Method for manufacturing semiconductor device and method for testing semiconductor device

By applying a high electric field voltage and annealing process to the gate insulating film of semiconductor devices, the threshold voltage deviation caused by sodium ions was solved, improving the yield and manufacturing efficiency of semiconductor devices and reducing the failure rate of packaging tests.

CN115116873BActive Publication Date: 2026-11-20FUJI ELECTRIC CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202210079478.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-03-17
Filing Date
2022-01-24
Publication Date
2026-11-20
Estimated Expiration
2042-01-24

AI Technical Summary

Technical Problem

During the electrode plating process of semiconductor devices, sodium ions may reach the gate insulating film, causing the threshold voltage to deviate from the design value and affecting the performance of the semiconductor device.

Method used

By applying a high electric field voltage to the gate insulating film during the manufacturing process, combined with an annealing process, semiconductor components that are significantly affected by sodium ions are screened out. After forming the plating layer, voltage measurement and judgment are performed to ensure the accuracy of the threshold voltage.

Benefits of technology

Effectively screen out defective semiconductor components, reduce the defect rate in packaging and testing, improve manufacturing efficiency, and reduce manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115116873B_ABST
    Figure CN115116873B_ABST
Patent Text Reader

Abstract

There is a case where threshold voltage of a semiconductor device deviates from a design value. The present invention provides a manufacturing method of a semiconductor device and a test method of a semiconductor device, the manufacturing method including: an element forming step of forming a semiconductor element on a semiconductor substrate and forming a metal electrode above the semiconductor substrate; a plating step of plating the metal electrode; an annealing step of annealing the semiconductor substrate; a voltage application step of applying a voltage corresponding to a thickness of a gate insulating film to the gate insulating film after the annealing step; and a determination step of measuring threshold voltage of the semiconductor element after the voltage application step, and determining whether or not the semiconductor element is acceptable based on a measurement result.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for manufacturing a semiconductor device and a method for testing a semiconductor device. Background Technology

[0002] Conventionally, it is known to plate the surface of the electrodes of a semiconductor device containing a transistor (see, for example, Patent Document 1).

[0003] Existing technical documents

[0004] Patent documents

[0005] Patent Document 1: Japanese Patent Application Publication No. 2017-157851 Summary of the Invention

[0006] Technical issues

[0007] If the electrodes of a semiconductor device are plated, sodium ions and other substances may reach the gate insulating film, causing the threshold voltage of the semiconductor device to deviate from the design value.

[0008] Technical solution

[0009] In a first aspect of the present invention, a method for manufacturing a semiconductor device is provided. The manufacturing method may include an element formation step of forming a semiconductor element including a gate insulating film on a semiconductor substrate and forming a metal electrode above the semiconductor substrate. The manufacturing method may include a plating step of plating the metal electrode. The manufacturing method may include an annealing step of annealing the semiconductor substrate. The manufacturing method may include a voltage application step of applying a voltage corresponding to the thickness of the gate insulating film to the gate insulating film after the annealing step. The manufacturing method may include a determination step of measuring a threshold voltage of the semiconductor element after the voltage application step and determining whether the semiconductor element is qualified based on the measurement result.

[0010] In the voltage application process, a voltage equivalent to an electric field greater than 3.64 kV / μm applied per unit thickness of the gate insulating film can be applied to the gate insulating film.

[0011] In the voltage application process, a voltage equivalent to an electric field of 4.55 kV / μm or more per unit thickness of the gate insulating film can be applied to the gate insulating film.

[0012] In the voltage application process, the voltage application time can be less than 10 seconds.

[0013] In the voltage application process, the voltage application time can be less than 1 second.

[0014] In the device formation process, a gate conductive portion that is insulated from the semiconductor substrate by a gate insulating film can be formed, and an interlayer insulating film that insulates the gate conductive portion from the metal electrode can be formed. In the annealing process, the semiconductor substrate can be annealed such that the average diffusion distance of sodium in the interlayer insulating film is more than 70% of the thickness of the interlayer insulating film.

[0015] In the annealing process, the annealing temperature can be above 240℃ and below 300℃.

[0016] The manufacturing method may include an assembly process for assembling a semiconductor package using semiconductor components that have been determined to be qualified through a judgment process.

[0017] In a second aspect of the present invention, a method for testing a semiconductor device is provided. The semiconductor device may include a semiconductor substrate having a semiconductor element comprising a gate insulating film, and a metal electrode formed on the semiconductor substrate with its upper surface plated. The testing method may include an annealing step of annealing the semiconductor substrate in a chip or wafer state before assembly into a semiconductor package. The testing method may include a voltage application step, after the annealing step, applying a voltage corresponding to the thickness of the gate insulating film to the gate insulating film. The testing method may include a determination step, after the voltage application step, measuring a threshold voltage of the semiconductor element and determining whether the semiconductor element is qualified based on the measurement result.

[0018] The semiconductor substrate may include: a gate conductive portion that is insulated from the semiconductor substrate by a gate insulating film, and an interlayer insulating film that insulates the gate conductive portion from the metal electrode.

[0019] It should be noted that the above summary of the invention does not list all the features of the invention. Furthermore, sub-combinations of these feature groups can also constitute an invention. Attached Figure Description

[0020] Figure 1 This is a cross-sectional view showing an example of a semiconductor device 100.

[0021] Figure 2 This is a diagram showing an outline of the manufacturing method of the semiconductor device 100.

[0022] Figure 3 This is a diagram showing an example of the voltage-current characteristics measured in the judgment process S214.

[0023] Figure 4 This is a diagram illustrating the conditions in the voltage application process S212.

[0024] Figure 5 This is a graph representing the average diffusion distance of sodium ions in the interlayer insulating film 38.

[0025] Figure 6 This is a diagram illustrating an example of the annealing conditions in the annealing process S210.

[0026] Figure 7 This is a diagram illustrating an example of the gate voltage-main current characteristics of a semiconductor device 100.

[0027] Figure 8 This is a diagram illustrating another example of a method for manufacturing a semiconductor device 100.

[0028] Figure 9 This is a circuit diagram showing an example of a circuit 200 disposed within the resin housing of a semiconductor module.

[0029] Figure 10 This is a top view showing an example of a semiconductor module 300.

[0030] Figure 11 It means Figure 10 A diagram of an example of the D-D' section.

[0031] Figure 12 This is a cross-sectional view showing an example of a semiconductor discrete device 400.

[0032] Symbol Explanation

[0033] 10: Semiconductor substrate; 12: Emitter region; 14: Base region; 18: Drift region; 21: Top surface; 37: Through-hole; 38: Interlayer insulating film; 39: Contact hole; 40: Gate trench; 42: Gate insulating film; 44: Gate conductive part; 52: Metal electrode; 53: Plating layer; 84: Through-hole; 86: Main terminal; 88: Housing; 93: Recess; 94: Bottom surface; 95: Cooling fin; 99: Control terminal; 100: Semiconductor device; 101: Sealing part; 102: Terminal; 103: Connection part; 104: Wiring; 105: Connection part; 106: Connection part; 107: Wiring; 108: Chip mounting part; 114: Cooling part; 162: Circuit board; 200: Circuit; 300: Semiconductor module; 400: Discrete semiconductor device. Detailed Implementation

[0034] The present invention will now be described through embodiments thereof, but these embodiments do not limit the invention as defined in the claims. Furthermore, not all combinations of the features described in the embodiments are necessarily necessary for the technical means of the invention.

[0035] In this specification, the side parallel to the depth direction of the semiconductor substrate is referred to as "upper" and the other side as "lower". One of the two main surfaces of a substrate, layer, or other component is referred to as the upper surface and the other as the lower surface. The directions "upper" and "lower" are not limited to the direction of gravity or the direction in which the semiconductor device is mounted.

[0036] In this specification, the terms "same" or "equal" may also include cases with errors caused by manufacturing deviations, etc. Such errors are, for example, within 10%.

[0037] In this specification, the conductivity type of the doped region containing impurities is described as P-type or N-type. In this specification, when referred to as P+ or N+ type, it means that the doping concentration is higher than that of P-type or N-type; when referred to as P- or N- type, it means that the doping concentration is lower than that of P-type or N-type.

[0038] Figure 1 This is a cross-sectional view showing an example of a semiconductor device 100. The semiconductor device 100 includes a semiconductor substrate 10. The semiconductor substrate 10 is a substrate formed of a semiconductor material. As an example, the semiconductor substrate 10 is a silicon substrate, but the material of the semiconductor substrate 10 is not limited to silicon. Figure 1 The image shows only a portion of the area on the upper surface 21 side of the semiconductor device 100.

[0039] In this cross-section, the semiconductor device 100 of this example includes a semiconductor substrate 10, an interlayer insulating film 38, a metal electrode 52, and a plating layer 53. The interlayer insulating film 38 is disposed on the upper surface 21 of the semiconductor substrate 10. The interlayer insulating film 38 is a film comprising at least one layer of an insulating film such as silicate glass with impurities such as boron or phosphorus, a thermally oxidized film, or other insulating films. Contact holes 39 are provided in the interlayer insulating film 38 to expose a portion of the upper surface 21 of the semiconductor substrate 10.

[0040] A metal electrode 52 is disposed above the interlayer insulating film 38. The metal electrode 52 can be formed of a metal or alloy such as aluminum. The metal electrode 52 can be formed to a thickness of 2.5 μm to 7.5 μm by sputtering. The metal electrode 52 is, for example, the emitter electrode in an IGBT (Insulated Gate Bipolar Transistor) or the source electrode in a MOSFET. The metal electrode 52 contacts the semiconductor substrate 10 through the contact hole 39 of the interlayer insulating film 38. A barrier metal layer such as titanium can be disposed between the interlayer insulating film 38, the semiconductor substrate 10, and the metal electrode 52. The barrier metal layer can be formed to a thickness thinner than the metal electrode 52. A plug electrode such as tungsten can be embedded in the contact hole 39 of the interlayer insulating film 38, and the metal electrode 52 can be disposed on it.

[0041] The semiconductor substrate 10 has, sequentially from its upper surface 21, an N-type emitter region 12, a P-type base region 14, and an N-type drift region 18. The emitter region 12 and the base region 14 can be formed by locally implanting impurities into the semiconductor substrate 10. In addition to these regions, the semiconductor substrate 10 may also have regions where impurities are locally implanted. Depending on the type of semiconductor device 100, an N-type or P-type region may be provided below the drift region 18, but... Figure 1 Omitted in .

[0042] One or more gate trench portions 40 are provided on the upper surface 21 of the semiconductor substrate 10. The gate trench portions 40 extend from the upper surface 21 of the semiconductor substrate 10 to the drift region 18. The emitter region 12 and the base region 14 are in contact with the sidewalls of the gate trench portions 40.

[0043] The gate trench portion 40 has a gate insulating film 42 and a gate conductive portion 44. The gate insulating film 42 is configured to cover the inner wall of the trench (groove portion) disposed on the upper surface 21 of the semiconductor substrate 10. The gate insulating film 42 can be formed by oxidizing or nitriding the semiconductor of the inner wall of the trench. In this example, the gate insulating film 42 is a thermal oxide film obtained by oxidizing the inner wall of the trench. The gate conductive portion 44 is disposed inside the trench at a position further inward than the gate insulating film 42. That is, the gate insulating film 42 insulates the gate conductive portion 44 from the semiconductor substrate 10. The gate conductive portion 44 is formed of a conductive material such as polysilicon.

[0044] In this example, the thickness of the gate insulating film 42 is set to T1 (μm). Thickness T1 is the thickness of the gate insulating film 42 in the direction perpendicular to the inner wall of the trench. Thickness T1 can also be the thickness of the gate insulating film 42 in the direction parallel to the upper surface 21 of the semiconductor substrate 10. Thickness T1 can also be the average thickness of the portion of the gate insulating film 42 that contacts the base region 14.

[0045] The gate conductive portion 44 is set to be longer than the base region 14 in the depth direction. The gate trench portion 40 at this cross-section is covered by an interlayer insulating film 38 on the upper surface 21 of the semiconductor substrate 10. Thus, the gate insulating film 42 and the gate conductive portion 44 of the gate trench portion 40 are insulated from the metal electrode 52. In this example, the thickness of the interlayer insulating film 38 is set to T2 (μm). Thickness T2 is the thickness of the interlayer insulating film 38 in the direction perpendicular to the upper surface 21 of the semiconductor substrate 10. Thickness T2 can also be the minimum thickness of the portion of the interlayer insulating film 38 in contact with the gate insulating film 42.

[0046] The gate conductive portion 44 is electrically connected to a gate wiring (not shown) that is insulated from the metal electrode 52. If a predetermined gate voltage is applied to the gate conductive portion 44, an electron-based inversion layer channel is formed on the surface of the interface in the base region 14 that contacts the gate trench portion 40. Thus, the semiconductor device 100 becomes a conductive state in which current flows between the upper surface 21 and the lower surface of the semiconductor substrate 10. The gate voltage at which the semiconductor device 100 becomes conductive is called the threshold voltage.

[0047] exist Figure 1 In one example, a gate voltage is applied to the entire gate trench 40. In other examples, a portion of the gate trench 40 may be connected to the metal electrode 52 without a gate voltage being applied. In this case, the gate trench 40 does not function as the gate for the transistor switch, but as a dummy gate. By configuring the dummy gate, the carrier concentration in the drift region 18 can be adjusted, thereby adjusting the on-resistance of the semiconductor device 100.

[0048] A plating layer 53 is provided on the metal electrode 52. The plating layer 53 is formed of materials such as gold, copper, and nickel alloys, and is formed by single layer or stacking. For example, if the metal electrode 52 is an alloy layer with aluminum as the main component, a nickel alloy can be first plated on the metal electrode 52 with a thickness of 2.0 μm to 6.0 μm, and then gold can be plated on it with a thickness of 0.01 μm to 0.10 μm. Wiring such as lead frames (not shown) can be soldered to the upper surface of the plating layer 53.

[0049] In the plating process of forming the plating layer 53, the upper surface of the metal electrode 52 may be immersed in a plating solution containing ions such as sodium. During the plating process, there is a possibility that ions contained in the plating solution may reach the semiconductor substrate 10. For example, in processes such as sputtering that form the metal electrode 52, unintended through-holes 37 may sometimes be formed on the metal electrode 52. If the interlayer insulating film 38 is exposed through the through-hole 37, sodium ions or the like may reach the interlayer insulating film 38 through the through-hole 37 and then the semiconductor substrate 10. Similarly, if the upper surface 21 of the semiconductor substrate 10 is exposed through the through-hole 37, sodium ions or the like may reach the semiconductor substrate 10 through the through-hole 37.

[0050] If sodium ions or the like that reach the semiconductor substrate 10 are implanted into the gate insulating film 42, the charged state of the gate insulating film 42 changes, resulting in a change in the threshold voltage. For example, when the semiconductor device 100 is placed in a high-temperature environment, the likelihood of sodium ions or the like reaching the gate insulating film 42 increases, leading to a change in the threshold voltage. Therefore, in the manufacturing process of the semiconductor device 100, it is preferable to pre-screen devices with a high likelihood of their threshold voltage changing due to the influence of sodium ions or the like.

[0051] Figure 2 This is a diagram illustrating a general method for manufacturing the semiconductor device 100. The manufacturing method may include only... Figure 2 This is part of the process shown. In this example, multiple semiconductor chips are formed using a semiconductor wafer. First, in the device formation process S202, semiconductor devices are formed on the semiconductor substrate 10, and metal electrodes 52 are formed above the semiconductor substrate 10. The semiconductor substrate 10 in the device formation process S202 is wafer-shaped.

[0052] Semiconductor components include MOSFETs and IGBTs. Figure 1 In this example, the semiconductor device has an emitter region 12, a base region 14, a drift region 18, and a gate trench 40. In the device formation process S202, a device can be formed... Figure 1 The interlayer insulating film 38 is shown. In addition, during the device formation process S202, a metal electrode can also be formed on the lower surface of the semiconductor substrate 10.

[0053] Next, in plating step S204, a plating layer 53 is formed by plating the upper surface of the metal electrode 52. In plating step S204, the upper surface of the metal electrode 52 can be immersed in a plating solution containing ions such as sodium and plating materials such as gold, copper, and nickel alloys. In plating step S204, the plating layer 53 can be formed by chemical plating or the like.

[0054] Next, the semiconductor wafer is cut into multiple semiconductor chips through a cutting process S206. The cutting process S206 may include a process of attaching a cutting tape to the semiconductor wafer before cutting to prevent the multiple semiconductor chips from scattering.

[0055] Next, in testing step S208, each of the chip-shaped semiconductor devices 100 is tested. In this example, testing step S208 tests the threshold voltage of the semiconductor device 100 through an annealing step S210, a voltage application step S212, and a judgment step S214. Testing step S208 can also test the semiconductor device 100 for items other than the threshold voltage test. In testing step S208, each semiconductor device 100 is sorted into qualified and unqualified products.

[0056] In annealing step S210, the semiconductor substrate 10 is annealed. In annealing step S210, the semiconductor device 100 can be placed in an annealing furnace or the like, and the entire semiconductor device 100 is annealed. In annealing step S210, it is preferable that at least a portion of the sodium ions that have entered the upper surface of the interlayer insulating film 38 can pass through the interlayer insulating film 38 in the thickness direction. As an example, the annealing temperature in annealing step S210 is 240°C or higher and 300°C or lower.

[0057] Next, in the voltage application step S212, a predetermined voltage is applied to the gate insulating film 42. In the voltage application step S212, a predetermined voltage is applied to the gate conductive portion 44 via the gate wiring. The potential of the upper surface 21 of the semiconductor substrate 10 can be the same as the potential of the metal electrode 52. As an example, the potential of the metal electrode 52 can be ground potential.

[0058] In the voltage application step S212, by applying a predetermined voltage to the gate insulating film 42, sodium ions and the like present near the gate insulating film 42 are attracted to the gate insulating film 42. The polarity of the voltage applied to the gate conductive portion 44 is opposite to the polarity of the ions attracted to the gate insulating film 42. In this example, sodium ions, which are positive ions, are attracted; therefore, a negative voltage is applied to the gate conductive portion 44.

[0059] Furthermore, in the voltage application step S212, in order to allow sodium ions to enter the gate insulating film 42, it is preferable to apply a voltage corresponding to the film thickness T1 of the gate insulating film 42 to the gate insulating film 42 (or the gate conductive portion 44). In the voltage application step S212 of this example, a negative voltage, such as an electric field larger than 3.64 kV / μm, is applied to the gate conductive portion 44 per unit thickness of the gate insulating film 42. This makes the influence of sodium ions and the like on the threshold voltage more apparent.

[0060] Next, in the judgment step S214, the threshold voltage of the semiconductor element (semiconductor device 100 in this example) is measured, and the semiconductor element is judged to be qualified based on the measurement result. In the judgment step S214, the qualification of each semiconductor device 100 can be determined by comparing the measured threshold voltage with a preset reference value.

[0061] Next, in assembly step S216, the semiconductor device 100, which has been determined to be a qualified product, is used to assemble a semiconductor package. The semiconductor package may be a semiconductor module that includes a control circuit for controlling the semiconductor device 100 in addition to the semiconductor device 100. The semiconductor module may have a resin housing that houses the semiconductor device 100 and the control circuit.

[0062] Next, in the packaging and testing step S218, the semiconductor package is tested. The packaging and testing step S218 may include tests to assess the operation of the semiconductor device 100. In this example, a semiconductor device 100 that passes the threshold voltage test is used to assemble the semiconductor package. Therefore, the number of semiconductor packages deemed unqualified in the packaging and testing step S218 can be reduced, and the overall manufacturing cost can be reduced.

[0063] In this manufacturing method, the semiconductor device 100 is annealed and tested before the assembly step S216. The packaging and testing step S218 may not include testing items that heat the semiconductor package or semiconductor device 100 to above 100°C. The semiconductor package can be a semiconductor module or a discrete semiconductor device.

[0064] Figure 3 This is a diagram showing an example of the voltage-current characteristics measured in the judgment process S214. Figure 3 In the diagram, a single line represents a characteristic of a semiconductor device 100. In the determination process S214, the gate voltage Vge applied to the gate conductive portion 44 of the semiconductor device 100 is varied, and the main current Ic flowing through the semiconductor device 100 is measured. The main current Ic is, for example, the collector current of an IGBT or the drain current of a MOSFET.

[0065] The threshold voltage is the gate voltage Vge at which the main current Ic begins to flow. For example... Figure 3 As shown in the non-conforming group, if sodium ions are implanted into the gate insulating film 42, the main current Ic will begin to flow through a low gate voltage Vge. In the judgment process S214, this can be determined by measuring... Figure 3 The voltage-current characteristics shown are used to calculate the threshold voltage of each semiconductor device 100.

[0066] Figure 4This diagram illustrates the conditions in the voltage application step S212. In this example, an electric field is applied to the gate insulating film 42 while the multiple semiconductor devices 100 are at 175°C. Furthermore, an experiment was conducted to determine whether a defect could be detected in the judgment step S214 when various electric fields were applied with different applied electric fields. The circle in the judgment column indicates a condition where a defect could be detected in the judgment step S214 when the electric field application time is set to 0.2 seconds. Conversely, conditions marked with an cross in the judgment column indicate that even when the electric field application time is set to 15 minutes, a defect could not be detected in the judgment step S214.

[0067] like Figure 4 As shown, in the example where an electric field of 3.64 kV / μm was applied to the gate insulating film 42, the semiconductor device 100 failed to be screened in the judgment step S214. On the other hand, in the example where an electric field greater than 3.64 kV / μm was applied, the semiconductor device 100 was able to be screened in the judgment step S214. In the voltage application step S212, it is preferable to apply a voltage to the gate insulating film 42 that corresponds to an electric field greater than 3.64 kV / μm per unit thickness of the gate insulating film 42. In the voltage application step S212, a voltage that corresponds to an electric field of 4.55 kV / μm or more per unit thickness of the gate insulating film 42 can be applied to the gate insulating film 42. As an example, when the thickness T1 of the gate insulating film 42 is 110 nm, the voltage Vge applied to the gate insulating film 42 can be -50 V or more.

[0068] In the voltage application step S212, the temperature of the semiconductor device 100 can be 100°C or higher and 250°C or lower. The temperature can be 150°C or higher. The temperature can be 200°C or lower. In the voltage application step S212, the higher the temperature, the smaller the applied electric field can be.

[0069] In the voltage application step S212, the voltage application time can be 10 seconds or less. As described above, by setting an appropriate electric field, the semiconductor device 100 can be screened with a short application time. This improves manufacturing efficiency. The voltage application time can be 1 second or less. The voltage application time can be 0.1 seconds or more, or 0.2 seconds or more.

[0070] Furthermore, in the annealing process S210, the semiconductor substrate 10 can be annealed such that the average diffusion distance of sodium ions in the interlayer insulating film 38 is 70% or more of the thickness T2 of the interlayer insulating film 38. This facilitates the diffusion of sodium ions that have entered the interlayer insulating film 38 into the semiconductor substrate 10. In the annealing process S210, the semiconductor substrate 10 can be annealed such that the average diffusion distance is 85% or more of the thickness T2 of the interlayer insulating film 38, or it can be annealed such that the average diffusion distance is 100% or more of the thickness T2 of the interlayer insulating film 38.

[0071] Figure 5 This is a graph representing the average diffusion distance of sodium ions in the interlayer insulating film 38. Average diffusion distance x of sodium ions in interlayer insulating film 38 ave [cm 2 The following formula is given.

[0072] x ave = 2 × (Dt) 0.5

[0073] D = D0exp(-Q / kT)

[0074] Where t is time [s], and D is the diffusion coefficient [cm]. 2 / s], D0 is the diffusion constant [cm 2 / s], Q is the activation energy [eV], k is the Boltzmann constant, and T is the absolute temperature [K].

[0075] The diffusion constant D0 and activation energy Q are constants used for the target ion. In this example, the target ion is the sodium ion, and D0 = 3.4 × 10⁻⁶. -2 cm 2 / s, Q = 1.22eV.

[0076] exist Figure 5 In this example, the thickness T2 of the interlayer insulating film 38 is 1 μm. In this case, it is preferable to make the average diffusion distance x ave To achieve a metal electrode thickness of 0.7 μm or greater, at least one of the annealing temperature and annealing time of the semiconductor substrate 10 is adjusted. The annealing temperature can be 240°C or higher and 300°C or lower. Alternatively, the annealing temperature can be 260°C or higher, or 280°C or higher. By increasing the annealing temperature, the annealing time can be shortened, thereby improving manufacturing efficiency. Furthermore, by setting the annealing temperature to 300°C or lower, cracking of the metal electrode 52 can be prevented. The annealing temperature can also be 290°C or lower.

[0077] Figure 6 This diagram illustrates an example of the annealing conditions in annealing process S210. In this example, the thickness T2 of the interlayer insulating film 38 is 1 μm. Figure 6 In the decision column, circles indicate cases where the semiconductor device 100 can be screened in decision process S214, and crosses indicate cases where it cannot be screened. In decision process S214, the electric field application time is set to 0.2 seconds, and the electric field applied to the gate insulating film 42 is set to 4.55 [kV / μm].

[0078] like Figure 6 As shown, the boundary between the cases that can be screened and those that cannot be screened is the condition of an annealing temperature of 260℃ and an annealing time of 4 hours. (Refer to...) Figure 5 Under these conditions, the average diffusion distance of sodium ions is approximately 70% of the thickness T2 of the interlayer insulating film 38. As described above, in the annealing process S210, the annealing conditions can be set such that the ratio of the average diffusion distance of sodium ions in the interlayer insulating film 38 to the thickness T2 of the interlayer insulating film 38 is 70% or more, or such that the ratio is 85% or more, or such that the ratio is 100% or more.

[0079] Figure 7 This is a diagram illustrating an example of the gate voltage-main current characteristics of a semiconductor device 100. Figure 7 The characteristics of a qualified semiconductor device 100 are shown in the diagram. Among the characteristics of the qualified semiconductor device 100, the extension line of the rising current waveform (…) Figure 7 The voltage at which the dashed line (Vge) intersects the horizontal axis is set as the reference threshold voltage Vth. The reference threshold voltage Vth can be a preset value, such as the design value of the semiconductor device 100. The range from the reference threshold voltage Vth to 0V is set as the low current range.

[0080] In the judgment step S214, the threshold voltage of each semiconductor device 100 can be measured by varying the gate voltage Vge within a low current range. Through the annealing step S210 and the voltage application step S212, the threshold voltage of the defective semiconductor device 100 varies within a low current range. By measuring the threshold voltage within this range, threshold variations caused by sodium ions, etc., can be detected efficiently.

[0081] Figure 8 This diagram illustrates another example of a manufacturing method for the semiconductor device 100. In this example, a testing step S208 is performed after the plating step S204 and before the dicing step S206. That is, in the testing step S208, the semiconductor device 100 in its wafer state is tested. The content of each step is similar to... Figure 2 The examples are the same.

[0082] In the testing step S208, multiple semiconductor devices 100 within a semiconductor wafer can be tested in parallel. In the annealing step S210, by placing the semiconductor wafer into an annealing furnace, multiple semiconductor devices 100 can be annealed simultaneously.

[0083] In the voltage application step S212 and the judgment step S214, by contacting the probes with each semiconductor device 100, electrical tests can be performed on multiple semiconductor devices 100 in parallel. In this example, since multiple semiconductor devices 100 can be processed in parallel, the test time will not become too long even if the voltage application time in the voltage application step S212 is extended. The voltage application time in this example can be less than 20 minutes, less than 10 minutes, less than 5 minutes, or less than 1 minute. By extending the voltage application time, the influence of sodium ions, etc., on the threshold voltage can be made more apparent.

[0084] Figure 9 This is a circuit diagram illustrating an example of a circuit 200 disposed within the resin housing of a semiconductor module. Circuit 200 supplies power to loads such as motors. A semiconductor module may include multiple circuits 200. For example, a semiconductor module may be a three-phase inverter comprising three sets of circuits 200.

[0085] Circuit 200 includes one or more Figures 1 to 8 The semiconductor device 100 described herein. Figure 9 In this example, circuit 200 includes four semiconductor devices 100. For example... Figure 9 As shown, semiconductor devices 100-1 and 100-2 are connected in parallel to form the upper arm of the inverter. Semiconductor devices 100-3 and 100-4 are connected in parallel to form the lower arm of the inverter. The upper and lower arms are connected in series.

[0086] Circuit 200 may include gate terminals G, P, N, and output terminals. An external power supply is connected to the P and N terminals. The gate voltage of each semiconductor device 100 is controlled by input at gate terminal G. The output terminal is connected to the node between the upper and lower arms. Additionally, an external load is connected to the output terminal.

[0087] Figure 10 This is a top view illustrating an example of a semiconductor module 300. The semiconductor module 300 is a semiconductor package containing multiple semiconductor devices 100. The semiconductor module 300 includes a housing 88 and circuitry 200. The housing 88 houses the circuitry 200. The circuitry 200 can be mounted on the bottom surface 94 of the housing 88. The housing 88 is, for example, a resin housing formed of resin. In this example, the housing 88 houses three sets of... Figure 9The circuit 200 shown is an example of this. In this example, the semiconductor module 300 functions as a three-phase inverter.

[0088] The housing 88 has multiple main terminals 86 and multiple control terminals 99. The main terminals 86 serve as... Figure 9 The P-terminal, N-terminal, and output terminals function as follows. Control terminal 99 serves as... Figure 9 The gate terminal G in the semiconductor device 100 performs a function. The control terminal 99 may include a terminal for detecting the current flowing in each semiconductor device 100, a terminal for detecting the temperature of the semiconductor device 100, etc.

[0089] A circuit board 162 is mounted on the bottom surface 94 of the housing 88. A plurality of semiconductor devices 100 and wiring patterns are disposed on the circuit board 162. The wiring patterns connect the terminals, main terminals 86, and control terminals 99 of the semiconductor devices 100. In addition, wiring such as leads or lead frames connecting the nodes may be provided in the housing 88.

[0090] Below the housing 88, a cooling section for cooling the semiconductor module 300 can be configured. Figure 10 The cooling section is omitted. The housing 88 may have a through hole 84 for securing the semiconductor module 300 to the outside.

[0091] Figure 11 It means Figure 10 A diagram showing an example of the D-D' cross-section. The D-D' cross-section is a cross-section passing through semiconductor devices 100-2 and 100-4. As described above, a cooling section 114 is provided under the housing 88. A refrigerant such as water flows inside the cooling section 114. Cooling fins 95, used to increase the contact area with the refrigerant, can be provided inside the cooling section 114. The cooling fins 95 can be connected to the lower surface of the housing 88.

[0092] The housing 88 may have a recess 93 for accommodating the circuit 200. The interior of the recess 93 may be filled with a sealing material such as silicone gel to seal the circuit 200.

[0093] Figure 12 This is a cross-sectional view showing an example of a semiconductor discrete device 400. The semiconductor discrete device 400 is a semiconductor package that includes a semiconductor device 100. The semiconductor discrete device 400 in this example includes a sealing portion 101, one or more terminals 102, a connection portion 103, a connection portion 105, a connection portion 106, wiring 104, wiring 107, and a chip mounting portion 108.

[0094] The chip mounting portion 108 houses the semiconductor device 100. The chip mounting portion 108 can be electrically connected to electrodes formed on the lower surface of the semiconductor device 100 via the connecting portion 106. The chip mounting portion 108 can be formed of a conductive material such as copper. The chip mounting portion 108 can function as a terminal for electrical connection to external circuitry. Alternatively, the chip mounting portion 108 can be fixed to an external cooling device. The connecting portions 103, 105, and 106 are formed of a conductive material such as solder.

[0095] Terminal 102 is connected to each electrode of semiconductor device 100. For example, semiconductor discrete device 400 may have terminals 102 connected to a main electrode formed on the upper surface of semiconductor device 100, and terminals 102 connected to a control electrode formed on the upper surface of semiconductor device 100. The main electrode is, for example, the emitter electrode in an IGBT. The control electrode is, for example, the gate electrode in an IGBT.

[0096] Wiring 104 and wiring 107 electrically connect each terminal 102 to the semiconductor device 100. Wiring 104 and wiring 107 are, for example, wires or lead frames. In this example, wiring 104 is a lead frame and wiring 107 is a wire. Connector 103 connects wiring 104 to terminal 102. Connector 105 connects wiring 104 to the electrodes of the semiconductor device 100. Wiring 107 can be bonded to terminal 102 and electrodes of semiconductor device 100.

[0097] The sealing portion 101 seals the semiconductor device 100 in such a way that it prevents the semiconductor device 100 from being exposed to the outside. The sealing portion 101 is formed of an insulating material. The sealing portion 101 can be a resin such as epoxy resin or ceramic. The sealing portion 101 can seal the wiring 104 and wiring 107 in such a way that they are not exposed to the outside. The sealing portion 101 can also seal the individual terminals 102. However, the ends of the terminals 102 are exposed to the outside of the sealing portion 101. The sealing portion 101 can also seal the chip mount portion 108. The lower surface of the chip mount portion 108 may be exposed to the outside of the sealing portion 101.

[0098] As in Figure 8 As explained, after the semiconductor device 100 is tested through the testing process S208, the qualified semiconductor devices are assembled into semiconductor modules such as semiconductor module 300 or semiconductor discrete device 400. Therefore, the defect rate in the packaging and testing process S218 can be reduced, thereby reducing manufacturing costs.

[0099] The present invention has been described above using embodiments, but the technical scope of the present invention is not limited to the scope described in the above embodiments. It will be apparent to those skilled in the art that various modifications or improvements can be made to the above embodiments. As can be seen from the claims, such modifications or improvements can also be included within the technical scope of the present invention.

[0100] It should be noted that the execution order of actions, processes, steps, and stages in the apparatus, system, program, and method shown in the claims, specification, and drawings can be implemented in any order unless specifically stated as "earlier than" or "before," and unless the result of a previous process is used in a subsequent process. Even if terms such as "firstly" or "next" are used for convenience in describing the flow of actions in the claims, specification, and drawings, this does not mean that they must be implemented in this order.

Claims

1. A method for manufacturing a semiconductor device, characterized in that, include: The device formation process involves forming a semiconductor device including a gate insulating film on a semiconductor substrate and forming a metal electrode on top of the semiconductor substrate. The plating process involves plating the metal electrode. The annealing process involves annealing the semiconductor substrate. In the voltage application process, after the annealing process, a voltage corresponding to the thickness of the gate insulating film is applied to the gate insulating film; as well as The determination process involves measuring the threshold voltage of the semiconductor element after the voltage application process, and determining whether the semiconductor element is qualified based on the measurement result.

2. The method for manufacturing a semiconductor device according to claim 1, characterized in that, In the voltage application process, a voltage equivalent to an electric field greater than 3.64 kV / μm applied per unit thickness of the gate insulating film is applied to the gate insulating film.

3. The method for manufacturing a semiconductor device according to claim 1, characterized in that, In the voltage application process, a voltage equivalent to an electric field of 4.55 kV / μm or more per unit thickness of the gate insulating film is applied to the gate insulating film.

4. The method for manufacturing a semiconductor device according to any one of claims 1 to 3, characterized in that, In the voltage application process, the voltage application time is less than 10 seconds.

5. A method for manufacturing a semiconductor device according to any one of claims 1 to 3, characterized in that, In the voltage application process, the voltage application time is less than 1 second.

6. A method for manufacturing a semiconductor device according to any one of claims 1 to 3, characterized in that, In the device formation process, a gate conductive portion that is insulated from the semiconductor substrate by the gate insulating film is formed, and an interlayer insulating film that insulates the gate conductive portion from the metal electrode is formed. In the annealing process, the semiconductor substrate is annealed such that the average diffusion distance of sodium in the interlayer insulating film is more than 70% of the thickness of the interlayer insulating film.

7. The method for manufacturing a semiconductor device according to claim 6, characterized in that, In the device formation process, the gate insulating film is formed to cover the inner wall of a trench disposed on the upper surface of the semiconductor substrate, and the gate conductive portion is formed inside the trench at a position further inward than the gate insulating film.

8. A method for manufacturing a semiconductor device according to any one of claims 1 to 3, characterized in that, In the annealing process, the annealing temperature is above 240°C and below 300°C.

9. A method for manufacturing a semiconductor device according to any one of claims 1 to 3, characterized in that, The manufacturing method further includes: The assembly process uses the semiconductor components that have been determined to be qualified in the judgment process to assemble semiconductor packages.

10. A testing method, characterized in that, Testing a semiconductor device, the semiconductor device comprising: a semiconductor substrate on which a semiconductor element including a gate insulating film is formed, and a metal electrode formed on the semiconductor substrate and whose upper surface is plated. The testing method includes: The annealing process involves annealing the semiconductor substrate in its chip or wafer state before it is assembled into a semiconductor package. A voltage application step, following the annealing step, involves applying a voltage corresponding to the thickness of the gate insulating film to the gate insulating film; and The determination process involves measuring the threshold voltage of the semiconductor element after the voltage application process, and determining whether the semiconductor element is qualified based on the measurement result.

11. The test method according to claim 10, characterized in that, The semiconductor substrate includes: a gate conductive portion that is insulated from the semiconductor substrate by the gate insulating film, and an interlayer insulating film that insulates the gate conductive portion from the metal electrode.

Citation Information

Patent Citations

  • Semiconductor device and method for manufacturing semiconductor device

    JP2017157851A

  • Screening method of semiconductor device and semiconductor device

    JP2007327918A

  • Silicon carbide semiconductor device

    JP2018101796A