Composite negative electrode material, preparation method thereof and lithium ion battery

By preparing composite anode materials, including a core and a coating layer, the pulverization problem caused by the volume expansion of silicon anode materials was solved, achieving high-capacity, long-cycle-life, and low-expansion lithium-ion battery performance.

CN115172746BActive Publication Date: 2026-11-24BTR NEW MATERIAL GRP CO LTD +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202110363721.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-04-02
Publication Date
2026-11-24
Estimated Expiration
2041-04-02

AI Technical Summary

Technical Problem

Existing silicon anode materials suffer from significant volume expansion in lithium-ion batteries, leading to material pulverization, loss of electrical contact, and impact on electrochemical performance and cycle stability, making commercial application difficult.

Method used

The composite anode material is used, including a core and a coating layer. The core consists of primary particles and nanoparticle layers, with the nanoparticle layers forming micropores and mesopores. The coating layer is a carbon layer. It is prepared through in-situ reaction and dealloying heat treatment to form continuous channels and a stable structure.

Benefits of technology

It effectively alleviates volume expansion, improves conductivity and stability, enhances the safety and cycle life of lithium-ion batteries, and increases battery capacity and rate performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115172746B_ABST
    Figure CN115172746B_ABST
Patent Text Reader

Abstract

The application relates to the field of negative electrode materials, and provides a composite negative electrode material, a preparation method thereof and a lithium ion battery, the composite negative electrode material comprising a core and a coating layer located on the surface of the core; wherein the core comprises primary particles and a nanoparticle layer located on the surface of the primary particles; the primary particle comprises a skeleton, the skeleton comprises a main skeleton located in the interior of the primary particle and a plurality of branches extending from the main skeleton to the surface of the primary particle; and the nanoparticle layer is formed with micropores and / or mesopores. The composite negative electrode material, the preparation method thereof and the lithium ion battery provided by the application can effectively inhibit the volume expansion of the negative electrode material and improve the cycle performance of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of anode material technology, specifically to composite anode materials and their preparation methods, and lithium-ion batteries. Background Technology

[0002] Lithium-ion batteries are widely used in electric vehicles and consumer electronics due to their advantages such as high energy density, high output power, long cycle life, and low environmental pollution. To improve battery energy density, the research and development of silicon anode materials has become increasingly mature. However, silicon anode materials experience significant volume expansion (>300%) during lithium insertion / extraction. Furthermore, during charging and discharging, the silicon anode material can pulverize and fall off the current collector, causing a loss of electrical contact between the active material and the current collector. This results in deteriorated electrochemical performance, capacity decay, and decreased cycle stability, hindering commercial applications.

[0003] Therefore, there is an urgent need to develop a silicon anode material with low expansion rate and high cycle stability, as well as its preparation method. Summary of the Invention

[0004] In view of this, this application provides a composite anode material and its preparation method, and a lithium-ion battery, which can reduce the expansion rate of the anode material and improve the charge-discharge cycle performance of the anode material. The preparation method can reduce the preparation cost.

[0005] In a first aspect, this application provides a composite anode material, the composite anode material comprising a core and a coating layer located on the surface of the core; wherein,

[0006] The core includes primary particles and a nanoparticle layer on the surface of the primary particles; the primary particles include a framework, which includes a main framework located inside the primary particles and multiple branches extending from the main framework to the surface of the primary particles; the nanoparticle layer is formed with micropores and / or mesopores.

[0007] In the above scheme, the nanoparticle layer can effectively prevent material pulverization, alleviate material volume expansion, and ensure the structural stability of the primary particles inside the anode material. After coating, it has better conductivity and stability, can effectively prevent carbon from filling the internal pores of the material, improve the material's first efficiency, and enable the composite anode material to exhibit characteristics such as high capacity, long cycle life, high rate performance, and low expansion.

[0008] In one embodiment, the composite negative electrode material includes at least one of the following characteristics a to d:

[0009] a. The nanoparticle layer comprises multiple stacked nanoparticles;

[0010] b. The nanoparticles are selected from at least one of nano-silicon particles, nano-germanium particles, nano-antimony particles, nano-tin particles, and nano-boron particles;

[0011] c. The nanoparticle layer comprises a plurality of nanoparticles, wherein the median particle size of the nanoparticles is 20 nm to 200 nm;

[0012] d. The thickness of the nanoparticle layer is 20 nm to 2000 nm.

[0013] In one embodiment, the composite negative electrode material includes at least one of the following characteristics a to e:

[0014] a. The main framework is a three-dimensional mesh structure;

[0015] b. Each of the aforementioned branches is a separate grain.

[0016] c. Each of the branches is a separate grain, the size of which is 30nm-100nm;

[0017] d. The maximum width of the cross-section of the branch is 20nm-250nm, and the maximum length of the cross-section of the branch is 100nm-1500nm;

[0018] e. The branches are selected from at least one of rod-shaped nanoparticles, nanosheets, nanowires, and nanotubes.

[0019] Secondly, this application provides a composite anode material, the composite anode material comprising a core and a coating layer located on the surface of the core; wherein, the core comprises primary particles and a nanoparticle layer located on the surface of the primary particles; the nanoparticle layer is formed with micropores and / or mesopores;

[0020] The primary particle has a macroporous structure, and channels are formed inside the primary particle, which extend to the surface of the primary particle.

[0021] The pore structure of this negative electrode material, extending to the surface of the primary particles, offers the following advantages: First, it improves lithium storage performance while reducing lithium battery expansion. This not only alleviates volume expansion during lithium intercalation but also provides space for internal expansion during lithiation, allowing the electrode material to expand inwards after lithiation and reducing the overall electrode film thickness, thus significantly improving the safety of lithium-ion batteries. Second, it provides channels for electrolyte flow, facilitating electrolyte contact. The pore structure also results in higher tap density, increasing the battery's volumetric energy density.

[0022] In one embodiment, the diameter of the channel is 20 nm to 250 nm; the depth of the channel is 50 nm to 1000 nm; and / or

[0023] The pores account for 35% to 90% of the total volume of the pore structure, the mesopores account for 5% to 45% of the total volume of the pore structure, and the micropores account for 5% to 20% of the total volume of the pore structure.

[0024] In one embodiment, the composite negative electrode material includes at least one of the following characteristics a to d:

[0025] a. The porosity of the composite negative electrode material is 30% to 70%, wherein the porosity of the primary particles is 15% to 75%, and the porosity of the nanoparticle layer is 5% to 35%;

[0026] b. The ratio of the total porosity of mesopores to the total porosity of micropores in the nanoparticle layer is (2-10):1;

[0027] c. The proportion of open pore volume in all pore structures of the composite negative electrode material is 60% to 95%, and the proportion of closed pore volume is 5% to 40%.

[0028] d. Among all the openings in the pore structure, cross-linked pores account for 79% to 95% of the total volume of all openings, through-holes account for 4% to 20% of the total volume of all openings, and blind holes account for 1% to 10% of the total volume of all openings.

[0029] In one embodiment, the composite negative electrode material includes at least one of the following characteristics a to g:

[0030] a. The primary particles are selected from at least one of silicon, germanium, antimony, tin, and boron;

[0031] b. The median particle size of the primary particles is 0.1 μm to 10 μm;

[0032] c. The median particle size of the composite negative electrode material is 0.1 μm to 15 μm;

[0033] d. The specific surface area of ​​the composite negative electrode material is 1m². 2 / g~100m 2 / g;

[0034] e. The coating layer includes a carbon layer;

[0035] f. The coating layer includes a carbon layer, the thickness of which is 5 nm to 100 nm;

[0036] g. The carbon content in the composite anode material is 5% to 50% by mass.

[0037] Thirdly, this application provides a method for preparing a composite negative electrode material, comprising the following steps:

[0038] A coating layer is formed on the surface of the NM alloy to obtain an NM alloy containing the coating layer;

[0039] The NM alloy containing the coating layer was added to an ammonium salt solution for a redox reaction to obtain an intermediate;

[0040] The intermediate is subjected to dealloying heat treatment under a protective atmosphere, and the reaction product is acid-washed to obtain a composite negative electrode material. In the NM alloy, N includes at least one of silicon, germanium, antimony, tin, and boron, and M includes at least one of magnesium, aluminum, calcium, and zinc.

[0041] In the above-mentioned scheme, this application can prepare a composite anode material with two pore structures in one step through a simple in-situ reaction. The composite anode material is obtained by reacting the coated NM alloy with an ammonium salt solution and then heating it in a protective atmosphere. The morphology and pore structure of the composite anode material are easily controlled; the alloy composition can be controlled to change the pore size and porosity, and the pore depth can be controlled by the reaction time and temperature. The pores in the prepared anode material provide internal expansion space during lithium insertion / extraction and can also serve as channels for electrolyte flow. This improves lithium storage performance while reducing lithium battery expansion, which is beneficial for the inward expansion of the anode material after lithiation, thereby reducing the overall electrode film thickness and greatly improving the safety of lithium-ion batteries. The outer nanoparticle layer can effectively prevent material pulverization, alleviate volume expansion, and ensure the structural stability of the primary particles inside the anode material. After coating with the coating material, it has better conductivity and stability, effectively preventing carbon from filling the three-dimensional channels of the primary particles, improving the material's initial efficiency, and enabling the composite anode material to exhibit high capacity, long cycle life, high rate performance, and low expansion.

[0042] In one embodiment, the preparation method includes at least one of the following features a to d:

[0043] a. The method for forming the coating layer includes: forming a carbon layer on the surface of the NM alloy by coating with a carbon source;

[0044] b. The method for forming the coating layer includes: forming a carbon layer on the surface of the NM alloy by coating with a carbon source; the carbon source includes at least one of a gaseous carbon source and a solid carbon source, the gaseous carbon source includes at least one of methane, acetylene, acetone and alcohol; the solid carbon source includes at least one of calcium carbonate, lithium carbonate, iron carbonate, zinc carbonate and magnesium carbonate.

[0045] c. The thickness of the coating layer formed on the surface of the NM alloy is 5 nm to 100 nm;

[0046] d. The median grain size of the NM alloy is 0.1 μm to 15 μm.

[0047] In one embodiment, the preparation method includes at least one of the following features a to f:

[0048] a. The median grain size of the NM alloy containing the coating layer is 0.1 μm to 15 μm;

[0049] b. The ammonium salt includes at least one selected from ammonium fluoride, ammonium chloride, ammonium bromide, ammonium iodide, ammonium nitrate, ammonium carbonate, ammonium perchlorate, ammonium sulfate, and ammonium sulfide;

[0050] c. The mass concentration of the ammonium salt solution is 0.1 mol / L to 5 mol / L;

[0051] d. The molar ratio of the NM alloy containing the coating layer to the ammonium salt is 1:(0.1~2);

[0052] e. The redox reaction time between the NM alloy containing the coating layer and the ammonium salt solution is 0.5 h to 12 h;

[0053] f. The redox reaction temperature between the NM alloy containing the coating layer and the ammonium salt solution is 20℃~80℃.

[0054] In one embodiment, the preparation method includes at least one of the following features a to g:

[0055] a. The temperature of the dealloying heat treatment is 200℃~950℃;

[0056] b. The holding time for the dealloying heat treatment is 2h to 18h;

[0057] c. The heating rate of the dealloying heat treatment is 1℃ / min to 20℃ / min;

[0058] d. The protective atmosphere includes at least one of helium, neon, argon, krypton, and xenon;

[0059] e. The acid solution used for pickling includes at least one of hydrochloric acid, nitric acid, and sulfuric acid;

[0060] f. The mass concentration of the acid solution is 1 mol / L to 5 mol / L;

[0061] g. The pickling time is 1 hour to 10 hours.

[0062] Fourthly, this application provides a lithium-ion battery, the lithium-ion battery comprising the composite negative electrode material described above or a negative electrode material prepared by the method for preparing the composite negative electrode material. Attached Figure Description

[0063] Figure 1aThis is a schematic diagram of the structure of the composite negative electrode material provided in the embodiments of this application;

[0064] Figure 1b A schematic diagram of the structure of primary particles in the composite negative electrode material provided in the embodiments of this application;

[0065] Figure 1c This is a schematic diagram of the structure of the nanoparticle layer in the composite anode material provided in the embodiments of this application;

[0066] Figure 2 A flowchart illustrating the preparation method of the composite anode material provided in the embodiments of this application;

[0067] Figure 3 Scanning electron microscope (SEM) images of the silicon-carbon composite anode material provided in the embodiments of this application;

[0068] Figure 4 XRD pattern of silicon-carbon composite anode material provided in the embodiments of this application;

[0069] Figure 5 The cycling performance curve of the silicon-carbon composite anode material provided in the embodiments of this application is shown. Detailed Implementation

[0070] The following are preferred embodiments of the present application. It should be noted that those skilled in the art can make several improvements and modifications without departing from the principles of the embodiments of the present application, and these improvements and modifications are also considered to be within the protection scope of the embodiments of the present application.

[0071] Currently, in lithium-ion batteries, the anode material is one of the key materials affecting its charge-discharge performance. Existing anode materials are graphite-based carbon materials, but their theoretical lithium storage capacity is only 372 mAh / g, which cannot meet the demand for high-energy-density materials. Silicon, as a lithium-ion battery anode material, has a very high theoretical capacity (approximately 4200 mAh / g). However, silicon anode materials experience significant volume expansion (>300%) during lithium insertion / extraction, making them prone to pulverization and falling off the current collector during charge-discharge cycles. This results in a loss of electrical contact between the active material and the current collector, leading to deteriorated electrochemical performance. Therefore, the large volume change effect easily leads to poor cycle stability, hindering commercial application.

[0072] To improve the cycle stability of lithium-ion batteries, this application provides a composite anode material.

[0073] Specifically, such as Figure 1aAs shown, the composite negative electrode material includes a core and a coating layer 30 located on the surface of the core; wherein, the core includes primary particles 10 and a nanoparticle layer 20 located on the surface of the primary particles 10; the primary particles 10 include a framework, which includes a main framework 11 located inside the primary particles and a plurality of branches 12 extending from the primary particle 10 to the surface of the primary particles 10; the nanoparticle layer 20 is formed with micropores and / or mesopores.

[0074] Please refer to further information. Figure 1b The primary particle 10 has a macroporous structure, with channels 13 formed inside the primary particle, extending to the surface of the primary particle. According to the definition of the International Union of Pure and Applied Chemistry (IUPAC), pores with a diameter greater than 50 nm are called macropores.

[0075] In this embodiment, the main skeleton 11 inside the primary particle and the multiple branches 12 extending to the surface of the primary particle are integrated into a whole. The entire skeleton structure enhances the electron transfer and ion diffusion of the material, which can effectively release the stress after lithiation and avoid stress concentration at the grain boundaries, which can lead to material cracking and pulverization.

[0076] The pore structure of this composite anode material, extending to the surface of the primary particles, offers the following advantages: First, it improves lithium storage performance while reducing lithium battery expansion. This not only alleviates volume expansion during lithium intercalation but also provides space for internal expansion during lithiation, allowing the electrode material to expand inward after lithiation and reducing the overall electrode film thickness, thus significantly improving the safety of lithium-ion batteries. Second, it provides channels for electrolyte flow, facilitating electrolyte contact.

[0077] The nanoparticle layer, composed of nanoparticles, effectively prevents material pulverization. The nanoparticle layer forms micropores and / or mesopores, which effectively mitigate volume expansion, promote electrolyte wetting and contact surfaces, accelerate lithium-ion transport, and improve the overall rate performance of the material, while ensuring the structural stability of the primary particles within the anode material. After coating, it exhibits better conductivity and stability, effectively preventing carbon from filling the internal pores of the material, improving the material's initial efficiency, and enabling the composite anode material to exhibit high capacity, long cycle life, high rate performance, and low expansion.

[0078] In some implementations, the main framework is a three-dimensional mesh structure;

[0079] In some embodiments, each branch is a separate grain; there are no obvious grain boundaries between the branch and the main framework, and the surface of the primary particle is dispersed with grains. In the prior art, the branches on the porous silicon secondary particles are mainly composed of multiple small grains with many grain boundaries. Compared with this structure, in this embodiment, the branch on the primary particle is a single large grain with few grain boundaries. After lithiation, the stress can be better dispersed, avoiding stress concentration that could lead to material damage. At the same time, the crystal plane curves of a single grain are the same, which is more conducive to reducing the relative volume expansion of the material in a certain direction. In contrast, the structure composed of multiple small grains has a relatively large volume expansion and relatively poor structural stability, resulting in poor cycle stability.

[0080] Specifically, the grain size is 30nm-100nm; for example, the grain size can be 30nm, 45nm, 50nm, 60nm, 75nm, or 100nm.

[0081] Please continue reading. Figure 1b The maximum width 12W of the cross-section of branch 12 is 20nm to 250nm, and the maximum length 12L of the cross-section of branch 12 is 100nm to 1500nm.

[0082] For example, the maximum width 12W of the cross-section of branch 12 can be 20nm, 40nm, 80nm, 100nm, 120nm, 150nm, 180nm, 200nm or 250nm, and the maximum length 12L of the cross-section of branch 12 can be 100nm, 200nm, 300nm, 400nm, 500nm, 800nm, 1000nm, 1200nm or 1500nm, and is not limited here.

[0083] In some embodiments, the branches are selected from at least one of rod-shaped nanoparticles, nanosheets, nanowires, and nanotubes.

[0084] In some embodiments, the diameter of the pore 13 is measured to be 10 nm-150 nm using a mercury porosimetry method; the depth of the pore is 50 nm-1500 nm. For example, the pore diameter can specifically be 10 nm, 50 nm, 60 nm, 80 nm, 100 nm, or 150 nm, and is not limited thereto. The depth of the pore 13 can specifically be 50 nm, 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, 800 nm, or 1000 nm, and is not limited thereto. The pore depth can be changed by controlling the reaction time and reaction temperature (generally, the longer the reaction time and the higher the reaction temperature, the deeper the pore).

[0085] In some embodiments, the primary particles are selected from at least one of silicon, germanium, tin, boron, and antimony; their framework can be a silicon framework, germanium framework, tin framework, boron framework, antimony framework, etc.; if the primary particles are selected from silicon materials, the primary particles include a silicon framework, including a main framework located inside the primary particle and multiple branches of the self-framework extending to the surface of the primary particle. The framework structures of germanium, boron, tin, and antimony are similar to the silicon framework structures described above.

[0086] like Figure 1c As shown, the nanoparticle layer 20 includes multiple nanoparticles 21 stacked on top of each other. The shape of the nanoparticles 21 can be spherical, quasi-spherical, flat, or any other arbitrary shape, and is not limited herein. Micropores 22 and / or mesopores 23 are formed before the nanoparticles 21. The pore size of the micropores is less than 2 nm, and the pore size of the mesopores is greater than 2 nm and less than 50 nm. Understandably, the pore sizes of the micropores and mesopores are smaller than the pore size of the primary particle channels.

[0087] In some embodiments, the nanoparticles are selected from at least one of nano-silicon particles, nano-germanium particles, nano-antimony particles, nano-tin particles, and nano-boron particles.

[0088] In some embodiments, the porosity of the composite negative electrode material is 30% to 70%, specifically 30%, 40%, 50%, 60% or 70%, which is not limited here. The porosity of the composite negative electrode material is preferably 40% to 60%.

[0089] In some embodiments, the porosity of the primary particles 10 is 15% to 75%, specifically 15%, 20%, 35%, 40%, 50%, 60% or 75%, and is not limited here.

[0090] In some embodiments, the porosity of the nanoparticle layer is 5% to 35%, specifically 5%, 10%, 15%, 20%, 25%, 30%, or 35%. In this embodiment, the ratio of the total porosity of mesopores to the total porosity of micropores in the nanoparticle layer is (2-10):1. Understandably, the number of mesopores in the nanoparticle layer is greater than the number of micropores. A greater number of mesopores than micropores facilitates the flow of electrolyte.

[0091] Understandably, nanoparticles 21 are formed on the surface of primary particles 10 and are tightly bonded to primary particles 10 to form nanoparticle layer 20. There are obvious grain boundaries between nanoparticle layer 20 and primary particles 10. They are not bonded by van der Waals forces, but by higher bonding forces. The connection between primary particles 10 and nanoparticle layer 20 is more stable, and the overall structure is more stable.

[0092] More specifically, the pores account for 35% to 90% of the total volume of the pore structure, the mesopores account for 5% to 45% of the total volume of the pore structure, and the micropores account for 5% to 20% of the total volume of the pore structure.

[0093] In all the above-mentioned pore structures, the volume ratio of open pores is 60% to 95%, and the volume ratio of closed pores is 5% to 40%. Among them, the open pores can be classified into cross-linked pores, through pores, and blind pores according to the pore structure type. In all pore structures, cross-linked pores account for 79% to 95% of the total volume of all open pores, through pores account for 4% to 20% of the total volume of all open pores, and blind pores account for 1% to 10% of the total volume of all open pores.

[0094] It should be noted that blind pores are conductive holes that connect the surface and inner layers of primary particles without penetrating the primary particles, while cross-linked pores are formed by the intersection of multiple channels. Understandably, a higher proportion of cross-linked pores provides channels for electrolyte flow, allowing the electrolyte to circulate within the primary particles along these pores. This improves the lithium storage performance of silicon while reducing lithium battery expansion. Through pores also provide fluid channels for the electrolyte, but they reduce the electrolyte flow rate. Therefore, the volume percentage of through pores should be less than that of cross-linked pores. Furthermore, blind pores hinder electrolyte flow; electrolyte flowing into a blind pore can only flow out along the same path. Therefore, the formation of blind pores should be minimized during the manufacturing process.

[0095] In some embodiments, the median particle size of nanoparticles 21 is 20 nm to 200 nm; specifically, the median particle size of nanoparticles 21 can be 20 nm, 40 nm, 50 nm, 60 nm, 80 nm, 100 nm, 150 nm, or 200 nm. Of course, the median particle size of nanoparticles 21 can also be set according to actual conditions and is not limited here. Small-diameter nanoparticles 21 are coated on the surface of primary particles, which can avoid carbon layer filling and clogging of pores, increase the channels for electrolyte flow, thereby improving the silicon lithium storage performance while reducing the expansion of lithium batteries.

[0096] In some embodiments, the thickness of the nanoparticle layer 20 is 20nm to 2000nm, specifically 20nm, 50nm, 100nm, 200nm, 300nm, 500nm, 800nm, 1000nm or 2000nm, etc. Of course, the thickness of the nanoparticle layer 20 can also be set according to the actual situation, and is not limited here.

[0097] Understandably, a nanoparticle layer 20 of appropriate thickness can effectively prevent material pulverization, alleviate material volume expansion, and ensure the structural stability of primary particles inside the silicon material.

[0098] In some embodiments, the median particle size of the primary particles 10 is 0.1 μm to 10 μm, specifically 0.1 μm, 0.3 μm, 0.5 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 5 μm or 10 μm. Preferably, the median particle size of the primary particles 10 is 0.3 μm to 5 μm, but this is not limited here.

[0099] In some embodiments, the median particle size of the composite anode material is 0.1 μm to 15 μm. Optionally, it can be 0.1 μm, 0.5 μm, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, or 15 μm, etc., and is not limited thereto. The median particle size of the composite anode material is preferably 0.5 μm to 10 μm, and more preferably 1 μm to 8 μm.

[0100] In some embodiments, the specific surface area ratio of the composite negative electrode material is 1m². 2 / g~100m 2 / g. Optionally, the specific surface area of ​​the composite negative electrode material can be 1m². 2 / g、5m 2 / g, 10m 2 / g, 15m 2 / g、20m 2 / g、25m 2 / g、30m 2 / g、35m 2 / g、40m 2 / g、45m 2 / g, 50m 2 / g、60m 2 / g、80m 2 / g or 100m 2 / g, etc., are not limited here; the specific surface area of ​​the composite negative electrode material is preferably 10m². 2 / g~50m 2 / g. Understandably, an excessively large specific surface area easily leads to SEI film formation, excessive consumption of irreversible lithium salt, and reduced initial battery efficiency. Considering the cost of the fabrication process, the specific surface area is controlled at 10m². 2 / g~50m 2 / g.

[0101] In some embodiments, the coating layer in the composite anode material is a carbon layer with a thickness of 5nm to 100nm, specifically 5nm, 10nm, 20nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, or 100nm. If the carbon layer is too thick, the lithium-ion transport efficiency will be reduced, which is not conducive to the high-rate charge and discharge of the material and will reduce the overall performance of the anode material. If the carbon layer is too thin, it will not be conducive to increasing the conductivity of the anode material and the performance of suppressing the volume expansion of the material will be weak, resulting in a long-cycle performance-price difference.

[0102] In some embodiments, the carbon content in the composite anode material is 5% to 50% by mass, specifically 5%, 8%, 10%, 15%, 20%, 25%, 30%, 40%, or 50%, and is not limited thereto. Optionally, the carbon content is 10% to 30% by mass.

[0103] In this article, "dealloying" refers to a method of selectively removing one or more components from an alloy through chemical or electrochemical corrosion processes. The dealloying process involves the removal of old lattice sites and the formation of new lattice sites, as well as the nucleation and growth of new crystals. The formation of nanoporous structures during dealloying is closely related to the atomic-level recombination at the alloy / solution interface. This recombination process is accomplished through surface diffusion of undissolved metal atoms and vacancies, and the rate of surface diffusion significantly influences the size of the ligaments / channels in the final nanoporous metal.

[0104] When the coating layer is a carbon layer, one embodiment of a method for preparing a composite negative electrode material is as follows: Figure 2 As shown, the method includes the following steps S100 to S400:

[0105] S100, preparation of NM alloy;

[0106] S200, A coating layer is formed on the surface of the NM alloy to obtain an NM alloy containing a coating layer;

[0107] S300. The NM alloy containing the coating layer is added to an ammonium salt solution to carry out a redox reaction to obtain an intermediate.

[0108] S400. The intermediate is subjected to dealloying heat treatment under a protective atmosphere, and the reaction product is acid-washed to obtain a composite negative electrode material, wherein N in the NM alloy includes at least one of silicon, germanium, antimony, tin, and boron, and M in the NM alloy includes at least one of magnesium, aluminum, calcium, and zinc.

[0109] In this scheme, a composite anode material with two pore structures can be prepared in one step through a simple in-situ reaction. The carbon-coated NM alloy is reacted with a cheap and common ammonium salt solution to obtain an intermediate. Then, it is de-alloyed at high temperature in a protective atmosphere. During the de-alloying process, the active metal in the NM alloy is reacted, thereby forming a nanoparticle layer on the surface of the NM alloy, and finally obtaining the composite anode material. The obtained anode material has channels, mesopores and micropores at the same time, and the morphology and pore structure are easy to control. The alloy composition can be controlled to change the pore size and porosity, and the pore depth can be controlled by the reaction time and reaction temperature.

[0110] The primary particles obtained by dealloying the inner NM alloy have continuous, interconnected channels. These continuous channels provide pore size for internal expansion during the lithiation process and also provide channels for electrolyte flow, improving the lithium storage performance of the anode material while reducing the expansion of the lithium battery. The generated nanoparticle layer forms mesopores and micropores, which can prevent material pulverization and alleviate volume expansion, ensuring the structural stability of the anode material. Using carbon-coated NM alloy as a raw material can avoid the later carbon coating from blocking the pore structure, improving the battery's initial efficiency.

[0111] This method yields a composite anode material comprising a core and a coating layer located on the surface of the core; wherein,

[0112] The core includes primary particles and a nanoparticle layer on the surface of the primary particles; the primary particles include a framework, which includes a main framework located inside the primary particles and multiple branches extending from the main framework to the surface of the primary particles; the nanoparticle layer is formed with micropores and / or mesopores.

[0113] The preparation method is explained in detail below:

[0114] S100, used to prepare NM alloys;

[0115] In some embodiments, N in the NM alloy includes at least one of Si, Ge, Sn, B, and Sb; M in the NM alloy includes at least one of Mg, Al, Zn, and Ca. Specific examples include Si-Mg alloys, Si-Al alloys, Ge-Mg alloys, Ge-Al alloys, etc. Different types of alloys can yield branches of different shapes, including at least one of rod-shaped nanoparticles, nanosheets, nanowires, and nanotubes.

[0116] In some embodiments, the NM alloy is prepared by mixing N powder and active metal M and then heating and reacting them under a protective gas to obtain the NM alloy.

[0117] The particle size of the N powder is 0.1μm to 15μm, specifically it can be 0.1μm, 0.5μm, 1μm, 3μm, 5μm, 8μm, 10μm or 15μm, etc., and is not limited here.

[0118] The particle size of the active metal M powder is 0.1μm to 80μm, specifically 0.1μm, 5μm, 10μm, 20μm, 40μm, 50μm or 80μm, etc., which is not limited here.

[0119] The molar ratio of nitrogen powder to active metal M is 1:(1~3), specifically 1:1, 1:1.5, 1:2, 1:2.5 or 1:3, which is not limited here.

[0120] The temperature for the heating reaction is 400℃ to 900℃, specifically 400℃, 500℃, 600℃, 700℃, 800℃ or 900℃.

[0121] The holding time for the heating reaction is 2h to 8h, specifically 2h, 4h, 6h or 8h, and is not limited here.

[0122] The heating rate of the reaction is 1℃ / min to 10℃ / min, specifically 1℃ / min, 3℃ / min, 5℃ / min, 8℃ / min or 10℃ / min, and is not limited here.

[0123] In this application, by controlling parameters such as silicon powder particle size, active metal particle size, reaction temperature, and reaction time, it is beneficial to the formation of NM alloy and to improve the doping uniformity of metal elements in NM alloy.

[0124] Of course, NM alloys can also be prepared by other methods, such as high-energy ball milling, vacuum smelting, and hot pressing sintering. It is understood that NM alloys can be obtained commercially, in which case step S100 can be omitted.

[0125] In some embodiments, the mass percentage content of N in the NM alloy is 15% to 60%. Optionally, the mass percentage content of N can be 15%, 20%, 30%, 40%, 50%, or 60%, and is not limited thereto. In specific embodiments, the NM alloy can be at least one of silicon-magnesium alloy, silicon-aluminum alloy, silicon-calcium alloy, and silicon-zinc alloy. Understandably, the pore size and porosity of the N material can be changed by controlling the composition of the NM alloy; generally, the higher the N content in the NM alloy, the smaller the pore size. The pore depth can be changed by controlling the heating reaction time and reaction temperature; generally, the longer the reaction time and the higher the reaction temperature, the deeper the pores.

[0126] In a specific embodiment, the method further includes:

[0127] The obtained NM alloy is pulverized to adjust the particle size of the NM alloy powder to 0.1μm to 15μm, specifically 0.1μm, 0.5μm, 1μm, 2μm, 5μm, 10μm or 15μm, which is not limited here.

[0128] Specifically, the pulverizing equipment includes at least one of a planetary ball mill, a sand mill, and an air jet mill. Understandably, the smaller the particle size of the NM alloy, the larger its specific surface area, allowing for a more complete reaction during dealloying heat treatment.

[0129] Of course, NM alloys can also be prepared by other methods, such as high-energy ball milling, vacuum smelting, and hot pressing sintering.

[0130] It is understandable that NM alloys can be obtained commercially, in which case step S100 can be omitted.

[0131] Step S200: A coating layer is formed on the surface of the NM alloy to obtain an NM alloy containing a coating layer;

[0132] In this embodiment, a carbon layer is formed on the surface of the NM alloy by vapor deposition using a carbon source gas under a protective gas atmosphere. The carbon source gas used includes at least one of methane, acetylene, acetone, and alcohol. In other embodiments, a carbon layer can also be formed on the surface of the NM alloy using liquid-phase coating and solid-phase coating methods. The solid-phase carbon source includes at least one of calcium carbonate, lithium carbonate, iron carbonate, zinc carbonate, and magnesium carbonate.

[0133] When using vapor deposition, the protective gas used in the vapor deposition process includes at least one of helium, neon, argon, krypton, and xenon.

[0134] The volume ratio of carbon source gas to protective gas is 1:(0.1~100), specifically 1:0.1, 1:10, 1:20, 1:40, 1:60, 1:80 or 1:100.

[0135] The carbon source gas introduction time is 5 min to 60 min, specifically 5 min, 15 min, 25 min, 35 min, 45 min or 60 min. Of course, it can also be set according to the actual situation, and there is no limitation here.

[0136] The flow rate of the carbon source gas is 0.1L / min to 2L / min, specifically 0.1L / min, 0.5L / min, 0.8L / min, 0.8L / min, 1.5L / min or 2L / min. Of course, it can also be set according to the actual situation, and there is no limitation here.

[0137] The temperature for vapor deposition is 400℃ to 950℃, specifically 400℃, 500℃, 600℃, 700℃, 800℃, 900℃ or 950℃. Of course, it can also be set according to the actual situation, and there is no limitation here.

[0138] The heating rate is 1℃ / min to 20℃ / min, specifically 1℃ / min, 5℃ / min, 10℃ / min, 15℃ / min or 20℃ / min, thereby effectively improving the reaction efficiency.

[0139] It should be noted that within the aforementioned suitable range of carbon source introduction time or flow rate, vapor deposition temperature, and heating rate, it helps to improve the uniform deposition of carbon layers on the surface of NM alloys.

[0140] When using solid-phase coating, the molar mass ratio of solid carbon source to NM alloy is 2:(1-10), specifically 2:1, 2:3, 2:5, 2:7, 2:8, 2:9 or 2:10. Of course, it can also be set according to the actual situation, and no limit is made here.

[0141] The reaction temperature between the solid carbon source and the NM alloy is 500℃~1000℃, specifically 500℃, 600℃, 700℃, 800℃, 900℃ or 1000℃. Of course, it can also be set according to the actual situation, and there is no limitation here.

[0142] In this embodiment, the thickness of the carbon layer formed on the surface of the NM alloy is 5nm to 100nm, specifically 5nm, 10nm, 20nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm or 100nm, etc., and the deposition thickness of the carbon layer can be controlled according to the deposition time.

[0143] The median grain size of carbon-coated NM alloys is 0.1μm to 15μm, specifically 0.1μm, 0.5μm, 1μm, 2μm, 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, 10μm or 15μm, etc., which are not limited here.

[0144] In step S300, the NM alloy containing the coating layer is added to an ammonium salt solution to carry out a redox reaction to obtain an intermediate.

[0145] In this embodiment, the ammonium salt includes at least one selected from ammonium fluoride, ammonium chloride, ammonium bromide, ammonium iodide, ammonium nitrate, ammonium carbonate, ammonium perchlorate, ammonium sulfate, and ammonium sulfide. The mass concentration of the ammonium salt solution is 0.1 mol / L to 5 mol / L, specifically 0.1 mol / L, 0.5 mol / L, 1 mol / L, 1.5 mol / L, 2 mol / L, 2.5 mol / L, 3 mol / L, 4 mol / L, or 5 mol / L, and can be set according to actual conditions.

[0146] Optionally, the molar ratio of the NM alloy containing the coating layer to the ammonium salt is 1:(0.1~2), specifically 1:0.1, 1:0.5, 1:0.8, 1:1, 1:1.5 or 1:2, etc.

[0147] The redox reaction time of NM alloy with ammonium salt solution is 0.5h to 12h, specifically 0.5h, 1h, 2h, 3h, 6h, 9h, 10h or 12h, and the redox reaction temperature is 20℃ to 80℃, specifically 20℃, 40℃, 50℃, 60℃, 70℃ or 80℃.

[0148] For example, when the NM alloy is a Si-M alloy, the carbon-coated Si-M alloy is immersed in an ammonium salt solution. After the Si-M alloy reacts with the ammonium salt solution, a layer of silicic acid is formed on the surface of the Si-M alloy. The chemical formula of the reaction is shown below:

[0149] MSi+NH4Y+H2O→H2SiO3+MY+NH3+H2

[0150] For example, when a silicon-magnesium alloy is placed in an ammonium chloride solution, silicic acid, magnesium chloride, ammonia, and hydrogen are generated on the surface of the silicon-magnesium alloy. It should be noted that the silicic acid adheres to the surface of the silicon-magnesium alloy in the form of colloidal particles, precipitates, or gels. Further drying treatment causes silicic acid nanoparticles to adhere to the surface of the silicon-magnesium alloy.

[0151] In step S400, the intermediate is subjected to dealloying heat treatment under a protective atmosphere, and the reaction product is post-treated to obtain the composite anode material.

[0152] To illustrate, for example, when the NM alloy is a Si-M alloy, during the dealloying process, the active metal vapor evaporated from the Si-M alloy reacts with silicic acid, causing the silicic acid to reduce the nano-silicon particles in situ at high temperature. The nano-silicon particles stack up to form a nanoparticle layer, which has micropores and / or mesopores. That is, the silicic acid nanoparticles react with the active metal vapor to form oxides. After removing the oxides, the nanoparticle layer can form micropores or mesopores.

[0153] The chemical formula for the reaction is shown below:

[0154] M + H₂SiO₃ → Si + MO + H₂O

[0155] To ensure the mixture reacts fully, the dealloying heat treatment temperature is 200℃~950℃, specifically 200℃, 300℃, 400℃, 600℃, 800℃ or 950℃, and the holding time is 2h~18h, specifically 2h, 3h, 6h, 9h, 12h, 15h or 18h, which is not limited here.

[0156] The heating rate of dealloying heat treatment is 1℃ / min to 20℃ / min, specifically 1℃ / min, 5℃ / min, 10℃ / min, 15℃ / min or 20℃ / min, thereby effectively improving the reaction efficiency.

[0157] To improve the safety of the reaction, the dealloying heat treatment is carried out under the protection of an inert gas, which includes at least one of helium, neon, argon, krypton, and xenon. The flow rate of the inert gas can be controlled between 1 L / min and 10 L / min.

[0158] Understandably, within the aforementioned suitable range of temperature, time, and heating rate for heat treatment, it helps to improve dealloying efficiency, facilitates the formation of a framework structure in the Si-M alloy during the dealloying process, and helps to form a nanoparticle layer on the surface of the Si-M alloy.

[0159] In a specific embodiment, pickling involves using an acid solution to wash the reaction products, thereby removing the metal oxides in the reaction products. In one feasible embodiment, the acid solution used for pickling includes at least one of hydrochloric acid, nitric acid, and sulfuric acid.

[0160] The mass concentration of the acid solution is 1 mol / L to 5 mol / L, specifically 1 mol / L, 2 mol / L, 3 mol / L, 4 mol / L, or 5 mol / L. Of course, the mass concentration of the acid solution can be adjusted according to actual needs; no specific limit is imposed here.

[0161] The pickling time is 1 hour to 10 hours, specifically 1 hour, 3 hours, 5 hours, 7 hours, or 10 hours. In this embodiment, the pickling product can still be recycled.

[0162] Understandably, within the aforementioned suitable concentration and pickling time range of the acid solution, it is helpful to improve pickling efficiency and reduce impurities in the negative electrode material.

[0163] In this embodiment, a silica layer is formed on the surface of the Si-M alloy by reacting it with an ammonium salt solution. During the high-temperature dealloying process, the metal vapor of the active metal in the Si-M alloy reacts with the silica, causing the silica to be reduced in situ to nano-silicon particles at high temperature. These nano-silicon particles form a nanoparticle layer with micropores and / or mesopores. This results in a negative electrode material with a pore structure of various pore sizes, and the pore size of the silicon material surface layer is smaller than that of the inner layer, thereby alleviating the volume expansion of silicon, effectively inhibiting material pulverization, and enhancing structural stability. The prepared composite negative electrode material can also effectively improve the stability of lithium battery charge-discharge cycles, and has multiple advantages such as high capacity, long cycle life, high rate performance, and low expansion.

[0164] This application also provides a lithium-ion secondary battery negative electrode sheet and a lithium-ion secondary battery, using the composite negative electrode material provided in the above embodiments of this application or the negative electrode material prepared by the method of the composite negative electrode material provided in the above embodiments of this application.

[0165] The embodiments of this application will be further described below with reference to several examples. However, the embodiments of this application are not limited to the specific embodiments described below. Appropriate modifications can be made within the scope of the main claims.

[0166] Example 1

[0167] A method for preparing a composite anode material includes the following steps:

[0168] (1) Silicon powder with a particle size of 1 μm and magnesium powder are mixed evenly at a molar ratio of 1:2 and then placed in an atmosphere furnace. Under the protection of argon inert gas, the mixture is heated to 600°C at a heating rate of 3°C / min and held for 6 hours to allow it to react fully and obtain a silicon-magnesium alloy. The silicon-magnesium alloy is ball-milled to obtain silicon-magnesium alloy powder with a particle size of 1 μm.

[0169] (2) Place the silicon-magnesium alloy powder into a rotary atmosphere furnace and heat it to 500°C at a heating rate of 3°C / min under the protection of argon atmosphere. Then, introduce 0.5L / min of acetylene gas so that the volume ratio of argon to acetylene in the rotary atmosphere furnace is 9:1. After holding at the temperature for 30 minutes, turn off the acetylene gas and cool to obtain carbon-coated silicon-magnesium alloy powder.

[0170] (3) Take 1 mol of carbon-coated silicon-magnesium alloy powder and add it to 1 L of ammonium chloride solution. The concentration of the ammonium chloride solution is 1 mol / L. React for 1 h under water bath conditions at 60℃. After filtration and drying, the intermediate is obtained.

[0171] (4) The intermediate was placed in an argon atmosphere and heated to 700°C at a heating rate of 3°C / min and held for 8 hours to allow it to react fully and obtain the reaction product.

[0172] (5) The reaction product was mechanically stirred and acid-washed in 1 mol / L hydrochloric acid solution for 2 h, and then filtered, washed and dried to obtain the composite negative electrode material.

[0173] After testing, the median particle size of the obtained composite anode material was 1.2 μm, the carbon mass percentage content was 15%, and the specific surface area was 45 m². 2 / g, carbon layer thickness is 50nm. The porosity of the obtained composite anode material is 55%, the porosity of the primary particles is 40%, the porosity of the nanoparticle layer is 25%, the ratio of total mesopore porosity to total micropore porosity in the nanoparticle layer is 4:1, the open pore volume accounts for about 80% of the total pore structure, and the closed pore volume accounts for about 20%; the maximum cross-sectional width of the branches is about 40nm, and the thickness of the nanoparticle layer is 100nm.

[0174] Figure 3 These are scanning electron microscope images of the composite anode material. Figure 4 The XRD pattern of the composite anode material provided in this embodiment; Figure 5 This is the cycle performance curve of the porous silicon anode material in this embodiment, with a charge / discharge current of 0.5C. From... Figure 3 The scanning electron microscope images show that the fabricated porous silicon has a distinct porous structure, with a carbon layer coating its surface. Figure 4 The XRD pattern shows that the three strong peaks at 28.4°, 47.3° and 56.1° correspond to the three strong peaks of silicon (JCPDS No. 27-1402), indicating that there are basically no impurities. Figure 5 As can be seen, the material has excellent cycling performance, retaining a capacity of 997 mAh / g after 1000 cycles at a high current of 0.5C.

[0175] Example 2

[0176] (1) Mix 2μm silicon powder and magnesium powder at a molar ratio of 1:2 and place them in an atmosphere furnace. Under the protection of argon inert gas, heat to 650℃ at a heating rate of 3℃ / min and hold for 5h to allow them to react fully and obtain silicon-magnesium alloy. Ball mill the silicon-magnesium alloy to obtain 1.5μm silicon-magnesium alloy powder.

[0177] (2) Place the silicon-magnesium alloy powder into a rotary atmosphere furnace and heat it to 600°C at a heating rate of 3°C / min under the protection of argon atmosphere. Then, introduce acetylene gas at a rate of 0.5 L / mind so that the volume ratio of argon to acetylene in the rotary atmosphere furnace is 9:1. After holding at the temperature for 30 min, turn off the acetylene gas and cool to obtain carbon-coated silicon-magnesium alloy powder.

[0178] (3) Take 1 mol of carbon-coated silicon-magnesium alloy powder and add it to 1 L of ammonium chloride solution. The concentration of the ammonium chloride solution is 1 mol / L. React for 2 h under water bath conditions at 60℃. After filtration and drying, the intermediate is obtained.

[0179] (4) The intermediate was placed in an argon atmosphere and heated to 650°C at a heating rate of 1°C / min and held for 6 hours to allow it to react fully and obtain the reaction product.

[0180] (5) The reaction product was mechanically stirred and acid-washed in 1 mol / L hydrochloric acid solution for 2 h, and then filtered, washed and dried to obtain the composite negative electrode material.

[0181] After testing, the median particle size of the obtained composite anode material was 1.8 μm, the carbon mass percentage content was 16%, and the specific surface area was 55 m². 2 / g, with a carbon layer thickness of 53nm. The resulting composite anode material has a porosity of 55%, with the primary particles having a porosity of 35% and the nanoparticle layer having a porosity of 23%. The ratio of the total mesopore porosity to the total micropore porosity in the nanoparticle layer is 5:1. The open pore volume accounts for approximately 83% of the total pore structure, while the closed pore volume accounts for approximately 17%. The maximum cross-sectional width of the branches is approximately 35nm, and the thickness of the nanoparticle layer is 150nm.

[0182] Example 3

[0183] (1) After mixing 2μm silicon powder and aluminum powder at a molar ratio of 1:2, the mixture was placed in an atmosphere furnace and heated to 650℃ at a heating rate of 5℃ / min under the protection of argon inert gas. The mixture was then held for 5h to allow it to react fully and obtain a silicon-aluminum alloy. The silicon-magnesium alloy was ball-milled to obtain 3μm silicon-magnesium alloy powder.

[0184] (2) Place the silicon-magnesium alloy powder into a rotary atmosphere furnace and heat it to 600°C at a heating rate of 3°C / min under the protection of argon atmosphere. Then, introduce acetylene gas at a rate of 0.5 L / mind so that the volume ratio of argon to acetylene in the rotary atmosphere furnace is 9:1. After holding at the temperature for 30 min, turn off the acetylene gas and cool to obtain carbon-coated silicon-magnesium alloy powder.

[0185] (3) Take 1 mol of carbon-coated silicon-magnesium alloy powder and add it to 1 L of ammonium chloride solution. The concentration of the ammonium chloride solution is 0.5 mol / L. React for 1 h under water bath conditions at 60℃. After filtration and drying, the intermediate is obtained.

[0186] (4) The intermediate was placed in an argon atmosphere and heated to 650°C at a heating rate of 3°C / min and held for 6 hours to allow it to react fully and obtain the reaction product.

[0187] (5) The reaction product was mechanically stirred and acid-washed in 1 mol / L hydrochloric acid solution for 2 h, and then filtered, washed and dried to obtain the composite negative electrode material.

[0188] After testing, the median particle size of the obtained composite anode material was 3.5 μm, the carbon mass percentage content was 15%, and the specific surface area was 40 m². 2 / g, with a carbon layer thickness of 80nm. The resulting composite anode material has a porosity of 45%, with the primary particles having a porosity of 36% and the nanoparticle layer having a porosity of 27%. The ratio of the total mesopore porosity to the total micropore porosity in the nanoparticle layer is 5:1. The open pore volume accounts for approximately 83% of the total pore structure, while the closed pore volume accounts for approximately 17%. The maximum cross-sectional width of the branches is approximately 50nm, and the thickness of the nanoparticle layer is 50nm.

[0189] Example 4

[0190] (1) Mix 2μm silicon powder and aluminum powder at a molar ratio of 1:2 and place them in an atmosphere furnace. Under the protection of argon inert gas, heat to 650℃ at a heating rate of 3℃ / min and hold for 5h to allow them to react fully and obtain silicon-magnesium alloy. Ball mill the silicon-magnesium alloy to obtain 1μm silicon-aluminum alloy powder.

[0191] (2) Place the silicon-magnesium alloy powder into a rotary atmosphere furnace and heat it to 650°C at a heating rate of 3°C / min under the protection of argon atmosphere. Then, introduce 0.5L / mind of acetylene gas so that the volume ratio of argon to acetylene in the rotary atmosphere furnace is 9:1. After holding at the temperature for 30min, turn off the acetylene gas and cool to obtain carbon-coated silicon-magnesium alloy powder.

[0192] (3) Take 1 mol of carbon-coated silicon-magnesium alloy powder and add it to 1 L of ammonium chloride solution. The concentration of the ammonium chloride solution is 5 mol / L. React for 2 h under water bath conditions at 60℃. After filtration and drying, the intermediate is obtained.

[0193] (4) The intermediate was placed in an argon atmosphere and heated to 650°C at a heating rate of 3°C / min and held for 6 hours to allow it to react fully and obtain the reaction product.

[0194] (5) The reaction product was mechanically stirred and acid-washed in 1 mol / L hydrochloric acid solution for 2 h, and then filtered, washed and dried to obtain the composite negative electrode material.

[0195] After testing, the median particle size of the obtained composite anode material was 1.5 μm, the carbon mass percentage content was 18%, and the specific surface area was 90 m². 2 / g, with a carbon layer thickness of 50nm. The resulting composite anode material has a porosity of 45%, with the primary particles having a porosity of 30% and the nanoparticle layer having a porosity of 15%. The ratio of the total porosity of mesopores to the total porosity of micropores in the nanoparticle layer is 8:1. The open pore volume accounts for approximately 81% of the total pore structure, while the closed pore volume accounts for approximately 19%. The maximum cross-sectional width of the branches is approximately 30nm, and the thickness of the nanoparticle layer is 500nm.

[0196] Example 5

[0197] (1) Silicon powder with a particle size of 1 μm and magnesium powder are mixed evenly at a molar ratio of 1:2 and then placed in an atmosphere furnace. Under the protection of argon inert gas, the mixture is heated to 600°C at a heating rate of 3°C / min and held for 6 hours to allow it to react fully and obtain a silicon-magnesium alloy. The silicon-magnesium alloy is ball-milled to obtain silicon-magnesium alloy powder with a particle size of 1 μm.

[0198] (2) Place the silicon-magnesium alloy powder into a rotary atmosphere furnace and heat it to 500°C at a heating rate of 3°C / min under the protection of argon atmosphere. Then, introduce 0.5L / min of acetylene gas so that the volume ratio of argon to acetylene in the rotary atmosphere furnace is 9:1. After holding at the temperature for 60min, turn off the acetylene gas and cool to obtain carbon-coated silicon-magnesium alloy powder.

[0199] (3) Take 1 mol of carbon-coated silicon-magnesium alloy powder and add it to 1 L of ammonium chloride solution. The concentration of the ammonium chloride solution is 1 mol / L. React for 1 h under water bath conditions at 60℃. After filtration and drying, the intermediate is obtained.

[0200] (4) The intermediate was placed in an argon atmosphere and heated to 700°C at a heating rate of 3°C / min and held for 8 hours to allow it to react fully and obtain the reaction product.

[0201] (5) The reaction product was mechanically stirred and acid-washed in 1 mol / L hydrochloric acid solution for 2 h, and then filtered, washed and dried to obtain the composite negative electrode material.

[0202] After testing, the median particle size of the obtained composite anode material was 1.2 μm, the carbon mass percentage content was 20%, and the specific surface area was 50 m². 2 / g, carbon layer thickness is 100nm. The porosity of the obtained composite anode material is 55%, the porosity of the primary particles is 40%, the porosity of the nanoparticle layer is 25%, the ratio of total mesopore porosity to total micropore porosity in the nanoparticle layer is 4:1, the open pore volume accounts for about 80% of the total pore structure, and the closed pore volume accounts for about 20%; the maximum cross-sectional width of the branches is about 40nm, and the thickness of the nanoparticle layer is 100nm.

[0203] Example 6

[0204] (1) Silicon powder with a particle size of 1 μm and magnesium powder are mixed evenly at a molar ratio of 1:2 and then placed in an atmosphere furnace. Under the protection of argon inert gas, the mixture is heated to 600°C at a heating rate of 3°C / min and held for 6 hours to allow it to react fully and obtain a silicon-magnesium alloy. The silicon-magnesium alloy is ball-milled to obtain silicon-magnesium alloy powder with a particle size of 1 μm.

[0205] (2) Place the silicon-magnesium alloy powder into a rotary atmosphere furnace and heat it to 500°C at a heating rate of 3°C / min under the protection of argon atmosphere. Then, introduce 0.5L / min of acetylene gas so that the volume ratio of argon to acetylene in the rotary atmosphere furnace is 9:1. After holding at the temperature for 30 minutes, turn off the acetylene gas and cool to obtain carbon-coated silicon-magnesium alloy powder.

[0206] (3) Take 1 mol of carbon-coated silicon-magnesium alloy powder and add it to 1 L of ammonium chloride solution. The concentration of the ammonium chloride solution is 1 mol / L. React for 12 h under water bath conditions at 90℃. After filtration and drying, the intermediate is obtained.

[0207] (4) The intermediate was placed in an argon atmosphere and heated to 800°C at a heating rate of 3°C / min and held for 8 hours to allow it to react fully and obtain the reaction product.

[0208] (5) The reaction product was mechanically stirred and acid-washed in 1 mol / L hydrochloric acid solution for 2 h, and then filtered, washed and dried to obtain the composite negative electrode material.

[0209] After testing, the median particle size of the obtained composite anode material was 1.6 μm, the carbon mass percentage content was 20%, and the specific surface area was 30 m². 2 / g, carbon layer thickness is 50nm. The porosity of the obtained composite anode material is 55%, the porosity of the primary particles is 40%, the porosity of the nanoparticle layer is 32%, the ratio of total mesopore porosity to total micropore porosity in the nanoparticle layer is 4:1, the open pore volume accounts for about 80% of the total pore structure, and the closed pore volume accounts for about 20%; the maximum cross-sectional width of the branches is about 40nm, and the thickness of the nanoparticle layer is 100nm.

[0210] Example 7

[0211] (1) Silicon powder with a particle size of 1 μm and magnesium powder are mixed evenly at a molar ratio of 1:2 and then placed in an atmosphere furnace. Under the protection of argon inert gas, the mixture is heated to 600°C at a heating rate of 3°C / min and held for 6 hours to allow it to react fully and obtain a silicon-magnesium alloy. The silicon-magnesium alloy is ball-milled to obtain silicon-magnesium alloy powder with a particle size of 1 μm.

[0212] (2) Place the silicon-magnesium alloy powder into a rotary atmosphere furnace and heat it to 500°C at a heating rate of 3°C / min under the protection of argon atmosphere. Then, introduce 0.5L / min of acetylene gas so that the volume ratio of argon to acetylene in the rotary atmosphere furnace is 9:1. After holding at the temperature for 30 minutes, turn off the acetylene gas and cool to obtain carbon-coated silicon-magnesium alloy powder.

[0213] (3) Take 1 mol of carbon-coated silicon-magnesium alloy powder and add it to 1 L of ammonium chloride solution. The concentration of the ammonium chloride solution is 1 mol / L. React for 1 h under water bath conditions at 60℃. After filtration and drying, the intermediate is obtained.

[0214] (4) The intermediate was placed in an argon atmosphere and heated to 1000°C at a heating rate of 3°C / min and held for 8 hours to allow it to react fully and obtain the reaction product.

[0215] (5) The reaction product was mechanically stirred and acid-washed in 1 mol / L hydrochloric acid solution for 2 h, and then filtered, washed and dried to obtain the composite negative electrode material.

[0216] After testing, the median particle size of the obtained composite anode material was 1.3 μm, the carbon mass percentage content was 20%, and the specific surface area was 30 m². 2 / g, carbon layer thickness is 50nm. The porosity of the obtained composite anode material is 50%, the porosity of the primary particles is 65%, the porosity of the nanoparticle layer is 22%, the ratio of total mesopore porosity to total micropore porosity in the nanoparticle layer is 4:1, the open pore volume accounts for about 80% of the total pore structure, and the closed pore volume accounts for about 20%; the maximum cross-sectional width of the branches is about 60nm, and the thickness of the nanoparticle layer is 70nm.

[0217] Example 8

[0218] (1) After mixing germanium powder with a particle size of 1 μm and magnesium powder at a molar ratio of 1:2, the mixture was placed in an atmosphere furnace and heated to 650°C at a heating rate of 3°C / min under the protection of argon inert gas. The mixture was then held for 8 hours to allow it to react fully and obtain a germanium-magnesium alloy. The germanium-magnesium alloy was ball-milled to obtain germanium-magnesium alloy powder with a particle size of 1 μm.

[0219] (2) Place the germanium-magnesium alloy powder into a rotary atmosphere furnace and heat it to 500°C at a heating rate of 3°C / min under the protection of argon atmosphere. Then, introduce 0.5L / min of acetylene gas so that the volume ratio of argon to acetylene in the rotary atmosphere furnace is 9:1. After holding the temperature for 30 minutes, turn off the acetylene gas and cool to obtain carbon-coated germanium-magnesium alloy powder.

[0220] (3) Take 1 mol of carbon-coated germanium-magnesium alloy powder and add it to 1 L of ammonium chloride solution. The concentration of the ammonium chloride solution is 1 mol / L. React for 2 h under water bath conditions at 60℃. After filtration and drying, the intermediate is obtained.

[0221] (4) The intermediate was placed in an argon atmosphere and heated to 1000°C at a heating rate of 3°C / min and held for 8 hours to allow it to react fully and obtain the reaction product.

[0222] (5) The reaction product was mechanically stirred and acid-washed in 1 mol / L hydrochloric acid solution for 2 h, and then filtered, washed and dried to obtain the composite negative electrode material.

[0223] After testing, the median particle size of the obtained composite anode material was 1.3 μm, the carbon mass percentage content was 21%, and the specific surface area was 31 m². 2 / g, with a carbon layer thickness of 40nm. The resulting composite anode material has a porosity of 52%, with the primary particles having a porosity of 64% and the nanoparticle layer having a porosity of 23%. The ratio of the total mesopore porosity to the total micropore porosity in the nanoparticle layer is 4:1. The open pore volume accounts for approximately 81% of the total pore structure, while the closed pore volume accounts for approximately 19%. The maximum cross-sectional width of the branches is approximately 62nm, and the thickness of the nanoparticle layer is 73nm.

[0224] Comparative Example 1

[0225] (1) Silicon powder with a particle size of 1 μm and magnesium powder are mixed evenly at a molar ratio of 1:2 and then placed in an atmosphere furnace. Under the protection of argon inert gas, the mixture is heated to 600°C at a heating rate of 3°C / min and held for 6 hours to allow it to react fully and obtain a silicon-magnesium alloy. The silicon-magnesium alloy is ball-milled to obtain silicon-magnesium alloy powder with a particle size of 1 μm.

[0226] (2) Place the silicon-magnesium alloy powder into a rotary atmosphere furnace and heat it to 500°C at a heating rate of 3°C / min under the protection of argon atmosphere. Then, introduce 0.5L / min of acetylene gas so that the volume ratio of argon to acetylene in the rotary atmosphere furnace is 9:1. After holding at the temperature for 30 minutes, turn off the acetylene gas and cool to obtain carbon-coated silicon-magnesium alloy powder.

[0227] (3) The carbon-coated silicon-magnesium alloy powder was placed in an argon atmosphere and heated to 700°C at a heating rate of 3°C / min, and then kept at the temperature for 8 hours to allow it to react fully and obtain the reaction product.

[0228] (4) The reaction product was mechanically stirred and acid-washed in 1 mol / L hydrochloric acid solution for 2 h, and then filtered, washed and dried to obtain the composite negative electrode material.

[0229] After testing, the median particle size of the obtained composite anode material was 1.4 μm, the carbon mass percentage content was 20%, and the specific surface area was 15 m². 2 / g, with a carbon layer thickness of 50nm. The resulting composite anode material has a porosity of 70%, with open pores accounting for approximately 70% of the total pore volume and closed pores accounting for approximately 30%; the maximum diameter of the nano-silicon framework unit is approximately 65nm.

[0230] Comparative Example 2

[0231] (1) Silicon powder with a particle size of 1 μm and magnesium powder are mixed evenly at a molar ratio of 1:2 and then placed in an atmosphere furnace. Under the protection of argon inert gas, the mixture is heated to 600°C at a heating rate of 3°C / min and held for 6 hours to allow it to react fully and obtain a silicon-magnesium alloy. The silicon-magnesium alloy is ball-milled to obtain silicon-magnesium alloy powder with a particle size of 1 μm.

[0232] (2) Place the silicon-magnesium alloy powder into a rotary atmosphere furnace and heat it to 500°C at a heating rate of 3°C / min under the protection of argon atmosphere. Then, introduce 0.5L / min of acetylene gas so that the volume ratio of argon to acetylene in the rotary atmosphere furnace is 9:1. After holding at the temperature for 30 minutes, turn off the acetylene gas and cool to obtain carbon-coated silicon-magnesium alloy powder.

[0233] (3) Take 1 mol of carbon-coated silicon-magnesium alloy powder and add it to 1 L of ammonium chloride solution. The concentration of the ammonium chloride solution is 10 mol / L. React for 12 h under water bath conditions at 100℃. The intermediate is obtained after filtration and drying.

[0234] (4) The intermediate was placed in an argon atmosphere and heated to 700°C at a heating rate of 3°C / min and held for 8 hours to allow it to react fully and obtain the reaction product.

[0235] (5) The reaction product was mechanically stirred and acid-washed in 1 mol / L hydrochloric acid solution for 2 h, and then filtered, washed and dried to obtain the composite negative electrode material.

[0236] After testing, the median particle size of the obtained composite anode material was 1.8 μm, the carbon mass percentage content was 25%, and the specific surface area was 45 m². 2 / g, carbon layer thickness is 50nm. The porosity of the obtained composite anode material is 55%, the porosity of the primary particles is 40%, the porosity of the nanoparticle layer is 7%, the ratio of total mesopore porosity to total micropore porosity in the nanoparticle layer is 1.8:1, the open pore volume accounts for approximately 58% and the closed pore volume accounts for approximately 42% of all pore structures; the maximum cross-sectional width of the branches is approximately 40nm, and the thickness of the nanoparticle layer is 200nm.

[0237] Comparative Example 3

[0238] The composite anode material is Si / C, with a median particle size of 1.5 μm. The core of the composite material is a porous silicon structure composed of stacked nano-silicon particles, and the outer shell is encapsulated by a carbon layer. The carbon content is 22% by mass, and the specific surface area is 38 m². 2 / g, the carbon layer thickness is 50nm, and the porosity of the composite anode material is 67%. That is.

[0239] Performance testing:

[0240] (1) Observation of the microstructure of composite negative electrode material powder particles:

[0241] The surface condition of the material was characterized by observing the microstructure of powder using a scanning electron microscope. The selected instrument was an OXFORD EDS (X-max-20mm2), with an accelerating voltage of 10KV and the focal length adjusted. The observation magnification ranged from 50K for high-magnification observation and from 500 to 2000 for low-magnification observation, mainly to observe particle agglomeration.

[0242] (2) Particle size test:

[0243] Add approximately 0.02g of powder sample to a 50ml clean beaker, add approximately 20ml of deionized water, and then add a few drops of 1% surfactant to completely disperse the powder in the water. Sonicate the mixture in a 120W ultrasonic cleaner for 5 minutes and test the particle size distribution using a MasterSizer 2000.

[0244] (3) Method for testing the diameter of the skeleton:

[0245] Twenty negative electrode material cores were randomly selected using SEM to test the diameter and length of the framework and the size of the branches.

[0246] (4) Test method for carbon content in negative electrode materials:

[0247] The sample is heated at high temperature in a high-frequency furnace under oxygen-enriched conditions, causing carbon and sulfur to oxidize into carbon dioxide and sulfur dioxide. This gas is then processed and enters a corresponding absorption cell, where it absorbs the corresponding infrared radiation, which is then converted into a corresponding signal by a detector. This signal is sampled by a computer, linearly corrected, and converted into a value proportional to the concentrations of carbon dioxide and sulfur dioxide. The values ​​from the entire analysis process are then accumulated. After analysis, this accumulated value is divided by the weight value in the computer, multiplied by a correction factor, and the blank is subtracted to obtain the carbon percentage in the sample. The sample was tested using a high-frequency infrared carbon-sulfur analyzer (Shanghai Dekai HCS-140).

[0248] (5) Test method for specific surface area of ​​negative electrode material:

[0249] After measuring the amount of gas adsorbed on the solid surface at different relative pressures under constant temperature and low temperature, the amount of monolayer adsorption of the sample is obtained based on the Brownnor-Etter-Taylor adsorption theory and its formula (BET formula), thereby calculating the specific surface area of ​​the solid.

[0250] (6) Porosity test:

[0251] The porosity of the negative electrode material and negative electrode sheet was tested using the gas displacement method. Calculation method: P = (V - V0) / V * 100%, where V0 is the true volume and V is the apparent volume, representing the percentage of the sample pore volume to the total area.

[0252] (7) Cross-sectional testing of negative electrode materials:

[0253] The cross-sectional polishing instrument uses an ion source to ionize inert gas to generate inert ions. After acceleration and focusing, the high-speed inert ions bombard atoms or molecules on the sample surface, achieving ion polishing. After CP cutting, the sample is placed on a dedicated SEM stage for SEM testing. The instrument model is IB-09010CP, with an ion acceleration voltage of 2-6kV and using argon gas. By cutting the silicon-carbon anode material through cross-section testing, the thickness of the nanoparticle layer and the carbon layer can be measured.

[0254] The negative electrode materials prepared using Examples 1-8 and Comparative Examples 1-3 are numbered S1-S8 and R1-R3. The negative electrode materials are mixed with sodium carboxymethyl cellulose, styrene-butadiene rubber, conductive graphite (KS-6) and carbon black (SP) in a ratio of 92:2:2:2:2 to form a slurry. The slurry is uniformly coated onto copper foil and dried to form a negative electrode sheet. The negative electrode sheet is assembled into a button cell in an argon atmosphere glove box. The separator used is a polypropylene microporous membrane. The electrolyte used is 1 mol / L lithium hexafluorophosphate (the solvent is a mixture of ethylene carbonate, methyl ethyl carbonate and dimethyl carbonate). The counter electrode used is a lithium metal sheet.

[0255] The discharge specific capacity of the above 11 groups of batteries was tested on the Landian CT2001A battery testing system. The ratio of the discharge capacity to the battery capacity in 1 hour is the discharge specific capacity.

[0256] The first coulombic efficiency test was conducted on the above 11 groups of batteries on the Blue Electric CT2001A battery testing system. The charge and discharge current was 0.05C, and the first coulombic efficiency was measured.

[0257] The above 11 groups of batteries were subjected to a 100-cycle test on the Blue Electric CT2001A battery testing system with a charge / discharge current of 0.2C. After 100 cycles, the battery capacity and capacity retention rate after each cycle were calculated.

[0258] The capacity retention rate after 100 cycles at 0.2C is calculated as: discharge capacity of the 100th cycle / discharge capacity of the first cycle * 100%. The results are shown in Table 1.

[0259] Table 1. Comparison of Parameter Performance of Various Anode Materials

[0260]

[0261]

[0262] Table 2. Comparison of Parameter Performance of Various Batteries

[0263]

[0264] As can be seen from Tables 1 and 2 above, the main difference between Example 4 and Example 1 is that the ammonium chloride concentration is higher and the soaking time is longer, resulting in more silica particles generated on the surface of the carbon-coated silicon-magnesium alloy. This leads to a thicker nano-silicon particle layer in the final product, a reduction in mesopores and micropores in the nano-silicon particle layer, and less electrolyte flow into the primary particles in the inner layer. Consequently, the electrode expansion rate increases and the cycle stability deteriorates during the charging and discharging process of the battery.

[0265] Compared to Example 1, the negative electrode material of Comparative Example 1 was not soaked in ammonium chloride solution during preparation. As a result, no silica particles were generated on the surface of the silicon-magnesium alloy. Consequently, the final product consisted only of a carbon layer and primary particles. The carbon particles in the carbon layer easily blocked the pore structure of the primary particles, which led to an increase in the electrode expansion rate and a decrease in cycle stability during the charging and discharging process.

[0266] The main difference between Comparative Example 2 and Example 1 is that the ammonium chloride concentration is higher, the immersion temperature is higher, and the immersion time is longer, resulting in more silica particles generated on the surface of the carbon-coated silicon-magnesium alloy. This results in a thicker nano-silicon particle layer in the final product, a reduction in mesopores and micropores in the nano-silicon particle layer, and less electrolyte flow into the primary particles in the inner layer. Consequently, the electrode expansion rate increases and the cycle stability deteriorates during the charging and discharging process of the battery.

[0267] Comparative Example 3 is a carbon-coated porous silicon anode material. The battery made of this material showed a decrease in both capacity and capacity retention after 100 cycles at 0.2C, and the electrode film expansion rate of Comparative Example 3 was also higher than that of Example 1.

[0268] As can be seen from the above embodiments and comparative examples, the nanoparticle layer on the surface of the primary particles of the anode material of this application has excellent mesopores and micropores. This effectively avoids material pulverization, and after lithiation, a rigid silicon-lithium alloy layer is formed, further suppressing the volume expansion of the primary particles and ensuring the structural stability of the porous silicon. During lithiation, the expansion of silicon intercalation fills the mesopores, which can further prevent electrolyte solvent molecules from contacting the primary particles and forming side reactions, generating more SEI, and resulting in lower first-cycle efficiency. Furthermore, the pore structure on the primary particles is structurally different from the mesopores and micropores of the nanoparticle layer, which can further alleviate the stress generated by the volume expansion of porous silicon, reduce electrode film expansion, improve safety, avoid material structure damage, ensure material structural stability, and bring about a long cycle life. After the carbon layer encapsulates the silicon material, it has better conductivity and stability. By adopting the order of first encapsulating carbon and then reacting to prepare porous materials, it can effectively avoid carbon filling or closing the pore structure, reducing the material's first-cycle efficiency, and even triggering side reactions. Therefore, the composite anode material is beneficial to meeting the requirements of long cycle life, high capacity, and low expansion of batteries, and can be widely used in the field of lithium-ion battery anode materials.

[0269] In summary, the method for preparing the composite anode material provided in this application is simple and easy to operate, and the preparation process is safe and efficient; the manufacturing cost is effectively reduced, making it suitable for mass production; the obtained product, when used as a battery electrode, has good charge-discharge cycle performance.

[0270] Although this application discloses preferred embodiments as described above, it is not intended to limit the claims. Any person skilled in the art can make several possible changes and modifications without departing from the concept of this application. Therefore, the scope of protection of this application should be determined by the scope defined in the claims of this application.

Claims

1. A composite negative electrode material, characterized by, The composite anode material includes a core and a coating layer located on the surface of the core, wherein the coating layer includes a carbon layer; wherein, The core includes primary particles and a layer of nanoparticles on the surface of the primary particles; the primary particles include a framework, which includes a main framework located inside the primary particles and multiple branches extending from the main framework to the surface of the primary particles, the main framework being a three-dimensional network structure, and each branch being an individual grain; the primary particles have channels formed inside them, which extend to the surface of the primary particles. The nanoparticle layer has micropores and / or mesopores, and the porosity of the nanoparticle layer is 10% to 35%; the nanoparticles are selected from at least one of nano-silicon particles, nano-germanium particles, nano-antimony particles, nano-tin particles, and nano-boron particles.

2. The composite negative material of claim 1, wherein, The composite anode material includes at least one of the following characteristics a to c: a. The nanoparticle layer comprises multiple stacked nanoparticles; b. The nanoparticle layer comprises a plurality of nanoparticles, wherein the median particle size of the nanoparticles is 20 nm to 200 nm; c. The thickness of the nanoparticle layer is 20nm~2000nm.

3. The composite negative electrode material according to claim 1 or 2, characterized in that, The composite anode material includes at least one of the following characteristics a to c: a. The size of the grains is 30nm-100nm; b. The maximum width of the cross-section of the branch is 20nm-250nm, and the maximum length of the cross-section of the branch is 100nm-1500nm; c. The branches are selected from at least one of rod-shaped nanoparticles, nanosheets, nanowires, and nanotubes.

4. The negative electrode material according to claim 1, characterized in that, The primary particles have a macroporous structure.

5. The negative electrode material according to claim 4, characterized in that, The diameter of the channel is 20nm~250nm; the depth of the channel is 50nm~1000nm; and / or The pores account for 35% to 90% of the total volume of all pore structures, the mesopores account for 5% to 45% of the total volume of all pore structures, and the micropores account for 5% to 20% of the total volume of all pore structures.

6. The composite negative electrode material according to any one of claims 1 to 5, characterized in that, The composite anode material includes at least one of the following characteristics a to d: a. The porosity of the composite negative electrode material is 30%~70%, wherein the porosity of the primary particles is 15%~75%; b. The ratio of the total porosity of mesopores to the total porosity of micropores in the nanoparticle layer is (2~10):1; c. In the composite negative electrode material, the open pore volume accounts for 60%~95% and the closed pore volume accounts for 5%~40% of all pore structures; d. Among all the openings in the pore structure, cross-linked pores account for 79% to 95% of the total volume of all openings, through-holes account for 4% to 20% of the total volume of all openings, and blind holes account for 1% to 10% of the total volume of all openings.

7. The composite negative electrode material according to any one of claims 1 to 6, characterized in that, The composite anode material includes at least one of the following characteristics a to f: a. The primary particles are selected from at least one of silicon, germanium, antimony, tin, and boron; b. The median particle size of the primary particles is 0.1µm to 10µm; c. The median particle size of the composite negative electrode material is 0.1µm~15µm; d. The specific surface area of the composite negative electrode material is 1 m 2 / g~100 m 2 / g; e. The thickness of the carbon layer is 5 nm to 100 nm; f. The carbon content in the composite anode material is 5% to 50% by mass.

8. A lithium-ion battery, characterized in that, Includes the composite anode material as described in any one of claims 1 to 7.

Citation Information

Patent Citations

  • Honeycomb silicon and carbon composite material and preparation method and application thereof