A method to replace laminated film
By using prepregs containing fiberglass cloth to be laminated with production boards and copper foil in the manufacture of high-density packaging substrates, a uniform interlayer dielectric layer is formed, which solves the cost and bonding problems of conventional materials in high-precision circuit production and achieves Low-cost, high-precision circuit board production.
Patent Information
- Application Number
- CN202210770649.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-30
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-06-30
AI Technical Summary
When manufacturing high-density packaging substrates with circuit widths less than 50um using existing technology, conventional prepreg materials cannot meet the requirements of high precision and low cost. In particular, the presence of fiberglass cloth results in poor copper bonding and cannot effectively replace high-cost prepregs. ABF insulation material.
The prepreg containing fiberglass cloth is laminated with the production board and copper foil. The resin is melted and evenly coated through rapid lamination. After peeling off the fiberglass cloth, the fluidity and curability of the resin are used to form a uniform interlayer dielectric layer to avoid glass The fiber cloth combines the fluidity and shape retention of the thermosetting resin to achieve uniformity of the interlayer medium, and improves the bonding force between the copper layer and the resin layer through etching.
It realizes the production of fine lines with line width and line spacing less than 50um, reduces process costs, avoids the use of high-cost ABF insulation materials, and meets the production needs of high-precision circuit boards. The thickness of the interlayer medium is uniform and the bonding force is strong. It is suitable for high-precision circuit boards. density packaging.
Smart Images

Figure CN115087211B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of printed circuit board manufacturing, and in particular to a method for replacing a laminated adhesive film. Background Art
[0002] With the development of large-scale integrated circuits, the lines are getting thinner and thinner. 22nm technology has entered mass production. The thinning of the lines has brought unprecedented challenges to equipment and processes. In order to improve the chip density and signal processing capabilities per unit area, 3D packaging came into being. People put forward the concept of three-dimensional packaging, which integrates and packages the chips in three dimensions, and stacks the chips to form a three-dimensional package to improve the packaging density per unit area.
[0003] The development of three-dimensional high-density packaging has placed higher and higher requirements on organic substrates. The line width and line spacing of organic substrates have been reduced from 100um at the PCB level to 30-50um at the current mass production line width. As the line width decreases, the structural requirements for the copper surface of the circuit are also increasing. The copper roughness RZ of a common PCB is 5-7um, and the roughness of a carrier board is usually less than 5um. For a line with a line width and line spacing of 10-20um, the surface roughness Rz of the copper line is generally 2 microns. If it is too large, the line will be deformed or the copper residue between the lines will cause a short circuit, and high-precision and reliable interconnection cannot be achieved.
[0004] There are only three methods for the circuit manufacturing process of organic substrates and printed circuit boards: additive method, subtractive method, and semi-additive method. These methods are widely used in the manufacture of organic substrates. In the stage of high development of IC packaging, in high-density packaging, due to the gradual increase in circuit density, the characteristic size of the packaging substrate has dropped from the original minimum 100um of the printed circuit board to 50um. The current high-end packaging substrate has reached 25um-30um, and some high-end packaging substrate suppliers are already trying to mass produce circuits with a line width of 15um. For organic substrates with a line width less than 50um, the subtractive method is completely unsuitable. The additive method is rarely used due to the slow speed of chemical copper plating; semi-additive technology, namely SAP technology, has become the dominant technology for high-density packaging substrate processing technology. Since the line accuracy of the semi-additive method is higher than that of other methods, it is widely used in the production of high-precision lines; however, when the line width is less than 50um, due to the bonding force of the line, the electrical insulation requirements between the lines, and the line accuracy requirements, conventional prepreg materials are no longer suitable for the processing of fine lines.
[0005] For lines with a line width and line spacing of less than 50um, the subtractive method cannot guarantee the dimensional accuracy of the line, so only the semi-additive method can be used. The semi-additive method directly performs chemical copper plating on the resin surface, and the substrate surface needs to be roughened. The roughened surface has a certain degree of roughness, which provides the necessary conditions for the copper wire and the insulating resin to provide bonding strength. However, after the conventional semi-cured sheet is pressed and cured on the surface of the inner layer of the line, since the semi-cured sheet structure contains glass fiber, the resin flows during the curing process, exposing the glass fiber, and only a very thin layer of resin is left on the surface of the glass fiber. When the surface is roughened, the very thin resin on the surface of the glass fiber is etched away, exposing the glass fiber, resulting in problems such as partial inability to copperize or poor copper bonding strength.
[0006] In order to achieve the production of high-precision circuits, Japan's Ajinomoto Company provides a sheet-like semi-cured material called ABF (Ajinomoto Build-up Film), which does not contain glass fiber. Using this material as the insulation layer of the outer circuit can achieve a good SAP process and is currently widely used in the manufacturing of high-end substrates. Japan's Ajinomoto Company started the ABF technology project in 1996 and completed the prototype and sample development in just 4 months, but it took about 3 years to seek commercialization. It was not until 1999 that the ABF substrate was gradually accepted by the chip manufacturing industry. During the 3 years when it could not find a market, Japan's Ajinomoto Company remained optimistic about the market prospects of ABF, established an intellectual property protection system, and continuously improved technical barriers, enabling Ajinomoto to establish a dominant position in the ABF industry and maintain it to this day.
[0007] So far, almost all IC substrates (Integrated Circuit, IC for short) use ABF as the build-up material; ABF material does not contain fiberglass cloth. ABF is a three-layer structure consisting of a base film PET (polyester film), a resin composition with thermosetting resins such as epoxy resin as the main component, and a protective film OPP (uniaxially oriented polypropylene film).
[0008] The ABF material is laminated using a dedicated laminator (fast press machine). After fast pressing pre-curing, laser blind holes are formed, followed by de-drilling, copper plating, pattern transfer, post-curing and other processes to form circuits. The above process is repeated multiple times to laminate and manufacture a carrier board.
[0009] It will take a long time for the manufacturing technology of laminated film materials to mature and for the market to accept them. Although domestic companies are striving to catch up, there are still market barriers, technical barriers and the accumulation of experience and technology, making it difficult to replace ABF materials. Since ABF resin is very expensive and is a patented product of Ajinomoto, its selling price is very high, which is 4-5 times the price of the BT-based prepreg provided by Mitsubishi Gas. It can be seen that the cost of using the SAP process to produce fine lines with a width of less than 50 microns is very high. Summary of the invention
[0010] In view of the above-mentioned existing technical defects, the present invention provides a method for replacing the laminated film, which avoids the use of high-cost ABF insulating materials by adopting alternative insulating materials, reduces the process cost of the circuit board, and thus reduces the cost of the circuit board.
[0011] In a first aspect, in order to solve the above technical problems, the present invention provides a method for replacing a laminated adhesive film, comprising the following steps:
[0012] S1, stacking a production board, at least one prepreg and a copper foil in sequence to form a stacked board structure;
[0013] S2, laminating the laminate structure by means of rapid lamination, so that the prepreg is in a pre-cured state with fluidity;
[0014] S3. In the pre-cured state of the prepreg, the copper foil is first peeled off to attach a layer of resin to the inner side of the copper foil; then the glass fiber cloth in the prepreg is peeled off to expose the resin attached to the surface of the production board;
[0015] S4, then baking the production board or copper foil to solidify the resin on the production board or copper foil;
[0016] S5. The copper foil is then stacked on the production board and pressed, and the copper foil is in contact with the side of the production board to which the resin is attached, so that the resin on the copper foil is combined with the resin on the production board and solidified.
[0017] Furthermore, in step S1, a prepreg with a resin content of 55% is used between the production board and the copper foil, and a glass fiber cloth with a model number of 2116 is provided in the middle of the prepreg.
[0018] Furthermore, in step S2, a vacuum laminator is used for rapid lamination, and the vacuum time during rapid lamination is 60 seconds, the pressurization time is 120 seconds, and the pressure is 25Kg / cm 2 , the temperature is 130℃.
[0019] Furthermore, in step S1, a prepreg with a resin content of 65% is used between the production board and the copper foil, and two glass fiber cloths with a model number of 1080 are arranged in the middle of the prepreg.
[0020] Furthermore, in step S2, a vacuum laminator is used for rapid lamination, and the vacuum time during rapid lamination is 60 seconds, the pressurization time is 120 seconds, and the pressure is 20Kg / cm 2 , the temperature is 130℃.
[0021] Furthermore, in step S4, the production plate is placed in an oven for baking.
[0022] Furthermore, in step S4, the baking temperature is 180° C. and the baking time is 75 minutes.
[0023] Furthermore, after step S5, the following steps are also included:
[0024] S6. Remove the copper foil on the board by etching to expose the rough resin layer on the inner surface.
[0025] Furthermore, in step S1, the production board is a core board, and an inner layer circuit has been manufactured on the core board.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] In the present invention, a prepreg containing glass fiber cloth filler is first stacked with a production board and a copper foil in sequence and then pressed with a fast press, the resin in the prepreg is melted and then evenly coated on the production board and the copper foil, and then the copper foil is peeled off in a melted state of the prepreg to expose the glass fiber cloth in the inner prepreg, and then the glass fiber cloth is peeled off from the copper foil or the production board by utilizing the low bonding force between the glass fiber cloth in the prepreg and the resin, and then the resin layer on the production board or the copper foil is cured by baking, so that the shape of the resin layer on one of them remains stable after being completely cured, and its thickness remains unchanged during pressing, while the resin layer on the other one remains in a state of having fluidity. The pre-cured state of the thermosetting resin flows to fill the resin layer in the flat cured state during pressing, thereby utilizing the fluidity of the thermosetting resin in the pre-cured state and the shape retention after complete curing. The two work together to achieve uniformity in the thickness of the interlayer dielectric. Finally, the resin-attached copper foil is pressed onto the resin-attached core board to form a uniform interlayer dielectric layer. There is no glass fiber cloth in the interlayer dielectric layer, which achieves the characteristics of the laminated film of ABF insulating material, and can meet the production of fine lines with a line width and line spacing of less than 50um, thereby replacing ABF insulating material, avoiding the use of high-cost ABF insulating material, reducing the process cost of the circuit board, and thus reducing the cost of the circuit board.
[0028] In addition, after lamination, the copper foil is removed by etching, and the copper teeth of the copper foil are used to form a rough surface on the surface of the resin layer to improve the bonding force between the resin layer and the copper layer deposited thereon.
[0029] According to the different resin absorption capabilities of glass fiber cloths of different types, the present invention matches the parameters of rapid pressing with the semi-cured sheets of corresponding types and resin content, so that after pressing and peeling the copper foil and glass fiber cloth, a layer of resin with the same thickness and meeting the requirements will be evenly coated on the production board and the copper foil. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 A local scanning electron microscope image of a uniform interlayer dielectric layer formed on a multilayer board in Example 1;
[0031] Figure 2 This is a local scanning electron microscope image of forming a uniform interlayer dielectric layer on a multilayer board in Example 2. DETAILED DESCRIPTION
[0032] In order to more fully understand the technical content of the present invention, the technical solution of the present invention will be further introduced and illustrated in conjunction with specific embodiments below.
[0033] Example 1
[0034] A method for replacing a laminated adhesive film in a circuit board shown in this embodiment includes the following steps in sequence:
[0035] a. Stack the core board, prepreg and copper foil in sequence to form a laminate structure.
[0036] Among them, the core board is a double-sided copper-clad board, and its inner layer circuit has been made through a negative film process before stacking the boards.
[0037] Among them, a semi-cured sheet with a resin content of 55% is used between the core board and the copper foil, and a glass fiber cloth with model number 2116 is set in the middle of the semi-cured sheet, that is, the thickness of the resin layer on both sides of the glass fiber cloth is the same, and the thickness of the resin layer on both sides of the glass fiber cloth is generally 10-30μm; in addition, in the later peeling process, the peeling surface will appear on the bonding surface of the glass fiber cloth and the resin, so that the thickness of the resin left on the copper foil and the core board can be controlled respectively.
[0038] b. The laminate structure is pressed together by rapid pressing to melt the prepreg, that is, to put the prepreg in a fluid pre-cured state.
[0039] Preferably, a vacuum laminator is used for rapid lamination, and the vacuum time during rapid lamination is 60s, the pressurization time is 120s, and the pressure is 25Kg / cm 2, the temperature is 130℃; in addition, the resin content in the semi-cured sheet and the pressure during pressing will both determine the thickness of the resin left on the core board and the copper foil. Here, according to the actual resin content, the parameters during rapid pressing are matched with the semi-cured sheet of corresponding model and resin content, so that after pressing and peeling off the copper foil and glass fiber cloth, a layer of resin with the same thickness and meeting the requirements will be evenly coated on the production board and copper foil.
[0040] c. In the pre-cured state of the semi-cured sheet, the copper foil is first peeled off. By utilizing the low bonding force between the glass fiber cloth and the resin in the semi-cured sheet, the peeling surface during peeling will appear on the bonding surface between the glass fiber cloth and the resin, so that half of the resin on the upper layer of the glass fiber cloth is peeled off together with the copper foil, thereby attaching a layer of resin to the inner side of the copper foil; then the glass fiber cloth in the semi-cured sheet is peeled off to expose the resin attached to the surface of the core board, that is, the other half of the resin under the glass fiber cloth is attached to the surface of the core board; at this time, the copper foil and the resin layer on the core board are both in a pre-cured state with fluidity.
[0041] d. Place the core board or copper foil in an oven for baking so that the resin on the core board or copper foil is completely cured after baking; here, the shape of the resin layer on one of them remains stable after being completely cured, and its thickness remains unchanged during pressing, while the resin layer on the other is kept in a pre-cured state with fluidity, which flows to fill the flat cured resin layer during pressing, thereby utilizing the fluidity of half of the thermosetting resin in the pre-cured state and the shape retention of the other half after being completely cured, and the two cooperate with each other to achieve uniformity of interlayer dielectric thickness.
[0042] The baking temperature is 180°C and the baking time is 75 minutes.
[0043] e. Finally, the copper foil with the resin layer is stacked on the core board and pressed to form a multilayer board; and during pressing, the copper foil is in contact with the side of the core board with the resin attached, so that the resin on the copper foil is combined with the resin on the core board and solidified to form a uniform interlayer dielectric layer with a thickness of about 21μm (such as Figure 1 As shown in the figure, there is no glass fiber cloth in the interlayer dielectric layer, which achieves the characteristics of the laminated film of ABF insulating material, and can meet the production of fine lines with a line width and line spacing of less than 50um, thereby replacing ABF insulating material, avoiding the use of high-cost ABF insulating material, reducing the process cost of the circuit board, and thus reducing the cost of the circuit board.
[0044] In order to realize the production of the circuit board, the following steps are also included after the above step e:
[0045] f. Drilling: Based on the existing drilling technology, drilling processing is carried out on the multilayer board according to the design requirements.
[0046] g. Copper plating: Use chemical copper plating method to deposit a thin layer of copper on the board surface and hole wall. The backlight test is level 10, and the thickness of the copper plating in the hole is 0.5μm.
[0047] h. Full board electroplating: Full board electroplating is performed for 120 minutes at a current density of 18ASF to thicken the copper layer on the hole and the board surface.
[0048] i. Production of outer circuit (negative film process): Transfer of outer pattern, coating of photosensitive film with a vertical coating machine, the thickness of the photosensitive film is controlled at 8μm, and a fully automatic exposure machine is used to complete the exposure of the outer circuit with a 5-6 grid exposure ruler (21 grid exposure ruler), and the outer circuit pattern is formed after development; outer layer etching, etching the outer circuit on the production board after exposure and development, and the outer line width is measured to be 3mil; outer layer AOI, using an automatic optical inspection system, by comparing with the CAM data, detect whether the outer circuit has defects such as open circuit, gap, incomplete etching, short circuit, etc.
[0049] j. Solder mask and silk-screen characters: After silk-screening solder mask ink on the surface of the production board, it is sequentially processed through pre-curing, exposure, development and heat curing to solidify the solder mask ink into a solder mask layer; specifically, "UL mark" is added to the solder mask ink and the characters on the TOP surface, so that a layer is coated on the circuits and substrates that do not require soldering to prevent bridging between circuits during soldering, provide a permanent electrical environment and chemical corrosion resistance, and at the same time beautify the appearance.
[0050] k. Surface treatment (nickel-gold immersion): The copper surface of the pad at the solder mask opening is chemically treated to evenly deposit a nickel layer and a gold layer of a certain required thickness. The nickel layer thickness is 3-5μm; the gold layer thickness is 0.05-0.1μm.
[0051] 1. Electrical test: Test the electrical conductivity of the finished board. The test method used for this board is: flying probe test.
[0052] m. Molding: According to the existing technology and design requirements, the circuit board is manufactured with a shape tolerance of + / -0.05mm.
[0053] n. FQC: According to the customer's acceptance standards and our inspection standards, the circuit board appearance is inspected. If there are any defects, they will be repaired in time to ensure excellent quality control for customers.
[0054] o, FQA: re-test the circuit board's appearance, hole copper thickness, dielectric layer thickness, green oil thickness, inner layer copper thickness, etc. to see if they meet customer requirements.
[0055] p. Packaging: According to the packaging method and packaging quantity required by the customer, the circuit board is sealed and packed, and desiccant and humidity card are placed before shipment.
[0056] Example 2
[0057] The method for replacing a laminated adhesive film in a circuit board shown in this embodiment has the same steps as those in Embodiment 1, except for steps a and b, which are specifically as follows:
[0058] a. Stack the core board, prepreg and copper foil in sequence to form a laminate structure.
[0059] Among them, the core board is a double-sided copper-clad board, and its inner layer circuit has been made through a negative film process before stacking the boards.
[0060] Among them, a semi-cured sheet with a resin content of 65% is used between the core board and the copper foil, and two stacked glass fiber cloths with a model number of 1080 are arranged in the middle of the semi-cured sheet. The two glass fiber cloths are used to provide more resin to fill the gaps, increase the resin content, and facilitate the peeling of the glass fiber cloth (one 1080 glass fiber cloth is not easy to peel off). When the two sheets are stacked together and peeled off, it will not affect the thickness of the resin attached to the core board; in addition, in the later peeling process, the peeling surface will appear on the bonding surface of the glass fiber cloth and the resin, so that the thickness of the resin left on the copper foil and the core board can be controlled respectively.
[0061] b. The laminate structure is pressed together by rapid pressing to melt the prepreg, that is, to put the prepreg in a fluid pre-cured state.
[0062] Preferably, a vacuum laminator is used for rapid lamination, and the vacuum time during rapid lamination is 60s, the pressurization time is 120s, and the pressure is 20Kg / cm 2 , the temperature is 130℃; in addition, the resin content in the semi-cured sheet and the pressure during pressing will both determine the thickness of the resin left on the core board and the copper foil. Here, according to the actual resin content, the parameters during rapid pressing are matched with the semi-cured sheet of corresponding model and resin content, so that after pressing and peeling off the copper foil and glass fiber cloth, a layer of resin with the same thickness and meeting the requirements will be evenly coated on the production board and copper foil.
[0063] c. In the pre-cured state of the semi-cured sheet, the copper foil is first peeled off. By utilizing the low bonding force between the glass fiber cloth and the resin in the semi-cured sheet, the peeling surface during peeling will appear on the bonding surface between the glass fiber cloth and the resin, so that half of the resin on the upper layer of the glass fiber cloth is peeled off together with the copper foil, thereby attaching a layer of resin to the inner side of the copper foil; then the glass fiber cloth in the semi-cured sheet is peeled off to expose the resin attached to the surface of the core board, that is, the other half of the resin under the glass fiber cloth is attached to the surface of the core board; at this time, the copper foil and the resin layer on the core board are both in a pre-cured state with fluidity.
[0064] d. Place the core board or copper foil in an oven for baking so that the resin on the core board or copper foil is completely cured after baking; here, the shape of the resin layer on one of them remains stable after being completely cured, and its thickness remains unchanged during pressing, while the resin layer on the other is kept in a pre-cured state with fluidity, which flows to fill the flat cured resin layer during pressing, thereby utilizing the fluidity of half of the thermosetting resin in the pre-cured state and the shape retention of the other half after being completely cured, and the two cooperate with each other to achieve uniformity of interlayer dielectric thickness.
[0065] The baking temperature is 180°C and the baking time is 75 minutes.
[0066] e. Finally, the copper foil with the resin layer is stacked on the core board and pressed to form a multilayer board; and during pressing, the copper foil is in contact with the side of the core board with the resin attached, so that the resin on the copper foil is combined with the resin on the core board and solidified to form a uniform interlayer dielectric layer with a thickness of about 40μm (such as Figure 2 As described above, there is no glass fiber cloth in the interlayer dielectric layer, which achieves the characteristics of the laminated film of ABF insulating material, and can meet the production of fine lines with a line width and line spacing of less than 50um, thereby replacing ABF insulating material, avoiding the use of high-cost ABF insulating material, reducing the process cost of the circuit board, and thus reducing the cost of the circuit board.
[0067] f. Remove the copper foil on the board by etching to expose the rough inner surface of the resin layer, and use the copper teeth of the copper foil to form a rough surface on the surface of the resin layer to improve the bonding force between the resin layer and the copper layer deposited thereon.
[0068] In order to realize the production of the circuit board, the following steps are also included after the above step e:
[0069] g. Drilling: Based on the existing drilling technology, drilling processing is carried out on the multilayer board according to the design requirements.
[0070] h. Copper plating: Use chemical copper plating method to deposit a thin layer of copper on the board surface and hole wall. The backlight test is level 10, and the thickness of the copper plating in the hole is 0.5μm.
[0071] i. Full board electroplating: Full board electroplating is performed for 120 minutes at a current density of 18ASF to thicken the hole copper and board surface copper layers.
[0072] j. Production of outer circuit (negative film process): Transfer of outer pattern, coating of photosensitive film with a vertical coating machine, the thickness of the photosensitive film is controlled at 8μm, and a fully automatic exposure machine is used to complete the exposure of the outer circuit with a 5-6 grid exposure ruler (21 grid exposure ruler), and the outer circuit pattern is formed after development; outer layer etching, etching the outer circuit on the production board after exposure and development, and the outer line width is measured to be 3mil; outer layer AOI, using an automatic optical inspection system, by comparing with the CAM data, detect whether the outer circuit has defects such as open circuit, gap, incomplete etching, short circuit, etc.
[0073] k. Solder mask and silk-screen characters: After silk-screening solder mask ink on the surface of the production board, it is sequentially processed through pre-curing, exposure, development and heat curing to solidify the solder mask ink into a solder mask layer; specifically, "UL mark" is added to the solder mask ink and characters on the TOP surface, thereby coating a layer on the circuits and substrates that do not require soldering to prevent bridging between circuits during soldering, provide a permanent electrical environment and chemical corrosion resistance, and at the same time beautify the appearance.
[0074] 1. Surface treatment (nickel-gold immersion): The copper surface of the pad at the solder mask opening is chemically treated to uniformly deposit a nickel layer and a gold layer of a certain required thickness. The nickel layer thickness is 3-5μm; the gold layer thickness is 0.05-0.1μm.
[0075] m. Electrical test: Test the electrical conductivity of the finished board. The test method used for this board is: flying probe test.
[0076] n. Molding: According to the existing technology and design requirements, the circuit board is manufactured with a shape tolerance of + / -0.05mm.
[0077] o. FQC: Check the appearance of the circuit board according to the customer's acceptance standards and our inspection standards. If there are any defects, repair them in time to ensure that we provide customers with excellent quality control.
[0078] p. FQA: Re-test the circuit board's appearance, hole copper thickness, dielectric layer thickness, green oil thickness, inner layer copper thickness, etc. to see if they meet customer requirements.
[0079] q. Packaging: According to the packaging method and packaging quantity required by the customer, the circuit board is sealed and packed, and desiccant and humidity card are placed before shipment.
[0080] The interlayer dielectric layer formed of resin in the above two embodiments has the following characteristics:
[0081] Insulation: HAST (inter-layer, inter-line) test passed, dielectric thickness less than 30 microns and uniform;
[0082] Copper foil adhesion: The bonding strength with chemical copper or copper foil meets the requirements;
[0083] Low dielectric constant and dielectric loss: No glass fiber;
[0084] Heat resistance: reflow soldering (260°C), temperature cycle, thermal shock test;
[0085] Practicality: high mechanical strength, low warpage, and small thermal expansion rate;
[0086] Flame retardancy: UL-94V compliant, halogen-free;
[0087] Circuit formation: adhesive removal, flash etching, photoresist adhesion;
[0088] Hole formation: laser processability (CO2, UV-YAG), good slag removal at the bottom of the hole;
[0089] Low cost: The processing is simple and the materials are readily available.
[0090] The technical solutions provided by the embodiments of the present invention are introduced in detail above. Specific examples are used herein to illustrate the principles and implementation methods of the embodiments of the present invention. The description of the above embodiments is only applicable to help understand the principles of the embodiments of the present invention. At the same time, for those skilled in the art, according to the embodiments of the present invention, there will be changes in the specific implementation methods and application scopes. In summary, the content of this specification should not be understood as limiting the present invention.
Claims
1. A method for replacing a laminated film, characterized in that: The following steps are involved: S1, stacking the production board, prepreg and copper foil in sequence to form a stacked board structure; S2, laminating the laminate structure by means of rapid lamination, so that the prepreg is in a pre-cured state with fluidity; S3. In the pre-cured state of the prepreg, the copper foil is first peeled off to attach a layer of resin to the inner side of the copper foil; then the glass fiber cloth in the prepreg is peeled off to expose the resin attached to the surface of the production board; S4, then baking the production board or copper foil to solidify the resin on the production board or copper foil; S5. The copper foil is then stacked on the production board and pressed, and the copper foil is in contact with the side of the production board to which the resin is attached, so that the resin on the copper foil is combined with the resin on the production board and solidified.
2. The method for replacing a laminated adhesive film according to claim 1, characterized in that: In step S1, a prepreg with a resin content of 55% is used between the production board and the copper foil, and a glass fiber cloth with a model number of 2116 is provided in the middle of the prepreg.
3. The method for replacing a laminated adhesive film according to claim 2, characterized in that: In step S2, a vacuum laminator is used for rapid lamination, and the vacuum time during rapid lamination is 60 seconds, the pressurization time is 120 seconds, and the pressure is 25Kg / cm 2 , the temperature is 130℃.
4. The method for replacing a laminated adhesive film according to claim 1, characterized in that: In step S1, a prepreg with a resin content of 65% is used between the production board and the copper foil, and two glass fiber cloths with a model number of 1080 are arranged in the middle of the prepreg.
5. The method for replacing a laminated adhesive film according to claim 4, characterized in that: In step S2, a vacuum laminator is used for rapid lamination, and the vacuum time during rapid lamination is 60 seconds, the pressurization time is 120 seconds, and the pressure is 20Kg / cm 2 , the temperature is 130℃.
6. The method for replacing a laminated adhesive film according to claim 1, characterized in that: In step S4, the production plate is placed in an oven for baking.
7. The method for replacing a laminated adhesive film according to claim 1, characterized in that: In step S4, the baking temperature is 180° C. and the baking time is 75 minutes.
8. The method for replacing a laminated adhesive film according to any one of claims 1 to 7, characterized in that: After step S5, the following steps are also included: S6. Remove the copper foil on the board by etching to expose the rough resin layer on the inner surface.
9. The method for replacing a laminated adhesive film according to claim 1, characterized in that: In step S1, the production board is a core board, and the inner layer circuit has been made on the core board.