Multilayer film and method for manufacturing polarizing plate using the same

By co-extruding multilayer films and utilizing specific resin combinations and structural designs, the challenges of conveying and bonding ultra-thin polarizer protective films were solved, enabling stable and seamless polarizer manufacturing.

CN115113319BActive Publication Date: 2026-11-24NITTO DENKO CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202210265687.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-03-18
Filing Date
2022-03-17
Publication Date
2026-11-24
Estimated Expiration
2042-03-17

AI Technical Summary

Technical Problem

In the existing technology, problems such as breakage and wrinkles are prone to occur during the transportation and lamination of ultra-thin polarizing protective films, making it difficult to manufacture polarizing plates.

Method used

A multilayer film structure with specific Hansen solubility parameters and glass transition temperature difference is adopted. The first and second layers are formed by co-extrusion molding. The first layer contains a cyclic olefin resin, the second layer contains an acrylic resin, and the third layer can be made of the same resin to ensure good peelability and adhesion.

Benefits of technology

It achieves stable delivery and seamless bonding of ultra-thin polarizer protective films, avoiding breakage and wrinkles, and promoting the thinning of polarizer plates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115113319B_ABST
    Figure CN115113319B_ABST
Patent Text Reader

Abstract

This invention relates to multilayer films and a method for manufacturing a polarizing plate using the multilayer film. A multilayer film is provided that enables the unimpeded transport of an extremely thin protective film for a polarizing element and its unimpeded adhesion to a polarizing element. An embodiment of the multilayer film of this invention is a co-extruded film having a first layer and a second layer, wherein the first layer comprises a first thermoplastic resin, the second layer comprises a second thermoplastic resin, and the distance D between the Hansen solubility parameters of the first and second thermoplastic resins is specified. HSP The radius R of the Hansen sphere of the first thermoplastic resin satisfies D. HSP The relationship is / R≥1.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to multilayer thin films and a method for manufacturing polarizing plates using multilayer thin films. Background Technology

[0002] For image display devices (e.g., liquid crystal displays, organic EL displays), due to their image formation methods, polarizing plates are usually arranged on at least one side of the image display panel. In recent years, the thinning and flexibility of image display devices have been progressing, leading to a strong demand for thinner polarizing plates. Considering the ongoing progress in thinning polarizing elements, there is an urgent need for thinner protective films for polarizing elements. However, attempting to thin the protective film for polarizing elements presents the following problems: difficulties in transporting the protective film during the polarizing plate manufacturing process, and difficulties in bonding the film to the polarizing element due to breakage, wrinkles, etc.

[0003] Existing technical documents

[0004] Patent documents

[0005] Patent Document 1: Japanese Patent Application Publication No. 2006-220732 Summary of the Invention

[0006] The problem the invention aims to solve

[0007] The present invention was made to solve the above-mentioned existing problems, and its main objective is to provide a multilayer film that can transport an extremely thin protective film for polarizing elements without defects and adhere to the polarizing element without defects.

[0008] Solution for solving the problem

[0009] The multilayer film of this invention is a co-extruded film having a first layer and a second layer, wherein the first layer comprises a first thermoplastic resin, and the second layer comprises a second thermoplastic resin, and the distance D between the Hansen solubility parameters of the first thermoplastic resin and the second thermoplastic resin is specified. HSP And the radius R of the Hansen sphere of the first thermoplastic resin satisfies D HSP The relationship is / R≥1.

[0010] In one embodiment, the difference in glass transition temperature between the first thermoplastic resin and the second thermoplastic resin is 50°C or less.

[0011] In one embodiment, the thickness of the first layer is 7 μm or less, and the thickness of the second layer is 25 μm or more.

[0012] In one embodiment, the first thermoplastic resin is a cyclic olefin resin, and the second thermoplastic resin is an acrylic resin.

[0013] In one embodiment, the light transmittance of the multilayer film is 90% or more and the haze is 1.0% or less.

[0014] In one embodiment, the first layer functions as a protective film for the polarizer, and the second layer functions as a supporting substrate.

[0015] In one embodiment, the multilayer film further includes a third layer on the side of the second layer opposite to the first layer, the third layer comprising the first thermoplastic resin. In another embodiment, the third layer functions as a protective film for a polarizer.

[0016] According to another aspect of the present invention, a method for manufacturing a polarizing plate is provided. The method includes: bonding the first layer of a multilayer film having the first layer and the second layer to a polarizing element to obtain an intermediate laminate; and peeling the second layer from the intermediate laminate.

[0017] Another manufacturing method of the present invention includes: attaching the first layer of a multilayer film further comprising the third layer to a first polarizing element to obtain a first intermediate laminate; peeling the laminate of the second layer and the third layer from the first intermediate laminate to obtain a first polarizing plate; attaching the third layer of the peeled laminate to a second polarizing element to obtain a second intermediate laminate; and peeling the second layer from the second intermediate laminate to obtain a second polarizing plate.

[0018] In one embodiment, the thickness of the polarizing element is 20 μm or less.

[0019] The effects of the invention

[0020] According to embodiments of the present invention, it is possible to deliver an extremely thin protective film for polarizers without defects and to adhere a multilayer film to the polarizer without defects. Attached Figure Description

[0021] Figure 1 middle, Figure 1 (a) is a cross-sectional schematic diagram illustrating a multilayer thin film according to one embodiment of the present invention; Figure 1 (b) is a cross-sectional schematic diagram illustrating another embodiment of the multilayer thin film of the present invention.

[0022] Figure 2 middle, Figure 2 (a)~ Figure 2 (c) is for use Figure 1 A schematic diagram illustrating the manufacturing method of the multilayer thin film polarizing plate (a).

[0023] Figure 3 middle, Figure 3 (a)~ Figure 3 (f) is for use Figure 1 (b) is a schematic diagram illustrating the manufacturing method of a multilayer thin film polarizing plate.

[0024] Explanation of reference numerals in the attached figures

[0025] 10. Level 1

[0026] 20 Second Floor

[0027] 30 Third Floor

[0028] 100+ layer thin film

[0029] 101 Multilayer Thin Film

[0030] 200 polarizer

[0031] 201 First Polarizing Component

[0032] 202 Second polarizer

[0033] 300 polarizing plate

[0034] 301 No. 1 Polarizing Plate

[0035] 302 2nd polarizing plate Detailed Implementation

[0036] The embodiments of the present invention will be described below, but the present invention is not limited to these embodiments.

[0037] A. Multilayer thin films

[0038] A-1. Overall Structure of Multilayer Thin Films

[0039] Figure 1 (a) is a cross-sectional schematic diagram illustrating a multilayer film according to one embodiment of the present invention. The multilayer film 100 illustrated in the figure is a co-extruded film having a first layer 10 and a second layer 20. By forming the multilayer film through co-extrusion, the peel force between the first layer and the second layer can be made appropriate. The first layer 10 contains a first thermoplastic resin, and the second layer 20 contains a second thermoplastic resin. In an embodiment of the present invention, the distance D between the Hansen solubility parameter (hereinafter also referred to as the HSP value) of the first thermoplastic resin and the second thermoplastic resin is... HSP The radius R of the Hansen sphere of the first thermoplastic resin satisfies D. HSP The relationship is that / R≥1. (D) HSP / R is preferably 1.1 or higher, more preferably 1.3 or higher, even more preferably 1.4 or higher, and particularly preferably 1.5 or higher. D HSP / R can be, for example, below 3.0, or, for example, below 2.7. DHSP When / R is in such a range, due to the synergistic effect with the effect of forming a multilayer film by co-extrusion molding, the following excellent peeling characteristics can be achieved: the first layer and the second layer do not peel off before the multilayer film is actually used, and the first layer and the second layer peel off well when the first layer is peeled off from the multilayer film for use as a various functional film.

[0040] For the aforementioned Hansen solubility parameters, the Hildebrand solubility parameters are divided into three components: dispersion force (δD), permanent dipole intermolecular force (δP), and hydrogen bonding force (δH). These are represented by vectors obtained by plotting them in 3D space. Substances with similar vectors can be judged to have high solubility. That is, the similarity of solubility can be judged based on the distance between their HSP values ​​(HSP distance). The definition and calculation of the Hansen solubility parameters are recorded in Charles M. Hansen's *Hansen Solubility Parameters: A Users Handbook* (CRC Publishing, 2007).

[0041] Regarding HSP values, there are known values ​​for various resins and solvents that can be used directly, or values ​​calculated using computer software, namely HSPiP (Hansen Solubility Parameters in Practice). It should be noted that HSPiP also has a database of resins and solvents. In this specification, the HSP value of the first thermoplastic resin is calculated using the Hansen sphere method and HSPiP according to the following steps. First, the solubility of the first thermoplastic resin being evaluated is performed using solvents with known solubility parameters. Here, methyl ethyl ketone (MEK) is used as a good solvent, and n-hexane, methanol, trichlorobenzene, and γ-butyrolactone are used as poor solvents, respectively, to evaluate the solubility relative to a mixture of these good and poor solvents. Details of the evaluation method are described in the examples described later. Next, based on the obtained solubility evaluation results, δD, δP, and δH are calculated using HSPiP, a three-dimensional plot is created, and the Hansen sphere is determined based on their coordinates. The center coordinates of the Hansen sphere are the HSP value of the first thermoplastic resin, and the radius of the Hansen sphere is the interaction radius R of the first thermoplastic resin. Furthermore, the HSP value of the second thermoplastic resin can be determined in the same manner as for the first thermoplastic resin. The coordinate distance between the HSP values ​​of the first and second thermoplastic resins is D. HSP D HSP It is represented by the following formula. In the formula, the suffix "1" refers to the first thermoplastic resin and "2" refers to the second thermoplastic resin.

[0042] D HSP=√{4×(δD1-δD2)} 2 +2×(δP1-δP2) 2 +2×(δH1-δH2) 2}

[0043] The difference in glass transition temperature (Tg) between the first thermoplastic resin and the second thermoplastic resin is preferably 50°C or less, more preferably 40°C or less, further preferably 30°C or less, and particularly preferably 20°C or less. This Tg difference can, for example, be 3°C or more. When the Tg difference is within this range, the excellent peel properties described above can be ensured, and excellent tensile properties can be achieved. Specifically, uneven stretching and breakage can be well suppressed. When forming multilayer films by co-extrusion, including stretching for the purpose of film formation, if the Tg difference is too large, uneven thickness may sometimes occur. Such uneven thickness raises concerns about wrinkles, bends and / or twisting, or breakage during transport. As a result, the polarizer and the first layer may not adhere well. When the Tg difference is within the range described above, such undesirable conditions can be suppressed.

[0044] The light transmittance of the multilayer film is preferably 90% or more, more preferably 92% or more, and even more preferably 95% or more. Higher light transmittance is preferred; for example, it can be 100% or less, and also, for example, 99% or less. Furthermore, the haze of the multilayer film is preferably 1.0% or less, more preferably 0.8% or less, and even more preferably 0.5% or less. Lower haze is preferred; for example, it can be 0.1% or more. When the light transmittance and / or haze are in such ranges, the first layer can exhibit very good properties when functioning as a protective film for the polarizer, as described later. Light transmittance can be measured, for example, according to the method of ASTM-D-1003. Haze can be measured, for example, according to the method of JIS K 7136.

[0045] In one embodiment, the first layer functions as a protective film for the polarizing element, and the second layer functions as a supporting substrate for the first layer. By configuring the multilayer film as described above, even if the first layer is very thin (for example, a thickness of 7 μm or less, or even 1 μm), it can still function as a protective film for the polarizing element. That is, even if the first layer is very thin, it can be well transported in the form of a multilayer film during the polarizing plate manufacturing process, and as described above, the first layer can be well peeled from the second layer. Therefore, when the polarizing element is bonded to the first layer (during the transfer of the first layer to the polarizing element), breakage, wrinkles, etc., can be suppressed, and bonding (transfer) can be performed well. As a result, a very thin protective film for the polarizing element can function well in the polarizing plate. In other words, multilayer films are suitable for use in the manufacture of polarizing plates.

[0046] In another embodiment of the present invention, such as Figure 1 As shown in (b), the multilayer film 101 may further include a third layer 30 on the side of the second layer 20 opposite to the first layer 10. The third layer 30 typically contains the first thermoplastic resin. Therefore, the third layer preferably functions as a protective film for polarizing elements.

[0047] The first to the third layers will be explained in detail below through items A-2 to A-4. Furthermore, the method of using the first layer (and the third layer if present) as a multilayer film that functions as a protective film for polarizing elements will be explained in item B as a method of manufacturing a polarizing plate.

[0048] A-2. First Floor

[0049] The first layer, as described above, comprises a first thermoplastic resin. As the first thermoplastic resin, any suitable thermoplastic resin can be used in the multilayer film as long as it meets the characteristics described above. Examples of the first thermoplastic resin include cyclic olefin resins, polyester resins, and (meth)acrylic resins. These resins can be used alone or in combination. Cyclic olefin resins or polyester resins are preferred, and cyclic olefin resins are more preferred. This is because it has the desired radius R of the Hansen sphere and facilitates the bonding of D with the second thermoplastic resin. HSP / R should be adjusted to an appropriate range. Representative examples of cyclic olefin resins include norbornene resins. Representative examples of polyester resins include polyethylene terephthalate (PET); a polyester comprising terephthalic acid, isophthalic acid, ethylene glycol, and neopentyl glycol as monomer units. (Meth)acrylic resins will be described later in section A-3, under the section on thermoplastic resins.

[0050] The aforementioned norbornene-based resins are resins polymerized using norbornene monomers as polymerization units. Examples of such norbornene monomers include norbornene, and its alkyl and / or alkylidene substituted derivatives, such as 5-methyl-2-norbornene, 5-dimethyl-2-norbornene, 5-ethyl-2-norbornene, 5-butyl-2-norbornene, 5-ethylidene-2-norbornene, and their halogenated, ester- or other polar group substituted derivatives; dicyclopentadiene, 2,3-dihydrodicyclopentadiene, etc.; dimethylbridged octahydronaphthalene, and its alkyl derivatives... And / or alkylidene substituents, and polar substituents such as halogens and esters, for example, 6-methyl-1,4:5,8-dimethylbridged-1,4,4a,5,6,7,8,8a-octahydronaphthalene, 6-ethyl-1,4:5,8-dimethylbridged-1,4,4a,5,6,7,8,8a-octahydronaphthalene, 6-ethylidene-1,4:5,8-dimethylbridged-1,4,4a,5,6,7,8,8a-octahydronaphthalene, 6 -Chloro-1,4:5,8-dimethylbridged-1,4,4a,5,6,7,8,8a-octahydronaphthalene, 6-cyano-1,4:5,8-dimethylbridged-1,4,4a,5,6,7,8,8a-octahydronaphthalene, 6-pyridyl-1,4:5,8-dimethylbridged-1,4,4a,5,6,7,8,8a-octahydronaphthalene, 5-methyl-5-methoxycarbonylbicyclo[2.2.1]hept-2-ene, 6-methoxycarbonyl-1,4:5, 8-Dimethylbridged-1,4,4a,5,6,7,8,8a-octahydronaphthalene, etc.; 3- to 4-terpolymers of cyclopentadiene, such as 4,9:5,8-dimethylbridged-3a,4,4a,5,8,8a,9,9a-octahydro-1H-benzoindene, 4,11:5,10:6,9-trimethylbridged-3a,4,4a,5,5a,6,9,9a,10,10a,11,11a-dodecylhydro-1H-anthracene, tetracyclic [4.4.0.1] 2,5 .1 7,10 [Dodecyl-3-ene, tetracyclo[9.2.1.0]] 2,10 .0 3,8 [Tetradecene-3,5,7,12-tetraene, etc.] The above-mentioned norbornene resins can be copolymers of norbornene monomers with other monomers.

[0051] In one embodiment, the norbornene resin can be a copolymer comprising polar norbornene monomers (polar backbone) and nonpolar norbornene monomers (nonpolar backbone). Specific examples of polar norbornene monomers include 5-methyl-5-methoxycarbonylbicyclo[2.2.1]hept-2-ene and 6-methoxycarbonyl-1,4:5,8-dimethylbridge-1,4,4a,5,6,7,8,8a-octahydronaphthalene. Specific examples of nonpolar norbornene monomers include norbornene, 2,3-dihydrodicyclopentadiene, and tetracyclo[4.4.0.1].2,5 .1 7,10 [Dodecyl-3-ene, tetracyclo[9.2.1.0]] 2,10 .0 3,8 [Tetradecane-3,5,7,12-tetraene. In this case, the polar backbone content in the norbornene resin is preferably 35 mol% to 95 mol%, more preferably 40 mol% to 90 mol%, and even more preferably 42 mol% to 88 mol%. Furthermore, the nonpolar backbone content in the norbornene resin is preferably 5 mol% to 65 mol%, more preferably 10 mol% to 60 mol%, and even more preferably 12 mol% to 58 mol%. When the polar and nonpolar backbone contents in the norbornene resin are within this range, excellent exfoliation properties can be achieved. It should be noted that when the polar and nonpolar backbone contents in the norbornene resin are within the above range, the norbornene resin may contain other monomer units (backbone).]

[0052] The Tg of the first thermoplastic resin can be, for example, 100°C to 130°C, or, for example, 140°C to 160°C. When the Tg of the first thermoplastic resin is in such a range, the difference between it and the Tg of the second thermoplastic resin can be set to the aforementioned desired range.

[0053] The thickness of the first layer is preferably 10 μm or less, more preferably 7 μm or less, further preferably 5 μm or less, and particularly preferably 3 μm or less. The thickness of the first layer can, for example, be 0.7 μm or more. According to embodiments of the present invention, even if the thickness of the first layer is so very thin, the first layer can be transported without defects and adhered to the object without defects. Therefore, when the object to be adhered to is, for example, a polarizing element, an extremely thin polarizing plate can be manufactured well.

[0054] The light transmittance of the first layer is preferably 88% or more, more preferably 92% or more, and even more preferably 95% or more. A light transmittance within this range ensures the desired transparency. Higher light transmittance of the first layer is preferred; for example, it can be 100% or less, and also, for example, 99% or less. The haze of the first layer is preferably 1.0% or less, more preferably 0.8% or less, and even more preferably 0.5% or less. When the haze is within this range, when the first layer is used as, for example, a protective film for a polarizing element, it can impart good clarity to the polarizing plate. Furthermore, even when used as a polarizing plate on the visual recognition side of an image display device, the displayed content can be visually recognized well. Lower haze is preferred; for example, it can be 0.1% or more.

[0055] In one embodiment, the first layer can be substantially optically isotropic. This property can be imparted to the first layer by co-extruding a multilayer film using a specified material. In this specification, "substantially optically isotropic" means that the in-plane phase difference Re(550) is 0 nm to 10 nm, and the phase difference Rth(550) in the thickness direction is -20 nm to +10 nm. More preferably, the in-plane phase difference Re(550) is 0 nm to 5 nm, further preferably 0 nm to 3 nm, and particularly preferably 0 nm to 2 nm. More preferably, the phase difference Rth(550) in the thickness direction is -5 nm to +5 nm, further preferably -3 nm to +3 nm, and particularly preferably -2 nm to +2 nm. When the Re(550) and Rth(550) of the first layer are in such ranges, when the first layer is used as a polarizer protective film, and a polarizing plate containing this polarizer protective film is applied to an image display device, adverse effects on display characteristics can be suppressed. It should be noted that Re(550) is the in-plane phase difference of the thin film measured at 23℃ using light with a wavelength of 550nm. Re(550) is calculated using the formula: Re(550) = (nx - ny) × d. Rth(550) is the phase difference in the thickness direction of the thin film measured at 23℃ using light with a wavelength of 550nm. Rth(550) is calculated using the formula: Rth(550) = (nx - nz) × d. Here, nx is the refractive index in the direction of maximum in-plane refractive index (i.e., the slow axis direction), ny is the refractive index in the direction orthogonal to the slow axis (i.e., the fast axis direction), nz is the refractive index in the thickness direction, and d is the thickness of the thin film (nm).

[0056] A-3. Second Floor

[0057] The second layer, as described above, comprises a second thermoplastic resin. As the second thermoplastic resin, any suitable thermoplastic resin can be used, provided the multilayer film satisfies the characteristics described above. (Meth)acrylic resins are preferably cited as examples of the second thermoplastic resin. This is because it is easy to bond D with the first thermoplastic resin. HSP Adjust / R to the appropriate range. (Meth)acrylic resins can be used alone or in combination with different (meth)acrylic resins. In this specification, "(meth)acrylic acid" refers to acrylic acid and / or methacrylic acid. Hereinafter, (meth)acrylic acid will sometimes be simply referred to as acrylic acid.

[0058] As a (meth)acrylic resin, any suitable (meth)acrylic resin can be used. Typically, as a monomer unit, the (meth)acrylic resin contains an alkyl (meth)acrylic ester as the main component. Examples of alkyl (meth)acrylic esters constituting the main backbone of the (meth)acrylic resin include linear or branched alkyl esters with 1 to 18 carbon atoms. They can be used alone or in combination. Furthermore, any suitable comonomer can be introduced into the (meth)acrylic resin through copolymerization. The type, quantity, and copolymerization ratio of such comonomers can be appropriately set according to the purpose.

[0059] The above-mentioned alkyl methacrylates are typically represented by the following general formula (1):

[0060]

[0061] In general formula (1), R 4 R represents a hydrogen atom or a methyl group. 5 Represents a hydrogen atom, or an aliphatic or alicyclic hydrocarbon group having 1 to 6 carbon atoms that may be substituted. Examples of substituents include halogens and hydroxyl groups. Specific examples of alkyl methacrylates include methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, n-butyl methacrylate, tert-butyl methacrylate, n-hexyl methacrylate, cyclohexyl methacrylate, chloromethyl methacrylate, 2-chloroethyl methacrylate, 2-hydroxyethyl methacrylate, 3-hydroxypropyl methacrylate, 2,3,4,5,6-pentahydroxyhexyl methacrylate, and 2,3,4,5-tetrahydroxypentyl methacrylate. In general formula (1), R 5 The preferred atom is a hydrogen atom or a methyl group. Therefore, particularly preferred alkyl (meth)acrylates are methyl acrylate or methyl methacrylate.

[0062] The above-mentioned (meth)acrylic resins may contain only a single (meth)acrylic alkyl ester unit, or they may contain R in the above general formula (1). 4 and R 5 Different types of alkyl (meth)acrylate units.

[0063] The content of alkyl methacrylate units in the aforementioned (meth)acrylic resins is preferably 50 mol% to 98 mol%, more preferably 55 mol% to 98 mol%, further preferably 60 mol% to 98 mol%, particularly preferably 65 mol% to 98 mol%, and most preferably 70 mol% to 97 mol%. When the content is less than 50 mol%, there is a concern that the effects derived from the alkyl methacrylate units (e.g., high heat resistance, high transparency) may not be fully realized. When the content is greater than 98 mol%, there is a concern that the resin may become brittle and prone to cracking, resulting in insufficient high mechanical strength and poor productivity.

[0064] In one embodiment, the (meth)acrylic resin may further contain vinyl monomer units (other vinyl monomer units) that can copolymerize with the above-mentioned alkyl (meth)acrylic ester. Other vinyl monomers include, for example, acrylonitrile, methacrylonitrile, α-ethylacrylonitrile, allyl glycidyl ether, maleic anhydride, itaconic anhydride, N-methylmaleimide, N-ethylmaleimide, N-cyclohexylmaleimide, aminoethyl acrylate, propylaminoethyl acrylate, dimethylaminoethyl methacrylate, ethylaminopropyl methacrylate, cyclohexylaminoethyl methacrylate, N-vinyldiethylamine, N-acetylvinylamine, allylamine, methylallylamine, N-methylallylamine, 2-isopropenyl-oxazoline, 2-vinyl-oxazoline, 2-acryloyl-oxazoline, N-phenylmaleimide, phenylaminoethyl methacrylate, styrene, α-methylstyrene, p-glycidylstyrene, p-aminostyrene, 2-styrene-oxazoline, etc. These can be used alone or in combination. Styrene monomers such as styrene and α-methylstyrene are preferred. The content of other vinyl monomer units is preferably 0 to 1% by weight, more preferably 0 to 0.1% by weight. When it is in such a range, it is possible to suppress the manifestation of undesirable phase differences and the reduction of transparency.

[0065] In one embodiment, the (meth)acrylic resin comprises at least one selected from glutarimide units, lactone ring units, maleic anhydride units, maleimide units, and glutaric anhydride units. Acrylic resins comprising lactone ring units are described, for example, in Japanese Patent Application Publication No. 2008-181078, the description of which is incorporated herein by reference. The glutarimide unit is preferably represented by the following general formula (2):

[0066]

[0067] In general formula (2), R 1 and R 2 Each independently represents hydrogen or an alkyl group having 1 to 8 carbon atoms, R3 It represents an alkyl group having 1 to 18 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, or an aryl group having 6 to 10 carbon atoms. In general formula (2), R is preferred. 1 and R 2 Each is independently hydrogen or methyl, R 3 It is hydrogen, methyl, butyl, or cyclohexyl. More preferably, R 1 Methyl, R 2 For hydrogen, R 3 It is a methyl group.

[0068] The aforementioned acrylic resin may contain only a single glutarimide unit, or it may contain R from the above general formula (2). 1 R 2 and R 3 Different types of glutarimide units.

[0069] The content of glutarimide units in (meth)acrylic resins is preferably 2 mol% to 50 mol%, more preferably 2 mol% to 45 mol%, further preferably 2 mol% to 40 mol%, particularly preferably 2 mol% to 35 mol%, and most preferably 3 mol% to 30 mol%. When the content is less than 2 mol%, there is concern that the effects derived from the glutarimide units (e.g., high optical properties, high mechanical strength) may not be fully realized. When the content exceeds 50 mol%, there are concerns that, for example, heat resistance and transparency may be insufficient.

[0070] In one embodiment, the (meth)acrylic resin may contain, for example, 0 to 10% by weight of unsaturated carboxylic acid units that do not participate in the intramolecular imidization reaction. The content of the unsaturated carboxylic acid units is preferably 0 to 5% by weight, more preferably 0 to 1% by weight. When the content is in this range, transparency, retention stability, and moisture resistance can be maintained.

[0071] The imidization rate in the (meth)acrylic resin is preferably 2.5% to 20.0%. When the imidization rate is within this range, a resin with excellent heat resistance, transparency, and processability can be obtained, preventing scaling and reduction in mechanical strength during film forming. In the above-mentioned (meth)acrylic resin, the imidization rate is expressed as the ratio of glutarimide units to alkyl (meth)acrylic ester units. This ratio can be obtained, for example, from the NMR spectrum, IR spectrum, etc., of the (meth)acrylic resin. In this embodiment, the imidization rate can be... 1 HNMR BRUKER AvanceIII (400MHz), through resin 1The peak area of ​​the O-CH3 protons derived from alkyl (meth)acrylate near 3.5–3.8 ppm is set as A, and the peak area of ​​the N-CH3 protons derived from glutarimide near 3.0–3.3 ppm is set as B. The peak area is then determined by the following formula.

[0072] Imidization rate Im (%) = {B / (A+B)} × 100

[0073] The acid value of the (meth)acrylic resin is preferably 0.10 mmol / g to 0.50 mmol / g. A resin with an excellent balance of heat resistance, mechanical properties, and processability can be obtained within this acid value range. If the acid value is too low, problems may arise such as increased costs due to the use of modifiers to adjust the acid value to the desired level, and the formation of gel-like substances due to modifier residues. If the acid value is too high, foaming is likely to occur during film forming (e.g., melt extrusion), tending to reduce the productivity of molded products. In the above-mentioned (meth)acrylic resin, the acid value refers to the content of carboxylic acid units and carboxylic anhydride units in the (meth)acrylic resin. In this embodiment, the acid value can be calculated, for example, by the titration method described in WO2005 / 054311 or Japanese Patent Application Publication No. 2005-23272.

[0074] The weight-average molecular weight of the above-mentioned (meth)acrylic resin is preferably 1,000 to 2,000,000, more preferably 5,000 to 1,000,000, further preferably 10,000 to 500,000, particularly preferably 50,000 to 500,000, and most preferably 60,000 to 150,000. The weight-average molecular weight can be determined, for example, by gel permeation chromatography (GPC system, manufactured by Tosoh Corporation) and conversion to polystyrene. It should be noted that tetrahydrofuran can be used as a solvent.

[0075] The Tg of the second thermoplastic resin can be, for example, 100°C to 130°C. When the Tg of the second thermoplastic resin is in such a range, the difference between the Tg of the second thermoplastic resin and the Tg of the first thermoplastic resin can be set to the aforementioned desired range.

[0076] The thickness of the second layer is preferably 20 μm or more, more preferably 25 μm or more, further preferably 30 μm or more, and particularly preferably 35 μm or more. The thickness of the second layer can, for example, be 250 μm or less. When the thickness of the second layer is within this range, it can function well as a support substrate. As a result, even if the thickness of the first layer is very thin, the first layer can be transported without defects and adhered to the object without defects. Therefore, when the first layer is used as a protective film for the polarizer, a polarizing plate with a very thin protective film for the polarizer can be manufactured, which greatly contributes to the thinning of the polarizing plate.

[0077] The light transmittance of the second layer can be, for example, 90% or more, or, for example, 92% or more. The haze of the second layer can be, for example, 1.0% or less, or, for example, 0.8% or less. Since the second layer can function as a support substrate, strict optical properties are not required. However, by co-extruding the multilayer film, the light transmittance and haze of the first layer can be set to the ranges described above, and the light transmittance and haze of the second layer can also be set to such ranges.

[0078] The tensile modulus of the second layer is preferably 0.5 GPa or higher, more preferably 1 GPa or higher, and even more preferably 2 GPa or higher. The upper limit of the tensile modulus can be, for example, 20 GPa. If the tensile modulus is less than 0.5 GPa, sufficient mechanical strength may not be achieved. The tensile modulus can be determined, for example, according to ASTM-D-882-61T.

[0079] The tensile strength of the second layer is preferably 10 MPa or more but less than 100 MPa, more preferably 30 MPa or more but less than 100 MPa. If the tensile strength is less than 10 MPa, sufficient mechanical strength may not be achieved. If the tensile strength exceeds 100 MPa, there are concerns about insufficient processability. Tensile strength can be measured, for example, according to ASTM-D-882-61T.

[0080] The tensile elongation of the second layer is preferably 1.0% or more, more preferably 3.0% or more, and even more preferably 5.0% or more. The upper limit of the tensile elongation can be, for example, 100%. If the tensile elongation is less than 1%, the toughness may be insufficient. The tensile elongation can be determined, for example, according to ASTM-D-882-61T.

[0081] A-4. Third Floor

[0082] The specific structure of the third layer is as described in section A-2 regarding the first layer. The third layer may have the same structure as the first layer, or it may have a different structure.

[0083] B. Manufacturing method of polarizing plate

[0084] As described above, the multilayer film of the embodiments of the present invention is suitable for use in the manufacture of polarizing plates. Therefore, a method for manufacturing a polarizing plate using such a multilayer film is also included in the embodiments of the present invention. One embodiment of the present invention uses... Figure 1 A multilayer thin film having a first layer and a second layer, as shown in (a). Figure 2 (a)~ Figure 2 (c) is a schematic diagram illustrating the manufacturing method of such a polarizing plate. First, as... Figure 2As shown in (a), the first layer 10 of a multilayer film 100 having a first layer 10 and a second layer 20 is bonded to a polarizer 200 to obtain an intermediate laminate. Bonding can be performed using any suitable adhesive layer (typically an adhesive layer or a binder layer). Examples of adhesives constituting the adhesive layer include, for example, water-based adhesives (typically polyvinyl alcohol (PVA) based adhesives) and active energy radiation-cured adhesives. Examples of binders constituting the binder layer include, for example, acrylic adhesives. Bonding is typically performed by a so-called roll-to-roll method. The polarizer 200 can be a single resin film or a laminate of a substrate and a resin layer (polarizer). A typical polarizer is a polyvinyl alcohol (PVA) based resin film or resin layer containing a dichroic substance (e.g., iodine). As a polarizer, any suitable polarizer configuration can be used, therefore detailed description is omitted. Next, as... Figure 2 As shown in (b), the second layer is peeled off from the intermediate laminate. The result is as follows: Figure 2 As shown in (c), a polarizing plate 300 having a polarizing element 200 and a first layer (polarizing element protective film) 10 can be obtained. By using the multilayer film of the embodiment of the present invention, an extremely thin polarizing element protective film can be transported without defects and bonded to the polarizing element without defects. As a result, an extremely thin polarizing plate can be manufactured well. For example, the polarizing element obtained by using a laminate of a resin substrate and a PVA-based resin layer coated on the resin substrate, as described in Japanese Patent Application Publication No. 2012-73580 and Japanese Patent No. 6470455, can have a very thin thickness of 5 μm or less (e.g., 3 μm). As a result, the thinning of the polarizing element protective film becomes the dominant factor in the thinning of the polarizing plate as a whole. In other words, the difficulty in transporting and bonding the thin polarizing element protective film to the polarizing element becomes an obstacle to the thinning of the polarizing plate as a whole. According to embodiments of the present invention, as described above, extremely thin (e.g., 1 μm thick) polarizer protective films can be conveyed without defects and bonded to polarizers without defects, thus enabling the fabrication of extremely thin polarizing plates. Specifically, according to embodiments of the present invention, a first layer (polarizer protective film) with a thickness of 1 μm can be bonded to a polarizer with a thickness of 5 μm using a 1 μm thick PVA-based adhesive layer. As a result, extremely thin polarizing plates with a thickness of 7 μm can be fabricated.

[0085] Another embodiment of the present invention describes a method for manufacturing a polarizing plate using, as follows: Figure 1 (b) shows a multilayer film having a first layer, a second layer, and a third layer. Figure 3 (a)~ Figure 3 (f) is a schematic diagram illustrating the manufacturing method of such a polarizing plate. First, as... Figure 3As shown in (a), the first layer 10 of a multilayer thin film 101 having a first layer 10, a second layer 20, and a third layer 30 is bonded to the first polarizer 201 to obtain a first intermediate laminate. Next, as... Figure 3 As shown in (b), the second and third layers are peeled off from the first intermediate layer. The result is as follows: Figure 3 As shown in (c), a first polarizing plate 301 having a polarizing element 201 and a first layer (polarizing element protective film) 10 can be obtained. Furthermore, as... Figure 3 As shown in (d), the third layer 30 of the laminate of the second and third layers, which is peeled from the first intermediate laminate, is attached to the second polarizer 202 to obtain the second intermediate laminate. Next, as... Figure 3 As shown in (e), the second layer 20 is peeled off from the second intermediate laminate. The result is as follows: Figure 3 As shown in (f), a second polarizing plate 302 having a polarizing element 202 and a third layer (polarizing element protective film) 30 can be obtained. According to this embodiment, two polarizing plates can be obtained from one multilayer film, thus achieving excellent manufacturing efficiency. It should be noted that the structure of the polarizing element, the bonding method, the adhesive layer, the effect, etc., are as follows... Figure 2 (a)~ Figure 2 The embodiment shown in (c) is as described above.

[0086] The thickness of the polarizing element can be, for example, 20 μm or less, or for example, 15 μm or less, or for example, 12 μm or less, or for example, 10 μm or less, or for example, 8 μm or less, or for example, 5 μm or less, or for example, 3 μm or less. On the other hand, the thickness of the polarizing element can be, for example, 1 μm or more, or for example, 2 μm or more, or for example, 3 μm or more. As described above, according to embodiments of the present invention, it is possible to manufacture a polarizing plate having a very thin protective film for the polarizing element, so the thickness of the polarizing element can be appropriately set according to the purpose. For example, when using a thin polarizing element of 5 μm or less, an extremely thin polarizing plate can be achieved.

[0087] [Example]

[0088] The present invention will now be described in detail through examples, but the present invention is not limited to these examples. The methods for measuring each characteristic are as follows. It should be noted that, unless otherwise specified, "parts" and "%" in the examples are based on weight.

[0089] (1) Tensile properties

[0090] The multilayer films obtained in the examples and comparative examples were cut into 150 mm wide and 150 mm long pieces as test samples. Using an intermittent stretching machine, the films were stretched twice along the MD direction and twice along the TD direction at the glass transition temperature of the first layer +20°C, and the presence or absence of film fracture was observed. Evaluation was performed according to the following criteria.

[0091] ○: No film rupture was observed.

[0092] △: Slight film breakage was observed.

[0093] ×: Significant film fractures were observed.

[0094] (2) Peelability

[0095] Peel tests were performed on the multilayer films obtained in the examples and comparative examples to evaluate the peelability between the first and second layers. Specifically, the multilayer film was cut to a size of 200 mm wide and 15 mm long. A slit was made between the first and second layers using a cutting tool, and the film was then attached to a glass plate. Using a TENSILON, the first and second layers were peeled at a 135-degree angle at a peeling speed of 300 mm / min, and the condition was observed. The results were evaluated according to the following criteria.

[0096] ○: The film can be peeled off well without breaking.

[0097] △: Slight fractures were observed in the film, but it was able to be peeled off.

[0098] ×: The film is broken, cannot be peeled off, or has not been cut into the kerf of the cutting blade.

[0099] <Example 1>

[0100] A cyclic olefin resin (manufactured by JSR Corporation) was used as the material for forming the first layer, and an acrylic resin (manufactured by KURARAY CO.,LTD, product name "HRS") was used as the material for forming the second layer. The cyclic olefin resin contained 85 mol% of a polar backbone (monomer units of 6-methoxycarbonyl-1,4:5,8-dimethylbridge-1,4,4a,5,6,7,8,8a-octahydronaphthalene) and 15 mol% of a non-polar backbone (monomer units of 2,3-dihydrodicyclopentadiene), with a Tg of 132°C. This cyclic olefin resin was designated "COP A". The acrylic resin was polymethyl methacrylate (PMMA), with a Tg of 112°C. This acrylic resin was designated "Acrylic A". These materials exhibit D... HSP The relationship is R = 1.6. These materials were co-extruded using an extruder with a specified die to obtain a multilayer film with a first layer of 5 μm thickness and a second layer of 35 μm thickness. The obtained multilayer film was evaluated in (1) and (2) above. The results are shown in Table 1.

[0101] Furthermore, a polarizing plate is fabricated using the obtained multilayer film. Specifically, a long roll of a 30μm thick polyvinyl alcohol (PVA) resin film (manufactured by KURARAY CO.,LTD, product name "PE3000") is unidirectionally stretched along its length at a ratio of 5.9 times its length using a roll stretching machine. Simultaneously, swelling, dyeing, cross-linking, and cleaning processes are performed, followed by drying to create a 12μm thick polarizing element. The multilayer film and the obtained polarizing element are then bonded together roll-to-roll using a PVA-based adhesive (1μm thick) with the first layer of the multilayer film adjacent to the polarizing element, creating an intermediate laminate. The second layer is then peeled off from the intermediate laminate to obtain a polarizing plate consisting of a polarizing element and a first layer (polarizing element protective film). The polarizing plate can be fabricated without defects in any step of the conveying (roll-to-roll) and bonding processes.

[0102] <Examples 2-10>

[0103] The first and second layers use the materials shown in Table 1 (therefore, Tg and D...). HSP (R is the value shown in Table 1), and the thicknesses of the first and second layers are set to the thicknesses shown in Table 1. Otherwise, the process is the same as in Example 1 to obtain a multilayer film. The obtained multilayer films are subjected to the same evaluation as in Example 1. The results are shown in Table 1. Furthermore, using the obtained multilayer films, polarizing plates are fabricated, except that the process is the same as in Example 1. Each polarizing plate can be fabricated without defects in any step of the transport (roll-to-roll) and bonding process.

[0104] <Example 11>

[0105] The first and third layers used "COP A", and the second layer used "Acrylic A". These materials were co-extruded using an extruder with a specified die to obtain a multilayer film with a first layer of 1 μm thickness, a second layer of 38 μm thickness, and a third layer of 1 μm thickness. The obtained multilayer film was evaluated in the same manner as in Example 1. The results are shown in Table 1. Furthermore, a polarizing plate was fabricated using the obtained multilayer film. First, the multilayer film and the polarizing element (first polarizing element) used in Example 1 were bonded together roll-to-roll using a PVA-based adhesive (1 μm thickness) with the first layer of the multilayer film adjacent to the first polarizing element to create a first intermediate laminate. Next, the laminate of the second and third layers was peeled off from the obtained first intermediate laminate to obtain a first polarizing plate with a configuration of the first polarizing element / first layer (polarizing element protective film). Furthermore, the second and third layers of the laminate and the polarizing element (second polarizing element) used in Example 1 are bonded together in roll-to-roll fashion using a PVA-based adhesive (1 μm thick) with the third layer of the laminate adjacent to the second polarizing element, to create a second intermediate laminate. Then, the second layer is peeled off from the obtained second intermediate laminate to obtain a second polarizing plate having a configuration of the second polarizing element / third layer (polarizing element protective film). Both the first and second polarizing plates can be manufactured without defects in any step of the transport (roll-to-roll) and bonding processes.

[0106] <Comparative Examples 1-5>

[0107] The first and second layers use the materials shown in Table 1 (therefore, Tg and D...). HSP (R is the value shown in Table 1), and the thicknesses of the first and second layers were set to the thicknesses shown in Table 1. Otherwise, the process was the same as in Example 1 to obtain a multilayer film. The obtained multilayer films were evaluated in the same way as in Example 1. The results are shown in Table 1. Furthermore, using the obtained multilayer films, the fabrication of polarizing plates was attempted, except that the process was the same as in Example 1. However, in Comparative Examples 1-3, the first layer did not peel off smoothly and could not be adhered to the polarizing element. In Comparative Examples 4-5, due to insufficient stretchability, the thickness of the first layer was uneven, and it could not be well adhered to the polarizing element.

[0108] It should be noted that the materials shown in Table 1 have the following meanings. Additionally, in Example 11 of Table 1, "Layer 1" refers to "Layer 1 and Layer 3". Furthermore, "※" in Comparative Examples 4 and 5 of Table 1 indicates that a solvent capable of dissolving the resin at room temperature could not be obtained, making it impossible to calculate D. HSP / R.

[0109] COP B: Manufactured by JSR Corporation, containing 60 mol% of a polar skeleton (monomer unit of 6-methoxycarbonyl-1,4:5,8-dimethylbridge-1,4,4a,5,6,7,8,8a-octahydronaphthalene) and 40 mol% of a nonpolar skeleton (monomer unit of 2,3-dihydrodicyclopentadiene).

[0110] COP C: Manufactured by JSR Corporation, containing 45 mol% of a polar skeleton (monomer unit of 6-methoxycarbonyl-1,4:5,8-dimethylbridge-1,4,4a,5,6,7,8,8a-octahydronaphthalene), 8 mol% of a nonpolar skeleton (monomer unit of norbornene), and 47 mol% of a nonpolar skeleton (monomer unit of 2,3-dihydrodicyclopentadiene).

[0111] COP D: Manufactured by JSR Corporation, containing 66 mol% of a polar skeleton (monomer unit of 6-methoxycarbonyl-1,4:5,8-dimethylbridge-1,4,4a,5,6,7,8,8a-octahydronaphthalene), 3 mol% of a nonpolar skeleton (monomer unit of norbornene), and 31 mol% of a nonpolar skeleton (monomer unit of 2,3-dihydrodicyclopentadiene).

[0112] Acrylic acid B: An acrylic resin with a Tg of 120℃

[0113] Polyester A: Polyester resin with a Tg of 151℃

[0114] Polyester B: Manufactured by Bell Polyester Products, Inc., product name "E03", containing terephthalic acid, isophthalic acid, ethylene glycol and neopentyl glycol as monomer units.

[0115] PP: Manufactured by Japan Polypropylene Corporation, product name "FY6C", polypropylene

[0116] OP: Manufactured by Mitsui Chemicals, Ltd., product name "TPX-M002", polymethylpentene

[0117] [Table 1]

[0118]

[0119] <Evaluation>

[0120] As can be clearly seen from Table 1, the multilayer films of the embodiments of the present invention have excellent tensile and peel properties.

[0121] Industrial availability

[0122] The multilayer thin film of the present invention is suitable for use in the manufacture of polarizing plates.

Claims

1. A multilayer film, which is a co-extruded film having a first layer and a second layer, wherein the first layer comprises a first thermoplastic resin and the second layer comprises a second thermoplastic resin. The distance D between the Hansen solubility parameters of the first thermoplastic resin and the second thermoplastic resin HSP And the radius R of the Hansen sphere of the first thermoplastic resin satisfies D HSP The relationship is that / R≥1. The thickness of the first layer is less than 7 μm, and the thickness of the second layer is more than 25 μm.

2. The multilayer thin film according to claim 1, wherein, The difference in glass transition temperature between the first thermoplastic resin and the second thermoplastic resin is less than 50°C.

3. The multilayer thin film according to claim 1 or 2, wherein, The first thermoplastic resin is a cyclic olefin resin, and the second thermoplastic resin is an acrylic resin.

4. The multilayer film according to claim 1 or 2 has a light transmittance of 90% or more and a haze of 1.0% or less.

5. The multilayer thin film according to claim 1 or 2, wherein, The first layer functions as a protective film for the polarizing element, and the second layer functions as a supporting substrate.

6. The multilayer thin film according to claim 1 or 2, wherein, The second layer also includes a third layer on the side opposite to the first layer, the third layer containing the first thermoplastic resin.

7. The multilayer thin film according to claim 6, wherein, The third layer functions as a protective film for the polarizer.

8. A method for manufacturing a polarizing plate, comprising: The first layer of the multilayer film according to any one of claims 1 to 5 is bonded to a polarizing element to obtain an intermediate laminate; and The second layer is peeled off from the intermediate laminate.

9. A method for manufacturing a polarizing plate, comprising: The first layer of the multilayer film according to claim 6 or 7 is bonded to the first polarizer to obtain the first intermediate laminate; The first polarizing plate is obtained by peeling the laminate of the second layer and the third layer from the first intermediate laminate; The third layer of the peeled laminate is bonded to the second polarizer to obtain the second intermediate laminate; and The second polarizing plate is obtained by peeling off the second layer from the second intermediate laminate.

10. The manufacturing method according to claim 8 or 9, wherein, The thickness of the polarizing element is less than 20 μm.

Citation Information

Patent Citations

  • Method for producing imide polymer

    JP2005023272A

  • Polarizer protective film and manufacturing method thereof, polarizing plate and manufacturing method thereof, and image display device

    JP2006220732A

  • Polarizer protection film, polarizing plate and image display device

    JP2008181078A

  • Manufacturing method of thin polarizing film

    JP2012073580A

  • Imide resin, and production method and use thereof

    WO2005054311A1