0027] In some embodiments, wherein the first surface comprises a metal surface, the head group comprises a -COOH group, a -COOR group, a -CONNR2 group, a -PO(OH)2 group, a -PO(OR)2 group, a -NH2 group, a -NR2 group, an acetylacetone group, a pyrrole group, a pyridine group and a thiophene group, and wherein R is an alkyl or phenyl derivative. In some embodiments, the metal surface comprises a metal, a metal alloy, a metal oxide, a metal nitride, or a combination thereof. Non-limiting examples of metals can be copper, cobalt, nickel, tungsten, ruthenium, chromium, iron, platinum, gold, silver, molybdenum, gallium, indium, or a combination thereof. In some embodiments, wherein the first surface comprises a metal surface, and the second surface comprises a dielectric surface.
[0028] In some embodiments, wherein the first surface comprises a dielectric surface, the head group may be selected from the group consisting of a -SiCl3 group, a -Si(OR)3 group, and a -Si(NR2)3 group, wherein R is an alkyl or phenyl derivative. A non-limiting example of a dielectric surface may be SiO x 、Si x N y 、Si、SiON、AlO x 、Al2O3、HfO x 、ZrO2、TiO x 、TiN、Ta x O5, Ta2O5, Y2O3, La2O3, AlN, MgO, CaF2, LiF, SrO, SiC, BaO, HfSiO4, LaAlO3, Nb2O5, BaTiO3, SrTiO3, Bi4Ti3O 12 、Pb(Zr,Ti)O3、CaCu3Ti4O 12 , LiNbO3, BaTiO3, LiNbO3, and KNbO3, or a combination thereof. In some embodiments, the first surface comprises a dielectric surface, and the second surface comprises a metal surface.
[0029] In some embodiments, after depositing the seed layer, a chemical vapor deposition process is performed to deposit a CVD film. In other embodiments, after depositing the seed layer, an atomic layer deposition process is performed to deposit an ALD film. In some embodiments, the thickness of the ALD film is equal to or less than the thickness of the seed layer. In some embodiments, wherein the seed layer is deposited on a metal surface, and the ALD film comprises a dielectric material. Non-limiting examples of the dielectric material include SiO x 、Si x N y 、Si、SiON、AlO x 、Al2O3、HfO x 、ZrO2、TiO x 、TiN、Ta x O5, Ta2O5, Y2O3, La2O3, AlN, MgO, CaF2, LiF, SrO, SiC, BaO, HfSiO4, LaAlO3, Nb2O5, BaTiO3, SrTiO3, Bi4Ti3O 12 、Pb(Zr,Ti)O3、CaCu3Ti4O 12 , LiNbO3, BaTiO3, LiNbO3, KNbO3, or a combination thereof. In some embodiments, wherein the seed layer is deposited on a dielectric surface, the ALD film comprises a metal, a metal alloy, a metal oxide, a metal nitride, or a combination thereof. Non-limiting examples of metals may be copper, cobalt, nickel, tungsten, ruthenium, chromium, iron, platinum, gold, silver, molybdenum, gallium, indium, or a combination thereof. In some embodiments, after the ALD film is deposited, the passivation film is removed. In some embodiments, the passivation film is removed by exposing the substrate to O2 or O2 plasma.
[0030] In some embodiments, the substrate with the seed layer is cleaned before performing atomic layer deposition. In some embodiments, only the first surface with the seed layer is cleaned before performing atomic layer deposition. In some embodiments, wherein the first surface is a metal surface, the substrate or the first surface of the substrate is cleaned with a hydrogen plasma. In some embodiments, the hydrogen plasma is a conductively coupled plasma (CCP). In some embodiments, the hydrogen plasma is an inductively coupled plasma (ICP). In some embodiments, the hydrogen plasma comprises a plasma of H2.
[0031] In some embodiments, the seed layer remains bonded to the first surface at a higher temperature, wherein the higher temperature is in the range of 50°C to 100°C, 50°C to 150°C, 50°C to 200°C, 50°C to 250°C, 50°C to 300°C, 50°C to 350°C, 50°C to 400°C, or 50°C to 500°C.
[0032] In some embodiments, after performing atomic layer deposition of the dielectric film, the seed layer is removed from the substrate. The seed layer can be removed by any suitable selective etching process. Suitable selective etching processes include, but are not limited to, the use of oxygen, oxygen plasma, and fluorine plasma. In some embodiments, when the seed layer is removed using oxygen or oxygen plasma, a metal oxide layer is formed on the metal surface. In some embodiments, the metal oxide layer formed on the metal surface is removed by the use of a reduction process. Suitable reduction processes include, but are not limited to, the use of plasmas containing hydrogen or ammonia and thermal annealing containing hydrogen or ammonia. In some embodiments, oxygen plasma, fluorine plasma, hydrogen plasma, and ammonia plasma can be independently generated remotely or internally, and can be conductively coupled or inductively coupled. In some embodiments, the seed layer is removed by sequentially exposing the substrate to oxygen plasma and hydrogen plasma.
[0033] In some embodiments, the seed layer further reacts with a first monomer to form a passivation film. In some embodiments, the first monomer includes a tetrazine derivative. Non-limiting examples of tetrazine derivatives include 1,2,4,5-tetrazine; 3,6-dimethyl-1,2,4,5-tetrazine; 3,6-diethyl-1,2,4,5-tetrazine; 3,6-dipropyl-1,2,4,5-tetrazine; 3,6-diisopropyl-1,2,4,5-tetrazine; or combinations thereof.
[0034] Figure 2 A first monomer 1,2,4,5-tetrazine is shown forming a passivation film. In method 200, a first substrate surface 210 is provided. The substrate surface 210 is deposited with a seed layer 211. The method provides at 212 exposing the seed layer to a first monomer 1,2,4,5-tetrazine, which results in the formation of a passivation film 213. During the method at 214, the passivation layer 213 is exposed to a second monomer 1,4-diethynylbenzene, increasing the thickness of the passivation film 213. The passivation film 213 is again exposed to the first monomer 1,2,4,5-tetrazine, further increasing the thickness of the passivation film 213. The method includes cyclic deposition of the first monomer and the second monomer at 214, so that the passivation film 213 has a desired thickness.
[0035] In some embodiments, after forming the passivation film, atomic layer deposition is performed to deposit an ALD film or increase the thickness of the ALD film. In some embodiments, the thickness of the ALD film is equal to or less than the thickness of the passivation film. In some embodiments, where the passivation film is formed on a metal surface, the ALD film includes a dielectric material. Non-limiting examples of dielectric materials include SiO x 、Si x N y 、Si、SiON、AlO x 、Al2O3、HfO x 、ZrO2、TiO x 、TiN、Ta x O5, Ta2O5, Y2O3, La2O3, AlN, MgO, CaF2, LiF, SrO, SiC, BaO, HfSiO4, LaAlO3, Nb2O5, BaTiO3, SrTiO3, Bi4Ti3O 12 、Pb(Zr,Ti)O3、CaCu3Ti4O 12 , LiNbO3, BaTiO3, LiNbO3, KNbO3, or a combination thereof. In some embodiments, wherein the seed layer is deposited on a dielectric surface, the ALD film comprises a metal, a metal alloy, a metal oxide, a metal nitride, or a combination thereof. Non-limiting examples of metals may be copper, cobalt, nickel, tungsten, ruthenium, chromium, iron, platinum, gold, silver, molybdenum, gallium, indium, or a combination thereof. In some embodiments, after the ALD film is deposited, the passivation film is removed. In some embodiments, the passivation film is removed by exposing the substrate to O2 or an O2 plasma.
[0036] In some embodiments, the passivation film wherein the passivation film has a thickness is further exposed to a second monomer to increase the thickness of the passivation film. In some embodiments, the second monomer comprises an acetylenic derivative. In some embodiments, the acetylenic derivative comprises a diacetylenic or triacetylenic derivative. In some embodiments, the acetylenic derivative may be selected from the group consisting of 1,4-diethynylbenzene, 1,3,5-triacetylenic benzene, or a combination thereof. Figure 2 The passive film 1,4-diethynylbenzene is shown reacting with the second monomer.
[0037] Figure 33 is a flow chart illustrating a detailed exemplary embodiment of method 300. At 310, an anchor reactant is flowed into a substrate processing region to selectively deposit a seed layer on a first substrate surface. At 311, the anchor reactant is removed from the substrate processing region, at 312, a first monomer is flowed into the substrate processing region to form a passivation film on the seed layer, and at 313, the first monomer is removed from the substrate processing region. At 314, a second monomer is flowed into the substrate processing region to increase the thickness of the passivation film, and at 315, the second monomer is removed from the substrate processing region. At 316, the process is repeated until a desired film thickness is reached, and at 317, ALD is performed to deposit an ALD film. At 318, the process is repeated until a desired ALD film thickness is reached.
[0038] In some embodiments, after exposure to the second monomer, atomic layer deposition is performed to deposit an ALD film or to increase the thickness of the ALD film. In some embodiments, the thickness of the ALD film is equal to or less than the thickness of the passivation film. In some embodiments, where the passivation film is formed on a metal surface, the ALD film includes a dielectric material. Non-limiting examples of dielectric materials include SiO x 、Si x N y 、Si、SiON、AlO x 、Al2O3、HfO x 、ZrO2、TiO x 、TiN、Ta x O5, Ta2O5, Y2O3, La2O3, AlN, MgO, CaF2, LiF, SrO, SiC, BaO, HfSiO4, LaAlO3, Nb2O5, BaTiO3, SrTiO3, Bi4Ti3O 12 、Pb(Zr,Ti)O3、CaCu3Ti4O 12 , LiNbO3, BaTiO3, LiNbO3, KNbO3, or a combination thereof. In some embodiments, wherein the seed layer is deposited on a dielectric surface, the ALD film comprises a metal, a metal alloy, a metal oxide, a metal nitride, or a combination thereof. Non-limiting examples of metals may be copper, cobalt, nickel, tungsten, ruthenium, chromium, iron, platinum, gold, silver, molybdenum, gallium, indium, or a combination thereof. In some embodiments, after the ALD film is deposited, the passivation film is removed. In some embodiments, the passivation film is removed by exposing the substrate to O2 or an O2 plasma.
[0039] Another aspect of the present disclosure provides cyclic deposition of a passivation film and an ALD film, wherein the passivation film is cyclically grown alongside the ALD film such that the thickness of the ALD film remains equal to or less than the thickness of the passivation film. This method reduces the lateral growth problem, also known as the mushroom growth problem. Figure 2 The growth of the passivation film by cyclic deposition is shown. The atomic layer deposition can be performed intermittently so that the thickness of the resulting ALD film remains equal to or less than the thickness of the passivation film. In some embodiments, the steps of reacting with the first monomer, exposing to the second monomer, and performing atomic layer deposition are repeated sequentially at least once. In some embodiments, sequential repetitions are performed in the range of 1 to 1000 times, 1 to 950 times, 1 to 900 times, 1 to 850 times, 1 to 800 times, 1 to 750 times, 1 to 700 times, 1 to 650 times, 1 to 600 times, 1 to 550 times, 1 to 500 times, 1 to 450 times, 1 to 400 times, 1 to 350 times, 1 to 300 times, 1 to 250 times, 1 to 200 times, 1 to 150 times, 1 to 100 times, 1 to 75 times, 1 to 50 times, 1 to 25 times, 200 to 1000 times, 300 to 1000 times, 400 to 1000 times, 500 to 1000 times, 600 to 1000 times, 700 to 1000 times, 800 to 1000 times, 900 to 1000 times. In some embodiments, the sequence is repeated until the final thickness of the ALD film is within a desired range. In some embodiments, the desired range includes to to to to to to to to to to to to to to to to to to to to to to to to to to to to to to to to to to and to
[0040] In some embodiments, the steps of reacting with the first monomer and exposing to the second monomer increase the thickness of the passivation film with each repetition in the following ranges: 1 nm to 50 nm, 1 nm to 45 nm, 1 nm to 40 nm, 1 nm to 35 nm, 1 nm to 30 nm, 1 nm to 25 nm, 5 nm to 50 nm, 5 nm to 45 nm, 5 nm to 40 nm, 5 nm to 35 nm, 5 nm to 30 nm, 5 nm to 25 nm, 10 nm to 50 nm, 10 nm to 45 nm, 10 nm to 40 nm, 10 nm to 35 nm. m, 10nm to 30nm, 10nm to 25nm, 15nm to 50nm, 15nm to 45nm, 15nm to 40nm, 15nm to 35nm, 15nm to 30nm, 15nm to 25nm, 20nm to 50nm, 20nm to 45nm, 20nm to 40nm, 20nm to 35nm, 20nm to 30nm, 20nm to 25nm, 25nm to 50nm, 25nm to 45nm, 25nm to 40nm, 25nm to 35nm, or 25nm to 30nm.
[0041] In some embodiments, the passivation film remains bonded to the first surface at a higher temperature, wherein the higher temperature is in the range of 50°C to 100°C, 50°C to 150°C, 50°C to 200°C, 50°C to 250°C, 50°C to 300°C, 50°C to 350°C, 50°C to 400°C, or 50°C to 500°C.
[0042] In some embodiments, wherein the thickness of the ALD film is within a desired range, the passivation film is removed. In some embodiments, the passivation film is removed by exposing the substrate to O2 or O2 plasma.
[0043] In some embodiments, after performing atomic layer deposition, the passivation film is removed from the substrate. The passivation film can be removed by any suitable selective etching process. Suitable selective etching processes include, but are not limited to, the use of oxygen, oxygen plasma, and fluorine plasma. In some embodiments, when the seed layer is removed using oxygen or oxygen plasma, a metal oxide layer is formed on the metal surface. In some embodiments, the metal oxide layer formed on the metal surface is removed by the use of a reduction process. Suitable reduction processes include, but are not limited to, the use of plasma containing hydrogen or ammonia and thermal annealing containing hydrogen or ammonia. In some embodiments, oxygen plasma, fluorine plasma, hydrogen plasma, and ammonia plasma can be independently generated remotely or internally, and can be conductively coupled or inductively coupled. In some embodiments, the passivation film is removed by sequentially exposing the substrate to oxygen plasma and hydrogen plasma.
[0044] Figure 1A reaction schematic diagram of selectively depositing an ALD film on a substrate according to one or more embodiments of method 100 is shown. Substrate 101 includes a first surface 102 and a second surface 103. In method step 110, the first surface 102 reacts with an anchor reactant to deposit a seed layer 104 on the first surface 102. During method step 120, the seed layer 104 is exposed to a first monomer 105 to form a passivation film having a thickness 107. Then in method step 130, the seed layer combined with the first monomer 105 is exposed to a second monomer 106 to increase the thickness 107 of the passivation film. Subsequently, in method step 140, atomic layer deposition is performed to deposit an ALD film 103 on the second surface, so that the thickness 108 of the ALD film is not greater than the thickness 107 of the passivation film. The substrate then undergoes a cyclic deposition method step 150 sequentially with the first monomer 105, the second monomer 106, and the ALD deposition 103. Finally, the passivation film is removed. Removal can be achieved by exposing the substrate to O2 or O2 plasma.
[0045] In some embodiments, the reaction zone is located in a modular system including multiple chambers that perform various functions including substrate centering and orientation, degassing, annealing, deposition, and / or etching. According to one or more embodiments, the modular system includes at least a first processing chamber and a central transfer chamber. The central transfer chamber can house a robot that can transfer substrates back and forth between the processing chamber and the load lock chamber. The transfer chamber is typically maintained under vacuum conditions and provides an intermediate stage for transferring substrates from one chamber to another and / or to a load lock chamber at the front end of the cluster tool. Two well-known modular systems that may be applicable to the present disclosure are and Both are available from Applied Materials, Inc., Santa Clara, California. However, the exact arrangement and combination of chambers may be varied to perform specific steps of the process as described herein. Other processing chambers that may be used include, but are not limited to, cyclic layer deposition (CLD), atomic layer deposition (ALD), chemical vapor deposition (CVD), physical vapor deposition (PVD), etching, pre-cleaning, chemical cleaning, thermal treatments such as RTP, plasma nitridation, degassing, orientation, hydroxylation, and other substrate processing. By performing processing in the processing chambers of the modular system, surface contamination of the substrate with atmospheric impurities can be avoided without oxidation prior to deposition of subsequent films.
[0046] According to one or more embodiments, the substrate is continuously under vacuum or "load lock" conditions and is not exposed to ambient air when moving from one chamber to the next. The transfer chamber is therefore in a vacuum state and is "evacuated" under vacuum pressure. An inert gas may be present in the processing chamber or the transfer chamber. In some embodiments, the inert gas is used to purge or remove some or all reactants (e.g., reactants). According to one or more embodiments, an inert gas is injected at the outlet of the processing chamber to prevent reactants (e.g., reactants) from moving from the processing chamber to the transfer chamber and / or additional processing chambers. Thus, the inert gas flow forms a curtain at the outlet of the chamber.
[0047] The substrates may be processed in a single substrate deposition chamber, where a single substrate is loaded, processed, and unloaded before processing another substrate. The substrates may also be processed in a continuous manner similar to a conveyor system, where multiple substrates are individually loaded into a first portion of the chamber, moved through the chamber, and unloaded from a second portion of the chamber. The shape of the chamber and associated conveyor system may form a straight path or a curved path. In addition, the processing chamber may be a carousel, where multiple substrates move around a central axis and are exposed to deposition, etching, annealing, cleaning, etc. in a carousel path.
[0048] During processing, the substrate may be heated or cooled. Such heating or cooling may be accomplished by any suitable means, including but not limited to changing the temperature of the substrate support and flowing a heated or cooled gas to the substrate surface. In some embodiments, the substrate support includes a heater / cooler that may be controlled to conductively change the substrate temperature. In one or more embodiments, the gas (reactive gas or inert gas) employed is heated or cooled to locally change the substrate temperature. In some embodiments, the heater / cooler is located in a chamber adjacent to the substrate surface to convectively change the substrate temperature.
[0049] The substrate may also be stationary or rotated during processing. A rotating substrate may be rotated (about the substrate axis) continuously or in discrete steps. For example, the substrate may be rotated throughout processing, or the substrate may be rotated a small amount between exposures to different reactive or purge gases. Rotating the substrate during processing (continuously or in steps) can help produce a more uniform deposition or etch by minimizing the effects of local variations in, for example, gas flow geometry.
[0050] In the spatial ALD process, reactive gases flow into different processing areas within the processing chamber. Different processing areas are separated from adjacent processing areas so that the reactive gases do not mix. The substrate can be moved between processing areas to expose the substrate to reactive gases individually. During the movement of the substrate, different parts of the substrate surface or the material on the substrate surface are exposed to two or more reactive gases so that any given point on the substrate is not substantially exposed to more than one reactive gas at the same time. As will be understood by those skilled in the art, due to the diffusion of gases in the processing chamber, a small part of the substrate may be exposed to multiple reactive gases at the same time, and unless otherwise specified, simultaneous exposure is unintentional.
[0051] In another aspect of the spatial ALD process, the reactive gases are delivered simultaneously to the reaction zone, but separated by an inert gas curtain and / or a vacuum curtain. The gas curtain can be a combination of an inert gas flowing into the process chamber and a vacuum flow flowing out of the process chamber. The substrate moves relative to the gas delivery apparatus so that any given point on the substrate is exposed to only one reactive gas.
[0052] As used herein, "pulse" or "dose" refers to the amount of source gas that is intermittently or non-continuously introduced into a process chamber. The amount of a particular compound within each pulse may vary over time, depending on the duration of the pulse. A particular process gas may include a single compound or a mixture / combination of two or more compounds.
[0053] In some embodiments of a time-domain ALD process, each reactive gas exposure to, including but not limited to, metal and dielectric materials for the ALD film is separated by a time delay to allow each compound to adhere and / or react on the substrate surface and then be purged from the process chamber. Mixing of the reactive gases is prevented by purging the process chamber between subsequent exposures.
[0054] In another aspect of the time-domain ALD process of some embodiments, there are time delays between pulses of reactive gas. During each time delay, a purge gas (such as argon) is introduced into the processing chamber to purge the reaction zone or otherwise remove any residual reactive gas or reaction products or byproducts from the reaction zone. Alternatively, the purge gas can flow continuously throughout the deposition process, so that only the purge gas flows during the time delay between reactive gas pulses. The pulses of reactive gas and purge gas are pulsed alternately between multiple pulses. Purging can also be performed by applying a vacuum without flowing gas.
[0055] The duration of each pulse / dose is variable and can be adjusted to accommodate, for example, the spatial capacity of the processing chamber and the capabilities of the vacuum system coupled to the processing chamber. In addition, the dosage time of the reactive gas can vary depending on the flow rate of the reactive gas, the temperature of the processing gas, the type of control valve, the type of processing chamber employed, and the ability of the processing gas components to adsorb onto the substrate. The dosage time can also vary depending on the type of layer to be formed and the geometry of the device to be formed. The dosage time should be long enough to provide a volume of compound sufficient to adsorb / chemisorb onto and form a layer of the processing gas component on substantially the entire surface of the substrate.
[0056] Once the passivation film is deposited, the method may optionally include further processing (eg, bulk deposition of a dielectric film). In some embodiments, the further processing may be an ALD process.
[0057] In one or more embodiments, the process described herein can generally be stored in a memory as a software program, and when the software program is executed by a controller or a processor, the substrate processing chamber performs one or more processes of the present disclosure. The software program can also be stored and / or executed by a second controller or processor (not shown) away from the hardware controlled by the controller or processor. Some or all of the methods of the present disclosure can also be executed in hardware. Therefore, the process can be implemented in software and executed using a computer system, implemented in hardware (such as an application-specific integrated circuit or other type of hardware), or implemented in a combination of software and hardware. When the software program is executed by a processor or a controller, a general-purpose computer is converted into a special-purpose computer (controller) that controls the operation of the chamber, thereby executing the process. The process can be stored on a non-temporary computer-readable medium including instructions, and when the instructions are executed by a controller or a processor of a substrate processing chamber, the substrate processing chamber is exposed to an anchoring reactant, a first monomer, and a second monomer, and a passivation layer and an ALD reactant having a thickness are formed in a predetermined order, so that the thickness of the resulting ALD film remains less than, greater than, or equal to the thickness of the passivation layer.
[0058] References throughout this specification to "one embodiment," "certain embodiments," "one or more embodiments," or "an embodiment" mean that a particular feature, structure, material, or characteristic described in conjunction with a plurality of embodiments is included in at least one embodiment of the present disclosure. Thus, phrases such as "in one or more embodiments," "certain embodiments," "in an embodiment," or "in an embodiment" appearing in various places throughout this specification do not necessarily refer to the same embodiment of the present disclosure. Furthermore, particular features, structures, materials, or characteristics may be combined in any suitable manner in one or more embodiments.
[0059] Although the disclosure herein has been described with reference to a plurality of specific embodiments, it will be understood that these embodiments are merely illustrative of the principles and applications of the disclosure. It will be apparent to those skilled in the art that various modifications and variations may be made to the methods and apparatus of the disclosure without departing from the spirit and scope of the disclosure. Therefore, the disclosure is intended to include modifications and variations within the scope of the appended claims and equivalents of the appended claims.
Claims
1. A method for selectively depositing a passivation film on a substrate, the method comprising: exposing the substrate comprising a first surface and a second surface to an anchor reactant, wherein the first surface comprises a metal surface and the second surface comprises a dielectric surface, or the first surface comprises the dielectric surface and the second surface comprises the metal surface; selectively depositing the anchoring reactant on the first surface as a seed layer, wherein the anchoring reactant comprises an ethynyl derivative having a head group selectively targeted to the first surface; and The seed layer is exposed to a first monomer to form the passivation film, wherein the first monomer includes a tetrazine derivative.
2. The method of claim 1, wherein the ethynyl derivative comprises a 4-ethynylbenzene derivative.
3. The method of claim 1, wherein the first surface or the second surface comprises a metal selected from the group consisting of Cu, Co, Ni, W, Ru, Cr, Fe, Pt, Au, Ag, Mo, Ga, and In.
4. The method of claim 3, wherein the head group of the anchor reactant is selected from the group consisting of -COOH, -COOR, -CONNR2, -PO(OH)2, -PO(OR)2, -NH2, -NR2, acetylacetone, pyrrole, pyridine and thiophene, and wherein R is an alkyl or phenyl derivative.
5. The method according to claim 1, wherein the first surface or the second surface comprises a material selected from SiO x 、Si x N y 、Si、SiON、AlO x 、Al2O3、HfO x 、ZrO2、TiO x 、TiN、Ta x O5, Y2O3, La2O3, AlN, MgO, CaF2, LiF, SrO, SiC, BaO, HfSiO4, LaAlO3, Nb2O5, BaTiO3, SrTiO3, Bi4Ti3O 12 、Pb(Zr,Ti)O3、CaCu3Ti4O 12 , LiNbO3, BaTiO3, and KNbO3.
6. The method of claim 5, wherein the head group of the anchoring reactant is selected from the group consisting of -SiCl3, -Si(OR)3 and -Si(NR2)3, and wherein R is an alkyl or phenyl derivative.
7. The method of claim 1, wherein the tetrazine derivative is selected from the group consisting of 1,2,4,5-tetrazine; 3,6-dimethyl-1,2,4,5-tetrazine; 3,6-diethyl-1,2,4,5-tetrazine; 3,6-dipropyl-1,2,4,5-tetrazine; and 3,6-diisopropyl-1,2,4,5-tetrazine. 8 . The method of claim 1 , wherein the passivation film has a thickness, and the method further comprises exposing the passivation film to a second monomer to increase the thickness of the passivation film.
9. The method of claim 8, wherein the second monomer is an alkyne derivative.
10. The method of claim 9, wherein the alkyne derivative comprises a diyne or triyne derivative.
11. The method of claim 9, wherein the alkyne derivative is selected from the group consisting of 1,4-diethynylbenzene and 1,3,5-triethynylbenzene.
12. The method of claim 8, wherein the method further comprises performing an atomic layer deposition (ALD) process to deposit an ALD film having a thickness on the second surface, wherein the thickness of the ALD film is less than or equal to the thickness of the passivation film.
13. The method of claim 12, wherein the second surface is a metal surface and the ALD film is selected from the group consisting of Cu, Co, Ni, W, Ru, Cr, Fe, Pt, Au, Ag, Mo, Ga, and In.
14. The method of claim 12, wherein the second surface is a dielectric surface and the ALD film is selected from SiO x 、Si x N y 、Si、SiON、AlO x 、Al2O3、HfO x 、ZrO2、TiO x 、TiN、Ta x O5, Y2O3, La2O3, AlN, MgO, CaF2, LiF, SrO, SiC, BaO, HfSiO4, LaAlO3, Nb2O5, BaTiO3, SrTiO3, Bi4Ti3O 12 、Pb(Zr,Ti)O3、CaCu3Ti4O 12 , LiNbO3, BaTiO3, and KNbO3.
15. A method for depositing an ALD film, the method comprising: (a) exposing a substrate comprising a first surface and a second surface to an anchor reactant, wherein the anchor reactant is a 4-ethynylbenzene derivative having a head group selectively targeted to the first surface and forming a seed layer; (b) forming a passivation film, wherein the seed layer is exposed to a first monomer to form the passivation film having a thickness of Å; (c) increasing the thickness of the passivation film, wherein the passivation film reacts with a second monomer; (d) performing atomic layer deposition to deposit the ALD film having a thickness on the second surface, wherein the thickness of the ALD film is maintained equal to or less than the thickness of the passivation film; (e) sequentially repeating steps (b), (c) and (d) at least once, wherein with each repetition of (b) and (c), the passivation film increases in thickness in the range of from 1 nm to 50 nm; and (f) Removing the passivation film by exposure to O2 or O2 plasma.
16. The method of claim 15, wherein the method further comprises sequentially repeating (c), (d) and (e) at least once, wherein with each repetition, (c) and (d) increase the thickness of the passivation film within a range from 1 nm to 50 nm.
17. The method of claim 16, further comprising removing the passivation film, wherein the removing is performed by exposing the first surface to O2 or O2 plasma.
18. A non-transitory computer readable medium comprising instructions that, when executed by a controller of a substrate processing chamber, cause the substrate processing chamber to perform the method of claim 1.
Citation Information
Patent Citations
Surface-selective atomic layer deposition using hydrosilylation passivation
CN108028172A
Schemes for selective deposition for patterning applications
CN110226224A
Microelectronic process and structure
KR1020040017785A
Molecular self-assembly in substrate processing
US20060108320A1
Selective Deposition With Alcohol Selective Reduction And Protection
US20160064275A1