A method for tin-based coating of positive electrode material precursor and positive electrode material precursor

Through tin-based coating technology, a porous coating layer is formed, which solves the structural and electrochemical performance problems of lithium-ion battery cathode materials under high voltage, improves the migration rate and electrochemical performance of lithium ions, and extends the cycle life of the battery. .

CN114824211BActive Publication Date: 2024-10-15GUANGDONG BRUNP RECYCLING TECH CO LTD +2
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202210433703.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-04-24
Publication Date
2024-10-15
Estimated Expiration
2042-04-24

AI Technical Summary

Technical Problem

Existing lithium-ion battery cathode materials have problems such as structural phase change, transition metal dissolution, oxygen evolution, and electrolyte oxidative decomposition under high voltage, which limits their application in high-energy-density lithium batteries, and commonly used coating materials Low electronic conductivity hinders the migration of lithium ions and reduces electrochemical performance.

Method used

Using a tin-based coating method, a porous coating layer is formed by mixing nickel cobalt manganese hydroxide with a solution of carbonate ions and sulfide ions, adding a stannous source and performing solid-liquid separation, and then immersing it in a persulfide salt solution. , improve the conductivity and lithium ion migration rate of the cathode material.

Benefits of technology

It achieves high conductivity and excellent electrochemical performance of the cathode material, improves the intercalation and extraction capabilities of lithium ions, reduces side reactions with the electrolyte, and extends the cycle life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114824211B_ABST
    Figure CN114824211B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a tin-based coated positive electrode material precursor, comprising the following steps: (1) mixing nickel-cobalt-manganese hydroxide with a solution containing carbonate ions and sulfide ions; (2) adding a stannous source solution to the mixed solution of step (1) to react and separate the solid from the liquid to obtain a solid product; (3) soaking the solid product obtained in step (2) in a persulfide salt solution, performing solid-liquid separation, washing, and drying to obtain a positive electrode material precursor. The positive electrode material prepared by the positive electrode material precursor prepared by the preparation method has excellent electrical conductivity and lithium ion migration rate, ensuring that the positive electrode material has good electrochemical performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium battery positive electrode materials, and in particular relates to a method for tin-based coating of a positive electrode material precursor and a positive electrode material precursor. Background Art

[0002] As a new type of green power source, lithium-ion batteries have been widely used in consumer electronics and new energy vehicles due to their advantages such as high operating voltage, long cycle life, light weight, low self-discharge, no memory effect and high cost performance. Among them, the positive electrode material is one of the core parts of lithium-ion batteries, which determines the performance of lithium-ion batteries. The positive electrode material limits the energy density, power density and cycle life of lithium-ion batteries. It can be said that the development of positive electrode materials determines the development direction of lithium-ion batteries.

[0003] With the rapid development of electric vehicles, smart electronic devices and other fields, there is an urgent need for high-energy-density lithium batteries with long cycle life and high safety. Using a positive electrode with high voltage and high specific capacity is an effective way to improve the energy density of batteries. Among them, layered positive electrode materials have received widespread attention due to their high theoretical specific capacity, but their application under high voltage still has many problems and challenges, especially the structural phase change at the interface with the electrolyte, transition metal dissolution, oxygen precipitation, and continuous oxidation and decomposition of the electrolyte, which seriously limit their application in high-energy-density lithium batteries.

[0004] In view of the above problems, in the prior art, a coating layer can be formed on the surface of the positive electrode material precursor to optimize the structural performance and electrochemical performance of the particles, improve the corrosion resistance of the positive electrode material, and reduce the side reaction between the material and the electrolyte. The more common coating materials are oxides, fluorides, lithium ion conductors, etc. The coating layer reduces the contact resistance between the particles while separating the material from the electrolyte, reducing the side reaction between the material and the electrolyte, and preventing the HF gas decomposed by the electrolyte from corroding the positive electrode material.

[0005] However, the coating materials used in the existing methods for preparing positive electrode material precursors containing coating layers are mostly oxide materials with low electronic conductivity, thereby increasing the resistivity of the positive electrode material; and the coating layer on the prepared positive electrode material precursor is too dense, which hinders the migration rate of lithium ions and causes the electrochemical performance of the final positive electrode material to decline. Summary of the invention

[0006] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention provides a method for coating a tin-based positive electrode material precursor and a positive electrode material precursor. The positive electrode material prepared by the positive electrode material precursor prepared by the preparation method has excellent electrical conductivity and lithium ion migration rate, ensuring that the positive electrode material has good electrochemical performance.

[0007] The above technical objectives of the present invention are achieved through the following technical solutions:

[0008] A method for coating a positive electrode material precursor with a tin base comprises the following steps:

[0009] (1) mixing nickel-cobalt-manganese hydroxide with a solution containing carbonate ions and sulfide ions;

[0010] (2) adding a stannous source solution to the mixed solution of step (1) to react and separate the solid from the liquid to obtain a solid product;

[0011] (3) The solid product obtained in step (2) is immersed in a persulfide salt solution, and then the solid-liquid separation is performed, and the positive electrode material precursor is obtained after washing and drying.

[0012] Preferably, in step (1), the nickel-cobalt-manganese hydroxide is mixed with a solution containing carbonate ions and sulfide ions at a solid-to-liquid ratio of 1 g:(1-5) mL.

[0013] Preferably, the concentration of carbonate ions in the solution containing carbonate ions and sulfide ions in step (1) is 0.1-1.0 mol / L.

[0014] Preferably, the concentration of sulfide ions in the solution containing carbonate ions and sulfide ions in step (1) is 0.1-1.0 mol / L.

[0015] Preferably, the stannous source in the stannous source solution in step (2) is a soluble stannous salt.

[0016] Preferably, the stannous source in the stannous source solution in step (2) is at least one of stannous chloride and stannous sulfate.

[0017] Preferably, the concentration of stannous ions in the stannous source solution in step (2) is 0.01-1 mol / L.

[0018] Preferably, the stannous source solution in step (2) is added dropwise into the mixed solution of step (1).

[0019] Preferably, the dripping rate of the stannous source solution in step (2) is 25-50 mL / h.

[0020] Preferably, in step (2), when the pH of the mixed solution is between 8 and 9, the reaction is stopped and solid-liquid separation is performed.

[0021] Preferably, the persulfide salt in the persulfide salt solution in step (3) is at least one of sodium persulfide or ammonium persulfide.

[0022] Preferably, the concentration of the persulfide salt in the persulfide salt solution in step (3) is 0.1-1 mol / L.

[0023] Preferably, in step (3), the solid product is mixed with the persulfide salt solution at a solid-liquid ratio of 1 g:(1-5) mL.

[0024] Preferably, the soaking time in step (3) is 1-24 hours.

[0025] Preferably, the washing method in step (3) is to first wash with deionized water and then wash with ethanol or acetone.

[0026] Preferably, the drying method in step (3) is vacuum drying at 50-80° C. for 2-12 h.

[0027] Preferably, a method for coating a tin-based positive electrode material precursor comprises the following steps:

[0028] S1. Prepare a stannous ion concentration of 0.01-1 mol / L stannous source solution, the stannous source is stannous chloride, stannous sulfate, at least one;

[0029] S2. Prepare a mixed solution of sodium carbonate and sodium sulfide, wherein the concentration of sodium carbonate is 0.1-1.0 mol / L, and the concentration of sodium sulfide is 0.1-1.0 mol / L;

[0030] S3. The nickel-cobalt-manganese hydroxide was added to the mixed solution prepared in step (2) at a solid-liquid ratio of 1g: (1-5) mL;

[0031] S4. Under constant stirring at a stirring speed of 200-500r / min, the stannous source solution prepared in step (1) was added dropwise to the mixed solution at a drop rate of 25-50mL / h;

[0032] S5. When the pH of the mixed solution is detected to be 8-9, the reaction is stopped, and solid-liquid separation is performed to obtain a wet material;

[0033] S6. According to the solid-liquid ratio of 1g: (1-5) mL, the wet material was added to a 0.1-1mol / L sodium persulfide / ammonium persulfide solution and soaked for 1-24h;

[0034] S7. After solid-liquid separation, the solid is first washed with deionized water and then with ethanol or acetone;

[0035] S8. After washing, vacuum dry at 50-80°C for 2-12 hours to obtain a tin-based coated positive electrode material precursor.

[0036] A positive electrode material precursor is prepared by the preparation method described above.

[0037] A positive electrode material is prepared by mixing and sintering a lithium source and the positive electrode material precursor as described above.

[0038] A lithium-ion battery comprising the positive electrode material as described above.

[0039] The beneficial effects of the present invention are:

[0040] (1) The present invention mixes nickel cobalt manganese hydroxide into a mixed solution containing carbonate ions and sulfide ions, and then drops a stannous source solution to generate a mixed precipitate of stannous hydroxide and stannous sulfide, which is then coated on the surface of a precursor (nickel cobalt manganese hydroxide). Finally, a persulfide salt is used to further dissolve the coating layer on the surface of the precursor, thereby removing the stannous sulfide in the coating layer and leaving the position originally occupied by the stannous sulfide in the precursor coating layer vacant, thereby making the coating layer loose and porous, thereby obtaining a precursor material having a porous coating layer.

[0041] The reaction equation is as follows: After the stannous source solution is added, the stannous ions are hydrolyzed and stannous sulfide precipitates are generated: Sn 2+ +2OH - =Sn(OH)2↓、Sn 2+ +S 2- =SnS↓The coating further dissolves in the persulfide salt solution: SnS+S2 2- =SnS3 2- .

[0042] (2) The precursor prepared by this method has a layer of stannous hydroxide coated on its surface. When it is subsequently sintered with a lithium source to prepare a positive electrode material, the coating layer will be dehydrated and oxidized to form tin dioxide with high conductivity, thereby improving the electronic conductivity of the positive electrode material. At the same time, the positive electrode material inherits the morphological characteristics of the precursor, and its surface coating layer has a porous structure, which further improves the mobility of lithium ions, facilitates the embedding and extraction of lithium in the positive electrode material, and isolates the side reactions between the positive electrode material and the electrolyte, thereby improving the cycle performance of the material. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 This is a SEM image of the cathode material precursor prepared in Example 1 of the present invention, magnified 10,000 times;

[0044] Figure 2 This is a SEM image of the positive electrode material precursor prepared in Example 1 of the present invention, magnified 100,000 times. DETAILED DESCRIPTION

[0045] The present invention will be further described below in conjunction with specific embodiments.

[0046] Embodiment 1:

[0047] A method for coating a positive electrode material precursor with a tin base comprises the following steps:

[0048] S1. Prepare a 0.5 mol / L stannous chloride solution;

[0049] S2. Prepare a mixed solution of sodium carbonate and sodium sulfide, wherein the concentration of sodium carbonate is 0.5 mol / L, and the concentration of sodium sulfide is 0.5 mol / L;

[0050] S3. Nickel cobalt manganese hydroxide (molecular formula: Ni 0.62 Mn 0.2 Co 0.18 (OH)2) was added to the mixed solution prepared in step (2) at a solid-liquid ratio of 1 g:3 mL;

[0051] S4. Under constant stirring at a stirring speed of 300r / min, the stannous chloride solution prepared in step (1) was added dropwise to the mixed solution at a dropping rate of 35mL / h;

[0052] S5. When the pH of the mixed solution is detected to be 8-9, the reaction is stopped, and solid-liquid separation is performed to obtain a wet material;

[0053] S6. According to the solid-liquid ratio of 1g:3mL, the wet material was added to a 0.5mol / L sodium persulfide / ammonium persulfide solution and soaked for 12h;

[0054] S7. After solid-liquid separation, the solid is first washed with deionized water and then with ethanol;

[0055] S8. After washing, vacuum drying is performed at 65°C for 7 hours to obtain a tin-based coated positive electrode material precursor.

[0056] A positive electrode material precursor is prepared by the preparation method as described above, and its SEM image magnified 10000 times is as follows Figure 1 As shown, the SEM image magnified 100,000 times is as follows Figure 2 shown.

[0057] Embodiment 2:

[0058] A method for coating a positive electrode material precursor with a tin base comprises the following steps:

[0059] S1. Prepare a stannous chloride solution with a concentration of 0.01 mol / L;

[0060] S2. Prepare a mixed solution of sodium carbonate and sodium sulfide, wherein the concentration of sodium carbonate is 0.1 mol / L, and the concentration of sodium sulfide is 0.1 mol / L;

[0061] S3. Nickel-cobalt-manganese hydroxide (molecular formula: Ni 0.62 Mn0.2 Co 0.18 (OH)2) was added to the mixed solution prepared in step (2) at a solid-liquid ratio of 1 g:1 mL;

[0062] S4. Under constant stirring at a stirring speed of 200r / min, the stannous chloride solution prepared in step (1) was added dropwise to the mixed solution at a dropping rate of 25mL / h;

[0063] S5. When the pH of the mixed solution is detected to be 8-9, the reaction is stopped, and solid-liquid separation is performed to obtain a wet material;

[0064] S6. According to the solid-liquid ratio of 1g:1mL, the wet material was added to a 0.1mol / L sodium persulfide / ammonium persulfide solution and soaked for 1h;

[0065] S7. After solid-liquid separation, the solid is first washed with deionized water and then with ethanol;

[0066] S8. After washing, vacuum drying is performed at 50°C for 12 hours to obtain a tin-based coated positive electrode material precursor.

[0067] A positive electrode material precursor is prepared by the preparation method described above.

[0068] Embodiment 3:

[0069] A method for coating a positive electrode material precursor with a tin base comprises the following steps:

[0070] S1. Prepare a 1 mol / L stannous sulfate solution;

[0071] S2. Prepare a mixed solution of sodium carbonate and sodium sulfide, wherein the concentration of sodium carbonate is 1.0 mol / L, and the concentration of sodium sulfide is 1.0 mol / L;

[0072] S3. Nickel-cobalt-manganese hydroxide (molecular formula: Ni 0.85 Mn 0.08 Co 0.07 (OH)2) was added to the mixed solution prepared in step (2) at a solid-liquid ratio of 1 g:5 mL;

[0073] S4. Under constant stirring at a stirring speed of 500r / min, the stannous sulfate solution prepared in step (1) was added dropwise to the mixed solution at a dropping rate of 50mL / h;

[0074] S5. When the pH of the mixed solution is detected to be 8-9, the reaction is stopped, and solid-liquid separation is performed to obtain a wet material;

[0075] S6. According to the solid-liquid ratio of 1g:5mL, the wet material was added to a 1mol / L sodium persulfide / ammonium persulfide solution and soaked for 24h;

[0076] S7. After solid-liquid separation, the solid is first washed with deionized water and then with acetone;

[0077] S8. After washing, vacuum drying is performed at 80°C for 2 hours to obtain a tin-based coated positive electrode material precursor.

[0078] A positive electrode material precursor is prepared by the preparation method described above.

[0079] Test example:

[0080] The nickel cobalt manganese hydroxide used in Example 1-3 was used as Comparative Example 1-3. The positive electrode material precursor obtained in Example 1-3 and the nickel cobalt manganese hydroxide used in Example 1-3 were used as raw materials, and lithium hydroxide was prepared according to a Li / (Ni+Co+Mn) molar ratio of 1.04, and the temperature was raised to 750°C in an oxygen atmosphere furnace, kept warm for 10 hours, and then cooled, crushed, and sieved with the furnace to obtain the corresponding positive electrode material. The conductivity of each positive electrode material was tested, and the results are shown in Table 1:

[0081] Table 1: Test results of conductivity of positive electrode materials

[0082] Conductivity(s / cm) Volume resistivity (Ω·cm) Example 1 <![CDATA[3.46*10 -2 ]]> 36.1 Example 2 <![CDATA[1.73*10 -2 ]]> 38.9 Example 3 <![CDATA[3.98*10 -2 ]]> 34.3 Comparative Example 1 <![CDATA[2.88*10 -3 ]]> 358.6 Comparative Example 2 <![CDATA[2.84*10 -3 ]]> 359.3 Comparative Example 3 <![CDATA[2.86*10 -3 ]]> 358.8

[0083] As shown in Table 1, the positive electrode material prepared by the positive electrode material precursor of the present invention has excellent electrical conductivity, and its electrical conductivity is less than 3.98*10 -2 s / cm, and the volume resistivity is less than 34.3Ω·cm. By comparing Example 1 with Comparative Example 1, Example 2 with Comparative Example 2, and Example 3 with Comparative Example 3, it can be seen that the conductivity of the positive electrode material made from the tin-based coated positive electrode material precursor of the present invention is much better than that of the positive electrode material made from the positive electrode material precursor without tin-based coating.

[0084] At the same time, with each positive electrode material, acetylene black as a conductive agent, PVDF as a binder, the active material, conductive agent, and binder are weighed in a ratio of 92:4:4, and a certain amount of organic solvent NMP is added. After stirring, it is coated on aluminum foil to make a positive electrode sheet. The negative electrode uses a metal lithium sheet and is made into a lithium-ion battery in a glove box filled with argon. Charge and discharge at a current of 3.6A at room temperature to test the first efficiency (%), 0.1C discharge specific capacity, 1C discharge specific capacity, and 300-week cycle retention rate (%). The test results are shown in Table 2:

[0085] Table 2: Battery electrochemical performance test results

[0086]

[0087] It can be seen from Table 2 that after the positive electrode material prepared by the positive electrode material precursor of the present invention is assembled into a battery, the battery has excellent electrochemical properties, and its first efficiency reaches 92.3% or more, the 0.1C discharge specific capacity can reach 192.1mAh / g or more, the 1C discharge specific capacity can reach 178.4mAh / g or more, and the 0.1C cycle 300 times The capacity retention rate can reach 90.1% or more. At the same time, by comparing Example 1 with Comparative Example 1, Example 2 with Comparative Example 2, and Example 3 with Comparative Example 3, it can be seen that after the positive electrode material made of the tin-based coated positive electrode material precursor of the present invention is assembled into a battery, the electrochemical performance of the battery is better than that of the battery assembled with the positive electrode material made of the positive electrode material precursor without tin-based coating.

[0088] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A method for preparing a tin-based coated positive electrode material precursor, characterized in that: The steps include: (1) mixing nickel-cobalt-manganese hydroxide with a solution containing carbonate ions and sulfide ions; (2) adding a stannous source solution to the mixed solution of step (1) to react and separate the solid and liquid to obtain a solid product, wherein the solid product is a nickel-cobalt-manganese hydroxide having a coating layer on the surface, wherein the coating layer is a mixed precipitate of stannous hydroxide and stannous sulfide; (3) The solid product obtained in step (2) is immersed in a persulfide salt solution to remove the stannous sulfide in the coating layer, and then the solid-liquid is separated, washed, and dried to obtain a positive electrode material precursor.

2. The method for preparing a tin-based coated positive electrode material precursor according to claim 1, characterized in that: In step (1), nickel-cobalt-manganese hydroxide is mixed with a solution containing carbonate ions and sulfide ions at a solid-liquid ratio of 1 g:(1-5) mL.

3. The method for preparing a tin-based coated positive electrode material precursor according to claim 1, characterized in that: The concentration of sulfide ions in the solution containing carbonate ions and sulfide ions in step (1) is 0.1-1.0 mol / L.

4. The method for preparing a tin-based coated positive electrode material precursor according to claim 1, characterized in that: The concentration of stannous ions in the stannous source solution in step (2) is 0.01-1 mol / L.

5. The method for preparing a tin-based coated positive electrode material precursor according to claim 1, characterized in that: The stannous source solution in step (2) is added dropwise into the mixed solution of step (1).

6. The method for preparing a tin-based coated positive electrode material precursor according to claim 1, characterized in that: When the pH of the mixed solution in step (2) is between 8 and 9, the reaction is stopped and solid-liquid separation is performed.

7. The method for preparing a tin-based coated positive electrode material precursor according to claim 1, characterized in that: The concentration of the persulfide salt in the persulfide salt solution in step (3) is 0.1-1 mol / L.

8. The method for preparing a tin-based coated positive electrode material precursor according to claim 1, characterized in that: In step (3), the solid product is mixed with the persulfide salt solution at a solid-liquid ratio of 1 g: (1-5) mL.

9. A cathode material precursor, characterized in that: The invention is prepared by the preparation method according to any one of claims 1 to 8.

10. A positive electrode material, characterized in that: It is formed by mixing and sintering a lithium source and the positive electrode material precursor according to claim 9.

Citation Information

Patent Citations

  • Positive electrode of lithium manganate material battery, preparation method and lithium manganate battery

    CN111193007A

  • Lithium-rich manganese-based positive electrode material surface modification method and lithium-rich manganese-based positive electrode material

    CN113788500A

  • Metal sulfide sodium ion battery negative electrode material and preparation method thereof

    CN114229884A

  • Ni-rich positive composition for lithium secondary battery using spherical transition metal complex hydroxide with nano-titanate and manufacturing method thereof

    KR1020180105762A