Thermoplastic elastomer composition and thermoplastic elastomer manufactured using the same

By adjusting the composition and additives of EPDM/PP thermoplastic elastomer, the damping performance and compression set of the material were improved, the noise and vibration problems at low temperatures were solved, and the sealing performance and user experience of the inner weatherstripping were enhanced.

CN114989534BActive Publication Date: 2026-11-20HYUNDAI MOTOR CO LTD +3
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202111478270.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-03-02
Filing Date
2021-12-06
Publication Date
2026-11-20
Estimated Expiration
2041-12-06

AI Technical Summary

Technical Problem

EPDM/PP thermoplastic elastomers exhibit poor damping properties at low temperatures, leading to noise and vibration problems. Additionally, increased compression set affects the sealing performance of the inner weatherstripping.

Method used

A thermoplastic elastomer composition was prepared by adjusting the ratio of ethylene propylene diene monomer (EPDM) and polypropylene (PP), and adding appropriate amounts of plasticizers, crosslinking agents and other additives, which improves the material's damping performance and reduces compression set.

Benefits of technology

The sealing performance of the inner weatherstripping has been improved, reducing friction noise and vibration, and enhancing the emotional quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114989534B_ABST
    Figure CN114989534B_ABST
Patent Text Reader

Abstract

The present invention relates to a thermoplastic elastomer composition comprising: about 80 parts by weight of a ternary ethylene propylene diene rubber (EPDM) comprising 5-ethylidene-2-norbornene (ENB) and polyethylene, about 30 parts by weight to about 70 parts by weight of polypropylene, about 20 parts by weight to about 40 parts by weight of a filler, and about 60 parts by weight to about 90 parts by weight of a plasticizer, and a thermoplastic elastomer manufactured using the same.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Cross-references to related applications

[0002] This application claims priority and benefit to Korean Patent Application No. 10-2021-0027197, filed on March 2, 2021, with the Korean Intellectual Property Office, the entire contents of which are incorporated herein by reference. Technical Field

[0003] This application relates to compositions of EPDM / PP thermoplastic elastomers that simultaneously possess improved material damping properties and compression set, and thermoplastic elastomers manufactured using the same. Background Technology

[0004] Weatherstripping is installed around the vehicle body or doors to help the door glass follow the correct tracks or prevent it from detaching from the tracks during vertical movement. In addition, weatherstripping also serves as a seal, preventing foreign objects (such as snow and rain) from flowing between the door glass and the door.

[0005] Specifically, the inner weatherstripping seals the vehicle interior and door windows to prevent foreign objects from entering and wind noise from entering. The inner weatherstripping not only needs excellent sealing performance but also superior dustproofing and sound insulation. In other words, friction between the door windows and the inner weatherstripping can generate vibration and noise problems.

[0006] On the other hand, EPDM / PP thermoplastic elastomer is obtained through a blending process of thermosetting elastomer (EPDM) and thermoplastic (PP), specifically through dynamic crosslinking of EPDM during the blending process.

[0007] This EPDM / PP thermoplastic elastomer is made by incorporating thermoplastic plastic into a thermosetting elastomer (EPDM). Unlike traditional thermosetting elastomers, EPDM / PP thermoplastic elastomers can be remolded and recycled, and are characterized by being both environmentally friendly and having a lower density than EPDM. Therefore, EPDM / PP thermoplastic elastomers are being used in the automotive industry as an environmentally friendly and lightweight material.

[0008] However, due to the poor damping properties of EPDM / PP thermoplastic elastomers, when applied to inner weatherstripping, noise and vibration problems caused by friction occur at low temperatures (approximately -4°C to approximately 4°C). Furthermore, as material damping increases, compression set also increases, which adversely affects the sealing performance of the inner weatherstripping. Summary of the Invention

[0009] One embodiment provides a thermoplastic elastomer composition that simultaneously improves material damping properties and compression set, resulting in improved sealing performance when applied to inner weatherstripping, while reducing frictional noise and vibration to improve emotional quality.

[0010] According to one embodiment, the thermoplastic elastomer composition comprises: about 80 parts by weight of ethylene propylene diene monomer (EPDM) rubber comprising 5-ethylidene-2-norbornene (ENB) and polyethylene, about 30 parts by weight to about 70 parts by weight of polypropylene, about 20 parts by weight to about 40 parts by weight of filler, and about 60 parts by weight to about 90 parts by weight of plasticizer.

[0011] Based on the total weight of the EPDM rubber, the EPDM rubber may contain about 5% to about 10% by weight of 5-ethylidene-2-norbornene and about 50% to about 70% by weight of polyethylene.

[0012] Based on the total weight of the EPDM rubber, the EPDM rubber may contain about 8.9% to about 10% by weight of 5-ethylidene-2-norbornene and about 50% to about 58% by weight of polyethylene.

[0013] EPDM rubber can have a crystallinity of about 0% to about 15.8% and a crystallinity of about 2.26 × 10⁻⁶. -4 mol / ml to approximately 2.68 × 10⁻⁶ -4 Crosslinking density of mol / ml and molecular weight distribution of about 3.4 to about 4.3.

[0014] The thermoplastic elastomer composition may contain about 30 parts by weight to about 35 parts by weight of polypropylene.

[0015] Polypropylene can have a crystallinity of about 52% to about 60%.

[0016] The thermoplastic elastomer composition may contain about 85 parts by weight to about 90 parts by weight of plasticizer.

[0017] The thermoplastic elastomer composition may further comprise about 0.1 parts by weight to about 1.25 parts by weight of a crosslinking agent.

[0018] The thermoplastic elastomer composition may further comprise about 0.1 parts by weight to about 0.5 parts by weight of a crosslinking aid, about 0.1 parts by weight to about 0.5 parts by weight of an antioxidant, about 1 part by weight to about 3 parts by weight of a surface modifier, about 1 part by weight to about 3 parts by weight of a lubricant, about 1 part by weight to about 3 parts by weight of a crosslinking accelerator, about 1 part by weight to about 5 parts by weight of a UV stabilizer, or a mixture thereof.

[0019] According to another embodiment, the thermoplastic elastomer made from the thermoplastic elastomer composition according to one embodiment has a loss factor (Tanδ) greater than or equal to about 0.139 and a compression set less than or equal to about 45.44%.

[0020] Thermoplastic elastomers can have a loss factor (Tanδ) of about 0.144 to about 0.158 and a compression set of about 29.53% to about 35.35%.

[0021] During adhesive sliding, thermoplastic elastomers can have a static coefficient of friction less than or equal to about 0.9, a dynamic coefficient of friction less than or equal to about 0.69, and a maximum acceleration less than or equal to about 2.44g.

[0022] According to another embodiment, a method for manufacturing a thermoplastic elastomer includes: mixing a powder containing filler, introducing ethylene propylene diene monomer (EPDM), polypropylene (PP) and the mixed powder into an extruder, mixing EPDM and polypropylene in the extruder, and dynamically crosslinking the EPDM.

[0023] According to another embodiment, the weatherstripping for a vehicle comprises a thermoplastic elastomer according to another embodiment.

[0024] According to one embodiment, the thermoplastic elastomer composition simultaneously improves material damping properties and compression set, resulting in improved sealing performance when applied to inner weatherstripping, while reducing frictional noise and vibration to improve emotional quality. Attached Figure Description

[0025] Figure 1 This is a process flow diagram illustrating the manufacturing process of a thermoplastic elastomer according to one embodiment.

[0026] Figure 2 This is a cross-sectional view showing a weatherstripping for a vehicle according to one embodiment.

[0027] Figure 3 This is a graph showing the results of the material damping properties of the thermoplastic elastomer measured in Experimental Example 2 based on the changes in the crystallinity, crosslinking density, and molecular weight distribution of EPDM and the changes in the crystallinity of PP.

[0028] Figure 4 This is a graph showing the results of compression set of the thermoplastic elastomer measured in Experimental Example 2 based on changes in the crystallinity, crosslinking density, and molecular weight distribution of EPDM and changes in the crystallinity of PP.

[0029] Figures 5 to 7These are electron micrographs showing the particle size of EPDM based on its ENB content.

[0030] Figure 8 This is a graph showing the results of the material damping properties of the thermoplastic elastomer measured according to the changes in crosslinking agent content, plasticizer content and filler content in Experimental Example 3.

[0031] Figure 9 This is a graph showing the results of compression set of the thermoplastic elastomer measured according to the changes in crosslinking agent content, plasticizer content and filler content in Experimental Example 3.

[0032] Figure 10 This is a graph showing the results of measuring the change in the coefficient of friction of the thermoplastic elastomers prepared according to Examples 1 to 5 in Experimental Example 4.

[0033] Figure 11 This is a graph showing the results of measuring the magnitude of the frictional vibration acceleration of the thermoplastic elastomers prepared according to Examples 1 to 5 in Experimental Example 4. Detailed Implementation

[0034] The advantages and features of this application and its implementation methods will become apparent from the embodiments described below with reference to the accompanying drawings. However, the embodiments should not be construed as limited to those set forth herein. Unless otherwise defined, all terms (including technical and scientific terms) in this specification are to be interpreted as commonly understood by those skilled in the art. Furthermore, terms as defined in commonly used dictionaries should not be ideally or over-interpreted unless explicitly defined.

[0035] Furthermore, unless there is an explicit description to the contrary, the word “comprising” and variations such as “including” or “containing” will be understood to imply the inclusion of the stated element but not to exclude any other elements.

[0036] Furthermore, unless otherwise stated, the singular includes the plural.

[0037] The thermoplastic elastomer composition according to one embodiment comprises: about 80 parts by weight of ethylene propylene diene monomer (EPDM), about 30 parts by weight to about 70 parts by weight of polypropylene, about 20 parts by weight to about 40 parts by weight of filler, and about 60 parts by weight to about 90 parts by weight of plasticizer.

[0038] As used herein, the term “about” or its equivalents include stated and average values ​​of a particular value within an acceptable range of deviation, taking into account measurement errors associated with the measurement of a particular parameter, as determined by a person skilled in the art.

[0039] Thermoplastic elastomer compositions may contain a mixture of ethylene propylene diene monomer (EPDM) rubber and polypropylene as the base resin.

[0040] EPDM rubber can improve the extrusion molding properties and recyclability of door side extruded parts, and enhance weather resistance and heat resistance.

[0041] The amount of EPDM rubber included can be approximately 80 parts by weight. If the EPDM rubber content is too low, defects in product flowability may occur during extrusion molding, leading to reduced dimensional stability, difficulty in molding, and a lower product recycling rate. If the EPDM rubber content is too high, the hardness of the finished product will increase, and the characteristics of compression load and compression set, which have a significant impact on door side performance, may deteriorate, potentially causing handling difficulties when the final product is installed on the car door.

[0042] EPDM rubber can contain 5-ethylidene-2-norbornene (ENB) and polyethylene.

[0043] Based on the total weight of the EPDM rubber, the amount of polyethylene contained can be from about 50% to about 70% by weight, for example, less than or equal to about 76% by weight, less than or equal to about 62% by weight, less than or equal to about 58% by weight, or less than or equal to about 56% by weight. As the polyethylene content in the EPDM rubber decreases, the loss factor (Tanδ), a damping property of the material as a thermoplastic elastomer, may increase, while the compression set may decrease.

[0044] If, based on the total weight of the EPDM rubber, the polyethylene content is less than approximately 50% by weight, the tensile strength may decrease and physical properties may deteriorate. If the polyethylene content exceeds approximately 70% by weight, the crystallinity may increase, resulting in reduced compression set.

[0045] Based on the total weight of the EPDM rubber, the amount of 5-ethylidene-2-norbornene contained can be from about 5% by weight to about 10% by weight, for example, greater than or equal to about 5.7% by weight, greater than or equal to about 7.3% by weight, or greater than or equal to about 8.9% by weight. As the content of 5-ethylidene-2-norbornene in the EPDM rubber increases, the loss factor (Tanδ), a damping property of the thermoplastic elastomer, may increase, while the compression set may decrease.

[0046] When the content of 5-ethylidene-2-norbornene is less than about 5% by weight based on the total weight of EPDM rubber, it may be difficult to extrude and injection mold. When the content of 5-ethylidene-2-norbornene exceeds about 10% by weight, the hardness and strength of the product increase, making it difficult to cut during extrusion and injection molding.

[0047] As the polyethylene content in EPDM rubber increases, the crystallinity of EPDM rubber increases, while the crosslinking density of EPDM rubber increases with the increase of the 5-ethylidene-2-norbornene content. Therefore, EPDM rubber can have a crystallinity ranging from 0% to 15.8% and a crosslinking density of approximately 2.26 × 10⁻⁶. -4 mol / ml to approximately 2.68 × 10⁻⁶ -4 The crosslinking density is approximately 3.4 to approximately 4.3 mol / ml, and the molecular weight distribution is approximately 3.4 to approximately 4.3. Crystallinity increases with increasing PE content in EPDM. During EPDM preparation, the molecular weight distribution may vary depending on the polymerization catalyst (Ziegler-Natta-wide distribution, metallocene-narrow distribution). Therefore, as the crystallinity of EPDM decreases, the crosslinking density increases, the molecular weight distribution increases, and the loss factor (Tanδ), a damping property of the thermoplastic elastomer, may increase, while the compression set may decrease.

[0048] Polypropylene (PP) is used to form the matrix of ethylene propylene diene monomer (EPDM) rubber and to enhance its oil and heat resistance. Based on approximately 80 parts by weight of EPDM rubber, the amount of polypropylene contained can be from approximately 30 parts by weight to approximately 70 parts by weight, for example, from approximately 30 parts by weight to approximately 35 parts by weight. When the amount of polypropylene contained is less than approximately 30 parts by weight, extrusion molding is difficult due to low flowability; however, when the amount of polypropylene contained is greater than approximately 70 parts by weight, the performance may deteriorate due to increased finished product hardness, making it difficult to install door-side extruded parts.

[0049] Polypropylene can be homopolymer polypropylene with a crystallinity of about 52% to about 60%. Homopolymer polypropylene has a higher crystallinity than random copolymers or block copolymers of polyethylene. Due to the lower crystallinity of polypropylene, the loss factor (Tanδ), a damping property of the material as a thermoplastic elastomer, may increase, but its compression set may decrease.

[0050] The plasticizer can be, for example, a high-viscosity paraffin oil, and the kinematic viscosity of the high-viscosity paraffin oil at about 40°C can be about 170 or higher.

[0051] Plasticizers improve the processability of thermoplastic elastomer compositions and also promote the dispersion of fillers, etc. Furthermore, plasticizers reduce the hardness of thermoplastic elastomer compositions, thereby increasing plasticity and moldability.

[0052] Based on approximately 80 parts by weight of EPDM rubber, the amount of plasticizer contained can be from approximately 60 parts by weight to approximately 90 parts by weight, for example, greater than or equal to approximately 65 parts by weight, greater than or equal to approximately 75 parts by weight, or greater than or equal to approximately 85 parts by weight. With the increase of plasticizer content, the loss factor (Tanδ), a damping property of the thermoplastic elastomer, may increase, while the compression set may decrease.

[0053] When the amount of plasticizer contained is less than about 60 parts by weight, the flowability may deteriorate during extrusion molding, which may lead to molding and processing defects. However, when the amount of plasticizer contained is greater than about 90 parts by weight, the flowability may increase, the extruded shape may deteriorate, and a longer cooling time may be required.

[0054] The thermoplastic elastomer composition may further include a crosslinking agent. For example, the crosslinking agent may include a phenolic resin crosslinking agent, a peroxide crosslinking agent, a silane crosslinking agent, or a combination thereof.

[0055] The role of crosslinking agents is to crosslink the rubber segments to exhibit the properties of thermoplastic elastomers. By adding crosslinking agents to crosslink the rubber segments (which are soft segments), and using a twin-screw extruder for dynamic crosslinking, thermoplastic elastomers are prepared, giving them rubber-like viscosity and elasticity. Here, phenolic resin crosslinking agents are chemicals that are very sensitive to moisture, and therefore may cause problems due to water absorption in summer. However, compared to phenolic resin crosslinking agents, peroxide crosslinking agents have fewer problems caused by water absorption.

[0056] For example, a peroxide crosslinking agent can have the structure of 2,5-dimethyl-2,5-di-(tert-butylperoxy)-hexane, a half-life temperature of about 170°C, and a molecular weight greater than or equal to about 290.

[0057] Based on approximately 80 parts by weight of EPDM rubber, the amount of crosslinking agent contained can be from approximately 0.1 parts by weight to approximately 1.25 parts by weight, for example, less than or equal to approximately 1.0 parts by weight, or less than or equal to approximately 0.76 parts by weight. As the content of crosslinking agent decreases, the loss factor (Tanδ), a damping property of the thermoplastic elastomer, may increase.

[0058] When the amount of crosslinking agent contained is less than about 0.1 parts by weight, insufficient crosslinking occurs, resulting in poor properties and elasticity of the finished product. When the amount of crosslinking agent contained is greater than about 1.25 parts by weight, excessive crosslinking may cause foreign objects such as fish eyes to be observed externally, resulting in appearance defects and molding defects in the extrusion molding machine.

[0059] The filler can be an inorganic filler, for example, an inorganic filler can be calcium carbonate with a particle size of less than or equal to about 10 μm and a whiteness of greater than or equal to about 95%.

[0060] Based on approximately 80 parts by weight of EPDM rubber, the amount of filler contained can be from approximately 20 parts by weight to approximately 40 parts by weight. When the amount of filler contained is less than approximately 20 parts by weight, the cost of other materials may increase and the filler effect may be insufficient. However, when the amount of filler contained is greater than approximately 40 parts by weight, extrusion molding may be difficult due to the increased hardness and reduced flowability of the material.

[0061] The thermoplastic elastomer composition may further include other additives, such as crosslinking aids, antioxidants, surface modifiers, lubricants, crosslinking accelerators, UV stabilizers, or mixtures thereof. For example, based on 80 parts by weight of EPDM rubber, the thermoplastic elastomer composition may further include about 0.1 parts by weight to about 0.5 parts by weight of a crosslinking aid, about 0.1 parts by weight to about 0.5 parts by weight of an antioxidant, about 1 part by weight to about 3 parts by weight of a surface modifier, about 1 part by weight to about 3 parts by weight of a lubricant, about 1 part by weight to about 3 parts by weight of a crosslinking accelerator, about 1 part by weight to about 5 parts by weight of a UV stabilizer, or mixtures thereof.

[0062] For example, the crosslinking aid can be N,N'-isophthalimide, 1,2-polybutadiene, or a mixture thereof.

[0063] When the amount of crosslinking agent is less than about 0.1 parts by weight, its effect may not be obvious. However, when the amount of crosslinking agent is greater than about 0.5 parts by weight, fish eyes may appear on the surface of the product due to over-crosslinking, and the appearance of the product will be deteriorated.

[0064] The antioxidant has a melting point of about 120°C and a whiteness of about 95%, and may be, for example, tetra(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, tetra(3-dodecylthiopropionate) or a mixture thereof.

[0065] When the amount of antioxidant is less than about 0.1 parts by weight, the properties of the thermoplastic elastomer composition deteriorate, and the performance of the finished product may deteriorate with prolonged use. When the amount of antioxidant is about 0.5 parts by weight, the product may exhibit blooming.

[0066] The surface modifier can be, for example, a polypropylene-based wax. The polypropylene-based wax may have a specific gravity of about 0.90 or less and a melting point of about 160°C or higher.

[0067] When the content of the surface modifier is less than about 1 part by weight, the effect of improving the scratch resistance of the finished product may be insufficient, and its wear resistance may deteriorate. When the content of the surface modifier is greater than about 3 parts by weight, the surface modifier may transfer to the surface of the finished product and fail to achieve the product characteristics.

[0068] UV stabilizers can be, for example, benzotriazole type UV absorbers, oligomeric HALS (hindered amine light stabilizers) type UV stabilizers, or mixtures thereof.

[0069] When the content of UV stabilizer is less than about 1 part by weight, it may cause whitening and microcracks on the surface due to UV attack. However, when the content of UV stabilizer is greater than about 5 parts by weight, UV stabilizers with low molecular weight may transfer to the surface and cause frost on the exterior of the product.

[0070] According to another embodiment, a thermoplastic elastomer is prepared by using a thermoplastic elastomer composition.

[0071] As described above, as the content of polyethylene in the EPDM rubber of the thermoplastic elastomer composition decreases, but the content of 5-ethylidene-2-norbornene in the EPDM rubber increases, the crystallinity of the EPDM rubber decreases, but its crosslinking density increases. Furthermore, with the increase of molecular weight distribution, the loss factor (Tanδ), which is the material damping property of the thermoplastic elastomer, may increase, but the compression set may decrease.

[0072] Furthermore, due to the lower crystallinity of polypropylene in the thermoplastic elastomer composition, the plasticizer content increases, and with the decrease in crosslinking agent content, the loss factor (Tanδ), which is the material damping property of the thermoplastic elastomer, may increase, but the compression set may decrease.

[0073] Therefore, in thermoplastic elastomers prepared by using thermoplastic elastomer compositions, the material damping properties and compression set, which are in a trade-off, are simultaneously improved.

[0074] For example, when measured at room temperature (24°C), the loss factor (Tanδ) of the thermoplastic elastomer exhibiting material damping performance can be greater than or equal to about 0.139, such as greater than or equal to about 0.140, greater than or equal to about 0.141, greater than or equal to about 0.142, greater than or equal to about 0.143, greater than or equal to about 0.144, greater than or equal to about 0.145, greater than or equal to about 0.148, greater than or equal to about 0.149, greater than or equal to about 0.150, greater than or equal to about 0.152, greater than or equal to about 0.153, greater than or equal to about 0.155, or greater than or equal to about 0.158, or about 0.144 to about 0.158.

[0075] Furthermore, when measured at low temperatures (approximately -4°C to approximately 4°C), the loss factor (Tanδ) of the thermoplastic elastomer exhibiting material damping performance can be greater than or equal to approximately 0.110, for example, greater than or equal to approximately 0.114, greater than or equal to approximately 0.115, greater than or equal to approximately 0.116, greater than or equal to approximately 0.117, greater than or equal to approximately 0.118, greater than or equal to approximately 0.121, greater than or equal to approximately 0.122, greater than or equal to approximately 0.123, or greater than or equal to approximately 0.124.

[0076] The loss factor (Tanδ), which represents the damping performance of a material, can be obtained by performing a temperature scan at approximately 0.2% dynamic strain and approximately 10 Hz using a Q850 instrument (Dynamic Mechanical Analysis, DMA) manufactured by TA Instruments, and then calculating each average Tanδ at room temperature (approximately 24 °C) or at low temperature (approximately -4 °C to approximately 4 °C).

[0077] The compression set of the thermoplastic elastomer can be less than or equal to about 45.44%, for example less than or equal to about 43.75%, less than or equal to about 43.26%, less than or equal to about 43.13%, less than or equal to about 42.97%, less than or equal to about 40.49%, less than or equal to about 35.35%, less than or equal to about 34.59%, less than or equal to about 31.45%, less than or equal to about 30.94%, less than or equal to about 30.70%, less than or equal to about 30.44%, less than or equal to about 30.37%, less than or equal to about 30.29%, less than or equal to about 30.17%, less than or equal to about 30.04%, less than or equal to about 29.51%, less than or equal to about 28.17%, less than or equal to about 29.53%, less than or equal to about 29.51%, less than or equal to about 27.55%, or about 29.53% to about 35.35%.

[0078] Compression set can be measured by applying a strain of about 25% according to ISO 815 and then continuing in an oven at about 70°C for about 22 hours.

[0079] Furthermore, the static friction coefficient of the thermoplastic elastomer can be less than or equal to about 0.9, for example, less than or equal to about 0.83, or less than or equal to about 0.69; the kinetic friction coefficient can be less than or equal to about 0.69, for example, less than or equal to about 0.67, or less than or equal to about 0.64; and the maximum acceleration exhibiting noise acceleration during adhesive sliding can be less than or equal to about 2.44g, for example, less than or equal to about 1.38g, or less than or equal to about 1.03g (where g is the unit of gravitational acceleration, 1g = 9.81m / s²). 2 ).

[0080] The coefficient of friction and maximum acceleration during adhesive sliding can be obtained by measuring the coefficient of friction and peak acceleration during adhesive sliding using a device manufactured by Zins-Ziegler Instrument GmbH under a vertical load of about 5 N at a speed of about 3 mm / s.

[0081] Therefore, thermoplastic elastomers, when applied to internal weatherstripping, can improve sealing performance and reduce frictional noise and vibration, thus contributing to improved emotional quality, as both material damping properties and compression set are simultaneously improved.

[0082] Figure 1 This is a process flow diagram illustrating the process of manufacturing a thermoplastic elastomer according to another embodiment.

[0083] refer to Figure 1 The method for manufacturing thermoplastic elastomers includes: a powder mixing step (S1), an extruder input step (S2), a mixing step of ethylene propylene diene monomer (EPDM) and polypropylene (PP) (S3), and an EPDM dynamic crosslinking step (S4).

[0084] In the powder mixing step (S1), powders such as fillers and other additives, other than ethylene propylene diene monomer (EPDM) rubber and polypropylene (PP), are premixed. Specifically, various chemicals are mixed in a super mixer to allow the dispersed chemicals to be fed into the extruder.

[0085] In the extruder input step (S2), each raw material is fed into the extruder. Specifically, ethylene propylene diene monomer (EPDM), polypropylene (PP), and pre-mixed powder are fed into the extruder in a predetermined ratio using a metering device.

[0086] In the EPDM and PP mixing step (S3), each raw material is mixed through the air gap between the screw and barrel of the extruder.

[0087] In the EPDM dynamic crosslinking step (S4), EPDM is dynamically crosslinked. The barrel temperature is adjusted and the screw assembly is configured for optimal dynamic crosslinking reaction. To improve the efficiency of the dynamic crosslinking reaction, a kneading section (to enhance shear force) can be added to the screw assembly to reduce the size of the EPDM particles.

[0088] Finally, dynamically cross-linked thermoplastic elastomer products can be cut and granulated immediately after unloading (S5).

[0089] Additionally, a weatherstripping for a vehicle according to another embodiment comprises a thermoplastic elastomer according to another embodiment.

[0090] Figure 2 This is a cross-sectional view showing a weatherstripping used in vehicles. (Reference) Figure 2 The weatherstripping 10 may include a sealing lip 11, a flocked component 12, a main body 13, a fixing part 15, and an outer wall sealing lip 16. The flocked component 12 forms a contact surface with the door glass 2. The main body 13 includes a reinforcing core material made of SUS material that is inserted therein and acts as a support. The fixing part 15 is fixed to the outside along the waistline of the door panel 1. The outer wall sealing lip 16 is tightly supported by the door panel 1.

[0091] Here, the sealing lip 11, the fixing portion 15, the outer wall sealing lip 16, or a combination thereof may contain a thermoplastic elastomer.

[0092] Specific embodiments of this application are presented below. However, the embodiments described below are for illustrative purposes only, and the scope of this application is not limited thereto.

[0093] [Preparation Example: Preparation of Thermoplastic Elastomers]

[0094] (Preparation Example 1)

[0095] EPDM / PP thermoplastic elastomers were prepared by mixing the components in the proportions shown in Table 1 and using a twin-screw extruder.

[0096] (Preparation Example 2)

[0097] An EPDM / PP thermoplastic elastomer composition was prepared using the same method as in Preparation Example 1, except that 31 parts by weight of polypropylene (PP) were mixed as shown in Table 1.

[0098] (Preparation Example 3)

[0099] An EPDM / PP thermoplastic elastomer composition was prepared using the same method as in Preparation Example 2, except that it was mixed with EPDM containing 56% by weight of polyethylene (PE).

[0100] (Preparation Example 4)

[0101] An EPDM / PP thermoplastic elastomer composition was prepared using the same method as in Preparation Example 3, except that it was mixed with EPDM containing 8.9 wt% 5-ethylidene-2-norbornene (ENB).

[0102] (Preparation Example 5)

[0103] An EPDM / PP thermoplastic elastomer composition was prepared using the same method as in Preparation Example 4, except that 75 parts by weight of a plasticizer (processing oil) were mixed in.

[0104] (Table 1)

[0105]

[0106]

[0107] (Unit: parts by weight)

[0108] 1) Crosslinking agent: peroxide

[0109] 2) Crosslinking aid: Triallyl cyanurate

[0110] 3) Lubricant: Stearic acid

[0111] 4) Crosslinking accelerator: zinc oxide

[0112] 5) Fillers: calcium carbonate, carbon black

[0113] 6) Plasticizer: Paraffin oil

[0114] [Experimental Example 1]

[0115] The thermoplastic elastomer compositions of Examples 1 to 5 were formed into sheets 2 mm thick using an injection molding machine, and then processed into various samples for evaluating their properties.

[0116] The property tests were conducted as follows, and the results are shown in Tables 2 and 3.

[0117] 1) Tensile properties: measured at 500 mm / min using a DUT-500C device manufactured by Daekyung Engineering Co., Ltd., in accordance with ISO 37 standard.

[0118] 2) Compression set: After applying 25% strain according to ISO 815 standard, it is placed in an oven at 70°C for 22 hours.

[0119] 3) Material damping (Tanδ): The average Tanδ was calculated at room temperature (24°C) or low temperature (-4°C to 4°C) after a temperature scan at 0.2% dynamic strain and 10 Hz using a Q850 instrument (Dynamic Mechanical Analysis, DMA) manufactured by TA Instruments.

[0120] 4) Friction coefficient and noise acceleration: The friction coefficient and peak acceleration during adhesive sliding were measured by using equipment manufactured by Zins-Ziegler Instrument GmbH at a speed of 3 mm / s under a vertical load of 5 N.

[0121] (Table 2)

[0122]

[0123] (Table 3)

[0124] nature unit Preparation Example 1 Preparation Example 2 Preparation Example 3 static friction coefficient - 0.9 0.83 0.69 coefficient of kinetic friction - 0.67 0.69 0.64 Maximum acceleration g 2.44 1.38 1.03

[0125] Referring to Table 2, compared with Preparation Example 2, when the PP content was reduced from 51 parts by weight to 31 parts by weight, the 50% modulus, tensile strength and tensile elongation decreased by 50.0%, 38.5% and 36.7% respectively, but the compression set increased by 22.2% and the material damping also increased by 3.6%.

[0126] Compared to Preparation Example 3, when the PE content of EPDM decreased from 67 wt% to 56 wt%, the 50% modulus and tensile strength decreased by 15.6% and 7.7%, respectively, but the tensile elongation increased by 7.5%. Furthermore, the compression set and material damping increased by 11.0% and 3.5%, respectively.

[0127] Compared with Preparation Example 4, when the ENB content of EPDM increased from 5.7 wt% to 8.9 wt%, the 50% modulus, tensile strength, and tensile elongation increased by 3.2%, 14.3%, and 2.0%, respectively. Furthermore, compression set and material damping also increased by 6.2% and 4.0%, respectively.

[0128] Compared to Preparation Example 5, when the content of plasticizer (processing oil) increased from 75 parts by weight to 85 parts by weight, the 50% modulus, tensile strength, and elongation at break decreased by 16.4%, 9.7%, and 2.0%, respectively. Compression set was almost similar, but material damping increased by 1.9%, with Preparation Example 5 exhibiting a low compression set of 29.53% and the highest material damping of 0.158.

[0129] Referring to Table 3, compared to Preparation Examples 1 to 3, as the material damping increased, the static friction coefficients were 0.90, 0.83, and 0.69 (decreases of 7.8% and 16.9%), and the dynamic friction coefficients were 0.67, 0.69, and 0.64 (increases of 3.0% and decreases of 7.2%), with Preparation Example 5 exhibiting the lowest friction coefficient. When adhesive sliding occurred, the maximum accelerations were 2.44, 1.38, and 1.03 (decreases of 43.4% and 25.4%), confirming that Preparation Example 5 has noise reduction and vibration damping effects.

[0130] [Experimental Example 2]

[0131] In a thermoplastic elastomer comprising 35.4 wt% EPDM and 13.7 wt% PP, the material damping properties and compression set of the thermoplastic elastomer were measured based on variations in the crystallinity, crosslinking density, and molecular weight distribution of EPDM and the crystallinity of PP. The results are shown in [Table / Figure / Insert Table ... Figure 3 and Figure 4 The material damping properties and compressive permanent deformation were measured in the same manner as in Experimental Example 1.

[0132] exist Figure 3 and Figure 4In the table, TPV 60, TPV 70, and TPV 80 correspond to PP contents of 31 parts by weight (14 wt%), 51 parts by weight (21 wt%), and 71 parts by weight (27 wt%), respectively. The specific compositions of TPV 60, TPV 70, and TPV 80 are shown in Table 4. Low EPDM crystallinity, medium EPDM crystallinity, and high EPDM crystallinity correspond to EPDM PE contents of 56 wt%, 62 wt%, and 67 wt%, respectively. Low EPDM crosslinking density, medium EPDM crosslinking density, and high EPDM crosslinking density correspond to EPDM ENB contents of 5.7 wt%, 7.3 wt%, and 8.9 wt%, respectively.

[0133] (Table 4)

[0134] Components TPV60 TPV70 TPV80 EPDM 80 (35% by weight) 80 (33% by weight) 80 (30% by weight) PP 31 (14% by weight) 51 (21% by weight) 71 (27% by weight) <![CDATA[Crosslinking agent 1) > 0.76 0.76 0.76 <![CDATA[Crosslinking assistant 2) > 0.27 0.27 0.27 <![CDATA[lubricant 3) > 1.7 1.7 1.7 <![CDATA[Crosslinking accelerator 4) > 3 3 3 <![CDATA[First filler 5) > 13.5 13.5 13.5 <![CDATA[Second filler 6) > 6 6 6 <![CDATA[Plasticizer 7) > 75 75 75

[0135] (Unit: parts by weight)

[0136] 1) Crosslinking agent: peroxide

[0137] 2) Crosslinking aid: Triallyl cyanurate

[0138] 3) Lubricant: Stearic acid

[0139] 4) Crosslinking accelerator: zinc oxide

[0140] 5) First filler: calcium carbonate

[0141] 6) Second filler: carbon black

[0142] 7) Plasticizer: Paraffin oil

[0143] refer to Figure 3 and Figure 4 The lower the PE content in EPDM, the higher the crosslinking density, the lower the crystallinity of PP, and the better the damping properties of the material.

[0144] Figures 5 to 7 These are electron micrographs showing how the particle size of EPDM changes with the ENB content of EPDM. Figures 5 to 7 The results show the cases when the ENB content of EPDM is 5.7 wt%, 7.3 wt%, and 8.9 wt%, respectively.

[0145] refer to Figures 5 to 7 As the ENB content of EPDM increases, the particle size (e.g., average diameter) of EPDM decreases to 2.10 μm, 1.67 μm, and 0.85 μm, respectively. Therefore, with the improvement of EPDM dispersibility, the frictional loss at the EPDM-PP interface increases, which has the effect of improving elasticity and permanent deformation, as well as increasing damping.

[0146] [Experimental Example 3]

[0147] In a thermoplastic elastomer containing 35.4 wt% EPDM and 13.7 wt% PP, the material damping properties and compression set of the thermoplastic elastomer were measured according to the variations in the contents of crosslinking agent, plasticizer (processing oil), and filler. The results are shown in... Figure 8 and Figure 9 The material damping properties and compressive permanent deformation were measured in the same manner as in Experimental Example 1.

[0148] exist Figure 8 and Figure 9 In the text, "low, medium, and high" crosslinking agent content refers to crosslinking agent content of 0.76 parts by weight (0.34 wt%), 1.0 parts by weight (0.44 wt%), and 1.25 parts by weight (0.55 wt%), respectively; "low, medium, and high" processing oil content refers to plasticizer content of 65 parts by weight (30.1 wt%), 75 parts by weight (33.2 wt%), and 85 parts by weight (36.0 wt%), respectively; and "low, medium, and high" filler content refers to filler content of 10 parts by weight (4.71 wt%), 23.5 parts by weight (10.4 wt%), and 30 parts by weight (12.9 wt%), respectively.

[0149] refer to Figure 8 and Figure 9 When the plasticizer content increases, the damping performance improves; however, when the crosslinking agent content increases, the damping performance deteriorates. But the filler content is unrelated to the damping performance.

[0150] [Experimental Example 4]

[0151] The changes in the coefficient of friction and the magnitude of frictional vibration acceleration of the thermoplastic elastomers prepared according to Examples 1 to 5 were measured, and the results are shown in... Figure 10 and Figure 11 The results are summarized in Table 5.

[0152] (Table 5)

[0153] coefficient of friction Maximum acceleration Preparation Example 1 0.278 2.44 Preparation Example 2 0.213 1.69 Preparation Example 3 0.235 1.38 Preparation Example 4 0.181 1.59 Preparation Example 5 0.208 1.03

[0154] refer to Figure 10 , Figure 11 According to Table 4, when the damping is increased, the static friction coefficient and the magnitude of frictional vibration decrease.

[0155] Therefore, the EPDM / PP thermoplastic elastomer composition according to one embodiment has the effect of increasing material damping and thus reducing frictional noise and vibration. Then, when this composition is applied to inner weatherstripping, it is expected to improve the overall quality of the product by improving sealing performance and simultaneously reducing frictional vibration and noise. Furthermore, this composition can be applied in various ways by adjusting the physical properties of the final product according to variations in the composition of the components.

[0156] While this application has been described in conjunction with what are now considered practical exemplary embodiments, it should be understood that this application is not limited to the disclosed embodiments. Rather, this application is intended to cover various modifications and equivalent arrangements included within the spirit and scope of the appended claims.

Claims

1. A thermoplastic elastomer composition comprising... 80 parts by weight of ethylene propylene diene monomer (EPDM) rubber containing 5-ethylidene-2-norbornene and polyethylene. 30 to 35 parts by weight of polypropylene 20 to 40 parts by weight of filler, and 60 to 90 parts by weight of plasticizer, The crystallinity of polypropylene is 52% to 60%. Based on the total weight of the EPDM rubber, the EPDM rubber contains 8.9% to 10% by weight of 5-ethylidene-2-norbornene and 50% to 58% by weight of polyethylene. The crystallinity of EPDM rubber ranges from 0% to 15.8%, and the crosslinking density is 2.26 × 10⁻⁶. -4 mol / ml to 2.68×10 -4 mol / ml, with a molecular weight distribution of 3.4 to 4.3, and The thermoplastic elastomer composition further comprises 0.1 to 1.25 parts by weight of a crosslinking agent.

2. The thermoplastic elastomer composition according to claim 1, wherein the thermoplastic elastomer composition comprises 85 to 90 parts by weight of a plasticizer.

3. The thermoplastic elastomer composition according to claim 1, wherein the thermoplastic elastomer composition comprises 0.1 to 0.5 parts by weight of a crosslinking aid, 0.1 to 0.5 parts by weight of an antioxidant, 1 to 3 parts by weight of a surface modifier, 1 to 3 parts by weight of a lubricant, 1 to 3 parts by weight of a crosslinking accelerator, 1 to 5 parts by weight of a UV stabilizer, or a mixture thereof.

4. A thermoplastic elastomer manufactured from the thermoplastic elastomer composition of claim 1, comprising: A loss factor greater than or equal to 0.139 measured at low temperatures ranging from -4°C to 4°C, and The compression set is less than or equal to 45.44% as measured at 70°C for 22 hours.

5. The thermoplastic elastomer according to claim 4, wherein the thermoplastic elastomer has Loss factors ranging from 0.144 to 0.158 were measured at low temperatures from -4°C to 4°C. Compression settling was measured at 70°C for 22 hours, ranging from 29.53% to 35.35%.

6. The thermoplastic elastomer according to claim 4, wherein... The static friction coefficient of thermoplastic elastomers is less than or equal to 0.

9. The coefficient of kinetic friction is less than or equal to 0.69, and The maximum acceleration during the adhesive sliding period is less than or equal to 2.44 g.

7. A method for manufacturing the thermoplastic elastomer according to claim 4, comprising: The mixture contains filler powder, that is, pre-mixed filler powder (excluding EPDM and polypropylene) and other additives. EPDM rubber, polypropylene, and the mixed powder are introduced into the extruder. EPDM rubber and polypropylene are mixed in an extruder, and This enables dynamic cross-linking of EPDM rubber.

8. A weatherstripping for a vehicle, comprising the thermoplastic elastomer according to claim 4.

Citation Information

Patent Citations

  • Camera module

    KR1020210027197A

  • Ethylene / alpha-olefin / nonconjugated polyene based compositions for thermoplastic vulcanizates

    CN104583304A

  • Peroxide vulcanized thermoplastic elastomer material and preparation method thereof

    CN110437549A

  • Ethylene / alpha-olefin / nonconjugated polyene based compositions for thermoplastic vulcanizates

    US20150210838A1