High performance plain and high expansion elements for oil and gas applications
By using thiocarbamate/acrylate polymer and 3D printing technology, combined with anti-extrusion device design, the problem of insufficient material brittleness and toughness in downhole sealing applications is solved, and high-performance sealing under high temperature and high pressure conditions is achieved , reduces the number of components of the sealing device and improves operating efficiency.
Patent Information
- Application Number
- CN202180007250.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-01-20
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2041-01-20
Smart Images

Figure CN114846219B_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to U.S. application serial number 17 / 152,887, filed on January 20, 2021, entitled “HIGH PERFORMANCE REGULAR AND HIGH EXPANSION ELEMENTS FOR OIL AND GAS APPLICATIONS,” and claims the benefit of U.S. application serial number 62 / 965,539, filed on January 24, 2020, entitled “3D PRINTED HIGH PERFORMANCE REGULAR AND HIGH EXPANSION ELEMENTS FOR OIL AND GAS APPLICATIONS,” both of which are commonly assigned with this application and are incorporated herein by reference in their entirety. Background Art
[0003] Significant challenges exist in designing high performance plain and high expansion components (e.g., sealing components such as packer components, plugs, etc.) for oil and gas applications. Such component designs are often complex, for example involving many sealing components such as contained in a through-the-tubing bridge plug. One way to simplify the design is to build a single component (e.g., with internal features that control its own expansion). However, there are currently no robust single component materials for downhole sealing applications. Available rubbers, like 3D printed polymers, are typically brittle, with low fracture toughness and low elongation at break. BRIEF DESCRIPTION OF THE DRAWINGS
[0004] Reference is now made to the following description in conjunction with the accompanying drawings, in which:
[0005] Figure 1 and 2 is a perspective view of a well system including an exemplary operating environment in which the apparatus, systems, and methods disclosed herein may be employed;
[0006] Figure 3 A flow chart showing an exemplary method for preparing a VAT resin for a thiourethane polymer according to the principles of the present disclosure is shown;
[0007] Figure 4 A flow chart showing an example method of three-dimensional stereolithographic printing of thiourethane polymer parts according to the principles of the present disclosure;
[0008] Figure 5A cross-sectional view depicting a downhole sealing device having an elastomeric element designed, manufactured, and operated in accordance with the present disclosure is shown;
[0009] Figure 6 A cross-sectional view depicting an alternative downhole sealing device having an elastomeric element designed, manufactured, and operated in accordance with the present disclosure is shown;
[0010] Figure 7 shows a cross-sectional view depicting a downhole sealing device in an uncompressed state positioned within a tubular member according to certain aspects of the present disclosure;
[0011] Figure 8 A diagram illustrating some aspects of the present disclosure is shown. Figure 7 A cross-sectional view of a downhole sealing device in a compressed state (e.g., a set state);
[0012] Fig. 9 illustrates an end view of an anti-extrusion device in an expanded state according to certain aspects of the present disclosure;
[0013] Fig.10 According to certain aspects of the present disclosure Fig. 9 An isometric view of the anti-extrusion device in a retracted state;
[0014] Fig.11 According to certain aspects of the present disclosure Fig. 9 An isometric view of the anti-extrusion device in an expanded state; and
[0015] Fig.12 A flow chart depicting a process for forming a downhole sealing device according to certain aspects of the present disclosure is presented. DETAILED DESCRIPTION
[0016] In the drawings and description that follow, similar components are generally labeled with the same reference numerals throughout the specification and drawings, respectively. The drawings drawn are not necessarily, but may be to scale. For the sake of clarity and conciseness, certain features of the present disclosure may be shown exaggerated in scale or in slightly schematic form, and some details of certain elements may not be shown.
[0017] The present disclosure can be implemented in different forms of embodiments. Specific embodiments are described in detail and shown in the accompanying drawings, and it should be understood that the present disclosure is considered to be an example of the principles of the present disclosure, and is not intended to limit the present disclosure to the contents shown and described herein. It should be fully recognized that the different teachings of the embodiments discussed herein can be adopted individually or in any suitable combination to produce the desired results. In addition, all statements of the principles and aspects of the present disclosure and its specific examples described herein are intended to cover their equivalents. In addition, as used herein, unless otherwise indicated, the term "or" refers to a non-exclusive "or".
[0018] Unless otherwise stated, the use of the terms “connected,” “engaged,” “coupled,” “attached,” or any other similar terms describing the interaction between elements is not meant to limit the interaction to the direct interaction between the elements and may also include the indirect interaction between the elements described.
[0019] Unless otherwise specified, the use of the terms "upward", "upper", "upward", "uphole", "upstream" or other similar terms should be interpreted as generally toward the surface of the well; similarly, the use of the terms "downward", "lower", "downward", "downhole" or other similar terms should be interpreted as generally toward the bottom, end, of the well, regardless of the wellbore orientation. The use of any one or more of the above terms should not be interpreted as indicating a position along a completely vertical or horizontal axis. Unless otherwise specified, the use of the term "formation" should be interpreted to cover both areas beneath exposed land and areas beneath land covered by a body of water such as ocean or fresh water.
[0020] refer to Figure 1 , depicts a perspective view of a well system 100 including an exemplary operating environment in which the devices, systems, and methods disclosed herein may be employed. For example, the well system 100 may employ a downhole sealing device 170 designed, manufactured, and / or operated according to any embodiment, aspect, application, variation, design, etc. disclosed in the following paragraphs. Figure 1 The well system 100 shown in FIG. 1 includes a service rig 110 (e.g., a drilling rig, completion rig, workover rig, or other mast structure or combination thereof) extending above and around a wellbore 120 formed in a formation 130. As will be appreciated by those skilled in the art, the wellbore 120 may be a fully cased, partially cased, or open hole wellbore. Figure 1 In the illustrated embodiment, the wellbore 120 is partially cased and, therefore, includes a cased region 140 and an open hole region 145. As depicted, the cased region 140 may employ a casing 150 held in place by cement 160.
[0021] According to at least one embodiment, Figure 1The well system 100 shown in FIG. 1 includes a downhole sealing device 170 located in a wellbore 120. The downhole sealing device 170 can be supported by a conveying tool 190, which can be a wireline, a slickline, a cable, a tubular (e.g., a drill string, a casing string, a completion string, a coiled tubing, etc.) or other structure suitable for supporting the downhole sealing device 170. In some aspects, the service rig 110 can include a derrick with a drill floor, and the conveying tool 190 extends downward from the service rig 110 into the wellbore 120 through the drill floor. In an offshore situation, in some embodiments, the service rig 110 can be supported by a riser or buttress extending downward to the seabed. Alternatively, the service rig 110 can be supported by a column located on a ballasted hull or pontoon (or both) below the water surface, which can be referred to as a semi-submersible platform or rig. In an offshore location, tubing can extend from the service rig to remove seawater and contain drilling fluid return. Other mechanical features not shown can control the entry and exit of the conveying tool 190 in the wellbore 120. Examples of these other mechanical features include a winch coupled to a hoisting device, a wireline unit or cable unit including a winch device, another maintenance vehicle, or other such mechanism. The downhole sealing device 170 can be a bridge plug, a packer, or another type of sealing device that can be used downhole. In addition, the downhole sealing device 170 can be located in the open hole area 145 of the wellbore 120, or alternatively as a sealant between two downhole tools.
[0022] In at least one embodiment, the downhole sealing device 170 may include an elastomeric element 172. In one or more embodiments, the elastomeric element 172 includes a thiocarbamate / acrylate polymer that is operable to, for example, press against a tubular member of the seal (e.g., the wellbore casing 150 in the illustrated embodiment) within the wellbore 120. As used herein, the term thiocarbamate / acrylate polymer is intended to encompass thiocarbamate polymers, thiol acrylate polymers, and blended combinations of thiocarbamate polymers and thiol acrylate polymers. Thus, in certain embodiments, the elastomeric element 172 may include a thiocarbamate polymer, and in other embodiments, the elastomeric element 172 may include a thiol acrylate polymer. However, in yet certain other embodiments, the elastomeric element 172 may include a blend of a thiocarbamate polymer and a thiol acrylate polymer, for example using various different proportions.
[0023] In at least one embodiment, the elastomeric element 172 is operable to, for example, press against a tubular member (e.g., the wellbore casing 150 in the illustrated embodiment) within the wellbore 120, and is operable to seal a pressure differential of at least 6,900 kPa (e.g., approximately 1,000 psi) at a temperature of at least 80° C., depending on the specific manufacturing process and composition of the elastomeric element 172. In another embodiment, the elastomeric element 172 is operable to, for example, press against a tubular member (e.g., the wellbore casing 150 in the illustrated embodiment) within the wellbore 120, and is operable to seal a pressure differential of at least 20,700 kPa (e.g., approximately 3,000 psi) at a temperature of at least 80° C. In yet another embodiment, the elastomeric element 172 is operable to, for example, press against a tubular member (e.g., the wellbore casing 150 in the illustrated embodiment) within the wellbore 120, and is operable to seal a pressure differential of at least 20,700 kPa at temperatures as low as -65° C. and as high as 270° C., depending on the specific manufacturing process and composition of the elastomeric element 172. In other embodiments, the elastomeric element 172 is operable to, for example, press against a tubular member (e.g., the wellbore casing 150 in the illustrated embodiment) within the wellbore 120, and is operable to seal a pressure differential of at least 27,575 kPa (e.g., approximately 4,000 psi) at a temperature of at least 80° C. In at least one or more other embodiments, the elastomeric element 172 is operable to, for example, press against a tubular member (e.g., the wellbore casing 150 in the illustrated embodiment) within the wellbore 120 and is operable to seal a pressure differential of at least 27,575 kPa at temperatures as low as -65°C and as high as 270°C. Additionally, in at least one or more other embodiments, the elastomeric element 172 has a fracture toughness of at least 40 MJ / m 3 , and a tensile strength of at least 25 MPa. In at least one embodiment, elastomeric element 172 is susceptible to a high degree of elongation (eg, to at least about 200%).
[0024] In at least one embodiment, the downhole sealing device 170 is a first downhole sealing device, and the well system 100 additionally includes a second downhole sealing device 180. In at least this embodiment, the second downhole sealing device 180 can be placed proximate to the downhole sealing device 170, for example, to supplement the downhole sealing device 170. For example, the second downhole sealing device 180 can include a material different from the thiourethane / acrylate polymer (e.g., a polymer material), and thus accommodate applications that may lack the downhole sealing device 170. For example, the second downhole sealing device 180 may have a greater pressure rating at extremely high temperatures, where it has a lesser pressure rating at lower temperatures.
[0025] According to one embodiment, the elastomeric element 172 is coupled to one or more downhole sealing features. Figure 1 In an embodiment of the present invention, the one or more downhole sealing features are first and second end plates coupled to opposite ends of the elastomeric element 172, and the first and second end plates 174 are configured to move relative to each other to axially compress the elastomeric element 172 into engagement with the wellbore casing 150. If the downhole sealing device 170 is positioned in the open hole area 145 of the well system 100, the first and second end plates 174 axially compress the elastomeric element 172 into engagement with the wellbore 120 itself. In some cases, the elastomeric element 172 and the first and second end plates 174 are positioned between two anti-extrusion devices 176. As in Figure 1 As seen in FIG. 1 , the downhole seal 170 is in an uncompressed state and is able to move within the wellbore 120. Once located at the desired position, an axial compressive force can be applied to the first and second end plates 174 to axially compress the elastomeric element 172 into a compressed state, such as Figure 2 shown.
[0026] Figure 2 According to certain aspects of the present disclosure Figure 1 Schematic diagram of a well system 100 including a downhole sealing device 170 in a compressed state. An axial compressive force 205 is applied to the elastomeric element 172 through the first and second end plates 174 to deform the elastomeric element 172 so that the elastomeric element 172 forms a seal in the wellbore 120. In the event that an anti-extrusion device 176 is used, the axial compressive force 205 can cause the anti-extrusion device 176 to expand in diameter and provide a surface that the deformable elastomeric element 172 cannot easily pass through (e.g., to prevent the elastomeric element 172 from deforming too much and exceeding the end plates 174). In some cases, the axial compressive force 205 can be removed from the downhole sealing device 170 or an axial extension force can be applied to the downhole sealing device (e.g., in a direction opposite to the axial compressive force 205) to return the downhole sealing device 170 to an uncompressed state, such as in Figure 1 As seen in.
[0027] Elastomeric elements designed, manufactured and operated according to the present disclosure may be applied to, but are not limited to, the following: 1) O-ring applications manufactured using 3D printing or other conventional methods (e.g., at -65°C to 270°C); 2) T-seals, stacked seals, four-petal seals, bonded seals or any other sealing applications manufactured using 3D printing or other conventional methods (e.g., at -65°C to 270°C); 3) ExtremGrip ELH elastomer components manufactured using 3D printing or other conventional methods (e.g., at -40°C to 250°C); 4) Packer elements with external complex or simple geometric features manufactured using 3D printing or other conventional methods (e.g., at -65°C to 270°C); 5) Packer elements with internal geometric features and with or without external features manufactured using 3D printing methods (e.g., at -65°C to 270°C); 6) Seals for on-demand or one-time applications manufactured using 3D printing methods (e.g., at -6 5°C to 270°C); 7) legacy seals no longer in commercial production manufactured using 3D printing methods (at -65°C to 270°C); 8) sealing elements bonded to a rigid substrate manufactured directly using 3D printing methods (e.g., at -65°C to 270°C); and 9) multi-component packer elements and bonded sealing systems with crystalline or high Tg regions that act as an integrated backup system manufactured using 3D printing or other conventional methods (e.g., at -65°C to 270°C). The above seals can be any type of packer for recoverable, production, permanent packers, for bridge plugs, for plug and abandonment applications, for hydraulic fracturing, for onshore or offshore applications, for conventional and HPHT applications, and to a certain extent (e.g., up to 270°C) geothermal applications. In addition, the seals can be used statically or dynamically.
[0028] All seals described above and their variants may or may not have backup, for example depending on the pressure rating and / or application temperature. Typically, for high pressures and / or temperatures, appropriately designed backups are used, which significantly improve the performance of components made from this material.
[0029] Using elastomeric elements made in accordance with this disclosure has the following additional benefits: reducing the part count of high expansion packers / plugs; expanding the design space to elements with internal geometric features, as well as compositional changes within components that change the glass transition and / or crystallinity to affect mechanical behavior; allowing 3D printed elements with internal features to have very high expansion rates (e.g., 150% or 200%, instead of approximately 25%); significantly increasing the temperature range of sealing applications from -65°C to 270°C; improving operational efficiencies by manufacturing high expansion elements on-site on-demand for manufacturers, operators and their customers; and potentially replacing common oil and gas elastomers where acidic conditions are a concern.
[0030] Thiocarbamate polymer
[0031] As part of the present disclosure, VAT resin additives suitable for making thiourethane polymer parts are being used. One embodiment of the present disclosure includes a photopolymerizable thiourethane resin for additive manufacturing in an oxygen environment, the resin comprising: a first type of monomer, the first type of monomer comprising two or more thiol functional groups; a second type of monomer, the second type of monomer comprising two or more isocyanate functional groups; a photolatent base, wherein the photolatent base can decompose upon exposure to light to form a non-nucleophilic base catalyst having a pKa greater than 7; an anionic step-growth polymerization inhibitor, the inhibitor having an acidic group configured to form an acid-base pair with the non-nucleophilic base; and a light absorber, the light absorber having an absorbance in the liquid mixture greater than the absorbance of the photolatent base at the wavelength of the light used for the exposure.
[0032] In at least one embodiment, because thiourethane polymers are cured using non-nucleophilic Lewis bases, free radical initiators and free radical or oxygen inhibitor additives developed for use with acrylate-based resins may not be suitable for use with thiourethane polymer manufacturing methods and systems.
[0033] As further disclosed herein, embodiments of the VAT resin can include a combination of resin additives including anionic step-growth polymerization inhibitors (e.g., cationic inhibitors) and light absorbers. These resin additives can be provided in amounts to reduce or prevent the propagation of thiourethane polymer photopolymerization in areas outside of the photodefined development area of the VAT resin, thereby improving the photodefinition of the thiourethane polymer part.
[0034] Therefore, one aspect of the present disclosure is a VAT resin for three-dimensional (3D) SLA printing of thiourethane polymer parts (e.g., elastomeric elements). Some embodiments of the resin may include a liquid mixture comprising a first type of monomer, a second type of monomer, and a photolatent base. The first type of monomer may include two or more thiol functional groups, and the second type of monomer may include two or more isocyanate functional groups. The photolatent base decomposes when exposed to light to form a non-nucleophilic base catalyst with a pKa greater than 7. The VAT resin may further include an anionic step-growth polymerization inhibitor having an acidic group configured to form an acid-base pair with a non-nucleophilic base. The VAT resin may also include a light absorber having an absorbance in the liquid mixture greater than the absorbance of the photolatent base in the liquid mixture at the wavelength of light for exposure.
[0035] In some embodiments, the VAT resin is substantially free of water (e.g., in some embodiments, less than 0.1 wt % or less than 0.01 wt % or less than 0.001 wt %). For example, anhydride or non-hydrated forms of monomers, photolatent bases, inhibitors, and light absorbers are used in a liquid mixture of the resin.
[0036] Although not limiting the scope of the present disclosure by theoretical considerations, it is believed that the shelf life of the resin can be reduced by the presence of water, which may be due to the reaction between the water and the isocyanate functional groups of the second type of monomers, thereby reducing the total number of isocyanate functional monomers available to participate in the step-growth polymerization reaction to form the thiocarbamate polymer part, and may form cyanuric acid byproducts that can degrade the structure of the cured thiocarbamate polymer part. In addition, it is believed that one of the reaction products between water and the isocyanate functional groups can be carbonic acid, which in turn can form cyanuric anhydride. It is further believed that although cyanuric anhydride can extend the polymer chain, when the chain breaks, it releases CO2, which in turn can degrade the structure of the cured printed polymer part.
[0037] In some embodiments of the VAT resin, the molar ratio of photolatent base to anionic step-growth polymerization inhibitor is in the range of about 5: 1 to 15: 1, and in some embodiments is about 10: 1. Such ratios are advantageous in allowing polymerization to proceed in the target area illuminated by light, where the light causes a relatively high concentration of activated non-nucleophilic base catalyst molecules (e.g., photodecomposed photolatent base molecules), while still providing sufficient inhibitor molecules in the non-target area to form an acid-base pair with the activated non-nucleophilic base catalyst molecules that have diffused out of the target area.
[0038] In some embodiments, the anionic step-growth polymerization inhibitor is a strong organic acid and is non-oxidizing. In other words, the inhibitor is substantially completely ionized (e.g., greater than 90% ionized, and in some embodiments greater than 99% ionized) in the liquid mixture of the resin, and the inhibitor does not substantially oxidize the thiol functional groups of the first type of monomers in the liquid mixture. The use of anionic step-growth polymerization inhibitors that are strong acids promotes the availability of acid groups that can form acid-base pairs with activated non-nucleophilic base catalyst molecules that diffuse into non-target areas of the resin, for example. The use of non-oxidizing anionic step-growth polymerization inhibitors helps to promote the shelf life of the resin by maintaining the availability of thiol functional groups that can participate in the polymerization reaction.
[0039] Non-limiting exemplary embodiments of anionic step-growth polymerization inhibitors include: octanoic acid, methanesulfonic acid, trifluoromethanesulfonic acid, or carboxylic acid. For example, in some embodiments, the concentration of anionic step-growth polymerization inhibitor of p-toluenesulfonic acid in the liquid mixture ranges from about 0.001 wt% to 0.2 wt%, and in some embodiments, ranges from about 0.05 wt% to 0.2 wt%.
[0040] In some embodiments, the absorbance of the light absorber in the liquid mixture is at least about 1% higher than the absorbance of the photolatent base at the wavelength of light to which the resin is exposed. In certain other embodiments, it is 5%, 10%, or even 20% higher.
[0041] Such embodiments facilitate the photolatent base molecules to absorb sufficient light and thereby activate the non-nucleophilic base catalyst molecules in the target area to catalyze the polymerization reaction, while still allowing the light absorber to absorb light scattered into non-target areas of the resin and thereby reduce the amount of light available to activate the photolatent base molecules in the non-target areas.
[0042] In some embodiments, the light absorber is irradiated at a wavelength (e.g., at least about 10,000 nm) used to activate the photolatent base. -1 cm -1 ) at low concentrations. Having a high molar extinction coefficient facilitates the use of low (e.g., millimolar or lower concentrations) light absorbers in the fluid mixture of resins, which in turn facilitates complete dissolution of the light absorber in the mixture, for example, mitigating the light scattering effects of partially precipitated light absorbers.
[0043] Consider an example where the light absorber is or comprises 2,2'-(2,5-thiophenediyl)bis(5-tert-butylbenzoxazole (molar extinction coefficient at about 373 nm equal to about 47000 M -1 cm -1 ), whose concentration in the fluid mixture is in the range of about 0.001 wt% to 1 wt%. At a concentration of about 1 wt% (e.g., about 23 mM), the absorbance in the fluid mixture will be equal to about 1080. At a fluid concentration of about 0.01 wt% (e.g., about 0.23 mM), the absorbance in the fluid mixture will be equal to about 10.8, and at a fluid concentration of about 0.001 wt% (e.g., about 0.023 mM), the absorbance in the fluid mixture will be equal to about 1.08.
[0044] Based on this disclosure, one skilled in the relevant art will understand that the light absorber can be a molecule selected in the UV or visible light range to have a sufficiently high molar extinction coefficient to be soluble in the fluid mixture, and whose absorbance is greater than the absorbance of the photolatent base, and the wavelength of light is used to activate the photolatent base.
[0045] In some embodiments of the resin, the photolatent base is or comprises 5-(2'-(methyl)thioxanthone)-1,5-diazabicyclo[4.3.0]non-5-enetetraphenylborate. Other non-limiting examples of other photolatent bases may also be used.
[0046] In some embodiments, the first type of monomer in the resin is or comprises one or more of the following: 2,2'-(ethylenedioxy)diethylenethiol, decanedithiol, hexanedithiol, ethylene glycol dimercaptoacetate, ethylene glycol dimercaptopropionate, thiobisbenzenethiol, xylene dithiol, pentaerythritol tetrathioacetate, pentaerythritol tetrathiopropionate, dipentaerythritol hexamercaptopropionate, trimethylolpropane trimercaptoacetate, trimethylolpropane trimercaptoacetate, or tris[2-(3-mercaptopropionyloxy)ethyl]isocyanurate.
[0047] In some embodiments, the second type of monomer in the resin is or comprises one or more of the following: hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, octane diisocyanate, isophorone diisocyanate, xylene diisocyanate, toluene diisocyanate, phenylene diisocyanate, bis(isocyanatomethyl)cyclohexane, 4,4'-methylenebis(phenylisocyanate), 4,4'-methylenebis(cyclohexylisocyanate), or tris(6-isocyanatohexyl)isocyanurate.
[0048] Based on this disclosure, one skilled in the relevant art will understand that the amount of inhibitor and light absorber present in the resin will depend on the amount of photolatent base initiator present in the resin and the absorbance of the photolatent base at the wavelength of the light beam used to activate the exposure of the photolatent base to form the non-nucleophilic base catalyst.
[0049] Figure 3 Selected aspects of an example method 300 for preparing a VAT resin for a thiourethane polymer according to the principles of the present disclosure are presented by way of a flow chart.
[0050] Always continue to refer to Figure 3 , some embodiments of method 300 may include forming a liquid mixture (step 310). Forming the liquid mixture (step 310) includes combining a first type of monomer and a second type of monomer to form a monomer mixture (step 320). Any combination of the first type of monomer and the second type of monomer disclosed herein can be mixed together to form a homogenous monomer mixture. For example, the first type of monomer can contain two or more thiol functional groups, and the second type of monomer can contain two or more isocyanate functional groups.
[0051] Forming the liquid mixture (step 310) also includes adding an anionic step-growth polymerization inhibitor to the monomer mixture (step 330), for example, any anionic step-growth polymerization inhibitor having an acidic group configured to form an acid-base pair with a non-nucleophilic base.
[0052] Forming the liquid mixture (step 310) also includes adding a photolatent base to the monomer mixture (step 340), for example, any disclosed photolatent base that decomposes upon exposure to light to form a non-nucleophilic base catalyst having a pKa greater than 7.
[0053] Forming the liquid mixture (step 310) also includes adding a light absorber to the monomer mixture (step 350), for example, any light absorber having an absorbance in the liquid mixture greater than the absorbance at the wavelength of light to which the photolatent base is exposed.
[0054] Embodiments of method 300 may include sequentially adding any combination of anionic step-growth polymerization inhibitor, photolatent base, and light absorber to the monomer mixture, or simultaneously adding any two or all three thereof to the monomer mixture to form a homogenous liquid mixture.
[0055] Figure 4 Selected aspects of an example method 400 for three-dimensional stereolithographic printing of thiourethane polymer parts in accordance with the principles of the present disclosure are presented via a flow chart.
[0056] Always continue to refer to Figure 4 Some embodiments of method 400 may include adding a resin to a tank of a three-dimensional stereolithography printer (step 410). The resin may include any embodiment of a liquid mixture comprising a first type of monomer, a second type of monomer, a photolatent base, an anionic step-growth polymerization inhibitor, and a light absorber as disclosed herein.
[0057] Embodiments of method 400 may also include positioning (step 420) the resin or a platform of the build stage located in the tank such that the thin layer of resin is located above the platform.
[0058] In some embodiments, as part of positioning (step 420), the build table can be moved to allow a thin layer of resin (e.g., a layer having a thickness of 100 to 500 microns) to flow on top of a previously cured layer of the part. In other embodiments, as part of positioning (step 420), the amount of liquid platform in the tank can be increased by adding the liquid platform to the tank via a pump (e.g., a syringe or peristaltic pump) to increase the level of resin in the tank and thereby allow the thin layer of resin to flow on top of the previously cured layer. In some embodiments, a portion of the liquid platform can be subtracted from the tank via a pump to reduce the level of resin in the tank but leave the thin layer of resin on top of the previously cured layer.
[0059] In still other embodiments, the light source may be moved and / or the focal plane of the projected light beam may be adjusted so that only a thin layer of resin is exposed to the light beam (step 430).
[0060] Embodiments of method 400 may also include exposing target areas of the thin layer to a light beam (step 440), wherein the light has a pattern corresponding to a cross-section of the thiourethane polymer component, such that a photolatent base in the light-exposed target areas of the resin decomposes to form a non-nucleophilic base catalyst and thereby catalyzes polymerization of the first type of monomer and the second type of monomer together to form a patterned layer of the thiourethane polymer component.
[0061] In an embodiment of method 400 , inhibitor and light absorber additives in the resin may substantially prevent polymerization of the first type of monomer and the second type of monomer in regions of the resin outside of the target region.
[0062] Based on this disclosure, one skilled in the relevant art will understand how the process of selectively exposing targeted areas of successive thin layers of resin to a beam of light can be repeated until the final three-dimensional part is formed. The part is then removed from the tank, cleaned and post-cured.
[0063] Liquid thiourethane resins and additives are or will be available from the manufacturer Adaptive3D of Plano, TX.
[0064] Thiol acrylate polymer
[0065] As part of the present disclosure, VAT resin additives suitable for making thiol acrylate polymer parts are being used. One embodiment of the present disclosure includes a photopolymerizable thiol acrylate resin for additive manufacturing in an oxygen environment, the resin comprising: a crosslinking component; at least one monomer and / or oligomer; and a chain transfer agent, the chain transfer agent comprising at least one of a thiol, a secondary alcohol, and / or a tertiary amine, wherein the resin can be configured to react upon exposure to light to form a cured material.
[0066] Cross-linking component can comprise by forming chemical or physical connection (for example, ionic, covalent or physical entanglement) between resin components and react to form any compound of the polymer network connected. Cross-linking component can comprise two or more reactive groups that can be connected to other resin components. For example, the two or more reactive groups of cross-linking component can be chemically connected to other resin components. Cross-linking component can comprise terminal reactive groups and / or side chain reactive groups. The quantity and position of reactive groups may affect the cross-linking density and the structure of, for example, the polymer network.
[0067] The two or more reactive groups may include acrylic functional groups. For example, methacrylate, acrylate, or acrylamide functional groups. In some cases, the crosslinking component includes a difunctional acrylic oligomer. For example, the crosslinking component may include an aromatic urethane acrylate oligomer or an aliphatic urethane acrylate oligomer. The crosslinking component may include CN9167, CN9782, CN9004, (polyethylene glycol) diacrylate, bisacrylamide, tricyclo[5.2.1.0 2,6 ] at least one of decane dimethanol diacrylate and / or trimethylolpropane triacrylate. The size of the crosslinking component may affect, for example, the length of the crosslinks of the polymer network.
[0068] The number of crosslinks or the crosslink density can be selected to control the properties of the resulting polymer network. For example, a polymer network with fewer crosslinks can exhibit higher elongation, while a polymer network with more crosslinks can exhibit higher rigidity. This may be because the polymer chains between the crosslinks may stretch when stretched. Chains with low crosslink density may wrap themselves into a coil to squeeze more tightly and to satisfy entropy forces. When stretched, these chains may untie and stretch before pulling the crosslinks, and the chains may break before stretching. In highly crosslinked materials, a large number of crosslinked chains may result in little or no uncurled chain length and almost immediate bond breakage when strained.
[0069] The amount of the cross-linking component can be selected to control the cross-linking density and the properties of the resulting polymer network. In some cases, the cross-linking component is 1-95% by weight of the resin. In other cases, the cross-linking component is >1%, 1.0-4.99%, 5-10%, or about 20%, 30%, 40%, 50%, 60%, 70%, 80%, or 90% by weight of the resin.
[46] In some cases, the resin comprises at least one monomer and / or oligomer. In some embodiments, the at least one monomer and / or oligomer is 1-95% by weight of the resin. In other cases, the at least one monomer and / or oligomer is >1%, 1.0-4.99%, 5-10%, or about 20%, 30%, 40%, 50%, 60%, 70%, 80%, or 90% by weight of the resin. Monomers can include small molecules that combine with each other to form oligomers or polymers. Monomer can comprise difunctional monomer and / or each molecule has more than one functional group multifunctional monomer of two functional groups.Oligomer can comprise the molecule that is made up of several monomer units.For example, in some cases, oligomer can be made up of two, three or four monomers (for example, dimer, trimer or tetramer).Oligomer can comprise difunctional oligomer and / or each molecule has more than one functional group multifunctional oligomer of two functional groups.
[0070] The at least one monomer and / or oligomer may be capable of reacting with other resin components to form a connected polymer network. For example, the at least one monomer and / or oligomer may include one or more functional groups that can react with the two or more reactive groups of the crosslinking component. The at least one monomer and / or oligomer may include an acrylic acid functional group. For example, a methacrylate, an acrylate or an acrylamide functional group.
[0071] In some cases, at least one monomer and / or oligomer comprises one or more monomers. For example, the one or more monomers may be about 1-95% by weight of the resin. Alternatively, the resin may include at least about 50% or at least about 60% of one or more monomers. In other cases, at least one monomer and / or oligomer comprises an acrylic monomer. The molecular weight of the acrylic monomer may be less than 200Da, less than 500Da or less than 1,000Da. The acrylic monomer may comprise at least one of 2-ethylhexyl acrylate, hydroxypropyl acrylate, cyclic trimethylolpropane formal acrylate, isobornyl acrylate, butyl acrylate and / or N,N'-dimethylacrylamide.
[0072] Chain transfer agents can include any compound having at least one weak chemical bond that potentially reacts with a free radical site of a growing polymer chain and interrupts the growth of the chain. During free radical chain transfer, the free radical can be temporarily transferred to the chain transfer agent, which reinitiates growth by transferring the free radical to another component of the resin, such as a growing polymer chain or monomer. Chain transfer agents can affect the dynamics and structure of the polymer network. For example, chain transfer agents can delay the formation of the network. This delayed network formation can reduce stress in the polymer network, thereby causing favorable mechanical properties.
[0073] In some cases, the chain transfer agent can be configured to react with the oxygen radical to initiate the growth of at least one new polymer chain and / or reinitiate the growth of an oxygen-terminated polymer chain. For example, the chain transfer agent can contain a weak chemical bond so that the radical can be displaced from the oxygen radical and transferred to another polymer, oligomer or monomer.
[0074] Additive manufacturing processes such as 3D printing can produce three-dimensional objects by sequentially curing layers of photopolymerizable resin. Thus, articles produced by additive manufacturing can include a majority or multiple photocured layers. Additive manufacturing can be performed in an oxygen environment, where oxygen can diffuse into the deposited layers of resin.
[0075] In certain embodiments, oxygen free radicals can be formed by the reaction of diffused oxygen and growing polymer chains. For example, at the oxygen-rich surface of resin layer, oxygen can react with initiator free radicals or polymer free radicals to form oxygen free radicals. Oxygen free radicals can be connected to polymer side chains. Oxygen free radicals, for example peroxy free radicals can slow down the solidification of resin. This slowed-down solidification can cause, for example, to form thin uncured monomers and / or oligomer layers with viscosity at the oxygen-rich surface of previously solidified resin layer, which will otherwise minimize the adhesion with the adjacent resin layer that solidifies subsequently.
[0076] At least in part due to the presence of the chain transfer agent, at least some bonding between the previously cured resin layer and the subsequently cured resin layer may also occur despite the presence of an oxygen-rich surface on the previously cured resin layer at the interface between the previously cured resin layer and the adjacent subsequently cured resin layer. In some cases, bonding may be covalent. In some embodiments, bonding may be ionic. In some cases, bonding may be a physical entanglement of polymer chains. Additionally, in some cases, the chain transfer agent is 1 / 2-50% by weight of the resin. In some cases, the chain transfer agent is about 0.5-4.0%, 4.0-4.7%, 4.7-4.99%, 4.99-5%, or 5-50% by weight of the resin.
[0077] Thiol acrylate polymer resin materials can exhibit excellent interlayer strength when 3D printed in an air environment. Because 3D printing is built layer by layer, when printing in the open air, each resin layer has the opportunity to be oxygen-enriched at its surface exposed to air (e.g., during patterning). In the case of existing resins, this oxygen enrichment leads to weak interlayer adhesion because the oxygen available at the oxygen-enriched interface between the layers inhibits free radical polymerization, thereby limiting chain growth and delaying the reaction. However, the thiol acrylate polymer resin contains a chain transfer agent (e.g., a secondary thiol) that can overcome this problem and promote chemical and physical crosslinking between 3D printed layers even in the presence of elevated or ambient oxygen levels at the interface between the layers.
[0078] Further, the mercaptan acrylate polymer resin material can exhibit lower oxygen sensitivity. In free radical polymerization systems, oxygen reacts with the initially initiated or propagated free radicals to form peroxy radicals. In existing resins, these peroxy radicals will tend to terminate polymerization. However, in the mercaptan acrylate polymer resin, the mercaptan can act as a chain transfer agent, thereby allowing the polymerization reaction to propagate further. Lower oxygen sensitivity can achieve open-air manufacturing processes without reducing oxygen manufacturing costs (e.g., nitrogen blanket or argon blanket).
[0079] Thiol acrylate polymer resins can undergo chain transfer reactions during photocuring. Chain transfer is a reaction by which free radicals of a growing polymer chain can be transferred to a chain transfer agent. The newly formed free radicals can then reinitiate chain growth. It is believed that, among other benefits, chain transfer reactions can reduce stress in materials formed from thiol acrylate polymer resins.
[0080] In some cases, the chain transfer agent can be configured to transfer free radicals from a first polymer chain or chain branch within a previously cured resin layer to a second polymer chain or chain branch within the volume of the photopolymerizable resin. For example, this can achieve the formation of chemical or physical crosslinks between adjacent photocured layers in an article produced by additive manufacturing. In other cases, the chain transfer agent can be configured to promote the growth of at least one new polymer chain near an oxygen-rich surface present on a previously cured resin layer. For example, this can also achieve the formation of chemical or physical crosslinks between adjacent photocured layers in an article produced by additive manufacturing. Further, the thiol acrylate polymer resin can include monomers or oligomers having side chains that can cooperate with the chain transfer agent to affect a chain transfer mechanism.
[0081] The chain transfer agent may include at least one of a thiol, a secondary alcohol and / or a tertiary amine. The secondary alcohol may include at least one of isopropanol and / or hydroxypropyl acrylate. In some cases, the thiol is about 0.5% to 4.0%, 4.0% to 4.7%, 4.7% to 4.99%, 4.99-5% or 5-50% by weight of the resin. The thiol may include a secondary thiol. The secondary thiol may include pentaerythritol tetrakis (3-mercaptobutyrate); 1,4-bis (3-mercaptobutoxy) butane; and / or at least one of 1,3,5-tris (3-mercaptobutoxyethyl) -1,3,5-triazine. The tertiary amine may include at least one of an aliphatic amine, an aromatic amine and / or a reactive amine. The tertiary amine may include at least one of triethylamine, N,N'-dimethylaniline and / or N,N'-dimethylacrylamide.
[0082] Any suitable addition compound may be optionally added to the resin. For example, the resin may further include polyethylene glycol. The resin may further include polybutadiene. The resin may further include polydimethylsiloxane acrylate. The resin may further include a copolymer poly(styrene-maleic anhydride copolymer).
[0083] The resin may further include a photoinitiator, an inhibitor, a dye and / or a filler. A photoinitiator may be any compound that undergoes a photoreaction upon absorption of light to produce reactive free radicals. Therefore, a photoinitiator may be able to initiate or catalyze a chemical reaction, such as free radical polymerization. The photoinitiator may include at least one of phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, bisacylphosphine oxide, diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide and / or 2,2'-dimethoxy-2-phenylacetophenone. In some cases, the photoinitiator is 0.01-3% by weight of the resin.
[0084] The inhibitor may be any compound that reacts with free radicals to produce a product that may not cause further polymerization. The inhibitor may include at least one of hydroquinone, 2-methoxyhydroquinone, dibutylhydroxytoluene, diallylthiourea and / or diallylbisphenol A.
[0085] The dye may be any compound that changes the color or appearance of the resulting polymer. The dye may also be used to attenuate stray light within the print area, thereby reducing unwanted free radical generation and over-curing of the sample. The dye may comprise at least one of 2,5-bis(5-tert-butyl-benzoxazol-2-yl)thiophene, carbon black and / or Disperse Red 1.
[0086] Fillers can be any compound added to the polymer formulation that can occupy space and / or replace other resin components. The filler can include at least one of titanium dioxide, silicon dioxide, calcium carbonate, clay, aluminosilicate, crystalline molecules, crystalline oligomers, semi-crystalline oligomers, and / or polymers, wherein the molecular weight of the polymer is between about 1,000 Da and about 20,000 Da.
[0087] Resin viscosity can be any value that facilitates use in additive manufacturing (e.g., 3D printing) of an article. Resins with higher viscosity are more resistant to flow, while resins with lower viscosity are less resistant to flow. Resin viscosity can affect, for example, printability, print speed, or print quality. For example, a 3D printer may only be compatible with resins having a certain viscosity. Alternatively, increasing resin viscosity may increase the time required to smooth the surface of deposited resin between printed layers because the resin may not settle as quickly.
[0088] The thiol acrylate polymer resin of the disclosed material can also have a high curing rate and low viscosity. The object of additive manufacturing is created by building the material layer by layer. Each layer is built by depositing liquid resin and applying light for photocuring. Therefore, the viscosity and curing rate of the resin will affect the printing speed. Low viscosity resin will spread quickly (e.g., 1-30 seconds) into a flat layer without applying heat or mechanically manipulating the layer. Spreading can be accelerated by mechanical manipulation (e.g., 1-10 seconds). In addition, the lower viscosity can allow the recoating blade to move faster. The faster the curing rate, the faster the next subsequent layer can be built.
[0089] For example, the viscosity of the resin can be adjusted by adjusting the ratio of monomer to oligomer. For example, a resin with a higher monomer content may exhibit a lower viscosity. This may be because the lower molecular weight monomers are able to dissolve the oligomers, reduce oligomer-oligomer interactions, and thus reduce the overall resin viscosity. The viscosity of the resin at room temperature or above room temperature may be less than about 250 centipoise, less than about 500 centipoise, less than about 750 centipoise, or less than about 1,000 centipoise. In some cases, the viscosity of the resin at a temperature between 0°C and 80°C is less than about 1000 centipoise, less than about 500 centipoise, or less than about 100 centipoise.
[0090] Articles may be made from the resins as described in any of the embodiments. The articles may be made by a cast polymerization process or an additive manufacturing process such as 3D printing. The articles may include footwear midsoles, shape memory foams, implantable medical devices, wearable articles, automotive seats, seals, gaskets, dampers, hoses and / or accessories. Articles may be made having a majority of layers comprising the resins as described in any of the embodiments.
[0091] In some embodiments, the article made of the resin as described in any embodiment further comprises a topcoat. The topcoat can be applied to the article to potentially obtain the desired appearance or physical properties of the article. The topcoat can include a thiol. The topcoat can include a secondary thiol. The topcoat can include an alkane. The topcoat can include a siloxane polymer. The topcoat can include at least one of a semifluorinated polyether and / or a perfluorinated polyether.
[0092] In some embodiments, the photoinitiator can be configured to generate free radicals after exposure to light. In some embodiments, the cross-linking component and the at least one monomer and / or oligomer are configured to react with free radicals to provide growth of at least one polymer chain free radical within the volume of the photopolymerizable resin. In some embodiments, the at least one polymer chain free radical reacts with diffused oxygen to provide oxygen free radicals. In some embodiments, the chain transfer agent can be configured to transfer oxygen free radicals to initiate growth of at least one new polymer chain free radical.
[0093] In some embodiments, the cross-linking component and the at least one monomer and / or oligomer are configured to react upon exposure to light to provide one or more polymer chains. In some embodiments, the chain transfer agent can be configured to transfer a free radical associated with one of the polymer chains to another of the polymer chains.
[0094] In some embodiments, the photoinitiator can be configured to generate free radicals upon exposure to light, wherein the free radicals initiate a chain reaction between the cross-linking component and the at least one monomer and / or oligomer to provide one or more polymer chains within the volume of the photopolymerizable resin. In some embodiments, the chain transfer agent can be configured to reinitiate a chain reaction to provide one or more new polymer chains within the volume of the photopolymerizable resin.
[0095] The curing rate of the resin layer can depend on the tendency of the resin component to polymerize by free radical reaction during curing by a light source (e.g., ultraviolet light). The resin can optionally include a photoinitiator or inhibitor that can be used to accelerate or delay the curing process. When the resin layer of the present disclosure is provided with a thickness suitable for 3D printing or other additive manufacturing, the resin layer can be photocured within the time length required for the efficient production of articles. For example, in some cases, a resin layer with a thickness of about 100 mm can be configured to form a cured material in no more than 30 seconds, no more than 20 seconds, no more than 10 seconds, no more than 3 seconds, no more than 1 second, or no more than 1 / 10 second. In other cases, a resin layer with a thickness of about 400 mm can be configured to form a cured material in no more than 1 second. In other cases, a resin layer with a thickness of about 300 mm can be configured to form a cured material in no more than 1 second. In other cases, a resin layer with a thickness of about 200 mm can be configured to form a cured material in no more than 1 second. In other cases, a resin layer with a thickness of about 1000 mm can be configured to form a cured material in no more than 30 seconds. In other cases, a resin layer having a thickness of about 10 mm may be configured to form a cured material in no more than 2 seconds, no more than 1 second, no more than 1 / 2 second, or no more than 1 / 4 second.
[0096] Another embodiment of the present disclosure includes a photopolymerizable resin for additive manufacturing, the resin comprising: at least one monomer and / or oligomer; and less than about 5% thiol, wherein the resin can be configured to react upon exposure to light to form a cured material. In some cases, the resin can be configured to form a cured material in an aerobic environment.
[0097] Although mercaptans have an unpleasant odor, mercaptan acrylate resins can have little or no audible odor. It is believed that the low odor characteristic is at least partially due to the use of less than stoichiometric amounts of high molecular weight mercaptans to reduce or eliminate the mercaptan odor. Further, mercaptans can be almost completely incorporated into the polymer network.
[0098] Thiol volatiles may come from cured materials or are produced during the manufacturing process using thiols. Thiol volatiles can be customized to be below the threshold detectable by human olfaction. This can be achieved, for example, by a resin comprising less than about 5% of thiols. Thiol volatiles can be measured in a sample using a gas chromatograph mass spectrometer (GC-MS). In some cases, the cured material contains less than 1 part of 100 million thiol volatiles at ambient temperature and ambient pressure in an oxygen environment for 50 seconds. In some cases, the cured material contains less than 1 part of 10 billion thiol volatiles at ambient temperature and ambient pressure in an oxygen environment for 50 seconds. In some cases, the cured material contains less than 1 part of 10 billion thiol volatiles at ambient temperature and ambient pressure in an oxygen environment for 50 seconds. In some cases, the cured material contains less than 1 part of 10 billion thiol volatiles at ambient temperature and ambient pressure in an oxygen environment for 50 seconds. In some embodiments, the cured material contains less than 1 part of 10 billion thiol volatiles at ambient temperature and ambient pressure in an oxygen environment for 50 seconds.
[0099] The at least one monomer and / or oligomer and thiol used for additive manufacturing can be any monomer and / or oligomer or thiol compound as described in the present disclosure for the resin. For example, the at least one monomer and / or oligomer comprises olefins, alkynes, acrylates or acrylamides, methacrylates, epoxides, maleimides and / or isocyanates.
[0100] In some cases, the thiol has a molecular weight greater than about 200 or greater than about 500. In some embodiments, the thiol has a molecular weight greater than about 100 and contains a moiety comprising a hydrogen bond acceptor and / or a hydrogen bond donor, wherein the moiety undergoes hydrogen bonding.
[0101] In some cases, the resin comprises the thiol and the at least one monomer and / or oligomer in about a certain stoichiometric ratio. In other embodiments, the thiol is less than about 20%, less than about 10%, or less than about 5% by weight of the resin.
[0102] In other cases, the thiol comprises an ester-free thiol. In some embodiments, the thiol comprises a hydrolytically stable thiol. In some embodiments, the thiol comprises a tertiary thiol.
[0103] The curing rate can be such that a photopolymerizable resin layer having a thickness of about 100 mm is configured to cure in no more than 30 seconds. The fracture strain of the material can be greater than 100%, up to 1000%. The toughness of the material is between about 30 MJ / m 3About 100MJ / m 3 between.
[0104] In some embodiments, the resin includes at least about 50% of one or more acrylic monomers and about 0-45% of one or more acrylic functionalized oligomers. The thiol acrylate resin can be stored as a one-pot system at room temperature.
[0105] In some cases, the components of the resin can be combined and stored in a single tank (e.g., a suitable chemical storage container) at room temperature for at least 6 months without the viscosity of the resin increasing by more than 10-20% of the viscosity of the resin. In some cases, the components of the resin mixture can be combined and stored in a single tank at room temperature for at least 6 months without the viscosity of the resin increasing by more than 2%, 5%, 10%, 25%, 50%, or 100% of the viscosity of the resin.
[0106] Stable thiols can be any thiol that exhibits less environmental thermal reaction (e.g., nucleophilic substitution with monomers or oligomers) than other thiols. In some cases, stable thiols include bulky side chains. Such bulky side chains may include at least one chemical group, such as C1-C18 cyclic, branched or linear alkyl, aryl or heteroaryl. In some cases, stable thiols include secondary thiols. In other cases, stable thiols include multifunctional thiols. In some cases, stable thiols include at least one of difunctional thiols, trifunctional thiols and / or tetrafunctional thiols. In some embodiments, the stable thiol includes pentaerythritol tetrakis (3-mercaptobutyrate); and / or at least one of 1,4-bis (3-mercaptobutyryloxy) butane.
[0107] Thiol acrylate polymer resins can exhibit improved storage stability. Resin compositions containing thiol-reactive species and non-thiol-reactive species, such as olefins and acrylates, may undergo dark reactions (e.g., ambient thermal free radical polymerization or Michael addition reactions), which shorten the shelf life of these compositions. In order to account for the reduced shelf life of these resins, they can be stored under low temperature conditions or as a two-can system. In contrast, thiol acrylate resins such as thiol acrylate resins of disclosed materials may contain stable thiols (e.g., secondary thiols). Stable thiols may have reduced reactivity, which may potentially increase the shelf life of 3D printable resin compositions and enable storage as a single-can resin system at room temperature. In addition, the resin remaining at the completion of the 3D printing run can be reused in subsequent runs.
[0108] In some embodiments, the components of the resin mixture can be combined and stored in a single jar at room temperature for at least 6 months without the viscosity of the resin increasing by no more than 10% of the viscosity of the resin. The increase in shelf life, pot life, and / or print life may be due, at least in part, to the presence of stable thiols in the resin mixture. Resin compositions containing thiol-reactive species and non-thiol-reactive species, such as acrylates, may undergo dark reactions (e.g., ambient thermal free radical polymerization or nucleophilic Michael addition reactions). However, the reactivity of the stable thiols in the dark reaction may be reduced.
[0109] In some cases, the resin may be configured to be used continuously in a 3D printing operation in an air environment for 2 weeks without the viscosity of the resin increasing by no more than 2%, 5%, 10%, 25%, 50%, or 100% viscosity increase. In some cases, the resin may be configured to be used continuously in a 3D printing operation in an air environment for 4 weeks without the viscosity of the resin increasing by no more than 2%, 5%, 10%, 25%, 50%, or 100% viscosity increase, and in some cases, the resin may be configured to be used continuously in a 3D printing operation in an air environment for 10 weeks without the viscosity of the resin increasing by no more than 2%, 5%, 10%, 25%, 50%, or 100% viscosity increase. In some cases, the resin may be configured to be used continuously in a 3D printing operation in an air environment for 26 weeks without the viscosity of the resin increasing by no more than 2%, 5%, 10%, 25%, 50%, or 100% viscosity increase. In some cases, the resin can be configured to be used continuously in a 3D printing operation in an air environment for 1 year without the viscosity of the resin increasing by no more than 2%, 5%, 10%, 25%, 50%, or 100% viscosity increase.
[0110] In other cases, the at least one monomer and / or oligomer comprises one or more acrylic monomers. In some embodiments, the one or more acrylic monomers are at least about 50% by weight of the resin. In other cases, the resin includes less than about 5% of a stable thiol, the stable thiol comprising one or more thiol functional groups, wherein the stable thiol can be configured to inhibit a nucleophilic substitution reaction between the one or more thiol functional groups and the one or more monomers or oligomers.
[0111] Other embodiments of the present disclosure may include a photopolymerizable resin for additive manufacturing, the resin comprising: less than 5% thiol, at least about 50% of one or more monomers; wherein the resin may be configured to react upon exposure to light to form a cured material, wherein the cured material has a toughness of about 3-100 MJ / m 3 and the fracture strain is in the range of about 30-1000%.
[0112] Cured thiol acrylate resins may further exhibit time-temperature superposition, so that their properties vary with temperature and frequency. At temperatures below the onset temperature of the glass transition, the material is in a glassy state and brittle. However, at temperatures above the onset temperature, the material may become viscoelastic and ductile until the end temperature of the glass transition. The glass transition temperature of a thiol acrylate resin may be close to the use temperature. For example, the T of the resin may be g The starting temperature can be close to 20°C.
[0113] Above T g At a temperature of the onset temperature, the thiol acrylate resin can be a high strain, high toughness material. Specifically, the cured thiol acrylate resin exhibits a strength of between 3 and 100 MJ / m 3 The toughness is between 20% and the failure strain is between 30-800%.
[0114] The cured materials of the present disclosure can provide mechanical properties of toughness and flexibility (e.g., measured by percent strain at break), which can be suitable for use in manufactured products (e.g., midsoles, insoles, outsoles) that require these properties. Thus, in additive manufacturing processes, products including these cured materials can be produced at reduced cost, with greater potential efficiency and customizability of product design and mechanical properties. For example, customization of toughness and flexibility can be demonstrated in the cured resin materials disclosed above.
[0115] Due to the material properties of thiol acrylate resins, products 3D printed from the resin can be used in a variety of applications. Specific applications can include mattresses, game items and other small household items, as well as products worn on the body or used on the body or ears. The resin can also be suitable for forming prototypes and assembling prototypes. For example, the resin can be used to produce low-cost soles (midsoles, insoles, outsoles) for test manufacturing. In another embodiment, the toughness of the resin in a wide temperature range (e.g., 0°C to 80°C) is between 3 and 100 MJ / m 3 The resin can be used to produce low-density engineered soles (midsoles, insoles, outsoles) for large-scale manufacturing.
[0116] Specifically, toughness can be customized by controlling the percentage and type of monomers and the optional combination of additional oligomers, fillers and additives. Control of these parameters can allow for specific design of the material's ability to stretch (strain) and the force (stress) when this stretch occurs. In general, the stress / strain behavior of a material can affect its fracture toughness. In some cases, the toughness of the cured material is about 3 MJ / m 3 In some cases, the toughness of the cured material is about 5 MJ / m 3 In some cases, the toughness of the cured material is about 10 MJ / m 3 In some cases, the toughness of the cured material is about 15-25 MJ / m 3 In some cases, the toughness of the cured material is about 30-100 MJ / m 3 .
[0117] In addition, the fracture strain can be customized by the optional combination of the percentage and type of the control monomer and other oligomer, filler and additive.Control the density between the underlying network morphology, crosslinking and the tear strength of the material (realized by the interaction of filler and matrix filler) can allow the elongation (strain) of the control material.In some cases, the fracture strain of the material of the described solidification is about 100%.In some cases, the fracture strain of the material of the described solidification is about 200%.In some cases, the fracture strain of the material of the described solidification is about 300%.In some cases, the fracture strain of the material of the described solidification is about 400%.In some cases, the fracture strain of the material of the described solidification is about 500%.In some cases, the fracture strain of the material of the described solidification is about 600%.In some cases, the fracture strain of the material of the described solidification is about 700%.In some cases, the fracture strain of the material of the described solidification is about 800%.
[0118] In a specific case, the toughness of the cured material is about 3-30 MJ / m 3 In other cases, the toughness of the cured material is about 8-15 MJ / m 3 In some cases, the toughness of the cured material is less than about 1 MJ / m 3 In some cases, the fracture strain of the cured material is in the range of about 50-250%. In some cases, the glass transition temperature of the cured material is in the range of about 10-30° C. In other cases, the toughness of the resin is in the range of about 3-100 MJ / m 3 In some cases, the toughness of the cured material is about 3-8 MJ / m 3In some cases, the fracture strain of the cured material is in the range of about 350-500%. In some cases, the toughness of the cured material at about 20° C. is in the range of about 3-30 MJ / m 3 In other cases, the toughness of the cured material at about 20°C is about 10 MJ / m 3 In some embodiments, the cured material has a strain at break at about 20° C. in the range of about 30-100%.
[0119] In some cases, the cured material has a glass transition temperature in the range of about 10-30° C. In some cases, the cured material has a Shore A hardness of about 95 at about 20° C. In some cases, the cured material has a toughness of about 1-5 MJ / m at about 20° C. 3 In certain cases, the toughness of the cured material at about 20°C is about 3 MJ / m 3 .
[0120] In certain cases, the cured material has a toughness of about 20-40 MJ / m at about 20°C. 3 In other cases, the toughness of the cured material at about 0°C is about 40 MJ / m 3 In other cases, the cured material has a toughness of about 30 MJ / m at about 20°C. 3 In other embodiments, the cured material has a toughness of about 20 MJ / m at about 40°C. 3 In other embodiments, the cured material has a toughness of about 1 MJ / m at about 80°C. 3 .
[0121] In some cases, the fracture strain of the cured material at about 0°C is in the range of about 250-300%. In some embodiments, the fracture strain of the cured material at about 20°C is in the range of about 400-500%. In some cases, the fracture strain of the cured material at about 40°C is in the range of about 400-500%. In some embodiments, the fracture strain of the cured material at about 80°C is in the range of about 275-375%. In some embodiments, the glass transition temperature of the cured material is in the range of about 35-55°C.
[0122] The curing rate of the resin layer can depend on the tendency of the resin component to polymerize by free radical reaction during curing by a light source (e.g., ultraviolet light). The resin can optionally include a photoinitiator or inhibitor that can be used to accelerate or delay the curing process. When the resin layer of the present disclosure is provided with a thickness suitable for 3D printing or other additive manufacturing, the resin layer can be photocured within the time length required for the efficient production of articles. The curing rate can be configured to cure in no more than 30 seconds for a photopolymerizable resin layer with a thickness of about 100 mm. For example, in some cases, a resin layer with a thickness of about 100 mm can be configured to form a cured material in no more than 30 seconds, no more than 20 seconds, no more than 10 seconds, no more than 3 seconds, no more than 1 second, or no more than 1 / 10 second. In other cases, a resin layer with a thickness of about 400 mm can be configured to form a cured material in no more than 1 second. In other cases, a resin layer with a thickness of about 300 mm can be configured to form a cured material in no more than 1 second. In other cases, a resin layer with a thickness of about 200 mm can be configured to form a cured material in no more than 1 second. In other cases, a resin layer having a thickness of about 1000 mm can be configured to form a cured material in no more than 30 seconds. In other cases, a resin layer having a thickness of about 10 mm can be configured to form a cured material in no more than 2 seconds, no more than 1 second, no more than 1 / 2 second, or no more than 1 / 4 second.
[0123] The cured material may also have a desired hardness suitable for the finished product. In some cases, the cured material has a Shore A hardness of about 30 at about 20°C. In some cases, the cured material has a Shore A hardness of about 90 at about 20°C.
[0124] The glass transition temperature (T g ) is the temperature at which a polymer changes from an amorphous rigid state to a more flexible state. The glass transition temperature of the cured material can be customized by controlling the percentage and type of monomers, oligomers, fillers, plasticizers, and percentages and types of curing additives (e.g., dyes, initiators, or inhibitors). In some cases, the glass transition temperature of the cured material is in the range of about 10°C to about 30°C. In some embodiments, the half-maximum full width of the glass transition temperature of the cured material exceeds 20°C, exceeds 30°C, exceeds 40°C, or exceeds 50°C. In specific cases, the half-maximum full width of the glass transition temperature of the cured material exceeds 50°C.
[0125] Additionally, below the glass transition temperature, the cured material is in a glassy state, and above the glass transition temperature, the cured material is in a tough state. In some cases, the tough state occurs in the range of about 5-50° C. In some cases, the tough state occurs in the range of about 20-40° C. In some cases, the glass transition temperature of the resin is in the range of about 20-25° C.
[0126] The fracture strain of the material may be greater than 100%, up to 1000%. The toughness of the material may be between about 30 MJ / m 3 About 100MJ / m 3 In specific cases, the fracture strain of the cured material at about 20°C is in the range of about 400-500%. In some cases, the glass transition temperature of the cured material is in the range of about 10-30°C. In some cases, the Shore A hardness of the cured material at about 20°C is about 30. In some cases, the Shore A hardness of the cured material at about 20°C is about 19. In some cases, the toughness of the cured material in the tough state is about 30 MJ / m 3 In some embodiments, the toughness of the cured material in the tough state is about 30-100 MJ / m 3 In some cases, the elastic modulus of the solidified material in the glassy state is less than 5 GPa, greater than 2 GPa, or greater than 1 GPa. In some cases, the elastic modulus of the solidified material in the glassy state is between 2 GPa and 5 GPa.
[0127] Additional embodiments of the present disclosure may include a photopolymerizable resin for additive manufacturing, the resin comprising: less than 5% thiol, at least about 50% one or more monomers; and a photoinitiator, wherein the photoinitiator may be configured to form free radicals after exposure to light, such that the free radicals initiate the growth of one or more polymer chains comprising at least a difunctional monomer and a monofunctional monomer; wherein the resin may be configured to react upon exposure to light to form a cured material, wherein the cured material has a glass transition temperature in the range of about 5-30°C.
[0128] In specific cases, the resin further includes a difunctional oligomer. In some cases, the difunctional oligomer is less than about 45% by weight of the resin. In some cases, the thiol is about 1 / 2-5% by weight of the resin. In some cases, the one or more monomers are about 1-95% by weight of the resin. In some cases, the photoinitiator is 0.01-3% by weight of the resin.
[0129] The resin may further include a trifunctional monomer. In some cases, the trifunctional monomer comprises trimethylolpropane triacrylate.
[0130] Another embodiment of the present disclosure provides a photopolymerizable resin for additive manufacturing, the resin comprising: about 5-15 parts of a thiol per hundred parts of rubber ("phr"); about 20-60% of a difunctional acrylic oligomer; and about 40-80% of one or more monofunctional acrylic monomers; wherein the resin can be configured to react upon exposure to light to form a cured material.
[0131] Another embodiment of the present disclosure provides a photopolymerizable resin for additive manufacturing, the resin comprising: about 4 to 6 phr of pentaerythritol tetrakis(3-mercaptobutyrate); about 40% to 50% of CN9167; and about 50% to 60% of hydroxypropyl acrylate; wherein the resin can be configured to react by exposure to light to form a cured material.
[0132] Another embodiment of the present disclosure provides a photopolymerizable resin for three-dimensional printing, the resin comprising: about 5-20 phr of thiol; about 0-5 phr of polydimethylsiloxane acrylate copolymer; about 20-100% of difunctional acrylic oligomer; and about 0-80% of at least one of monofunctional acrylic monomers; wherein the resin can be configured to react by exposure to light to form a cured material.
[108] Another embodiment of the present disclosure provides a photopolymerizable resin for three-dimensional printing, the resin comprising: about 4 to 6 phr of pentaerythritol tetrakis (3-mercaptobutyrate); about 20% to 40% of CN9004; and about 60% to 80% of hydroxypropyl acrylate; wherein the resin can be configured to react by exposure to light to form a cured material.
[0133] Another aspect of the present disclosure provides a photopolymerizable resin for three-dimensional printing, the resin comprising: about 5-10 phr of thiol; about 0-20% of trimethylolpropane triacrylate; about 30-50% of at least one of the difunctional acrylic oligomers; about 50-86% of isobornyl acrylate; and about 0-21% of hydroxypropyl acrylate; wherein the resin can be configured to react by exposure to light to form a cured material.
[0134] Another aspect of the present disclosure provides a photopolymerizable resin for three-dimensional printing, the resin comprising: about 4 to 6 phr of pentaerythritol tetrakis(3-mercaptobutyrate); about 0% to 5% of trimethylolpropane triacrylate; about 25% to 35% of CN9004; and about 65% to 75% of isobornyl acrylate; wherein the resin can be configured to react by exposure to light to form a cured material.
[0135] Another embodiment of the present disclosure provides a photopolymerizable resin for three-dimensional printing, the resin comprising: about 5-10 phr of thiol; about 0-5% of trimethylolpropane triacrylate; about 30-50% of at least one of the difunctional acrylic oligomers; about 5-75% of isobornyl acrylate; and about 0-80% of hydroxypropyl acrylate; wherein the resin can be configured to react by exposure to light to form a cured material.
[0136] The photopolymerizable resin for additive manufacturing can be prepared according to the following procedure.
[0137] The resin can be printed in a top-down DLP printer (such as Octave Light R1) in an open air atmosphere and ambient conditions. The Z fluid can be loaded into the printing tank (usually 70-95% of the total volume), and the printing resin is then placed on top of the Z fluid (at a commensurate level, for example, 5-30%). The following printing parameters are entered into the control software: exposure time (usually in the range of 0.1-20 seconds), layer height (usually in the range of 10-300 microns), and recoating the surface between each layer in 0.25-10 seconds. The computer-aided design ("CAD") file is loaded into the software, oriented and supported as needed, and then printing is started. The printing cycle is: the build table descends to allow the resin to coat the surface, rises to the layer height below the resin surface (also known as the Z-axis resolution), the recoater blade smoothes the surface of the resin, and the optical engine exposes the mask (a cross-sectional image of the printed portion at the current height), causing the liquid resin to gel. The process is repeated layer by layer until the product is printed. In some embodiments, the 3D printed resin part is post-processed by curing under UV radiation at 350-400 nm at a temperature between 0-100° C. for between 0-5 hours.
[0138] Liquid thiol acrylate resins and additives are available from manufacturer Adaptive3D of Plano, Texas, under the trade name Elastic Tough Rubber ("ETR90").
[0139] Figure 5is a cross-sectional view depicting a downhole sealing device 500 having an elastomeric element 510 designed, manufactured, and operated in accordance with the present disclosure. For example, the elastomeric element 510 may include a thiourethane / acrylate polymer manufactured using any one or a combination of the manufacturing processes discussed above. In the illustrated embodiment, the elastomeric element 510 is positioned between a first end plate and a second end plate 530. In one or more embodiments, the first end plate and the second end plate 530 include hook features 535 that secure the elastomeric element 510 sufficiently so that the first end plate and the second end plate 530 apply an expansion force (e.g., so that the first end plate and the second end plate 530 pull the elastomeric element 510). The elastomeric element 510 may include an inner surface 520 having an inner diameter and an outer surface 525 having an outer diameter.
[0140] Figure 6 is a cross-sectional view depicting an alternative downhole sealing device 600 having an elastomeric element 610 designed, manufactured, and operated in accordance with the present disclosure. For example, the elastomeric element 610 may include a thiourethane / acrylate polymer manufactured using any one or a combination of the manufacturing processes discussed above. In the illustrated embodiment, the elastomeric element 610 is positioned in a groove 635 in a sealing feature 630 (e.g., a single sealing feature). Thus, according to at least this embodiment, the elastomeric element 610 is an O-ring or other thin cross-section geometric sealing element positioned within the groove 635. In contrast to the downhole sealing device 500, the downhole sealing device 600 may employ fluid pressure to axially compress the elastomeric element 610 into engagement with a tubular, a wellbore, or the like. Further to Figure 6 In the embodiment of the present invention, the elastomeric element 610 is a single elastomeric element.
[0141] Figure 7 is a cross-sectional view depicting a downhole sealing device 700 in an uncompressed state positioned within a tubular member 705 in accordance with certain aspects of the present disclosure. The tubular member 705 may be any suitable tubular member, such as a wellbore, a casing string, or a downhole tool. The downhole sealing device 700 in accordance with the present disclosure includes an elastomeric element 710 designed, manufactured, and operated in accordance with the present disclosure. For example, the elastomeric element 710 may include a thiocarbamate / acrylate polymer manufactured using any one or a combination of the manufacturing processes discussed above. In the illustrated Figure 7 In the embodiment of the present invention, the elastomeric element 710 is positioned between the first end plate and the second end plate 730 and includes an inner diameter 720 and an outer diameter 725. The schematically shown first and second anti-extrusion devices 740 can be positioned adjacent to the first and second end plates 730, opposite the elastomeric element 710. The anti-extrusion devices 740 can be in a closed state, but can be actuated to an open state when an axial compressive force is applied.
[0142] In some embodiments, the mandrel 750 can be located within the inner diameter 720 of the elastomeric element 710 so that the elastomeric element 710 fits around the mandrel 750. The mandrel 750 can provide support for the elastomeric element 710 during axial compression to prevent the elastomeric element 710 from deforming radially inward (e.g., toward the central longitudinal axis 760). The mandrel 750 can have an inner diameter, but in other examples it does not have an inner diameter. The annulus that can be sealed by the downhole sealing device 700 can be an annulus between the outer diameter of the mandrel 750 and the inner diameter of the surrounding tubular 705.
[0143] When in an uncompressed state, the downhole sealing device 700 can move freely within the tubular member 705. In order to move the downhole sealing device 700 to a compressed state and seal the tubular member 705, an axial force (e.g., a force applied toward the elastomeric element 710 parallel to the longitudinal axis 760 of the elastomeric element 710) can be applied. The axial force can be applied through the first end plate and the second end plate 730. In some cases, the axial force can be applied by an axial compression tool 770. The axial compression tool 770 can be any tool capable of generating an axial compression force in the downhole sealing device 700. The axial compression tool 770 can include a linear actuator positioned in the wellbore (e.g., positioned adjacent to the downhole sealing device 700 or not adjacent to the downhole sealing device) or outside the wellbore. When positioned not adjacent to the downhole sealing device 700, the axial compression tool 770 can include a tubular member for transmitting the axial compression force to the downhole sealing device 700. When the axial compression force is applied, the elastomeric element 710 can be compressed, such as Figure 8 shown.
[0144] Figure 8 is a diagram illustrating certain aspects of the present disclosure Figure 7 8 is a cross-sectional view of a downhole sealing device 700 in a compressed state (e.g., a set state). An axial compressive force 810 is applied to the downhole sealing device 700, such as from an axial compression tool 770 and through the first end plate and the second end plate 730. The axial compressive force 810 causes the elastomeric element 710 to deform. Figure 8 As shown, the anti-extrusion device 740 extends in response to the axial compressive force 810 and is therefore in an open state. The anti-extrusion device 740 can help reduce the gap between the first and second end plates 730 and the tubular member 705, thereby inhibiting the elastomeric element 710 from being squeezed or deformed too much beyond the first and second end plates 730. When in a compressed state, the elastomeric element 710 can expand the outer diameter sufficiently to seal the tubular member 720, such as by filling the annulus between the mandrel 750 and the tubular member 705.
[0145] Fig. 99 is an end view of an anti-extrusion device 900 in an expanded state according to certain aspects of the present disclosure. The anti-extrusion device 900 can include a central hole 910 through which a mandrel or other tubular member can pass. When in an expanded state (e.g., under axial compression), a blocking surface 920 can be rotated to be perpendicular to the longitudinal axis of the anti-extrusion device 900. As described herein, the blocking surface 920 blocks the extrusion element from expanding too far beyond the end plate.
[0146] Rollers 930 may be present on the end of the blocking surface 920 adjacent to where the blocking surface 920 will contact or nearly contact the inner diameter of the tubular into which it has been placed. These rollers 930 may facilitate expansion of the anti-extrusion device 900. These rollers 930 may also facilitate positioning of the anti-extrusion device 900 within the tubular.
[0147] Fig.10 According to certain aspects of the present disclosure Fig. 9 900 is an isometric view of anti-extrusion device 900 in a retracted state. Anti-extrusion device 900 can be biased toward the retracted state such that removal of the axial compressive force causes anti-extrusion device 900 to move to the retracted state. In some cases, anti-extrusion device 900 can be moved to the retracted state by an axial tensile force applied thereto (e.g., opposite to the axial compressive force).
[0148] When in the retracted state, the blocking surface 920 moves to a position parallel or approximately parallel to the longitudinal axis of the anti-extrusion device 900. The rollers 930 positioned at the ends of the blocking surface 920 are thus retracted from the inner diameter of the tubular member in which the anti-extrusion device 900 is placed. The longitudinal supports 940 are shown in the retracted state, parallel or generally parallel to the longitudinal axis of the anti-extrusion device 900.
[0149] When an axial compressive force is applied to the anti-extrusion device 900, the rear body 950 is pushed toward the front body 960. As the rear body 950 moves toward the front body 960, the blocking surface 920 rotates outward with the distal end of the longitudinal support 940 to form a triangular support, wherein the angle between the blocking surface 920 and its longitudinal support 940 is less than 90°. Fig.10 The retracted state moves to Fig.11 expansion state.
[0150] Fig.11 According to certain aspects of the present disclosure Fig. 9 900 in an expanded state. Blocking surface 920 is shown extended and can be used to block the extrusion of the elastomeric element. Rollers 930 can be seen at the ends of blocking surface 920. Longitudinal supports 940 are shown to support blocking surface 920.
[0151] In some cases, one or more rollers 930 can be positioned on each blocking surface 920 or on the distal end of each longitudinal support 940 so that when the anti-extrusion device 900 is positioned within the tubular in an expanded state, the rollers 930 are positioned adjacent to the inner diameter of the tubular. These rollers 930 can be single-axis rollers (e.g., flat rollers) or can be multi-axis rollers (e.g., partially captured ball bearings).
[0152] Fig.12 is a flow chart depicting a process 1200 for forming a downhole sealing device according to certain aspects of the present disclosure. As described herein, any suitable technique may be used. In at least one embodiment, any suitable additive manufacturing technique may be used to allow individual layers (e.g., complete layers or portions of layers) to be sequentially applied to form a complete elastomeric element. The elastomeric element may be formed in isolation from other components of the downhole sealing device, or may be formed together with one or more components of the downhole sealing device. For example, the elastomeric element may be formed around a first end plate and a second end plate, a mandrel, or any combination thereof.
[0153] At optional block 1210, a base component may be provided. The base component may be a mandrel, one or more end plates, or any combination thereof. In some cases, block 1210 may be skipped when the elastomeric element is formed in isolation from other components of the downhole sealing device.
[0154] At block 1220, a pattern of the elastomeric material is determined. The pattern may be the first layer or any subsequent layer of the elastomeric material, including the last layer. The pattern may include the shape of the layer.
[0155] At optional block 1230, a material for the layer may be selected. The material may be any suitable elastomeric material consistent with the present disclosure. In at least one embodiment, the material may be any material disclosed above for forming an elastomeric element comprising a thiourethane / acrylate polymer. Additionally, additives may be included with the material to impart not only a higher thermal stability to the elastomeric element, but also a greater modulus amplitude.
[0156] At block 1240, a layer of elastomeric material may be applied. The layer may be applied directly to a base component, to a temporary component (e.g., a component that will be removed from the elastomeric element prior to incorporation into a wellbore sealing device), a build platform (e.g., a surface that may be used to temporarily build an elastomeric element prior to removal of the elastomeric element for incorporation into a wellbore sealing device), or a previously applied layer of elastomeric material. The layer may be applied using any suitable method appropriate to the style of additive manufacturing being used.
[0157] The process of applying the layers in block 1240 can be any known or hereafter discovered 3D printing process, including but not limited to SLA and / or DLP printing. For example, a commercially available desktop polymer 3D printer (e.g., an Octave Light printer) can be used to apply the layers in block 1240. Thus, the layers, and therefore the elastomeric element, can be manufactured on demand, such as in a field repair shop.
[0158] Blocks 1220, 1230, and 1240 may constitute layering iteration 1270. Multiple layering iterations 1270 may be used to produce an elastomeric element.
[0159] At block 1250, process 1200 can determine whether additional layers should be applied. If additional layers are to be applied, process 1200 can continue at block 1220 by performing another layering iteration 1270 to determine a pattern for the additional layers.
[0160] When multiple materials are used, two or more sequentially applied layers may be applied in the same plane as one another but be composed of different materials. For example, to produce a single layer of a first material having a solid circular appearance within a square area of a second material, a first layering iteration 1270 may be performed to apply the first material in a circular shape, and a second layering iteration 1270 may be performed to apply the second material in a square shape. Thus, at block 1240, if a current layer is applied to a previously applied layer of elastomeric material, the current layer does not necessarily need to be applied to a layer applied in an immediately previous iteration, but may be applied to a layer previously applied two or more iterations ago.
[0161] At box 1250, if process 1200 determines that no additional layers need to be applied, the component can be provided at box 1260. Providing the component can include providing an elastomeric element or any other component or combination of components formed using process 1200. Providing the component can include performing additional assembly of the component with one or more other components. Providing the component can include providing the component to another process or additional steps not shown in process 1200. In some cases, providing the component can include performing additional finishing, such as additional finishing of the elastomeric element. For example, the additional finishing can include surface polishing or texturing, or even subsequent processing. Providing the component can be providing the component for use, such as use in a wellbore or tubular.
[0162] Process 1200 describes how an elastomeric element may be formed by sequential layering iterations 1270. Layering iterations 1270 may form the elastomeric element in any suitable orientation. For example, each layer of the elastomeric element may be generally cylindrical in shape, with subsequent layers increasing in diameter. In another example, each layer may be generally annular or ring-shaped in shape, with each layer being perpendicular to the longitudinal axis (e.g., Figure 3 elastomeric element 310 if it is formed using sequential layers from left to right). Other layer orientations may be used.
[0163] In some cases, layering iteration 1270 can include applying a temporary material layer. The temporary material can be any material that can be easily removed from the elastomeric element without damaging the elastomeric element. For example, the temporary material can be a material with a melting point lower than the melting point of the elastomeric element. In some cases, the temporary material can be a water-soluble material or a loosely bonded material that can be washed off the elastomeric element. The temporary material can be applied in layering iteration 1270 to provide temporary structural support for subsequent layers applied in subsequent layering iterations 1270. Once the elastomeric element has been formed, the finishing operation can include removing any temporary material, thereby leaving gaps or channels where the temporary material was used.
[0164] In yet another embodiment, a layering process is not required. For example, in at least one other embodiment, the pattern can be a mold. Thus, the selected material (e.g., as discussed in the above paragraphs) can be placed within a mold having a specific three-dimensional shape. The selected material can then be subjected to UV light through a UV permeable mold, thereby forming an elastomeric element.
[0165] Aspects disclosed herein include:
[0166] A. A downhole sealing device, comprising: 1) one or more downhole sealing features, and 2) an elastomeric element, the elastomeric element comprising a thiocarbamate / acrylate polymer, the elastomeric element being coupled to the one or more downhole sealing features, the elastomeric element being operable to press against a tubular member in a downhole application.
[0167] B. A well system, comprising: 1) a wellbore, the wellbore being located in a formation, and 2) a downhole sealing device, the downhole sealing device being located in the wellbore, the downhole sealing device comprising: a) one or more downhole sealing features, and b) an elastomeric element, the elastomeric element comprising a thiocarbamate / acrylate polymer, the elastomeric element being coupled to the one or more downhole sealing features, the elastomeric element being operable to press against a surface in the wellbore.
[0168] C. A method for sealing in a wellbore, the method comprising: 1) positioning a downhole sealing device in a wellbore located in a formation, the downhole sealing device comprising: a) one or more downhole sealing features; and b) an elastomeric element, the elastomeric element comprising a thiocarbamate / acrylate polymer, the elastomeric element being coupled to the one or more downhole sealing features; and 2) subjecting the elastomeric element to an axial compressive force, the axial compressive force pressing the elastomeric element against a surface in the wellbore.
[0169] Aspects A, B and C may have one or more of the following additional combinations of elements: Element 1: wherein the thiourethane / acrylate polymer is a thiourethane polymer. Element 2: wherein the thiourethane / acrylate polymer is a thiol acrylate polymer. Element 3: wherein the thiourethane / acrylate polymer is a blended combination of a thiourethane polymer and a thiol acrylate polymer. Element 4: wherein the elastomeric element is operable to press against the tubular in the downhole application and is operable to seal a pressure differential of at least 6,900 kPa at a temperature of at least 80°C. Element 5: wherein the elastomeric element is operable to press against the tubular in the downhole application and is operable to seal a pressure differential of at least 20,700 kPa at a temperature of at least 80°C. Element 6: wherein the elastomeric element is operable to press against the tubular in the downhole application and is operable to seal a pressure differential of at least 20,700 kPa at a temperature of at least 80°C. Element 7: wherein the elastomeric element is operable to press against the tubular member in the downhole application and is operable to seal a pressure differential of at least 27,575 kPa at a temperature of at least 80°C. Element 8: wherein the elastomeric element is operable to press against the tubular member in the downhole application and is operable to seal a pressure differential of at least 27,575 kPa at a temperature as low as -65°C and as high as 270°C. Element 9: wherein the fracture toughness of the elastomeric element is at least 40 MJ / m 3, and the tensile strength is at least 25 MPa. Element 10: Wherein the one or more downhole sealing features are a first end plate and a second end plate coupled to opposite ends of the elastomeric element, the first end plate and the second end plate being configured to move relative to each other to axially compress the elastomeric element into engagement with the tubular member. Element 11: Wherein the elastomeric element and the first end plate and the second end plate are positioned between a first anti-extrusion device and a second anti-extrusion device, the first anti-extrusion device and the second anti-extrusion device being configured to expand in diameter when subjected to an axial compressive force so that the elastomeric element cannot axially deform beyond the first end plate and the second end plate. Element 12: Wherein the one or more metal sealing features are a single metal sealing feature, the single metal sealing feature having a groove located therein, and further wherein the elastomeric element is an O-ring positioned within the groove. Element 13: Wherein the elastomeric element is a single element. Element 14: wherein the elastomeric element is a 3D printed element made using a VAT resin, the VAT resin being formed using a liquid mixture comprising: a first type of monomer, the first type of monomer comprising two or more thiol functional groups; a second type of monomer, the second type of monomer comprising two or more isocyanate functional groups; a photolatent base, wherein the photolatent base can decompose when exposed to light to form a non-nucleophilic base catalyst having a pKa greater than 7; an anionic step-growth polymerization inhibitor, the inhibitor having an acidic group configured to form an acid-base pair with the non-nucleophilic base; and a light absorber, the light absorber having an absorbance in the liquid mixture greater than the absorbance of the photolatent base at the wavelength of the light used for the exposure. Element 15: wherein the elastomeric element is a 3D printed element manufactured using a VAT resin, the VAT resin being formed using a liquid mixture comprising: a cross-linking component; at least one monomer and / or oligomer; and a chain transfer agent, the chain transfer agent comprising at least one of a thiol, a secondary alcohol, and / or a tertiary amine, wherein the resin can be configured to react upon exposure to light to form a cured solid material. Element 16: wherein the surface in the wellbore is a wellbore casing. Element 17: wherein the one or more downhole sealing features are a first end plate and a second end plate coupled to opposite ends of the elastomeric element, the first end plate and the second end plate being configured to move relative to each other to axially compress the elastomeric element into engagement with the surface in the wellbore. Element 18: wherein the elastomeric element and the first end plate and the second end plate are positioned between a first anti-extrusion device and a second anti-extrusion device, the first anti-extrusion device and the second anti-extrusion device being configured to expand in diameter when subjected to an axial compressive force, such that the elastomeric element cannot axially deform beyond the first end plate and the second end plate.Element 19: wherein the one or more metal sealing features is a single metal sealing feature having a groove located therein, and further wherein the elastomeric element is an O-ring positioned within the groove. Element 20: wherein the downhole sealing device is a first downhole sealing device, and the well system further comprises a second downhole sealing device positioned proximate to the first downhole sealing device. Element 21: wherein the second downhole sealing device comprises a polymer material different from the thiourethane / acrylate polymer.
[0170] Those skilled in the art to which this application relates will appreciate that other and further additions, deletions, substitutions and modifications may be made to the described embodiments.
Claims
1. A downhole sealing device, comprising: one or more downhole sealing features; as well as an elastomeric element comprising a thiourethane / acrylate polymer, the elastomeric element coupled to the one or more downhole sealing features, the elastomeric element operable to press against a tubular in a downhole application; wherein the elastomeric element is a 3D printed element manufactured using a VAT resin, wherein the VAT resin is formed using a liquid mixture comprising: Cross-linking components; at least one monomer and / or oligomer; and A chain transfer agent comprising at least one of a thiol, a secondary alcohol, and / or a tertiary amine, wherein the resin is capable of being configured to react upon exposure to light to form a cured solid material. 2 . The downhole sealing device of claim 1 , wherein the thiourethane / acrylate polymer is a thiourethane polymer.
3. The downhole sealing device of claim 1, wherein the thiourethane / acrylate polymer is a thiol acrylate polymer. 4 . The downhole sealing device according to claim 1 , wherein the thiourethane / acrylate polymer is a blended combination of a thiourethane polymer and a thiol acrylate polymer.
5. The downhole sealing device of claim 1, wherein the elastomeric element is operable to press against the tubular member in the downhole application and is operable to seal a pressure differential of at least 6,900 kPa at a temperature of at least 80°C.
6. The downhole sealing device of claim 1, wherein the elastomeric element is operable to press against the tubular member in the downhole application and is operable to seal a pressure differential of at least 20,700 kPa at a temperature of at least 80°C.
7. The downhole sealing device of claim 1, wherein the elastomeric element is operable to press against the tubular member in the downhole application and is operable to seal a pressure differential of at least 20,700 kPa at temperatures as low as -65°C and as high as 270°C.
8. The downhole sealing device of claim 1, wherein the elastomeric element is operable to press against the tubular member in the downhole application and is operable to seal a pressure differential of at least 27,575 kPa at a temperature of at least 80°C.
9. The downhole sealing device of claim 1, wherein the elastomeric element is operable to press against the tubular member in the downhole application and is operable to seal a pressure differential of at least 27,575 kPa at temperatures as low as -65°C and as high as 270°C.
10. The downhole sealing device of claim 1, wherein the fracture toughness of the elastomeric element is at least 40 MJ / m 3 , and the tensile strength is at least 25 MPa.
11. A downhole sealing device according to claim 1, wherein the one or more downhole sealing features are a first end plate and a second end plate connected to opposite ends of the elastomeric element, and the first end plate and the second end plate are configured to move relative to each other to axially compress the elastomeric element into engagement with the tubular member.
12. A downhole sealing device according to claim 11, wherein the elastomeric element and the first end plate and the second end plate are positioned between a first anti-extrusion device and a second anti-extrusion device, and the first anti-extrusion device and the second anti-extrusion device are configured to expand in diameter when subjected to an axial compressive force, so that the elastomeric element cannot axially deform beyond the first end plate and the second end plate.
13. A downhole sealing device according to claim 1, wherein the one or more metal sealing features is a single metal sealing feature having a groove located therein, and further wherein the elastomeric element is an O-ring positioned within the groove.
14. The downhole sealing device of claim 1, wherein the elastomeric element is a single element.
15. The downhole sealing device according to claim 1, wherein the elastomeric element is a 3D printed element manufactured using a VAT resin, wherein the VAT resin is formed using a liquid mixture comprising: a first type of monomer, said first type of monomer comprising two or more thiol functional groups; a second type of monomer, said second type of monomer comprising two or more isocyanate functional groups; a photolatent base, wherein the photolatent base is capable of decomposing upon exposure to light to form a non-nucleophilic base catalyst with a pKa greater than 7; an anionic step-growth polymerization inhibitor having an acidic group configured to form an acid-base pair with the non-nucleophilic base; as well as A light absorber having an absorbance in the liquid mixture greater than an absorbance of the photolatent base at the wavelength of the light used for the exposing.
16. A well system comprising: a wellbore, the wellbore being located in a formation; as well as A downhole sealing device, the downhole sealing device is positioned in the wellbore, and the downhole sealing device comprises: one or more downhole sealing features; and an elastomeric element comprising a thiourethane / acrylate polymer, the elastomeric element coupled to the one or more downhole sealing features, the elastomeric element operable to press against a surface in the wellbore; wherein the elastomeric element is a 3D printed element manufactured using a VAT resin, wherein the VAT resin is formed using a liquid mixture comprising: Cross-linking components; at least one monomer and / or oligomer; and A chain transfer agent comprising at least one of a thiol, a secondary alcohol, and / or a tertiary amine, wherein the resin is capable of being configured to react upon exposure to light to form a cured solid material.
17. The well system of claim 16, wherein the elastomeric element is operable to press against a tubular in a downhole application and is operable to seal a pressure differential of at least 6,900 kPa at a temperature of at least 80°C.
18. The well system of claim 16, wherein the surface in the wellbore is a wellbore casing.
19. A well system according to claim 16, wherein the one or more downhole sealing features are a first end plate and a second end plate connected to opposite ends of the elastomeric element, and the first end plate and the second end plate are configured to move relative to each other to axially compress the elastomeric element into engagement with the surface in the wellbore.
20. A well system according to claim 19, wherein the elastomeric element and the first and second end plates are positioned between a first anti-extrusion device and a second anti-extrusion device, and the first and second anti-extrusion devices are configured to expand in diameter when subjected to an axial compressive force so that the elastomeric element cannot axially deform beyond the first and second end plates.
21. The well system of claim 16, wherein the one or more metal sealing features is a single metal sealing feature having a groove located therein, and further wherein the elastomeric element is an O-ring positioned within the groove.
22. The well system of claim 16, wherein the elastomeric element is a 3D printed element manufactured using a VAT resin formed using a liquid mixture comprising: a first type of monomer, said first type of monomer comprising two or more thiol functional groups; a second type of monomer, said second type of monomer comprising two or more isocyanate functional groups; a photolatent base, wherein the photolatent base is capable of decomposing upon exposure to light to form a non-nucleophilic base catalyst with a pKa greater than 7; an anionic step-growth polymerization inhibitor having an acidic group configured to form an acid-base pair with the non-nucleophilic base; as well as A light absorber having an absorbance in the liquid mixture greater than an absorbance of the photolatent base at the wavelength of the light used for the exposing.
23. The well system of claim 16, wherein the downhole sealing device is a first downhole sealing device, and the well system further comprises a second downhole sealing device positioned proximate to the first downhole sealing device.
24. The well system of claim 23, wherein the second downhole sealing device comprises a polymer material different from the thiourethane / acrylate polymer.
25. A method for sealing in a wellbore, the method comprising: A downhole sealing device is positioned in a wellbore located in a subterranean formation, the downhole sealing device comprising: one or more downhole sealing features; as well as an elastomeric element comprising a thiourethane / acrylate polymer, the elastomeric element coupled to the one or more downhole sealing features; as well as subjecting the elastomeric element to an axial compressive force that presses the elastomeric element against a surface in the wellbore; wherein the elastomeric element is a 3D printed element manufactured using a VAT resin, wherein the VAT resin is formed using a liquid mixture comprising: Cross-linking components; at least one monomer and / or oligomer; and A chain transfer agent comprising at least one of a thiol, a secondary alcohol, and / or a tertiary amine, wherein the resin is capable of being configured to react upon exposure to light to form a cured solid material.
26. The method of claim 25, wherein the compressed elastomeric element is operable to seal a pressure differential of at least 6,900 kPa at a temperature of at least 80°C.
27. A method according to claim 25, wherein the one or more downhole sealing features are a first end plate and a second end plate connected to opposite ends of the elastomeric element, and further wherein subjecting the elastomeric element to an axial compressive force includes moving the first end plate and the second end plate relative to each other to axially compress the elastomeric element into engagement with the surface in the wellbore.
28. The method of claim 25, wherein the one or more metal sealing features is a single metal sealing feature having a groove therein, the elastomeric element being an O-ring positioned within the groove, and further wherein subjecting the elastomeric element to an axial compressive force comprises subjecting the O-ring to fluid pressure to axially compress the elastomeric element into engagement with the surface in the wellbore.
29. The method of claim 25, further comprising 3D printing the elastomeric element using a VAT resin formed using a liquid mixture comprising: a first type of monomer, said first type of monomer comprising two or more thiol functional groups; a second type of monomer, said second type of monomer comprising two or more isocyanate functional groups; a photolatent base, wherein the photolatent base is capable of decomposing upon exposure to light to form a non-nucleophilic base catalyst with a pKa greater than 7; an anionic step-growth polymerization inhibitor having an acidic group configured to form an acid-base pair with the non-nucleophilic base; as well as A light absorber having an absorbance in the liquid mixture greater than an absorbance of the photolatent base at the wavelength of the light used for the exposing.
Citation Information
Patent Citations
High performance regular and high expansion elements for oil and gas applications
US11692412B2
Downhole tools comprising cast degradable sealing elements
US20160177655A1
Downhole expandable metal tubular
US20160369587A1
Wellbore Seals With Complex Features Through Additive Manufacturing
US20180187509A1