Semiconductor structure and method for forming the same
Patent Information
- Application Number
- CN202110162406.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-02-05
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-02-05
Smart Images

Figure CN114883408B_ABST
Abstract
Description
Technical Field
[0001] The embodiments of the present invention relate to the field of semiconductor manufacturing, and in particular to a semiconductor structure and a method for forming the same. Background Art
[0002] With the rapid development of semiconductor manufacturing technology, semiconductor devices are moving towards higher component density and higher integration, and semiconductor process nodes are continuously decreasing in accordance with Moore's Law. Transistors, as the most basic semiconductor devices, are currently being widely used. Therefore, with the increase in component density and integration of semiconductor devices, in order to adapt to the reduction of process nodes, the channel length of transistors has to be continuously shortened.
[0003] In order to better adapt to the requirements of device size reduction, semiconductor processes have gradually begun to transition from planar transistors to three-dimensional transistors with higher efficiency, such as gate-all-around (GAA) transistors. In a gate-all-around transistor, the gate surrounds the area where the channel is located from all sides. Compared with planar transistors, the gate of a gate-all-around transistor has a stronger control ability over the channel and can better suppress the short channel effect.
[0004] However, the performance of all-around gate transistors still needs to be improved. Summary of the invention
[0005] The problem solved by the embodiments of the present invention is to provide a semiconductor structure and a method for forming the same, which increases the filling volume of the gate electrode layer and the ratio of the volume of the gate electrode layer to the volume of the gate structure, which is beneficial to improving the problem of increased gate resistance caused by reduced gate length.
[0006] To solve the above problems, an embodiment of the present invention provides a semiconductor structure, comprising: a substrate; a channel structure layer, located on the substrate and spaced apart from the substrate, the channel structure layer comprising one or more spaced apart channel layers; a source-drain doping layer, located on both sides of the channel structure layer along the length direction of the channel layer and covering the sidewalls of the channel structure layer, the source-drain doping layer and the adjacent channel layer, or the source-drain doping layer and the substrate, and the channel layer adjacent to the substrate form a through groove; a gate opening, located between the source-drain doping layers and spanning the channel structure layer, the gate opening being connected to the through groove; a gate structure, filled in the gate opening and the through groove, the gate structure covering the top of the channel structure layer and surrounding the channel layer, the gate structure comprising a gate function layer surrounding the channel layer, and a gate electrode layer filled in the gate opening and the through groove formed with the gate function layer, the gate function layer exposing the sidewalls of the through groove and the gate opening, and the gate electrode layer contacting the sidewalls of the gate opening and the through groove.
[0007] Accordingly, an embodiment of the present invention further provides a method for forming a semiconductor structure, comprising: providing a substrate, on which one or more channel stacks stacked in sequence from bottom to top are formed, each of the channel stacks comprising a sacrificial layer and a channel layer located on the sacrificial layer; forming a dummy gate structure across the channel stack on the substrate, the dummy gate structure covering a portion of the top and a portion of the sidewall of the channel stack; forming a source-drain doping layer in the channel stack on both sides of the dummy gate structure; after forming the source-drain doping layer, removing the dummy gate structure to form a gate opening to expose the channel stacking; removing the sacrificial layer to form a through groove connected to the gate opening, the through groove is surrounded by the adjacent channel layer and the source-drain doped layer, or the through groove is surrounded by the substrate, the channel layer adjacent to the substrate and the source-drain doped layer; forming a gate function layer surrounding the gate opening and the channel layer exposed by the through groove, the gate function layer exposing the side walls of the gate opening and the through groove; filling the gate opening and the through groove with the gate function layer, the gate electrode layer is in contact with the side walls of the gate opening and the through groove, and the gate electrode layer and the gate function layer are used to constitute a gate structure.
[0008] Compared with the prior art, the technical solution of the embodiment of the present invention has the following advantages:
[0009] In the semiconductor structure provided by an embodiment of the present invention, the gate functional layer exposes the side walls of the gate opening and the through-groove, and the gate functional layer is not formed on the side walls of the gate opening and the through-groove, thereby being able to provide a larger process space for forming a gate electrode layer. The gate electrode layer can correspondingly contact the side walls of the gate opening and the through-groove, thereby increasing the filling volume of the gate electrode layer and the proportion of the volume of the gate electrode layer to the volume of the gate structure, which is beneficial to improving the problem of increased gate resistance caused by a reduction in the gate length Lg, and further beneficial to reducing the gate RC delay and increasing the circuit speed, thereby improving the performance of the semiconductor structure.
[0010] In the method for forming a semiconductor structure provided by an embodiment of the present invention, in the process of forming the gate functional layer, the gate functional layer exposes the side walls of the gate opening and the through-groove, so that the gate functional layer is not formed on the side walls of the gate opening and the through-groove. Therefore, in the process of forming the gate electrode layer, a larger process space can be provided for forming the gate electrode layer, and the gate electrode layer can correspondingly contact the side walls of the gate opening and the through-groove, thereby increasing the filling volume of the gate electrode layer and the proportion of the volume of the gate electrode layer to the volume of the gate structure, which is beneficial to improving the problem of increased gate resistance caused by reduced gate length, and further beneficial to reducing gate RC delay and increasing circuit speed, and the performance of the semiconductor structure is improved.
[0011] In an optional scheme, the step of forming the gate functional layer includes one or more deposition and removal processes; the deposition and removal process includes: forming a gate functional film on the bottom and side walls of the gate opening and the side walls of the through groove, wherein the gate functional film surrounds the channel layer; removing the gate functional film located on the side walls of the gate opening and the through groove; the substrate includes a first area for forming a first device and a second area for forming a second device, and forming the gate functional layer includes: performing a first number of deposition and removal processes to form a gate functional layer on the first area, and performing a second number of deposition and removal processes to form a gate functional layer on the second area, and the second number of times is different from the first number, so that by adjusting the number of deposition and removal processes for forming the gate functional layer on different areas, the thickness of the gate functional layer formed on different areas is different, and accordingly the performance of the first device and the second device is different, so as to meet the demand for diversified device functions. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 It is a schematic diagram of the structure of a semiconductor structure;
[0013] Figure 2 is a schematic structural diagram of an embodiment of a semiconductor structure of the present invention;
[0014] Figures 3 to 17 It is a schematic structural diagram corresponding to each step in an embodiment of a method for forming a semiconductor structure of the present invention. DETAILED DESCRIPTION
[0015] As can be seen from the background technology, the performance of the current all-around gate transistor needs to be improved. The reason why the performance of the semiconductor structure needs to be improved is now analyzed in combination with a semiconductor structure. Figure 1 It is a structural diagram of a semiconductor structure.
[0016] The semiconductor structure includes: a substrate 10; a channel structure layer 11, which is located on the substrate 10 and is spaced apart from the substrate 10, and the channel structure layer 11 includes one or more spaced apart channel layers 12; a source-drain doped layer 17, which is located on both sides of the channel structure layer 11 along the length direction of the channel layer 12 and covers the sidewalls of the channel structure layer 11, and the source-drain doped layer 17 and the adjacent channel layer, or the source-drain doped layer 17 and the substrate 10, and the channel layer 12 adjacent to the substrate 10 form a through groove (not shown). Marked); an inner sidewall 18, located on the sidewall of the source-drain doped layer 17 exposed by the through groove; a gate structure 13, spanning the channel structure layer 11 and covering the top of the channel structure layer 11, the gate structure 13 is located between the source-drain doped layers 17 and surrounds the channel layer 12, the gate structure 13 includes a high-k gate dielectric layer 16 surrounding the channel layer 12 and located on the sidewall of the through groove, a work function layer 15 located on the high-k gate dielectric layer 16, and a gate electrode layer 14 located on the work function layer 15 and filling the through groove.
[0017] The semiconductor structure is a fully enclosed gate transistor. As the device size gradually decreases, the length Lg of the gate structure 13 decreases accordingly, and the gate resistance increases accordingly. Moreover, as the length Lg of the gate structure 13 continues to decrease, the gate resistance increases to a greater extent, and the impact on the overall circuit is further increased. The increase in gate resistance causes gate RC delay, thereby reducing the speed of the logic circuit. In particular, in the semiconductor structure, a high-k gate dielectric layer 16 and a work function layer 15 stacked in sequence are formed on the sidewalls, bottom walls and top walls of the through groove. The remaining space in the through groove for forming the gate electrode layer 14 is small, resulting in a small volume of the gate electrode layer 14, and the resistivity of the gate electrode layer 14 material is generally lower than the resistivity of the work function layer 15 material. As the length Lg of the gate structure 13 further decreases, the problem of increased resistance of the gate electrode layer 14 becomes more significant, and the impact on device performance is becoming increasingly difficult to ignore.
[0018] In order to solve the technical problem, an embodiment of the present invention provides a semiconductor structure, wherein the gate functional layer exposes the side walls of the gate opening and the through-groove, thereby providing a larger filling space for the gate electrode layer. The gate electrode layer can correspondingly contact the side walls of the gate opening and the through-groove, thereby increasing the filling volume of the gate electrode layer and the proportion of the volume of the gate electrode layer to the volume of the gate structure, which is beneficial to improving the problem of increased gate resistance caused by reduced gate length, and further beneficial to reducing gate RC delay and increasing circuit speed, thereby improving the performance of the semiconductor structure.
[0019] In order to make the above-mentioned purposes, features and advantages of the embodiments of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below with reference to the accompanying drawings. Figure 2 , showing a schematic structural diagram of an embodiment of a semiconductor structure of the present invention.
[0020] In this embodiment, the semiconductor structure includes: a substrate 100; a channel structure layer 200, which is located on the substrate 100 and is spaced apart from the substrate 100, and the channel structure layer 200 includes one or more spaced apart channel layers 210; a source-drain doped layer 110, which is located on both sides of the channel structure layer 200 along the length direction of the channel layer 210 and covers the sidewalls of the channel structure layer 200, and the source-drain doped layer 110 and the adjacent channel layer 210, or the source-drain doped layer 110 and the substrate 100, and the channel layer 210 adjacent to the substrate 100 form a through groove 170 (combined with reference Fig.16 ); Gate opening 160 (combined with reference Fig.16), located between the source and drain doping layers 110 and across the channel structure layer 200, the gate opening 160 is connected to the through groove 170; the gate structure 300 is filled in the gate opening 160 and the through groove 170, the gate structure 300 covers the top of the channel structure layer 200 and surrounds the channel layer 210, the gate structure 300 includes a gate function layer 310 surrounding the channel layer 210, and a gate electrode layer 320 filled in the gate opening 160 and the through groove 170 formed with the gate function layer 310, the gate function layer 310 exposes the side walls of the through groove 170 and the gate opening 160, and the gate electrode layer 320 is in contact with the side walls of the gate opening 160 and the through groove 170.
[0021] The gate functional layer 310 exposes the side walls of the gate opening 160 and the through groove 170. The gate functional layer 310 is not formed on the side walls of the gate opening 160 and the through groove 170, thereby providing a larger process space for forming the gate electrode layer 320. The gate electrode layer 320 can correspondingly contact the side walls of the gate opening 160 and the through groove 170, thereby increasing the filling volume of the gate electrode layer 320 and the proportion of the volume of the gate electrode layer 320 to the volume of the gate structure 300, which is beneficial to improving the problem of increased gate resistance caused by the reduction of the gate length Lg, and further beneficial to reducing the gate RC delay and increasing the circuit speed, thereby improving the performance of the semiconductor structure.
[0022] The substrate 100 is used to provide a process platform for forming a semiconductor structure. In this embodiment, the semiconductor structure is an all-around gate (GAA) transistor as an example for description. In other embodiments, the semiconductor structure can also be a forksheet transistor or a complementary field effect transistor (CFET).
[0023] In this embodiment, the substrate 100 includes a substrate. In other embodiments, the substrate may also include a substrate and a fin located on the substrate. The channel structure layer is correspondingly located on the fin. In this embodiment, the substrate 100 is a silicon substrate. In other embodiments, the substrate may also be other suitable materials.
[0024] In this embodiment, the substrate 100 includes a first region (not shown) for forming a first device and a second region (not shown) for forming a second device. Specifically, the first device and the second device have different performances, such as different threshold voltages and breakdown voltages, to meet the demand for diversified device functions.
[0025] The channel layer 210 is used to provide a conductive channel for the field effect transistor. The stacking direction of the plurality of stacked channel layers 210 is perpendicular to the surface of the substrate 100. In this embodiment, an NMOS transistor is formed, and the material of the channel layer 210 is Si. In other embodiments, when a PMOS transistor is formed, in order to improve the performance of the PMOS transistor, SiGe channel technology can be used, and the material of the channel layer is SiGe.
[0026] In this embodiment, the number of the channel layers 210 is three for illustration. In other embodiments, the number of the channel layers may be other numbers.
[0027] When the field effect transistor is working, the source-drain doped layer 110 is used to provide a carrier source. In this embodiment, the source-drain doped layer 110 includes a stress layer doped with ions, and the stress layer is used to provide stress to the channel region, thereby improving the mobility of carriers. In this embodiment, when a PMOS transistor is formed, the material of the stress layer is Si or SiGe, and the doped ions in the source-drain doped layer 110 are P-type ions; when an NMOS transistor is formed, the material of the stress layer is Si or SiC, and the doped ions in the source-drain doped layer 110 are N-type ions.
[0028] The through slot 170 and the gate opening 160 together provide a spatial location for the gate structure 300 .
[0029] When the device is working, the gate structure 300 is used to control the opening and closing of the conductive channel. In this embodiment, the gate structure 300 is a metal gate structure.
[0030] In this embodiment, the portion of the gate structure 300 located in the through groove 170 is the first portion 300 (1), and along the length direction of the channel layer 210, the side wall of the first portion 300 (1) is indented relative to the side wall of the channel layer 210; the portion of the gate structure 300 located in the gate opening 160 is the second portion 300 (2).
[0031] The gate functional layer 310 exposes the sidewalls of the gate opening 160 and the through groove 170 . The gate functional layer 310 is not formed on the sidewalls of the gate opening 160 and the through groove 170 , which can provide a larger formation space for the gate electrode layer 320 .
[0032] The gate functional layer is a gate dielectric layer; or, the gate functional layer is a work function layer; or, the gate functional layer includes a gate dielectric layer and a work function layer located on the gate dielectric layer.
[0033] In this embodiment, the gate function layer 310 includes a gate dielectric layer 31 and a work function layer 32 located on the gate dielectric layer 31. The gate dielectric layer 31 and the work function layer 32 both expose the sidewalls of the gate opening 160 and the through groove 170, thereby significantly improving the effect of increasing the formation space of the gate electrode layer 320.
[0034] In other embodiments, when the gate function layer is a gate dielectric layer or a work function layer, the gate dielectric layer or the work function layer exposes the sidewalls of the gate opening and the through groove, which can also increase the formation space of the gate electrode layer.
[0035] The gate dielectric layer 31 is used to achieve electrical isolation between the work function layer 32 and the gate electrode layer 320 and the channel layer 210. In this embodiment, the gate dielectric layer 31 is a high-k gate dielectric layer, and the material of the high-k gate dielectric layer is a high-k dielectric material; wherein the high-k dielectric material refers to a dielectric material having a relative dielectric constant greater than the relative dielectric constant of silicon oxide. Specifically, the material of the high-k gate dielectric layer is HfO2. In other embodiments, the material of the high-k gate dielectric layer can also be selected from ZrO2, HfSiO, HfSiON, HfTaO, HfTiO, HfZrO or Al2O3.
[0036] The work function layer 32 is used to adjust the work function of the gate structure, and then adjust the threshold voltage of the field effect transistor. When forming an NMOS transistor, the work function layer 32 is an N-type work function layer, and the material of the work function layer 32 includes one or more of titanium aluminide, tantalum carbide, aluminum or titanium carbide; when forming a PMOS transistor, the work function layer 32 is a P-type work function layer, and the material of the work function layer 32 includes one or more of titanium nitride, tantalum nitride, titanium carbide, tantalum silicon nitride, titanium silicon nitride and tantalum carbide.
[0037] In this embodiment, the substrate 100 includes a first region for forming a first device and a second region for forming a second device; the thickness of the gate functional layer 310 located in the first region is different from the thickness of the gate functional layer 320 in the second region, so that by adjusting the thickness of the gate functional layer 310 located in different regions, the performance of the first device and the second device are made different accordingly to meet the demand for diversified device functions.
[0038] Specifically, when the thickness of the gate dielectric layer is different, the breakdown voltage of the device is different; when the thickness of the work function layer is different, the threshold voltage of the device is different.
[0039] The gate electrode layer 320 serves as an electrode for electrically leading out the gate structure 300 , thereby achieving electrical connection between the gate structure 300 and an external circuit.
[0040] As can be seen from the above records, the gate functional layer 310 exposes the side walls of the gate opening 160 and the through groove 170, which is conducive to providing a larger process space for the gate electrode layer 320. The gate electrode layer 320 can correspondingly contact the side walls of the gate opening 160 and the through groove 170, thereby increasing the filling volume of the gate electrode layer 320 and the ratio of the volume of the gate electrode layer 320 to the volume of the gate structure 300, which is conducive to improving the problem of increased gate resistance caused by the reduction of the gate length Lg, and further helps to reduce the gate RC delay and increase the circuit speed, thereby improving the performance of the semiconductor structure.
[0041] Specifically, compared with the work function layer 32, the resistivity of the gate electrode layer 320 material is lower. By increasing the volume of the gate electrode layer 320 and increasing the proportion of the volume of the gate electrode layer 320 to the volume of the gate structure 300, it is beneficial to significantly improve the problem of increased gate resistance caused by the reduction of the gate length Lg.
[0042] The material of the gate electrode layer 320 is a conductive material. In this embodiment, the material of the gate electrode layer 320 is W. In other embodiments, the material of the gate electrode layer may also be Al, Cu, Ag, Au, Pt, Ni or Ti.
[0043] In this embodiment, the semiconductor structure further includes: an interlayer dielectric layer 130, which is located on the substrate 100 at the side of the gate structure 300 and covers the source-drain doped layer 110. The interlayer dielectric layer 130 is used to achieve electrical isolation between adjacent semiconductor structures. In this embodiment, the material of the interlayer dielectric layer 130 is silicon oxide.
[0044] In this embodiment, the semiconductor structure further includes an inner spacer 120, which is located between the first portion 300 (1) and the source-drain doped layer 110. The inner spacer 120 is used to isolate the source-drain doped layer 110 from the gate structure 300, and also increases the distance between the gate structure 300 and the source-drain doped layer 110, which is beneficial to reducing the parasitic capacitance between the gate structure 300 and the source-drain doped layer 110.
[0045] In this embodiment, the material of the inner sidewall 120 is an insulating material, so as to achieve isolation between the source-drain doped layer 110 and the gate structure 300. The material of the inner sidewall 120 includes silicon nitride, silicon oxide, silicon oxynitride, low-k dielectric material or ultra-low-k dielectric material. As an example, the material of the inner sidewall 120 is silicon nitride.
[0046] In this embodiment, the semiconductor structure further includes: a gate spacer 140 located between the second portion 300 (2) and the interlayer dielectric layer 130. The gate spacer 140 is used to define the position of the source-drain doped layer 110 and to protect the sidewall of the gate structure 300.
[0047] In this embodiment, the material of the gate spacer 140 includes silicon nitride, silicon oxide, silicon oxynitride, low-k dielectric material or ultra-low-k dielectric material, and the gate spacer 140 is a single-layer or stacked structure. As an example, the gate spacer 140 is a single-layer structure, and the material of the gate spacer 140 is silicon nitride.
[0048] In this embodiment, the semiconductor structure further includes an interface layer 330 located between the gate structure 300 and the channel layer 210 .
[0049] The process of forming the gate functional layer 310 includes one or more deposition removal processes, and the deposition removal processes include: forming a gate functional film on the bottom and side walls of the gate opening 160 and the side walls of the through groove 170, and the gate functional film surrounds the channel layer 210; and removing the gate functional film located on the side walls of the gate opening 160 and the through groove 170. The interface layer 330 is used as an interface layer (Interface layer) between the gate functional layer and the channel layer 210, and is used to provide good interface quality for forming the gate functional layer. Moreover, the interface layer 330 is also used to increase the growth rate of the gate functional film on the channel layer 210 formed with the interface layer 330, so that the growth rate of the gate functional film on the interface layer 330 and the side walls of the gate opening 160 and the through groove 170 is different, so that the thickness of the gate functional film surrounding the channel layer 210 is greater than the thickness of the gate functional film formed on the side walls of the through groove 170 and the gate opening 160, so that when the gate functional film located on the side walls of the gate opening 160 and the through groove 170 is etched away, since the gate functional film surrounding the channel layer 210 is thicker, part of the thickness can be retained to form the gate functional layer 310.
[0050] Specifically, in this embodiment, the interface layer 330 is used to improve the bonding ability of the atoms of the gate dielectric layer 31 on the surface of the interface layer 330, so that in the process of forming the gate dielectric film, the growth rate of the gate dielectric film on the interface layer 330 is greater than the growth rate on the gate sidewall 140 or the inner sidewall 120.
[0051] In this embodiment, the material of the interface layer 330 includes silicon oxide. In other embodiments, the material of the interface layer may also be other suitable materials.
[0052] In the actual process, the semiconductor structure may further include: a work function interface layer (not shown), which is located between the gate dielectric layer 31 and the work function layer 32. The work function interface layer is used to provide good interface quality for forming the work function layer 32, and the material of the work function interface layer is selected as follows: the bonding ability of the atoms of the work function layer 32 on the work function interface layer is greater than the bonding ability on the gate sidewall 140 or the inner sidewall 120, so that in the process of forming the work function layer 32, it is beneficial to make the growth rate of the work function film on the channel layer 210 formed with the work function interface layer greater than the growth rate on the sidewall of the gate opening 160 or the through groove 170.
[0053] Correspondingly, the present invention also provides a method for forming a semiconductor structure. Figures 3 to 17 It is a schematic structural diagram corresponding to each step in an embodiment of a method for forming a semiconductor structure of the present invention.
[0054] The method for forming the semiconductor structure of this embodiment is described in detail below with reference to the accompanying drawings.
[0055] refer to Figure 3 A substrate 100 is provided, on which one or more channel stacks 230 stacked sequentially from bottom to top are formed, and each channel stack 230 includes a sacrificial layer 220 and a channel layer 210 located on the sacrificial layer 220 .
[0056] The substrate 100 is used to provide a process platform for subsequent processes. In this embodiment, the formation of a gate-all-around (GAA) transistor is used as an example for description. In other embodiments, the formation method can also be used to form a forksheet transistor or a complementary field effect transistor (CFET).
[0057] In this embodiment, the substrate 100 includes a substrate. In other embodiments, the substrate may also include a substrate and a fin located on the substrate. The channel stack is stacked on the fin accordingly.
[0058] In this embodiment, the substrate 100 includes a first region (not shown) for forming a first device and a second region (not shown) for forming a second device. Specifically, the first device and the second device have different performances, such as different threshold voltages and breakdown voltages, to meet the demand for diversified device functions.
[0059] The stacking direction of the plurality of stacked channel stacks 230 is perpendicular to the surface of the substrate 100 .
[0060] In the channel stack 230 , the sacrificial layer 220 is used to support the channel layer 210 and to occupy a space for the subsequent formation of a gate structure. The channel layer 210 is used to provide a conductive channel of the field effect transistor.
[0061] In this embodiment, an NMOS transistor is formed, the material of the channel layer 210 is Si, and the material of the sacrificial layer 220 is SiGe. In the subsequent process of removing the sacrificial layer 220, the etching selectivity of SiGe and Si is relatively high. By setting the material of the sacrificial layer 220 to SiGe and the material of the channel layer 210 to Si, the effect of the removal process of the sacrificial layer 220 on the channel layer 210 can be effectively reduced, thereby improving the quality of the channel layer 210, and further facilitating the improvement of device performance. In other embodiments, when a PMOS transistor is formed, in order to improve the performance of the PMOS transistor, SiGe channel technology can be used, the material of the channel layer is SiGe, and the material of the sacrificial layer is Si.
[0062] In this embodiment, the number of the channel stacks 230 is three for illustration. In other embodiments, the number of the channel stacks 230 may be other numbers.
[0063] Continue to refer Figure 3 A dummy gate structure 150 is formed on the substrate 100 and crosses the channel stack 230 . The dummy gate structure 150 covers a portion of the top and a portion of the sidewall of the channel stack 230 .
[0064] The dummy gate structure 150 occupies a space for a gate structure to be formed subsequently.
[0065] In this embodiment, the dummy gate structure 150 is a stacked structure, and the dummy gate structure 150 includes a dummy gate oxide layer (not shown) and a dummy gate layer (not shown) located on the dummy gate oxide layer. The dummy gate oxide layer is located on the surface of the channel stack 230. In the subsequent process of removing the dummy gate structure 150, the dummy gate layer is removed first. The dummy gate oxide layer can temporarily define the position where the etching stops in the process of removing the dummy gate layer, thereby reducing the probability of causing damage to the channel stack 230.
[0066] In this embodiment, the material of the dummy gate oxide layer is silicon oxide or silicon oxynitride. The dummy gate layer is located on the dummy gate oxide layer and crosses the channel stack 230. In this embodiment, the material of the dummy gate layer is polysilicon.
[0067] In this embodiment, the formation method further includes: after forming the dummy gate structure 150, forming a gate sidewall 140 on the sidewall of the dummy gate structure 150. The gate sidewall 140 is used together with the dummy gate structure 150 as an etching mask for a subsequent etching process to define the formation position of the source and drain doping layer, and the gate sidewall 140 is also used to protect the sidewalls of the dummy gate structure 150 and the subsequent gate structure.
[0068] In this embodiment, the material of the gate spacer 140 includes silicon nitride, silicon oxide, silicon oxynitride, low-k dielectric material or ultra-low-k dielectric material, and the gate spacer 140 is a single-layer or stacked structure. As an example, the gate spacer 140 is a single-layer structure, and the material of the gate spacer 140 is silicon nitride.
[0069] refer to Figure 4 After forming the dummy gate structure 150, the forming method further includes: forming a groove 240 in the channel stack 230 on both sides of the dummy gate structure 150. The groove 240 is used to provide a spatial position for forming a source and drain doping layer. The sidewall of the groove 240 exposes the channel stack 230, so as to facilitate the subsequent etching of the sacrificial layer 220 along the length direction of the channel layer 210.
[0070] In this embodiment, an anisotropic etching process (eg, an anisotropic dry etching process) is used to etch the channel stack 230 on both sides of the dummy gate structure 150 , which is beneficial to improving the cross-sectional morphology quality of the groove 240 .
[0071] refer to Figure 5 , along the length direction of the channel layer 210, the partial thickness of the sacrificial layer 220 exposed by the sidewall of the groove 240 is etched to form a groove 250, and the groove 250 is surrounded by the adjacent channel layer 210 and the sacrificial layer 220, or surrounded by the substrate 100, the channel layer 210 adjacent to the substrate 100, and the sacrificial layer 220.
[0072] The groove 250 is used to provide a space for the subsequent formation of an inner sidewall, so that after a gate structure is subsequently formed at the location of the sacrificial layer 220 , the inner sidewall can achieve isolation between the source and drain doping regions and the gate structure.
[0073] In this embodiment, a wet etching process is used to etch the partial thickness of the sacrificial layer 220 exposed by the sidewall of the groove 240. The wet etching process is an isotropic etching process, so that the sacrificial layer 220 can be etched along the length direction of the channel layer 210, and the wet etching process is easy to achieve a large etching selectivity, which is conducive to reducing the difficulty of etching the sacrificial layer 220 and reducing the probability of damage to other film layer structures.
[0074] In this embodiment, the material of the sacrificial layer 220 is SiGe, the material of the channel layer 210 is Si, and the exposed sacrificial layer 220 is wet-etched by HCl vapor. The etching rate of HCl vapor on SiGe material is much greater than that on Si material, which can effectively reduce the probability of damage to the channel layer 210.
[0075] In other embodiments, when the material of the channel layer is SiGe and the material of the sacrificial layer is Si, the etching solution for wet etching is TMAH (tetramethylammonium hydroxide) solution. The difference between the etching rate of TMAH solution for Si and the etching rate for SiGe is large, which can also effectively reduce the probability of the channel layer being damaged.
[0076] refer to Figure 6 , an inner spacer 120 is formed in the trench 250 .
[0077] Subsequently, a source-drain doped layer is formed in the groove 240, and a gate structure is formed at the position of the pseudo-gate structure 150 and the sacrificial layer 220. The inner sidewall 120 is used to achieve isolation between the source-drain doped layer and the gate structure, and also increases the distance between the gate structure and the source-drain doped layer, which is beneficial to reducing the parasitic capacitance between the gate structure and the source-drain doped layer.
[0078] In this embodiment, the material of the inner sidewall 120 is an insulating material to achieve isolation between the source-drain doping layer and the gate structure. In this embodiment, the material of the inner sidewall 120 includes silicon nitride, silicon oxide, silicon oxynitride, low-k dielectric material or ultra-low-k dielectric material. As an example, the material of the inner sidewall 120 is silicon nitride.
[0079] In this embodiment, the step of forming the inner sidewall 120 includes: forming a sidewall film (not shown) on the top of the pseudo gate structure 150, the top and sidewall of the gate sidewall 140, and the bottom and sidewall of the groove 240, and the sidewall film is filled in the groove 250; using an isotropic etching process to remove the sidewall film located on the top of the pseudo gate structure 150, the top and sidewall of the gate sidewall 140, the bottom of the groove 240, and the sidewall of the channel layer 210, and the remaining sidewall film located in the groove 250 is used as the inner sidewall 120.
[0080] In this embodiment, an atomic layer deposition process is used to form the sidewall film. In this embodiment, the isotropic etching process includes an isotropic dry etching process.
[0081] refer to Figure 7 , a source-drain doped layer 110 is formed in the channel stack 230 on both sides of the dummy gate structure 150 .
[0082] When the field effect transistor is working, the source-drain doping layer 110 is used to provide a carrier source. In this embodiment, the source-drain doping layer 110 includes a stress layer doped with ions, and the stress layer is used to provide stress for the channel region, thereby improving the mobility of carriers.
[0083] Specifically, the step of forming the source-drain doped layer 110 includes: forming the source-drain doped layer 110 in the groove 240 . Accordingly, the source-drain doped layer 110 covers the sidewalls of the channel layer 210 and the inner spacer 120 .
[0084] When forming a PMOS transistor, the material of the stress layer is Si or SiGe, and the doped ions in the source and drain doping layer 110 are P-type ions; when forming an NMOS transistor, the material of the stress layer is Si or SiC, and the doped ions in the source and drain doping layer 110 are N-type ions.
[0085] refer to Figure 8In this embodiment, the formation method further includes: forming an interlayer dielectric layer 130 on the substrate 100 at the side of the dummy gate structure 150. The interlayer dielectric layer 130 is used to achieve electrical isolation between adjacent devices, and is also used to support the channel layer 210 in the subsequent process of removing the dummy gate structure 150 and removing the sacrificial layer 220. In this embodiment, the material of the interlayer dielectric layer 130 is silicon oxide.
[0086] Continue to refer Figure 8 After forming the source-drain doping layer 110, the dummy gate structure 150 is removed to form a gate opening 160, exposing the channel stack 230. The gate opening 160 is used to provide a space for forming a gate structure. The gate opening 160 exposes the channel stack 230, so that the sacrificial layer 220 can be removed through the gate opening 160 later.
[0087] In this embodiment, the gate opening 160 crosses the channel stack 230 and is located between the source and drain doping layers 110. In this embodiment, the gate opening 160 is located in the interlayer dielectric layer 130 and is surrounded by the gate spacer 140.
[0088] refer to Fig. 9 , remove the sacrificial layer 220 to form a through groove 170 connected to the gate opening 160, and the through groove 170 is surrounded by the adjacent channel layer 210 and the source-drain doped layer 110, or the through groove 170 is surrounded by the substrate 100, the channel layer 210 adjacent to the substrate 100, and the source-drain doped layer 110.
[0089] The through slot 170 and the gate opening 160 together provide a space for forming a gate structure.
[0090] The sacrificial layer 220 is removed after the source-drain doped layer 110 is formed. Therefore, after removing the sacrificial layer 220 , both ends of the channel layer 210 are connected to the source-drain doped layer 110 along the length direction of the channel layer 210 , and are suspended in the gate opening 160 so that the subsequent gate structure can surround the channel layer 210 .
[0091] After the sacrificial layer 220 is removed, the channel layers 210 are arranged at intervals, and the remaining channel layers 210 constitute the channel structure layer 200 . The channel structure layer 200 is located on the substrate 100 and is arranged at intervals from the substrate 100 .
[0092] In this embodiment, a wet etching process is used to remove the sacrificial layer 220. Specifically, the material of the channel layer 210 is Si, and the material of the sacrificial layer 220 is SiGe, so the sacrificial layer 220 exposed by the gate opening 160 is removed by HCl vapor.
[0093] Combined with reference Fig.10After forming the through-groove 170 , the forming method further includes: forming an interface layer 330 surrounding the gate opening 160 and the channel layer 210 exposed by the through-groove 170 .
[0094] The subsequent formation of the gate functional layer includes one or more deposition removal processes, which include: forming a gate functional film on the bottom and side walls of the gate opening 160 and the side walls of the through groove 170, wherein the gate functional film surrounds the channel layer 210; and removing the gate functional film located on the side walls of the gate opening 160 and the through groove 170.
[0095] The interface layer 330 is used as an interface layer between the gate functional layer and the channel layer 210, and is used to provide good interface quality for forming the gate functional layer. Moreover, the interface layer 330 is also used to increase the growth rate of the gate functional film on the channel layer 210 formed with the interface layer 330, so that the growth rate of the gate functional film on the interface layer 330 and the side walls of the gate opening 160 and the through groove 170 is different, so that the thickness of the gate functional film surrounding the channel layer 210 is greater than the thickness of the gate functional film formed on the side walls of the through groove 170 and the gate opening 160, so that when the gate functional film located on the side walls of the gate opening 160 and the through groove 170 is etched away, since the gate functional film surrounding the channel layer 210 is thicker, part of the thickness can be retained to form the gate functional layer.
[0096] In this embodiment, the material of the interface layer 330 includes silicon oxide. In other embodiments, the material of the interface layer may also be other suitable materials.
[0097] In this embodiment, the step of forming the interface layer 330 includes: performing plasma oxidation treatment on the surface of the channel layer 210. By performing plasma oxidation treatment on the surface of the channel layer 210, the interface layer 330 is formed only on the surface of the channel layer 210 exposed by the gate opening 160 and the through groove 170. Specifically, in an oxygen atmosphere, the surface of the channel layer 210 is subjected to plasma treatment (Plasma treatment), so that a portion of the thickness of the channel layer 210 is oxidized to form the interface layer 330.
[0098] refer to Figures 11 to 16 , a gate function layer 310 is formed to surround the gate opening 160 and the channel layer 210 exposed by the through groove 170 , and the gate function layer 310 exposes the sidewalls of the gate opening 160 and the through groove 170 .
[0099] The gate functional layer 310 is used to form a gate structure with a subsequent gate electrode layer. After the gate functional layer 310 is formed, the remaining space of the gate opening 160 and the through groove 170 is used to form a gate electrode layer.
[0100] The gate functional layer 310 exposes the sidewalls of the gate opening 160 and the through groove 170 , so that the gate functional layer 310 is not formed on the sidewalls of the gate opening 160 and the through groove 170 , which can provide a larger process space for forming the gate electrode layer in the subsequent process of forming the gate electrode layer.
[0101] The gate functional layer is a gate dielectric layer; or, the gate functional layer is a work function layer; or, the gate functional layer includes a gate dielectric layer and a work function layer located on the gate dielectric layer.
[0102] In this embodiment, the gate function layer 310 includes a gate dielectric layer 31 and a work function layer 32 located on the gate dielectric layer 31. The gate dielectric layer 31 and the work function layer 32 both expose the sidewalls of the gate opening 160 and the through groove 170, so that the effect of increasing the formation space of the gate electrode layer is more significant.
[0103] In other embodiments, when the gate function layer is a gate dielectric layer or a work function layer, the gate dielectric layer or the work function layer exposes the sidewalls of the gate opening and the through groove, which can also increase the formation space of the gate electrode layer.
[0104] The gate dielectric layer 31 is used to achieve electrical isolation between the work function layer 32 and the subsequent gate electrode layer and the channel layer 210. In this embodiment, the gate dielectric layer 31 is a high-k gate dielectric layer, and the material of the high-k gate dielectric layer is a high-k dielectric material. Specifically, the material of the high-k gate dielectric layer is HfO2. In other embodiments, the material of the high-k gate dielectric layer can also be selected from ZrO2, HfSiO, HfSiON, HfTaO, HfTiO, HfZrO or Al2O3.
[0105] The work function layer 32 is used to adjust the work function of the gate structure, and then adjust the threshold voltage of the field effect transistor. When forming an NMOS transistor, the work function layer 32 is an N-type work function layer, and the material of the work function layer 32 includes one or more of titanium aluminide, tantalum carbide, aluminum or titanium carbide; when forming a PMOS transistor, the work function layer 32 is a P-type work function layer, and the material of the work function layer 32 includes one or more of titanium nitride, tantalum nitride, titanium carbide, tantalum silicon nitride, titanium silicon nitride and tantalum carbide.
[0106] In this embodiment, the step of forming the gate functional layer 310 includes one or more deposition and removal processes; the deposition and removal process steps include: forming a gate functional film on the bottom and side walls of the gate opening 160 and the side walls of the through groove 170, and the gate functional film surrounds the channel layer 210; and removing the gate functional film located on the side walls of the gate opening 160 and the through groove 170.
[0107] Specifically, the deposition removal process includes: using a deposition process to form a gate functional film; and using an etching process to remove the gate functional film located on the sidewalls of the gate opening 160 and the through groove 170 .
[0108] In the actual process, the process conditions of the deposition process and the etching process can be adjusted respectively so that the thickness of the gate functional film obtained by each deposition removal process is different, which is conducive to the precise control of the thickness of the gate functional film obtained by each deposition removal process.
[0109] Specifically, adjusting the process conditions of the deposition process may include: adjusting the gas flow, pressure, temperature, time and other process parameters of the deposition process; adjusting the process conditions of the etching process may include: adjusting the gas flow or etching solution concentration, temperature, pressure, time and other process parameters of the etching process.
[0110] As an example, the step of forming the gate functional layer 310 includes multiple deposition and removal processes, so that the gate functional layer 310 with a desired thickness can be obtained through multiple deposition and removal processes.
[0111] In this embodiment, the substrate 100 includes a first area for forming a first device and a second area for forming a second device; forming a gate functional layer includes: performing a first number of deposition and removal processes to form a gate functional layer surrounding the gate opening 160 and the channel layer 210 exposed by the through groove 170 on the first area, and performing a second number of deposition and removal processes to form a gate functional layer surrounding the gate opening 160 and the channel layer 210 exposed by the through groove 170 on the second area, and the second number is different from the first number, so that by adjusting the number of deposition and removal processes for forming the gate functional layer 310 on different areas, the thickness of the gate functional layer 310 formed on different areas is different, and the performance of the first device and the second device is adjusted accordingly to meet the demand for diversified device functions.
[0112] Specifically, when the thickness of the gate dielectric layer is different, the breakdown voltage of the device is different; when the thickness of the work function layer is different, the threshold voltage of the device is different.
[0113] In the step of performing the deposition removal process, in the process of forming the gate functional film, the thickness of the gate functional film surrounding the channel layer 210 is greater than the thickness of the gate functional film formed on the sidewalls of the gate opening 160 and the through groove 170. The gate functional film surrounding the channel layer 210 is thicker, so that while the gate functional film located on the sidewalls of the gate opening 160 and the through groove 170 is etched away, the gate functional film surrounding the channel layer 210 can retain a portion of its thickness for forming the gate functional layer 310.
[0114] In this embodiment, the process for forming the gate functional film includes an atomic layer deposition (ALD) process. The ALD process is a self-limiting reaction process based on the ALD process, which is conducive to obtaining a thinner film and accurately controlling the thickness of the deposited film. The ALD process has a high step coverage capability and is easy to form a gate functional film surrounding the channel layer 210 on the bottom and sidewalls of the gate opening 160 and the sidewalls of the through groove 170.
[0115] In this embodiment, the gate functional film is surrounded on the channel layer 210 formed with the interface layer 330. Specifically, during the formation of the gate functional film, the growth rate of the gate functional film on the channel layer 210 formed with the interface layer 330 or the gate functional film is greater than the growth rate on the sidewalls of the gate opening 160 and the through groove 170.
[0116] The growth of the atomic layer deposition process is selective, that is, the growth rate of the atomic layer deposition process on different materials is different. In this embodiment, since the interface layer 330 is surrounded by the channel layer 210, the interface layer 330 is made of a different material from the gate sidewall 140 of the gate opening 160 or the inner sidewall 120 of the through groove 170. Compared with the gate sidewall 140 or the inner sidewall 120, the atoms of the gate functional film have a stronger bonding ability with the surface of the interface layer 330, so that at the same time, the number of atomic layers deposited on the surface of the interface layer 330 by the atomic layer deposition process is greater than the number of atomic layers deposited on the surface of the gate sidewall 140 or the inner sidewall 120, and the growth rate of the gate functional film on the interface layer 330 is correspondingly greater.
[0117] In this embodiment, the step of removing the gate functional film on the sidewalls of the gate opening 160 and the through groove 170 includes: etching the gate functional film using an isotropic etching process until the gate functional film on the sidewalls of the gate opening 160 and the through groove 170 is removed.
[0118] In this embodiment, during the process of etching the gate functional film, since the gate functional film surrounding the channel layer 210 is thicker, when the gate functional film located on the side walls of the gate opening 160 and the through groove 170 is removed, the gate functional film surrounding the channel layer 210 still retains a portion of its thickness for forming the gate functional layer.
[0119] The isotropic etching process has the characteristic of isotropic etching, that is, the etching rate along the direction parallel to the surface of the substrate 100 is slightly different from the etching rate along the direction perpendicular to the surface of the substrate 100, so that the gate functional film can be etched along the direction perpendicular to the side walls of the gate opening 160 and the through groove 170 until the gate functional film located on the side walls of the gate opening 160 and the through groove 170 is removed.
[0120] In this embodiment, the isotropic etching process includes an atomic layer etching (ALE) process. The atomic layer etching process includes multiple cycles of two steps of modification and removal, each cycle removes a thinner film layer, and the multiple cycles are repeated until the desired etching thickness is reached, which is conducive to accurately controlling the etching thickness of the gate functional film, and the atomic layer etching process has the characteristics of self-limiting etching, which is conducive to improving the consistency of etching thickness in different directions.
[0121] In other embodiments, the isotropic etching process may also be a wet etching process or an isotropic dry etching process.
[0122] In this embodiment, the gate functional layer 310 includes a gate dielectric layer 31 and a work function layer 32 located on the gate dielectric layer 31 . The specific steps of forming the gate functional layer 310 in this embodiment will be described in detail below with reference to the accompanying drawings.
[0123] like Figures 11 to 13 As shown, one or more first sub-deposition and removal processes are performed to form a gate dielectric layer 31 surrounding the gate opening 160 and the channel layer 210 exposed by the through groove 170 .
[0124] Specifically, the steps of the first sub-deposition removal process include: Fig.11 As shown, a gate dielectric film 301 is formed on the bottom and sidewalls of the gate opening 160 and the sidewalls of the through groove 170, and the gate dielectric film 301 surrounds the channel layer 210; Fig.12 As shown, the gate dielectric film 301 located on the sidewalls of the gate opening 160 and the through groove 170 is removed.
[0125] In this embodiment, the bonding ability of the atoms of the gate dielectric film 301 to the surface of the interface layer 330 is greater than the bonding ability to the surface of the gate sidewall 140 or the inner sidewall 120 , so that the growth rate of the gate dielectric film 301 on the interface layer 330 is greater than the growth rate on the gate sidewall 140 or the inner sidewall 120 .
[0126] like Fig.13 As shown, in this embodiment, the gate dielectric layer 31 is formed by repeating the first sub-deposition removal process twice. In other embodiments, based on the actual required thickness of the gate dielectric layer, forming the gate dielectric layer may also include performing the first sub-deposition removal process for other times.
[0127] like Figures 14 to 16 As shown, one or more second sub-deposition and removal processes are performed to form a work function layer 32 surrounding the channel layer 210 on the channel layer 210 formed with the gate dielectric layer 31 .
[0128] Specifically, the step of forming the work function layer 32 includes one or more second sub-deposition removal processes, and the second sub-deposition removal process includes: Fig.14 As shown, a deposition process is used to form a work function film 302 on the sidewalls of the gate opening 160 and the through groove 170 formed with the gate dielectric layer 31, and the work function film 302 surrounds the channel layer 210 formed with the gate dielectric layer 31; as shown Fig.15 As shown, the work function film 302 on the sidewalls of the gate opening 160 and the through groove 170 is removed.
[0129] In this embodiment, the deposition process is an atomic layer deposition process. In the process of forming the work function film 302, the atoms of the work function film 302 material have different bonding abilities on different materials, so that the time required for the work function film 302 to bond on different material film layers is different, so that at the same time, the number of atomic layers of the work function film 302 deposited on different material film layers is different. Specifically, the bonding ability of the atoms of the work function film 302 material on the gate dielectric layer 31 or the work function film 302 is greater than the bonding ability on the gate sidewall 140 or the inner sidewall 120, which correspondingly makes the growth rate of the work function film 302 on the gate dielectric layer 31 or the work function film 302 greater than the growth rate on the sidewalls of the gate opening 160 and the through groove 170, so that the work function film 302 surrounding the channel layer 210 is thicker.
[0130] It should be noted that in the actual process, after forming the gate dielectric layer 31 and before forming the work function film 302, a work function interface layer can also be formed on the gate dielectric layer 31 to provide good interface quality for forming the work function film 302, and the work function interface layer material is selected as follows: the bonding ability of the atoms of the work function film 302 on the work function interface layer is greater than the bonding ability on the gate sidewall 140 or the inner sidewall 120, which is conducive to making the growth rate of the work function film 302 on the channel layer 210 where the work function interface layer is formed greater than the growth rate on the sidewall of the gate opening 160 or 170.
[0131] like Fig.16 As shown, in this embodiment, the second sub-deposition and removal process is performed twice to form the work function layer 32. The number of times the second sub-deposition and removal process is performed to form the work function layer is not limited to this.
[0132] refer to Fig.17 A gate electrode layer 320 is filled in the gate opening 160 and the through groove 170 formed with the gate functional layer 310 . The gate electrode layer 320 contacts the sidewalls of the gate opening 160 and the through groove 170 . The gate electrode layer 320 and the gate functional layer 310 are used to form a gate structure 300 .
[0133] The gate electrode layer 320 is used as an electrode to lead out the electrical properties of the gate structure 300, thereby realizing the electrical connection between the gate structure 300 and the external circuit. When the device is working, the gate structure 300 is used to control the opening and closing of the conductive channel. In this embodiment, the gate structure 300 is a metal gate structure.
[0134] The gate functional layer 310 exposes the side walls of the gate opening 160 and the through groove 170, which is conducive to providing a larger process space for forming the gate electrode layer 320. It is not only conducive to reducing the difficulty of filling the gate electrode layer 320 in the gate opening 160 and the through groove 170, but also the gate electrode layer 320 can contact the side walls of the gate opening 160 and the through groove 170, thereby increasing the filling volume of the gate electrode layer 320 and the proportion of the volume of the gate electrode layer 320 to the volume of the gate structure 300, which is conducive to improving the problem of increased gate resistance caused by the reduction of the gate length Lg, and further conducive to reducing the gate RC delay and increasing the circuit speed, thereby improving the performance of the semiconductor structure.
[0135] Specifically, compared with the work function layer 32, the resistivity of the gate electrode layer 320 material is lower. By increasing the volume of the gate electrode layer 320 and increasing the proportion of the volume of the gate electrode layer 320 to the volume of the gate structure 300, it is beneficial to significantly improve the problem of increased gate resistance caused by the reduction of the gate length Lg.
[0136] In this embodiment, the portion of the gate structure 300 located in the through-slot 170 is the first portion 300 ( 1 ), and the portion of the gate structure 300 located in the gate opening 160 is the second portion 300 ( 2 ).
[0137] In this embodiment, the sidewall of the gate opening 160 has a gate sidewall 140, and the sidewall of the through groove 170 has an inner sidewall 120. Therefore, the first portion 300 (1) contacts the sidewall of the inner sidewall 120, and the second portion 300 (2) contacts the sidewall of the gate sidewall 140.
[0138] The material of the gate electrode layer 320 is a conductive material. In this embodiment, the material of the gate electrode layer 320 is W. In other embodiments, the material of the gate electrode layer may also be Al, Cu, Ag, Au, Pt, Ni or Ti.
[0139] In this embodiment, the process of forming the gate electrode layer 320 includes an atomic layer deposition process. The atomic layer deposition process has a high gap filling capability, which is beneficial to improving the filling capability and filling quality of the gate electrode layer 320 in the gate opening 160 and the through groove 170, thereby improving the performance of the device.
[0140] Specifically, the step of forming the gate electrode layer 320 includes: filling the gate opening 160 and the through groove 170 with a gate electrode material layer (not shown), the gate electrode material layer also being formed on the interlayer dielectric layer 130; and using a planarization process to remove the gate electrode material layer above the top surface of the interlayer dielectric layer 130. The process of forming the gate electrode material layer includes an atomic layer deposition process. The planarization process includes a chemical mechanical planarization process.
[0141] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.
Claims
1. A semiconductor structure, characterized in that: include: substrate; A channel structure layer, located on the substrate and spaced apart from the substrate, the channel structure layer comprising one or more spaced apart channel layers; A source-drain doped layer, located on both sides of the channel structure layer along the length direction of the channel layer and covering the sidewalls of the channel structure layer, wherein the source-drain doped layer and the adjacent channel layer, or the source-drain doped layer and the substrate, and the channel layer adjacent to the substrate form a through groove; A gate opening, located between the source and drain doping layers and spanning the channel structure layer, the gate opening being connected to the through groove; A gate structure filled in the gate opening and the through groove, the gate structure covers the top of the channel structure layer and surrounds the channel layer, the gate structure includes a gate function layer surrounding the channel layer, and a gate electrode layer filled in the gate opening and the through groove formed with the gate function layer, the gate function layer exposes the sidewalls of the through groove and the gate opening, and the gate electrode layer contacts the sidewalls of the gate opening and the through groove; the step of forming the gate function layer includes one or more deposition removal processes, and the steps of the deposition removal process include: forming a gate function film on the bottom and sidewalls of the gate opening and the sidewalls of the through groove, and the gate function film surrounds the channel layer; The gate function film on the sidewalls of the gate opening and the through groove is removed.
2. The semiconductor structure according to claim 1, wherein: The gate functional layer is a gate dielectric layer; Alternatively, the gate function layer is a work function layer; Alternatively, the gate function layer includes a gate dielectric layer and a work function layer located on the gate dielectric layer.
3. The semiconductor structure according to claim 2, wherein: The substrate includes a first region for forming a first device and a second region for forming a second device; the thickness of the gate functional layer in the first region is different from the thickness of the gate functional layer in the second region.
4. The semiconductor structure according to claim 1, wherein: The semiconductor structure further includes an interface layer located between the gate structure and the channel layer.
5. The semiconductor structure according to claim 4, characterized in that The material of the interface layer includes silicon oxide.
6. The semiconductor structure according to claim 1, wherein: The portion of the gate structure located in the through groove is the first portion, and along the length direction of the channel layer, the sidewall of the first portion is indented relative to the sidewall of the channel layer; the semiconductor structure also includes: an inner sidewall located between the first portion and the source and drain doping layer.
7. The semiconductor structure according to claim 6, wherein: The material of the inner sidewall includes silicon nitride, silicon oxide, silicon oxynitride, low-k dielectric material or ultra-low-k dielectric material.
8. The semiconductor structure according to claim 1, wherein: The portion of the gate structure located within the gate opening is the second portion; the semiconductor structure further includes: an interlayer dielectric layer located on the substrate at the side of the gate structure and covering the source and drain doped layer; and a gate sidewall located between the second portion and the interlayer dielectric layer.
9. A method for forming a semiconductor structure, characterized in that: include: Providing a substrate, on which one or more channel stacks stacked sequentially from bottom to top are formed, each of the channel stacks comprising a sacrificial layer and a channel layer located on the sacrificial layer; forming a dummy gate structure across the channel stack on the substrate, wherein the dummy gate structure covers a portion of the top and a portion of the sidewall of the channel stack; forming source-drain doping layers in the channel stacks on both sides of the dummy gate structure; After forming the source-drain doping layer, removing the dummy gate structure to form a gate opening to expose the channel stack; The sacrificial layer is removed to form a through groove connected to the gate opening, wherein the through groove is surrounded by the adjacent channel layer and the source-drain doped layer, or the through groove is surrounded by the substrate, the channel layer adjacent to the substrate, and the source-drain doped layer; forming a gate function layer surrounding the gate opening and the channel layer exposed by the through groove, wherein the gate function layer exposes the sidewalls of the gate opening and the through groove; The step of forming the gate functional layer includes one or more deposition removal processes, and the deposition removal process includes: forming a gate functional film on the bottom and sidewalls of the gate opening and the sidewalls of the through groove, wherein the gate functional film surrounds the channel layer; removing the gate functional film on the sidewalls of the gate opening and the through groove; A gate electrode layer is filled in the gate opening and the through groove formed with the gate function layer, the gate electrode layer is in contact with the sidewalls of the gate opening and the through groove, and the gate electrode layer and the gate function layer are used to form a gate structure.
10. The method for forming a semiconductor structure according to claim 9, wherein: The gate functional layer is a gate dielectric layer; or, the gate functional layer is a work function layer; or, the gate functional layer includes a gate dielectric layer and a work function layer located on the gate dielectric layer.
11. The method for forming a semiconductor structure according to claim 10, wherein: The gate function layer includes a gate dielectric layer and a work function layer located on the gate dielectric layer; The step of forming the gate functional layer includes: performing one or more first sub-deposition removal processes to form a gate dielectric layer surrounding the gate opening and the channel layer exposed by the through groove; Performing one or more second sub-deposition and removal processes to form a work function layer surrounding the channel layer on the channel layer formed with the gate dielectric layer.
12. The method for forming a semiconductor structure according to claim 9, wherein: In the step of deposition and removal, in the process of forming the gate functional film, the thickness of the gate functional film surrounding the channel layer is greater than the thickness of the gate functional film formed on the gate opening and the sidewall of the through groove; The step of removing the gate functional film on the sidewalls of the gate opening and the through groove comprises: etching the gate functional film using an isotropic etching process until the gate functional film on the sidewalls of the gate opening and the through groove is removed.
13. The method for forming a semiconductor structure according to claim 12, wherein: The isotropic etching process includes an atomic layer etching process, a wet etching process or an isotropic dry etching process.
14. The method for forming a semiconductor structure according to claim 9, wherein: The process of forming the gate functional film includes an atomic layer deposition process.
15. The method for forming a semiconductor structure according to claim 14, wherein: After forming the through groove and before forming the gate functional layer, the method for forming the semiconductor structure further includes: forming an interface layer surrounding the gate opening and the channel layer exposed by the through groove; During the process of forming the gate functional film, the growth rate of the gate functional film on the channel layer formed with the interface layer or the gate functional film is greater than the growth rate on the gate opening and the sidewall of the through groove.
16. The method for forming a semiconductor structure according to claim 15, wherein: The step of forming the interface layer includes performing plasma oxidation treatment on the surface of the channel layer.
17. The method for forming a semiconductor structure according to claim 15, wherein: After forming the dummy gate structure and before forming the source-drain doping layer, the method for forming the semiconductor structure further includes: forming a groove in the channel stack on both sides of the dummy gate structure; etching a portion of the sacrificial layer exposed by the sidewall of the groove along the length direction of the channel layer to form a groove, wherein the groove is surrounded by the adjacent channel layer and the sacrificial layer, or surrounded by the substrate, the channel layer adjacent to the substrate, and the sacrificial layer; and forming an inner sidewall in the groove; The step of forming the source-drain doping layer includes: forming the source-drain doping layer in the groove.
18. The method for forming a semiconductor structure according to claim 15, wherein: The method for forming the semiconductor structure further comprises: after forming the dummy gate structure and before forming the source-drain doping layer, forming a gate sidewall on the sidewall of the dummy gate structure.
19. The method for forming a semiconductor structure according to claim 9 or 10, characterized in that: In the step of providing a substrate, the substrate includes a first region for forming a first device and a second region for forming a second device; Forming the gate functional layer includes: performing a first number of deposition and removal processes to form a gate functional layer surrounding the gate opening and the channel layer exposed by the through groove on the first area, and performing a second number of deposition and removal processes to form a gate functional layer surrounding the gate opening and the channel layer exposed by the through groove on the second area, and the second number of times is different from the first number.