Thermal insulation mat and method of making same, battery pack, and device
The thermal insulation pad formed by the composite of silicone rubber and aerogel solves the problem of thermal runaway propagation in battery packs, effectively blocks heat conduction, and improves the safety performance and cycle life of battery packs.
Patent Information
- Application Number
- CN202110236896.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-03-03
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2041-03-03
AI Technical Summary
When a battery pack experiences thermal runaway, it is prone to propagation of thermal runaway, posing a safety hazard. Existing technologies are unable to effectively block heat conduction between individual battery cells, affecting the safety performance of the battery pack.
The heat insulation pad is made of silicone rubber and aerogel composite. After one side of the heat insulation pad comes into contact with a 600℃ hot surface, the temperature difference between the two sides is ≥150℃. The thermal conductivity is ≤0.13W/(m·K), the compressive strength is 1MPa~30MPa, the compressive elastic modulus is 1MPa~40MPa, the thickness is 1mm~10mm, and the aerogel particles are spherical or near-spherical with a particle size of 0.1mm~5mm and a pore size of 1nm~500nm.
It effectively blocks heat conduction between battery cells, slows down the spread of thermal runaway, improves the safety performance and cycle life of the battery pack, reduces thermal conductivity, enhances compressive strength and elastic modulus, and improves the safety performance and energy density of the battery pack.
Smart Images

Figure CN115036622B_ABST
Abstract
Description
Technical Field
[0001] This application belongs to the field of energy storage device technology, specifically relating to a heat insulation pad and its preparation method, a battery pack and a device. Background Technology
[0002] Secondary batteries have advantages such as high energy density, long cycle life, and no pollution or memory effect, and are therefore widely used in various consumer electronics products and large-scale devices such as electric vehicles and energy storage systems. For example, as environmental protection issues receive increasing attention, new energy electric vehicles are becoming more and more popular.
[0003] To meet the range requirements of electric vehicles, battery packs typically use a large number of individual cells connected in series and parallel. When one or more individual cells in the battery pack experience thermal runaway, it can easily lead to the propagation of thermal runaway within the pack, posing a safety hazard. Since the safety performance of the battery pack directly affects the safety of the electric vehicle and its passengers, effectively improving the safety performance of battery packs has become an urgent technical problem to be solved. Summary of the Invention
[0004] In view of the technical problems existing in the background art, this application provides a heat insulation pad and its preparation method, battery pack and device, which are intended to effectively improve the safety performance of the battery pack.
[0005] The first aspect of this application provides a heat insulation pad for a battery pack. The heat insulation pad includes silicone rubber and aerogel dispersed in the silicone rubber. The heat insulation pad satisfies the following condition: after one side surface of the heat insulation pad is in contact with a hot surface at 600°C for 5 minutes at a pressure of 0.9 MPa and then depressurized, and then continues to be in contact with the hot surface at 600°C for 20 minutes, the temperature difference between the one side surface of the heat insulation pad and the opposite side surface is ≥150°C.
[0006] The heat insulation pad provided in this application is formed by a composite of silicone rubber and aerogel, and the temperature difference between the surface of the heat insulation pad in pressurized contact with the hot surface and the surface on the opposite side is ≥150℃. Therefore, applying the heat insulation pad to the battery pack can effectively block heat conduction between battery cells, significantly slow down the spread of thermal runaway within the battery pack, and thus improve the safety performance of the battery pack.
[0007] In some embodiments, the temperature difference is ≥200℃. In some embodiments, the temperature difference is ≥300℃. In some embodiments, the temperature difference is 200℃~465℃. In some embodiments, the temperature difference is 300℃~465℃.
[0008] In any embodiment of the first aspect of this application, the thermal conductivity of the heat insulation pad at 100°C is ≤0.13 W / (m·K), optionally 0.022 W / (m·K) to 0.09 W / (m·K), and more preferably 0.023 W / (m·K) to 0.05 W / (m·K). A low thermal conductivity of the heat insulation pad is beneficial for improving the barrier effect against heat conduction between battery cells, thereby enhancing the safety performance of the battery pack. When the thermal conductivity of the heat insulation pad is within an appropriate range, it not only improves the safety performance of the battery pack but also allows the battery pack to have a longer cycle life.
[0009] In any embodiment of the first aspect of this application, the compressive strength of the heat insulation pad is 1 MPa to 30 MPa, optionally 3 MPa to 25 MPa, and further optionally 5 MPa to 20 MPa. When the compressive strength of the heat insulation pad is within an appropriate range, it ensures that it is not easily broken or yielded under the cyclic expansion force of the battery cell, thereby effectively performing its functions of heat insulation and buffering cyclic expansion over a long period.
[0010] In any embodiment of the first aspect of this application, the compressive modulus of the heat insulation pad is 1 MPa to 40 MPa, optionally 5 MPa to 40 MPa, further optionally 10 MPa to 30 MPa, and even more optionally 15 MPa to 25 MPa. The heat insulation pad has a good compressive modulus, which can buffer the cyclic expansion stress of the battery cells, thereby further improving the safety performance of the battery pack and also contributing to a higher cycle capacity retention rate of the battery pack.
[0011] In any embodiment of the first aspect of this application, the thickness of the heat insulation pad is 1 mm to 10 mm, optionally 2 mm to 6 mm. A heat insulation pad thickness within an appropriate range enables the battery to achieve higher safety performance and higher volumetric or gravimetric energy density.
[0012] In any embodiment of the first aspect of this application, the aerogel is a spherical or near-spherical particle. The spherical or near-spherical morphology of the aerogel reduces stress concentration under pressure, thereby ensuring that the particles are not easily broken and that the internal pore structure of the particles is not easily damaged, thus enabling the thermal insulation pad to have better long-term thermal insulation performance.
[0013] In any embodiment of the first aspect of this application, the particle size of the aerogel is 0.1 mm to 5 mm, optionally 0.3 mm to 3 mm. A particle size within an appropriate range ensures both good uniformity of aerogel particle dispersion and a high aerogel volume ratio in the insulation pad, thus enabling the insulation pad to achieve high thermal insulation performance.
[0014] In any embodiment of the first aspect of this application, the aerogel includes aerogel with a particle size of 1.8 mm to 2.2 mm, aerogel with a particle size of 0.8 mm to 1.2 mm, and aerogel with a particle size of 0.4 mm to 0.6 mm. By using a reasonable particle size distribution, the volume ratio of aerogel in the thermal insulation pad can be further increased, while also reducing the thermal bridging phenomenon that may occur due to excessive silicone rubber between particles, thereby further improving the thermal insulation effect of the thermal insulation pad.
[0015] In any embodiment of the first aspect of this application, the volume ratio of aerogel with a particle size of 1.8 mm to 2.2 mm, aerogel with a particle size of 0.8 mm to 1.2 mm, and aerogel with a particle size of 0.4 mm to 0.6 mm is (25 to 40):(5 to 10):(1 to 3). By further optimizing the particle size distribution, the thermal insulation performance of the thermal insulation pad can be further improved.
[0016] In any embodiment of the first aspect of this application, the pore size of the aerogel is 1 nm to 500 nm, optionally 10 nm to 100 nm, and more preferably 30 nm to 50 nm. The aerogel has a nanoscale porous structure of appropriate size, which can further improve the thermal insulation performance of the thermal insulation pad.
[0017] In any embodiment of the first aspect of this application, the aerogel is selected from one or more of inorganic oxide aerogels, carbon-based aerogels, and organic polymer aerogels. In some embodiments, the aerogel is selected from inorganic oxide aerogels. Optionally, the aerogel is selected from one or more of silica aerogels, alumina aerogels, zirconia aerogels, and yttrium oxide aerogels.
[0018] In any embodiment of the first aspect of this application, the surface of the aerogel particles is modified with a polymer selected from one or more of polyacrylic acids, polyacrylates, polyethers, polyols, polyolefins, their derivatives, and copolymers thereof. In some embodiments, the polymer is selected from one or more of polyacrylic acid, polymethyl methacrylate, polyethyl methacrylate, polyethylene glycol, polyvinyl alcohol, polystyrene, polybutadiene, polypropylene, their derivatives, and copolymers thereof. The use of polymer-modified aerogels enables the thermal insulation pad to perform better thermal insulation.
[0019] In any embodiment of the first aspect of this application, the silicone rubber is a condensation-type or addition-type silicone rubber, optionally a two-component addition-type silicone rubber. Two-component addition-type silicone rubber is less prone to shrinkage during vulcanization, and the resulting heat insulation pad has higher structural strength.
[0020] In any embodiment of the first aspect of this application, the silicone rubber includes one or more of silicone rubber, methyl vinyl silicone rubber, methyl phenyl vinyl silicone rubber, nitrile silicone rubber, and silicone nitrile rubber. In some embodiments, the silicone rubber includes a two-component addition-type silicone rubber.
[0021] In any embodiment of the first aspect of this application, the silicone rubber includes foamed silicone rubber.
[0022] A second aspect of this application provides a battery pack comprising a plurality of battery cells arranged in an array, wherein a heat insulation pad is disposed between at least two adjacent battery cells, and at least one heat insulation pad is the heat insulation pad according to this application. Because the battery pack of this application uses the heat insulation pad according to this application, it can achieve at least higher safety performance.
[0023] A third aspect of this application provides an electrical device that includes a battery pack according to this application. Because the electrical device of this application uses the battery pack according to this application, it can achieve at least a high level of safety performance.
[0024] The fourth aspect of this application provides a method for preparing a heat insulation pad, the method comprising the following steps: dispersing aerogel in liquid silicone rubber and forming a film; subjecting the film to vulcanization to obtain a heat insulation pad; wherein the heat insulation pad satisfies the following: after one side surface of the heat insulation pad is in contact with a hot surface at 600°C for 5 minutes at a pressure of 0.9 MPa and then depressurized, and then continues to be in contact with a hot surface at 600°C for 20 minutes, the temperature difference between the one side surface of the heat insulation pad and the opposite side surface is ≥150°C.
[0025] In any embodiment of the second aspect of this application, the mass ratio of liquid silicone rubber to aerogel is 1:(0.2 to 2).
[0026] In any embodiment of the second aspect of this application, the volume ratio of liquid silicone rubber to aerogel is 50:50 to 8:92, and optionally 30:70 to 10:90.
[0027] In any embodiment of the second aspect of this application, the viscosity of the liquid silicone rubber is 0.1 Pa·s to 50 Pa·s, optionally 0.3 Pa·s to 25 Pa·s, and further optionally 0.5 Pa·s to 15 Pa·s. Attached Figure Description
[0028] To more clearly illustrate the technical solutions of the embodiments of this application, the drawings used in the embodiments of this application will be briefly described below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on the drawings without creative effort. It should be noted that the drawings are not drawn to scale.
[0029] Figure 1 This is a schematic diagram of a vehicle provided in one embodiment of this application.
[0030] Figure 2 This is an exploded view of a battery pack provided in one embodiment of this application.
[0031] Figure 3 This is a schematic diagram of another battery pack provided in an embodiment of this application, wherein the outer packaging and other accessories of the battery pack are omitted.
[0032] Figure 4 This is a schematic diagram of the structure of a heat insulation pad provided in an embodiment of this application. Detailed Implementation
[0033] To make the inventive objectives, technical solutions, and beneficial technical effects of this application clearer, the following detailed description is provided in conjunction with embodiments. It should be understood that the embodiments described in this specification are merely illustrative and not intended to limit the scope of this application.
[0034] For simplicity, this paper only explicitly discloses some numerical ranges. However, any lower limit can be combined with any upper limit to form an undefined range; and any lower limit can be combined with other lower limits to form an undefined range, just as any upper limit can be combined with any other upper limit to form an undefined range. Furthermore, although not explicitly stated, every point or individual value between the endpoints of a range is included within that range. Therefore, each point or individual value can serve as its own lower or upper limit and be combined with any other point or individual value, or with other lower or upper limits, to form an undefined range.
[0035] In this description, it should be noted that, unless otherwise stated, the numerical range indicated by "~" includes both endpoints and any value between them. For example, "1~30" includes 1, 30, and any value between 1 and 30 (such as 4.5, 5, 7, 10, 13, 15, 16.3, 20, 23, etc.). "Several" means one or more; "multiple / types" means two / more than two (including two / types); "above" and "below" include the stated number; the terms "above," "below," "inner," and "outer," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings, and are only for the convenience and simplification of description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of this document.
[0036] In the description of this application, it should also be noted that, unless otherwise expressly specified and limited, the terms "installation," "connection," and "joining" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a direct connection or an indirect connection through an intermediate medium. Those skilled in the art can understand the specific meaning of the above terms in this application depending on the specific circumstances.
[0037] The foregoing description of this invention is not intended to describe every disclosed embodiment or implementation. Instead, the following description provides more specific examples of exemplary embodiments. Throughout the application, guidance is provided through a series of embodiments that can be used in various combinations. The examples listed are merely representative and should not be construed as exhaustive.
[0038] The device described in the embodiments of this application can be any battery-powered device. Examples of the device include, but are not limited to, mobile devices (e.g., mobile phones, laptops, portable devices, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), power tools (e.g., electric drills, electric grinders, electric wrenches, electric screwdrivers, electric hammers, impact drills, concrete vibrators, electric planers, etc.), electric trains, ships and satellites, energy storage systems, etc.
[0039] The device includes a battery pack according to embodiments of this application. The battery pack can be used as a power source for the device to provide electrical energy, or it can be used as an energy storage unit for the device.
[0040] Figure 1 This is a schematic diagram of an example device. The device is an electric vehicle 1, which can be a pure electric vehicle, a hybrid electric vehicle, or a range-extended electric vehicle, etc. A battery pack 10 can be installed inside the electric vehicle 1. The battery pack 10 serves as the power source for the electric vehicle 1, providing power to the device or meeting other operational power needs such as navigation, air conditioning, and audio systems. The number of battery cells in the battery pack 10 and its mounting position can be adjusted according to actual needs. As an example, the battery pack 10 can be located at the bottom of the electric vehicle 1, and can be located at the front or rear of the vehicle. The electric vehicle 1 can also be equipped with a controller 20 and a motor 30. The controller 20 is used to control the power supply from the battery pack 10 to the motor 30.
[0041] The battery pack 10 includes multiple battery cells to meet the requirements of high voltage and high capacity. These battery cells can be connected in series, in parallel, or a combination of both (referred to as hybrid connection). The battery pack 10 can be a battery pack or a battery module.
[0042] Figure 2This is an exploded view of battery pack 10 as an example. Battery pack 10 is a battery stack. (See reference...) Figure 2 The battery pack may include multiple battery cells 60 connected in series, parallel, or a combination thereof. The battery pack may also include a housing (or enclosure). The housing may include a first housing 51 and a second housing 52, which can be interlocked to form a housing with a closed chamber. Multiple battery cells 60 are housed within the housing. The number of battery cells 60 contained in the battery pack can be adjusted according to actual needs.
[0043] Figure 3 This is a schematic diagram of another battery pack 10 provided in this application. The battery pack 10 is a battery module 40. (Refer to...) Figure 3 The battery module 40 includes multiple battery cells 60 arranged in series, parallel, or mixed connections. The number of battery cells 60 in the battery module 40 can be adjusted according to actual needs. In this application, the battery cells 60 can be selected from lithium-ion secondary batteries, lithium-ion primary batteries, lithium-sulfur batteries, sodium-lithium-ion batteries, sodium-ion batteries, magnesium-ion batteries, etc., and this application is not limited to these. The battery cells 60 can be cylindrical, flat, cuboid, or other shapes, and this application is not limited to these either.
[0044] In the battery module 40, a heat insulation pad 70, according to any embodiment of this application, is disposed between at least two adjacent battery cells 60. The heat insulation pad 70 serves to block heat. In some embodiments, multiple battery cells 60 are arranged along the length of the battery module 40, with the larger surfaces of two adjacent battery cells 60 facing each other. Here, the larger surface refers to the side with the largest area (measured from the outer surface) of the battery cell. A heat insulation pad 70 is disposed between two adjacent groups of battery cells 60. The heat insulation pad 70 may be in contact with the surfaces of the battery cells 60 or may not be in contact with them. The number of battery cells 60 contained in each group of battery cells 60 may be one or more, for example, 1 to 5, or 2 to 4, or even 1, 2, or 3.
[0045] The battery module 40 may also include a fixing assembly (not shown) for fixing a plurality of battery cells 60. As an example, the fixing assembly may include a housing and a cover, the housing having a receiving space and an opening communicating with the receiving space. The battery cells 60 are placed within the receiving space, and the cover is placed on the housing to close the opening. Of course, the fixing assembly may also employ other structures known in the art for fixing the battery cells 60.
[0046] The heat insulation pad 70 provided in the embodiments of this application will now be described in detail.
[0047] Figure 4 This is a schematic diagram of an example heat insulation pad 70. (See reference...) Figure 4The heat insulation pad 70 provided in this application embodiment includes silicone rubber 71 and aerogel 72 dispersed in silicone rubber 71. The heat insulation pad 70 satisfies the following condition: after one side surface of the heat insulation pad 70 is in contact with a hot surface at 600°C for 5 minutes at a pressure of 0.9MPa and then depressurized, and then continues to be in contact with a hot surface at 600°C for 20 minutes, the temperature difference between one side surface of the heat insulation pad 70 and the opposite side surface is ≥150°C.
[0048] The hot surface can be a heat-conducting plate. The heat-conducting plate can be selected from known plates capable of withstanding 0.9 MPa pressure and 600°C temperature, and possessing good thermal conductivity. For example, the heat-conducting plate can be made of alloy steel. The shape of the heat-conducting plate is the same as that of the heat insulation pad 70, and the edges are aligned. The thickness of the heat-conducting plate can be 10 mm to 30 mm, for example, 26 mm.
[0049] The heat insulation pad 70 has two opposing surfaces in the thickness direction, one surface of which is in contact with a heat-conducting plate, and the other surface of which is in contact with another heat-conducting plate. The aforementioned temperature difference is the temperature difference between these two surfaces.
[0050] As an example, the heat insulation pad 70 is sandwiched between two heat-conducting plates to form a composite. A pressure of 0.9 MPa is applied to the composite, and the heat-conducting plate on one side of the heat insulation pad 70 is heated to 600°C. After holding for 5 minutes, the pressure is released, and the heat insulation pad 70 is kept in contact with the 600°C heat-conducting plate for another 20 minutes. The temperature difference between the surface of the heat insulation pad 70 in contact with the 600°C heat-conducting plate and the opposite side surface of the surface is ≥150°C.
[0051] As a more specific example, one side surface of the heat insulation pad 70 in its thickness direction is brought into contact with the surface of an alloy steel plate and the edges are aligned. The other side surface of the heat insulation pad 70 in its thickness direction is brought into contact with the surface of another alloy steel plate and the edges are aligned, forming a composite body in which the heat insulation pad 70 is sandwiched between two alloy steel plates. A pressure of 0.9 MPa is applied to the composite body along the stacking direction (i.e., the thickness direction of the heat insulation pad 70). Then, the alloy steel plate on one side of the heat insulation pad 70 is heated to 600°C, held at the temperature and pressure for 5 minutes, and then the pressure is released. After the heat insulation pad 70 continues to be in contact with the 600°C alloy steel plate for 20 minutes, the temperature of the side surface of the heat insulation pad 70 in contact with the 600°C alloy steel plate (i.e., the hot surface temperature of the heat insulation pad 70) T1 and the temperature of the other side surface opposite to the one side surface (i.e., the cold surface temperature of the heat insulation pad 70) T2 are measured, wherein T1-T2≥150°C.
[0052] There are no particular restrictions on the shape of the heat insulation pad 70, which can be selected according to the shape and structure of the battery cell 60. As an example, the heat insulation pad 70 can be a circular, rectangular or other polygonal sheet.
[0053] The heat insulation pad 70 provided in this application is formed by combining silicone rubber 71 and aerogel 72. Aerogel 72 possesses a nanoporous structure and excellent properties such as low thermal conductivity. Silicone rubber 71 not only has excellent heat resistance, ensuring it is not easily decomposed at high temperatures, but also, due to its molecular structure, gives the heat insulation pad 70 good compressive mechanical properties. The inventors have discovered that the aforementioned temperature difference of the heat insulation pad 70 is a comprehensive reflection of its thermal conductivity, thickness, and compressive mechanical properties, and can serve as a performance indicator reflecting the heat insulation pad 70's ability to block heat conduction from thermally runaway battery cells 60 within the battery pack 10. When the heat insulation pad 70 satisfies the aforementioned temperature difference within an appropriate range, applying the heat insulation pad 70 to the battery pack 10 can more effectively block heat conduction from thermally runaway battery cells 60 to adjacent battery cells 60, significantly slowing down the spread of thermal runaway within the battery pack 10, thereby improving the safety performance of the battery pack 10.
[0054] In some embodiments, the temperature difference is ≥200℃, ≥300℃, ≥350℃, or ≥400℃. Optionally, the temperature difference is 150℃~500℃, 200℃~480℃, 200℃~465℃, 270℃~470℃, 300℃~465℃, 350℃~465℃, 310℃~450℃, or 320℃~400℃. The temperature difference of the heat insulation pad 70 being within an appropriate range indicates that the heat insulation pad 70 not only has a low thermal conductivity but also can withstand the cyclic expansion stress of the battery cell 60, thereby better performing its heat insulation function and enabling the battery pack 10 to achieve higher safety performance.
[0055] In some embodiments, the thermal conductivity of the heat insulation pad 70 at 100°C is ≤0.13 W / (m·K). The lower the thermal conductivity of the heat insulation pad 70, the better its heat insulation performance, thereby further improving the safety performance of the battery. In some embodiments, the thermal conductivity of the heat insulation pad 70 at 100°C is 0.022 W / (m·K) to 0.09 W / (m·K), optionally 0.022 W / (m·K) to 0.085 W / (m·K), 0.025 W / (m·K) to 0.065 W / (m·K), 0.023 W / (m·K) to 0.05 W / (m·K), 0.03 W / (m·K) to 0.06 W / (m·K), or 0.03 W / (m·K) to 0.05 W / (m·K), etc. If the thermal conductivity of the heat insulation pad 70 is within an appropriate range, then the ratio of silicone rubber 71 and aerogel 72 is more suitable. This allows it to have high thermal insulation performance, as well as good compressive elastic modulus and compressive strength, thereby enabling the battery pack 10 to have high safety performance and long cycle life.
[0056] In some embodiments, the compressive strength of the heat insulation pad 70 is 1 MPa to 45 MPa, optionally 1 MPa to 30 MPa, 2 MPa to 26 MPa, 3 MPa to 25 MPa, 4 MPa to 22 MPa, or 5 MPa to 20 MPa. During the use of the battery pack 10, the battery cells 60 will generate significant cyclic expansion forces. With the compressive strength of the heat insulation pad 70 within an appropriate range, it can ensure that it is not easily broken or yielded under the cyclic expansion forces of the battery cells 60, thereby effectively providing heat insulation and buffering against cyclic expansion over a long period.
[0057] In some embodiments, the compressive elastic modulus of the heat insulation pad 70 is 1 MPa to 40 MPa, 5 MPa to 40 MPa, 3 MPa to 30 MPa, 10 MPa to 30 MPa, 4 MPa to 28 MPa, 5 MPa to 25 MPa, 6 MPa to 20 MPa, 10 MPa to 25 MPa, 10 MPa to 20 MPa, or 15 MPa to 25 MPa, etc. When the compressive elastic modulus of the heat insulation pad 70 is within an appropriate range, it can provide good heat insulation while also meeting the expansion requirements of the battery cell 60. In particular, it can effectively buffer the cyclic expansion of the battery cell 60, thereby controlling the internal stress of the cell. This reduces the risk of short circuits or leakage within the battery cell 60 caused by cell compression, and also reduces the risk of excessive internal pressure within the battery cell 60 breaking through the explosion-proof valve, thus further improving the safety performance of the battery pack 10.
[0058] In addition, the heat insulation pad 70 reduces the cyclic expansion stress of the battery cell 60 and is also conducive to the full wetting of the electrolyte inside the cell, so as to maintain a good ion transport interface inside the cell, which is also conducive to the battery pack 10 having a high cycle capacity retention rate.
[0059] In some embodiments, the thickness of the heat insulation pad 70 is 1mm to 10mm, optionally 1mm to 8mm, 1.5mm to 5mm, 2mm to 6mm, or 2mm to 4mm, etc. When the thickness of the heat insulation pad 70 is within an appropriate range, it can effectively block heat and buffer expansion stress, while also helping the battery pack 10 to have a smaller volume or weight, thereby enabling the battery to achieve higher safety performance and higher volumetric energy density or gravimetric energy density.
[0060] In some embodiments, the aerogel 72 is a spherical or near-spherical particle. Optionally, the sphericity of the aerogel is ≥0.8. Sphericity is the ratio of the average (including the largest diameter) of multiple (e.g., 5) different oriented diameters of the particle to the largest diameter of the particle. The particle diameter can be determined using methods known in the art, such as vernier calipers. The closer the sphericity is to 1, the closer the particle morphology is to spherical. The aerogel 72 has a spherical or near-spherical morphology, which results in a more uniform stress distribution when subjected to pressure (e.g., the compression molding pressure in the preparation of the heat insulation pad 70, or the cyclic expansion force of the battery cell 60 during use), reducing stress concentration. This ensures that the particles are not easily broken and that the internal pore structure of the particles is not easily damaged, thereby enabling the heat insulation pad 70 to have better long-term thermal insulation performance. In addition, the spherical or near-spherical aerogel particles themselves have good fluidity, which is conducive to their uniform dispersion in silicone rubber 71, and has a large contact area with silicone rubber 71 to avoid powder shedding, thereby enabling the heat insulation pad 70 to have good mechanical property consistency and high heat insulation effect as a whole.
[0061] In some embodiments, the particle size of aerogel 72 is 0.1 mm to 5 mm, optionally 0.2 mm to 4 mm, 0.3 mm to 3 mm, or 0.5 mm to 2 mm, etc. The particle size of aerogel 72 is within an appropriate range, which ensures both good uniformity of aerogel 72 particle dispersion and a high aerogel 72 volume fraction in the heat insulation pad 70, thus enabling the heat insulation pad 70 to achieve high heat insulation performance. Furthermore, the appropriate particle size of aerogel 72 also facilitates the fabrication and molding of the heat insulation pad 70, ensuring its adhesion even with a high aerogel 72 volume fraction, and preventing particle shedding or detachment.
[0062] In some embodiments, the aerogel 72 includes aerogels with particle sizes of 1.8 mm to 2.2 mm, aerogels with particle sizes of 0.8 mm to 1.2 mm, and aerogels with particle sizes of 0.4 mm to 0.6 mm. By appropriately matching particle sizes, the volume ratio of aerogel 72 in the heat insulation pad 70 can be further increased, while also reducing the thermal bridging phenomenon that may occur due to excessive silicone rubber 71 between particles, thereby further improving the heat insulation effect of the heat insulation pad 70.
[0063] In some embodiments, the volume ratio of aerogel particles with a particle size of 1.8 mm to 2.2 mm, aerogel particles with a particle size of 0.8 mm to 1.2 mm, and aerogel particles with a particle size of 0.4 mm to 0.6 mm is (25 to 40):(5 to 10):(1 to 3); optionally, it is (28 to 37):(6 to 10):(1.5 to 3), or (30 to 35):(7 to 9):(1.5 to 2.5). For example, this volume ratio is 32:8:2. By further optimizing the particle size distribution, the thermal insulation performance of the thermal insulation pad 70 can be further improved.
[0064] In some embodiments, the pore size of the aerogel 72 is 1 nm to 500 nm, optionally 10 nm to 100 nm, 10 nm to 70 nm, 15 nm to 50 nm, or 30 nm to 50 nm. The aerogel 72 has a nanoscale porous structure of appropriate size, which can "lock in" air molecules to reduce heat convection, thereby further reducing the thermal conductivity of the insulation pad 70 and thus further improving the thermal insulation performance. In addition, the pore size of the aerogel 72, within an appropriate range, can structurally prevent the infiltration of liquid silicone rubber during the fabrication of the insulation pad 70, avoiding damage to the particulate pore structure, thereby contributing to the high thermal insulation performance of the insulation pad 70.
[0065] In some embodiments, aerogel 72 is selected from one or more of inorganic oxide aerogels, carbon-based aerogels, and organic polymer aerogels. In some embodiments, aerogel 72 is selected from inorganic oxide aerogels. For example, inorganic oxide aerogels are selected from one or more of silica aerogels, alumina aerogels, zirconia aerogels, and yttrium oxide aerogels. Optionally, aerogel 72 may include silica aerogels. Examples of carbon-based aerogels include one or more of graphene aerogels and carbon nanotube aerogels. Examples of organic polymer aerogels include phenolic resin aerogels. A suitable aerogel 72 has a low thermal conductivity, enabling the thermal insulation pad 70 to have high thermal insulation performance.
[0066] In some embodiments, the surface of the aerogel 72 is modified with a polymer. This modification may involve a polymer coating the surface of the aerogel 72 particles. The polymer may be selected from one or more of polyacrylic acids, polyacrylates, polyethers, polyols, polyolefins, their derivatives, and copolymers thereof. Optionally, the polymer is selected from one or more of polyacrylic acids and polyacrylates. As a specific example, the polymer is selected from one or more of polyacrylic acid, polymethyl methacrylate, polyethyl methacrylate, polyethylene glycol, polyvinyl alcohol, polystyrene, polybutadiene, polypropylene, their derivatives, and copolymers thereof. In some embodiments, the polymer is selected from one or more of polyacrylic acid, polymethyl methacrylate, and polyethyl methacrylate.
[0067] Modifying the surface of aerogel 72 with a polymer not only gives the aerogel 72 particles higher strength, making them less prone to breakage under pressure, but also protects the pore structure of the particles from damage during the composite process of aerogel 72 and liquid silicone rubber. Furthermore, it enhances the adhesion between the aerogel 72 particles and the silicone rubber 71. Therefore, polymer-modified aerogel 72 enables the thermal insulation pad 70 to perform its insulation function better.
[0068] In this application, the silicone rubber 71 can be selected according to actual application requirements without significantly impairing the heat insulation and cushioning effects of the heat insulation pad 70. In some embodiments, the silicone rubber 71 can be a condensation-type or addition-type silicone rubber. The condensation-type silicone rubber can be a one-component condensation-type silicone rubber or a two-component condensation-type silicone rubber. The addition-type silicone rubber can be a one-component addition-type silicone rubber or a two-component addition-type silicone rubber. In some embodiments, the silicone rubber 71 is a two-component addition-type silicone rubber. Two-component silicone rubber offers better controllability during the preparation of the heat insulation pad 70 and is easier to handle. Two-component addition-type silicone rubber is less prone to shrinkage during vulcanization, and the resulting heat insulation pad 70 has higher structural strength.
[0069] In some embodiments, silicone rubber 71 may be one or more of silicone rubber, methyl vinyl silicone rubber, methyl phenyl vinyl silicone rubber, nitrile silicone rubber, and silicone-nitrogen rubber. Optionally, silicone rubber 71 is a two-component addition-type silicone rubber. Silicone rubber has the advantages of low thermal conductivity, high strength, and good adhesion. Two-component addition-type silicone rubber also has the advantage of low shrinkage during vulcanization.
[0070] In some embodiments, the silicone rubber 71 comprises foamed silicone rubber. For example, a foaming agent may be added to the silicone rubber 71. Using foamed silicone rubber allows closed-cell pores to be formed within the silicone rubber 71 matrix of the heat insulation pad 70, thereby further reducing the thermal conductivity of the heat insulation pad 70 and further improving its heat insulation performance. As an example, one component of the two-component silicone rubber contains 1 to 8% by weight of a vulcanizing agent and greater than 0 and less than or equal to 5% by weight of a foaming agent. The vulcanizing agent and foaming agent can be of types known in the art. By rationally controlling the ratio of vulcanizing agent to foaming agent, the foaming rate can be matched with the vulcanization rate during the preparation of the heat insulation pad 70, resulting in a heat insulation pad 70 with high structural strength while forming closed-cell pores of appropriate size.
[0071] In this application, the compressive modulus of the thermal insulation pad has a meaning known in the art and can be determined using instruments and methods known in the art. For example, an electronic universal testing machine (e.g., CMT4204 model). Testing can be referenced to GB / T7757-2009. An exemplary testing method is as follows: Cut a thermal insulation pad sample with a length * width = 80mm * 80mm; using a CMT4204 electronic universal testing machine, compress the thermal insulation pad along its thickness direction at a compression rate of 2mm / min at 25°C until the strain reaches 50%, obtaining a stress-strain curve; divide the stress in the linear interval by the strain to calculate the compressive modulus of the thermal insulation pad. To make the test results more accurate, the average value of the test results of multiple samples (e.g., 10) can be taken as the compressive modulus of the thermal insulation pad.
[0072] In this application, the compressive strength of the thermal insulation pad has a meaning known in the art and can be determined using instruments and methods known in the art. For example, an electronic universal testing machine (e.g., CMT4204 model). The test can be performed with reference to GB / T7757-2009. As an example, the thermal insulation pad can be compressed according to the compressive modulus test method to obtain the maximum compressive stress that the thermal insulation pad withstands when it ruptures or yields, which is the compressive strength of the thermal insulation pad.
[0073] In this application, the thermal conductivity of the insulation pad has a meaning known in the art and can be measured using instruments and methods known in the art. For example, a dual-plate thermal conductivity meter (e.g., WNK-200D type). The test can be referenced to GB / T10294-2008. An exemplary test method is as follows: cut an insulation pad sample with a diameter of 100 mm; use a WNK-200D type dual-plate thermal conductivity meter to test the thermal conductivity of the insulation pad at a test temperature of 100°C.
[0074] In this application, the thickness of the thermal insulation pad has a meaning known in the art and can be measured using instruments and methods known in the art, such as thickness gauges.
[0075] In this application, the particle size of the aerogel has a meaning known in the art and can be determined using instruments and methods known in the art. An exemplary test method is as follows: particles are sieved using a sieve, and then the particle size is measured using vernier calipers. To make the test results more accurate, the average value of the test results for multiple particles (e.g., 20) can be taken as the particle size of the aerogel. For the particle size of the aerogel in the insulation pad, a scanning electron microscope (SEM) can be used to capture SEM images. The test can be referenced in JY / T010-1996. An exemplary test method is as follows: SEM images of the test sample are captured using a scanning electron microscope. The particle size of the aerogel is calculated based on the SEM images.
[0076] In this application, the pore size of the aerogel has a meaning known in the art and can be determined using instruments and methods known in the art. For example, a porosity analyzer (e.g., ASAP 2020).
[0077] This application also provides a method for preparing a heat insulation pad, the method comprising the following steps: dispersing aerogel in liquid silicone rubber and forming a film; and vulcanizing the film to obtain a heat insulation pad.
[0078] Aerogel can be dispersed in liquid silicone rubber using a physical mixing method, allowing the aerogel and liquid silicone rubber to adhere fully and form a film. As an example, aerogel and liquid silicone rubber can be mixed using a mechanical mixing method, such as stirring. The mixture is then added to a mold and pressed into shape.
[0079] As another example, aerogel can be laid in a single or multiple layers in a mold, and then liquid silicone rubber can be injected into the gaps between the aerogel particles. The injection process can employ a multi-point injection method. This facilitates the uniform injection of liquid silicone rubber into all gaps between the aerogel particles, thereby effectively bonding the particles, significantly improving the overall structural strength, and giving the thermal insulation pad a good compressive modulus. After the silicone rubber is injected, it is pressed into shape. Pressing can be performed using a die-casting process. Through pressing, especially hot pressing, the overall structure becomes smoother, and the silicone rubber further penetrates the gaps between the particles to achieve bonding and strength support effects. As an example, liquid silicone rubber can be injected using an injection molding method.
[0080] In some embodiments, the mass ratio of liquid silicone rubber to aerogel is 1:(0.2-2), optionally 1:(1-2), or 1:(1.5-2).
[0081] In some embodiments, the volume ratio of liquid silicone rubber to aerogel is 50:50 to 8:92, and optionally 30:70 to 10:90, 40:60 to 10:90, 40:60 to 20:80, or 30:70 to 20:80.
[0082] When the ratio of liquid silicone rubber to aerogel is within an appropriate range, the resulting thermal insulation pad can have high thermal insulation performance, as well as good compressive modulus and compressive strength.
[0083] In some embodiments, the viscosity of the liquid silicone rubber is 0.1 Pa·s to 50 Pa·s, optionally 0.3 Pa·s to 25 Pa·s, 0.5 Pa·s to 15 Pa·s, 0.5 Pa·s to 10 Pa·s, 1 Pa·s to 20 Pa·s, or 1 Pa·s to 10 Pa·s, etc. A viscosity within an appropriate range facilitates uniform mixing of the aerogel and the liquid silicone rubber, improves the adhesion of the aerogel, and simultaneously enables the thermal insulation pad to have good compressive strength and compressive modulus.
[0084] In any embodiment, the compression molding temperature can be 0℃~150℃, 20℃~100℃, 50℃~100℃, 60℃~80℃, or 70℃~75℃. The compression molding pressure can be 0.05MPa~2MPa, 0.08MPa~1MPa, 0.1MPa~0.5MPa, or 0.1MPa~0.3MPa.
[0085] The temperature and time for vulcanizing the film can be determined based on the type of liquid silicone rubber and its vulcanization mechanism. In some embodiments, the vulcanization temperature can be 20℃~150℃, 100℃~150℃, 25℃~120℃, 50℃~100℃, or 80℃~100℃, etc. The vulcanization time can be 20min~300min, 30min~200min, 50min~150min, 80min~240min, 80min~150min, 80min~120min, or 100min~200min, etc.
[0086] In the preparation method, the aerogel and silicone rubber can be of the types described above, and will not be repeated here. Furthermore, both aerogel and liquid silicone rubber are commercially available.
[0087] In some embodiments, aerogels can be prepared using the following methods.
[0088] A silicon source, water, alcohol, and acid are mixed to obtain a mixed solution. In some embodiments, the mass ratio of silicon source, water, alcohol, and acid in the mixed solution can be 1:3–5:4–7:1.5 × 10⁻⁶. -3 ~2×10 -3 For example, 1:4:6:2×10 -3 As an example, the silicon source can be selected from methyl orthosilicate, ethyl orthosilicate, or butyl orthosilicate. The alcohol can be selected from ethanol, propanol, or butanol. The acid can be selected from acetic acid, hydrochloric acid, or sulfuric acid.
[0089] The mixed solution is subjected to a hydrolysis reaction to form a silica sol. In some embodiments, the hydrolysis reaction temperature can be 20°C to 30°C, or 25°C to 30°C. The hydrolysis reaction time can be 5h to 15h, or 8h to 12h.
[0090] The silica sol is mixed with ammonia to adjust the pH of the mixture to 7–8.5, or 7.5–8. In some embodiments, the volume of ammonia can be 2–3 times, for example, 2.5 times, the volume of the silica sol. The concentration of ammonia can be 0.3 mol / L to 0.5 mol / L.
[0091] The mixed system is injected into the oil phase, where the sol rapidly gels to form spherical or near-spherical silica gels suspended on the surface of the oil phase. In some embodiments, the oil phase may be selected from one or more of vegetable oils, mineral oils, and synthetic oils. As an example, the oil phase may be selected from one or more of soybean oil, peanut oil, paraffin oil, and glycerin. The aerogel prepared by this method has most of its hydrophilic functional groups facing inward, reducing the possibility of silicone rubber components penetrating and damaging the aerogel pores, thereby protecting the integrity of the pore structure and giving the aerogel a low thermal conductivity. At the same time, the resulting aerogel can maintain its own morphology, reducing stress concentration caused by structural rupture and ensuring the overall structural strength of the thermal insulation pad.
[0092] The gel is aged with ethanol. In some embodiments, the aging time can be 2 to 4 days, for example, 3 days.
[0093] The aged gel is subjected to supercritical drying to obtain silica aerogel. Supercritical drying can reduce the damage to the pores caused by liquid evaporation, protect the integrity of the aerogel's pore structure, and reduce thermal conductivity. In some embodiments, supercritical drying with carbon dioxide can be used. The supercritical drying pressure can be 10 MPa to 20 MPa, or 12 MPa to 16 MPa, etc. The supercritical drying temperature can be 50°C to 80°C, or 60°C to 70°C. The supercritical drying time is 100 min to 500 min, 150 min to 600 min, or 300 min to 500 min. Suitable supercritical drying conditions can further protect the integrity of the aerogel's pore structure.
[0094] In the aerogel preparation examples, by controlling the concentration and ratio of reactants, hydrolysis reaction temperature, hydrolysis reaction time, aging time, and supercritical drying time, the resulting hydrogel can achieve a more optimized pore structure. For example, the pore size of the aerogel can be 10 nm to 100 nm, especially 15 nm to 50 nm, or even 30 nm to 50 nm.
[0095] In some embodiments, the step of polymer modification of the aerogel may also be included. As an example, the aerogel is mixed with a silane coupling agent solution; polymer monomers are added to the mixture, and the polymerization reaction of the monomers is initiated in the presence of an initiator; the mixture is then filtered, washed, and dried to obtain a polymer-coated aerogel.
[0096] In the mixing step of the aerogel and the silane coupling agent solution, the silane coupling agent solution can be a mixture of silane coupling agent, water, and alcohol. The silane coupling agent can be selected from methacryloyloxypropyltrimethoxysilane (MPS) or 3-(methacryloyloxy)propyltrimethoxysilane (KH-570). The alcohol can be selected from ethanol, propanol, or butanol. The mass ratio of silane coupling agent, water, and alcohol in the silane coupling agent solution is 1:3 to 5:7 to 9, for example, 1:4:8. The ratio of aerogel to silane coupling agent solution is 10 g / L to 40 g / L.
[0097] The aerogel and silane coupling agent solution can be mixed by stirring, such as mechanical stirring, magnetic stirring, or ultrasonic stirring. The stirring time can be 10 h to 24 h.
[0098] Add the monomer of the polymer to the mixture. The amount of monomer added can be 1 to 5 times or 3 to 4.5 times the mass of the aerogel.
[0099] The monomer undergoes a polymerization reaction, and there are no particular limitations on the type of initiator; any conventional choice in the art can be used. The polymerization conditions and the amount of initiator are not particularly limited and can be selected based on the specific types of monomer and initiator. According to a specific embodiment, the monomer is methyl methacrylate (MMA), and the initiator is potassium persulfate (KPS). The amount of initiator relative to 100 parts by weight of monomer can be 0.1 to 0.5 parts by weight. The polymerization can be carried out under a protective atmosphere. The protective atmosphere can be a nitrogen atmosphere or an inert gas atmosphere. The polymerization temperature is 60°C to 80°C. The polymerization is carried out at atmospheric pressure. The polymerization time is 4 to 8 hours.
[0100] Washing can be performed using methods known in the art, such as rinsing with deionized water. Drying can be carried out at temperatures ranging from 60°C to 100°C, for example, 70°C to 80°C.
[0101] In this application, an exemplary test method for determining the proportion of aerogels in different particle size ranges within an aerogel mixture is as follows: The weights m1, m2, ... m of the aerogels in each particle size range are measured using an electronic balance. n n is an integer greater than or equal to 3; according to (m1 / ρ1):(m2 / ρ2):……:(m n / ρ n Calculate the aerogel percentage in different particle size ranges. ρ1, ρ2, ..., ρ n The density of the aerogel within each particle size range can be calculated based on the weight / volume of the aerogel particles. The volume of the aerogel particles can be calculated using the formula for the volume of a sphere. To improve accuracy, multiple particles (e.g., 32) within each particle size range can be analyzed to calculate their density separately, and the average value can be taken as the density of the aerogel within that range.
[0102] In this application, the mass ratio of liquid silicone rubber to aerogel has a meaning known in the art and can be determined using instruments and methods known in the art. For example, the mass of silicone rubber and aerogel can be measured separately using an electronic balance, and then the mass ratio can be calculated.
[0103] In this application, the volume ratio of liquid silicone rubber to aerogel has a meaning known in the art and can be determined using instruments and methods known in the art. For example, a measuring cup can be used to test the volume of liquid silicone rubber; the volume of aerogel can be tested according to the method described above; and then the volume ratio can be calculated.
[0104] In this application, the viscosity of liquid silicone rubber has a meaning known in the art and can be measured using instruments and methods known in the art. For example, a viscometer. Another example is a JJAVD type viscosity-average molecular weight analyzer.
[0105] Example
[0106] The following embodiments describe the disclosure of this application in more detail. These embodiments are merely illustrative, as various modifications and variations will be apparent to those skilled in the art within the scope of the disclosure of this application. Unless otherwise stated, all parts, percentages, and ratios reported in the following embodiments are based on weight, and all reagents used in the embodiments are commercially available or synthesized by conventional methods and can be used directly without further processing, and the instruments used in the embodiments are commercially available.
[0107] I. Battery Pack Preparation
[0108] 1.1. Preparation of Aerogels
[0109] (1) According to the ratio of ethyl silicate:water:ethanol:HCl = 1:4:6:2×10 -3 A mixed solution was obtained by mass ratio of the two solutions, and the mixed solution was subjected to hydrolysis reaction at 25°C for 12 hours to form silica sol.
[0110] (2) Add ammonia water equivalent to 2.5 times the volume of silica sol to make the pH of the mixture 7.5-8.
[0111] (3) Quickly inject the mixed system into the oil phase (soybean oil). The sol in the oil phase will quickly gel and form spherical silica gel suspended on the surface of the oil phase.
[0112] (4) Immerse the silica gel in ethanol for 3 days to age.
[0113] (5) The aged silica gel was subjected to supercritical carbon dioxide drying for 500 min at a pressure of 14 MPa and a temperature of 60 °C to obtain silica aerogel spheres. The pore size of the aerogel was 15 nm to 50 nm.
[0114] 1.2. Modification of Aerogels
[0115] (1) Add 10g of silica aerogel to 400mL of silane coupling agent MPS solution (mass ratio MPS:water:ethanol = 1:4:8) and stir for 24h.
[0116] (2) Add 43g of methyl methacrylate (MMA) to the mixture in step (1), introduce nitrogen gas, and add 0.2g of potassium persulfate (KPS) as an initiator. The polymerization reaction is carried out at 75°C for 6 hours with stirring.
[0117] (3) After the reaction is terminated, the mixture is filtered, rinsed with deionized water, and then dried at 80°C to obtain polymethyl methacrylate (PMMA) coated aerogel.
[0118] 2. Preparation of heat insulation pads
[0119] (1) PMMA-coated modified silica aerogel with a particle size of 2±0.2mm, PMMA-coated modified silica aerogel with a particle size of 1±0.2mm, and PMMA-coated modified silica aerogel with a particle size of 0.5±0.1mm are mixed in a volume ratio of 32:8:2; the mixed aerogel is then mixed uniformly with silicone rubber (Pt-catalyzed two-component addition type) with a viscosity of 1Pa·s by physical stirring.
[0120] (2) The mixture obtained in step (1) is evenly spread in the mold and pressed into a plate with uniform thickness by die casting at 75°C and 0.1MPa pressure.
[0121] (3) The molded board is cured at 80℃ for 150 minutes to obtain the heat insulation pad. The thickness of the heat insulation pad is 4mm.
[0122] 3. Preparation of battery cells
[0123] Preparation of positive electrode sheet
[0124] LiNi, the positive electrode active material 0.5 Co 0.2 Mn 0.3O2, conductive agent Super-P, and binder polyvinylidene fluoride (PVDF) are dispersed in NMP solvent at a weight ratio of 95:2:3 and thoroughly mixed to obtain a positive electrode slurry. The positive electrode slurry is coated onto two opposite surfaces of a positive electrode current collector aluminum foil, and after drying and cold pressing, a positive electrode sheet is obtained. The single-sided coating density of the positive electrode film is 18.83 mg / cm³. 2 (Solvent-free), compacted density is 3.25 g / cm³. 3 .
[0125] Preparation of negative electrode sheet
[0126] Natural graphite (anode active material), Super-P (conductive agent), styrene-butadiene rubber (SBR) (binder), and sodium carboxymethyl cellulose (CMC-Na) (thickener) were dispersed in deionized water at a weight ratio of 93:3:2:2. After thorough mixing, a negative electrode slurry was obtained. This slurry was then coated onto the two opposite surfaces of a copper foil current collector. Following drying and cold pressing, the negative electrode sheet was obtained. The single-sided coating density of the negative electrode film was 11.62 mg / cm³. 2 (Solvent-free), compacted density is 1.45 g / cm³. 3 .
[0127] Preparation of electrolyte
[0128] Ethyl carbonate (EC), propylene carbonate (PC), and dimethyl carbonate (DMC) were mixed evenly in a weight ratio of 1:1:1 to obtain an organic solvent; lithium salt LiPF6 was then dissolved in the organic solvent and mixed evenly to obtain an electrolyte, wherein the concentration of LiPF6 was 1 mol / L.
[0129] Preparation of battery cells
[0130] The positive electrode, separator, and negative electrode are wound together to obtain the battery cell; the battery cell is then placed in an outer packaging, injected with electrolyte, and sealed to obtain a single battery cell.
[0131] 4. Battery Pack Fabrication
[0132] Multiple battery cells are arranged side-by-side in a row, with the large surfaces of adjacent battery cells facing each other. A heat-insulating pad is placed between every two adjacent battery cells. The heat-insulating pad is in surface contact with the adjacent battery cells. The battery cells are then secured using a fixing assembly, which includes end plates located at both ends of the battery pack.
[0133] Examples 1-7 and Comparative Example 1: Battery packs were prepared according to the above preparation method, wherein the difference between each example is that the ratio of aerogel and silicone rubber in the heat insulation pad is adjusted, as detailed in Table 1.
[0134] Examples 8-13: Similar to Examples 1-6, except that unmodified aerogels were used.
[0135] II. Testing Section
[0136] 1. Insulation pad test
[0137] (1) The parameters of the heat insulation pad were tested using the method described above.
[0138] (2) Compression stress retention rate test
[0139] The compression retention rate test was conducted using a non-standard test based on GB / T1685-2008. A sample of the thermal insulation pad, measuring 80mm x 80mm, was cut. The sample was placed in a clamp, and the clamp pressure was adjusted to maintain the sample at 20% compression. The pressure value was recorded. This compression was maintained at room temperature for 30 days, and the pressure value at the same compression level after 30 days was recorded. The final output was the compression stress retention rate test result after 30 days.
[0140] 2. Battery pack performance testing
[0141] (1) Temperature difference test
[0142] A heat insulation pad sample with dimensions of 140mm x 70mm was cut. The sample was sandwiched between two alloy steel plates with dimensions of 140mm x 70mm x 26mm, forming a sandwich structure. The heat insulation pad sample was in surface contact with the alloy steel plates, and their edges were aligned. A pressure of 0.9MPa was applied to the composite, and one side of the alloy steel plate was heated to 600℃. After holding this temperature for 5 minutes, the pressure was released, and the sample was kept in contact with the 600℃ alloy steel plate for another 20 minutes. The hot side temperature T1 and the cold side temperature T2 of the heat insulation pad were measured, and the temperature difference T1-T2 was calculated. A pressure sensor was used to monitor the pressure, and a temperature sensor was used to monitor the temperature.
[0143] (2) Battery pack thermal runaway safety performance test
[0144] Charge the battery pack to 100% SOC (State of Charge). Induce thermal runaway in one cell of the battery pack (e.g., by puncturing or heating the cell; a cell temperature exceeding 60°C and rising rapidly is considered thermal runaway). Record the time t (min) for the adjacent cell to experience thermal runaway. That is, without additional cooling measures, calculate the time t for the second cell to experience thermal runaway from the time the first cell experiences thermal runaway. The longer this time t, the better the thermal runaway safety performance of the battery pack.
[0145] (3) Battery pack cycle performance test
[0146] The maximum end stress F (maximum force on the battery pack end divided by the end plate area) after cyclic expansion was simulated using the battery pack stress simulation software Abaqus. To maintain a good battery pack cycle life, the maximum end stress F after cyclic expansion should be <215MPa. The simulation parameters are as follows: A preload of 5000N is applied to the battery pack. At 25°C, the battery pack is charged from 5% SOC to 50% SOC at a constant current rate of 3C, then at a constant current rate of 2C to 70% SOC, then at a constant current rate of 1C to 80% SOC, and finally discharged at a constant current rate of 1C to 5% SOC. This constitutes one charge-discharge cycle. The battery pack is subjected to 2500 charge-discharge cycles.
[0147] Table 1: Relevant Parameters of Thermal Insulation Pads
[0148]
[0149] The temperature difference is a comprehensive reflection of the thermal conductivity, thickness, and compressive mechanical properties of the heat insulation pad. As shown in Table 1, within an appropriate temperature difference range, the heat insulation pad not only has a low thermal conductivity but also suitable compressive strength, compressive modulus, and compressive stress retention rate. When applied to battery packs, this heat insulation pad can effectively prevent heat transfer from thermally runaway battery cells to adjacent battery cells, thus improving the safety performance of the battery pack.
[0150] Furthermore, surface modification of the aerogel with polymers can further improve the compressive strength, compressive modulus, and compressive stress retention rate of the thermal insulation pad. Under the cyclic expansion forces of the battery pack, the thermal insulation pad is less prone to cracking or yielding, thus effectively providing thermal insulation over a long period. Simultaneously, the thermal insulation pad can also buffer the cyclic expansion stress of the battery over a long timescale, thereby further improving the safety performance of the battery pack and contributing to a longer cycle life.
[0151] Table 2: Performance Testing
[0152]
[0153] As shown in Table 2, the heat insulation pad of this application can significantly delay the thermal runaway of individual cells within the battery pack from spreading to adjacent cells, thereby effectively improving battery safety performance. Simultaneously, the heat insulation pad of this application can also buffer the cyclic expansion of the battery pack, which is beneficial for maintaining a good cycle life.
[0154] The above description is merely a specific embodiment of this application, but the scope of protection of this application is not limited thereto. Any person skilled in the art can easily conceive of various equivalent modifications or substitutions within the technical scope disclosed in this application, and these modifications or substitutions should all be covered within the scope of protection of this application. Therefore, the scope of protection of this application should be determined by the scope of the claims.
Claims
1. A battery pack, characterized in that, The device includes multiple battery cells arranged in an array, with a heat insulation pad disposed between at least two adjacent battery cells. The heat insulation pad comprises silicone rubber and an aerogel dispersed in the silicone rubber. The heat insulation pad satisfies the following condition: after one side surface of the heat insulation pad is in contact with a hot surface at 600°C for 5 minutes under a pressure of 0.9MPa and then depressurized, and then continues to be in contact with a hot surface at 600°C for 20 minutes, the temperature difference between the one side surface of the heat insulation pad and the opposite side surface is 200°C ~ 465°C. The thermal conductivity of the heat insulation pad at 100℃ is 0.022 W / (m·K) ~ 0.09 W / (m·K); The compressive elastic modulus of the heat insulation pad is 5MPa ~ 40MPa; The aerogel includes aerogels with a particle size of 1.8 mm to 2.2 mm, aerogels with a particle size of 0.8 mm to 1.2 mm, and aerogels with a particle size of 0.4 mm to 0.6 mm. The volume ratio of the aerogel with a particle size of 1.8 mm to 2.2 mm, the aerogel with a particle size of 0.8 mm to 1.2 mm, and the aerogel with a particle size of 0.4 mm to 0.6 mm is (25 to 40): (5 to 10): (1 to 3). The silicone rubber is dispersed between aerogel particles, and the aerogel is selected from silica aerogel.
2. The battery pack according to claim 1, characterized in that, The compressive strength of the heat insulation pad is 1 MPa ~ 30 MPa.
3. The battery pack according to claim 1, characterized in that, The surface of the aerogel is modified with a polymer selected from one or more of polyacrylic acids, polyacrylates, polyethers, polyols, polyolefins, their derivatives, and their copolymers.
4. The battery pack according to claim 1, characterized in that, The silicone rubber used is either condensation-type or addition-type silicone rubber.
5. The battery pack according to claim 1, characterized in that, The silicone rubber is a two-component addition-type silicone rubber, which includes one or more of silicone rubber, methyl vinyl silicone rubber, methyl phenyl vinyl silicone rubber, nitrile silicone rubber, and silicone nitrogen rubber.
6. The battery pack according to claim 1, characterized in that, The silicone rubber includes foamed silicone rubber.
7. An electrical device comprising a battery pack according to any one of claims 1 to 6.
8. A method for preparing a heat insulation pad, characterized in that, Includes the following steps: Aerogel is dispersed in liquid silicone rubber and formed into a film; The membrane is vulcanized and molded to obtain a heat insulation pad; The heat insulation pad satisfies the following condition: after one side surface of the heat insulation pad is in contact with a hot surface at 600°C for 5 minutes under a pressure of 0.9MPa, the pressure is released, and then it continues to be in contact with a hot surface at 600°C for 20 minutes, the temperature difference between the one side surface of the heat insulation pad and the opposite side surface is 200°C ~ 465°C. The thermal conductivity of the heat insulation pad at 100℃ is 0.022 W / (m·K) ~ 0.09 W / (m·K); The compressive elastic modulus of the heat insulation pad is 5MPa ~ 40MPa; The aerogel includes aerogels with a particle size of 1.8 mm to 2.2 mm, aerogels with a particle size of 0.8 mm to 1.2 mm, and aerogels with a particle size of 0.4 mm to 0.6 mm. The volume ratio of the aerogel with a particle size of 1.8 mm to 2.2 mm, the aerogel with a particle size of 0.8 mm to 1.2 mm, and the aerogel with a particle size of 0.4 mm to 0.6 mm is (25 to 40): (5 to 10): (1 to 3). The silicone rubber is dispersed between aerogel particles, and the aerogel is selected from silica aerogel.
Citation Information
Patent Citations
High heat-conducting insulating silicon rubber and preparation method thereof
CN102618041A
Battery module
CN110265591A
Aerogel-containing heat-insulating silicone rubber foam material and preparation method thereof
CN110551397A
Diaphragm with self-crosslinking effect and preparation method thereof
CN111180641A
Thermal insulation material used between power battery cells, and preparation method and application thereof