Nitride semiconductor substrate, semiconductor element, and method for manufacturing nitride semiconductor substrate
By sputtering and annealing AlN thin films on sapphire substrates, the problems of numerous crystal defects and uneven surfaces in AlN thin films in the prior art are solved, and high-quality nitride semiconductor substrates are realized, which are suitable for high-efficiency ultraviolet light-emitting devices.
Patent Information
- Application Number
- CN202180016240.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-02-27
- Filing Date
- 2021-02-26
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2041-02-26
AI Technical Summary
Existing technologies make it difficult to grow high-quality AlN films on sapphire substrates, resulting in numerous crystal defects and uneven surfaces, as well as large half-widths of X-ray diffraction rocking curves, requiring further high crystallinity.
An AlN thin film was deposited on a sapphire substrate by sputtering and annealed at a temperature above 1500℃. The film thickness was controlled to be below 10000 nm, the through dislocation density to be below 2×10⁸ cm⁻², the oxygen concentration to be above 10¹⁸ cm⁻³ and below 10²¹ cm⁻³, and the hydrogen concentration to be above 10¹⁶ cm⁻³ and below 2×10¹⁷ cm⁻³.
High-quality nitride semiconductor substrates were achieved, reducing through-dislocation density and improving crystallinity and surface flatness, thus meeting the requirements of high-efficiency ultraviolet light-emitting devices.
Smart Images

Figure CN115176049B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to nitride semiconductor substrates, semiconductor devices, and methods for manufacturing nitride semiconductor substrates. Background Technology
[0002] Group III nitride semiconductors such as aluminum nitride (AlN), aluminum gallium nitride (AlGaN), and aluminum gallium indium nitride (AlGaInN) have attracted much attention as materials for optical semiconductor devices such as ultraviolet light-emitting elements.
[0003] For example, AlN has a very wide bandgap among semiconductor materials, enabling it to efficiently extract ultraviolet light, making it a promising substrate for high-efficiency light-emitting devices. However, bulk AlN single-crystal substrates are expensive and difficult to fabricate in large areas, making cost a significant issue when used as substrate materials for ultraviolet light-emitting devices.
[0004] Given this situation, there is an expectation, for example, of fabricating high-quality AlN thin films on inexpensive sapphire substrates as nitride semiconductor substrates.
[0005] However, the lattice mismatch between AlN and sapphire is significant, resulting in multiple through dislocations in the AlN film grown on the sapphire substrate. Consequently, it is difficult to obtain a flat surface for the AlN film deposited on the sapphire substrate, and there is also an increase in crystal defects.
[0006] As a method for obtaining a high-quality AlN thin film formed by suppressing the defect density of AlN crystals to a low level, there is, for example, the technique described in Patent Document 1.
[0007] Existing technical documents
[0008] Patent documents
[0009] Patent Document 1: Japanese Patent Application Publication No. 2017-055116
[0010] Non-patent literature
[0011] Non-Patent Document 1: Fabrication of +cAlN / -cAlN Structures for Near-Infrared Wavelength Transformation at the 80th Autumn Academic Lecture of the Chinese Society of Applied Physics, by Yu-Suke Hayashi et al. Summary of the Invention
[0012] The problem the invention aims to solve
[0013] Patent Document 1 discloses a method for manufacturing a nitride semiconductor substrate, wherein the substrate on which the nitride semiconductor is formed is annealed to cover the hermetically sealed state of the main surface of the nitride semiconductor by a cover member for suppressing the dissociation of the components of the nitride semiconductor from the main surface of the nitride semiconductor.
[0014] However, Patent Document 1 discloses that the full width at half maximum (WHM) of the X-ray diffraction rocking curve in the (10-12) plane of the nitride semiconductor substrate manufactured by the above manufacturing method is 300 arcsec, which requires further high crystallinity.
[0015] The present invention was made to solve the above-mentioned problems, and its purpose is to provide high-quality nitride semiconductor substrates, etc.
[0016] means for solving problems
[0017] To achieve the above objectives, one aspect of the present invention relates to a nitride semiconductor substrate comprising a substrate and an AlN-containing film disposed above the substrate, wherein the thickness of the AlN-containing film is less than 10000 nm, and the through dislocation density of the AlN-containing film is 2 × 10⁻⁶. 8 cm -2 the following.
[0018] Furthermore, one embodiment of the present invention relates to a nitride semiconductor substrate comprising a substrate and an AlN-containing film disposed above the substrate, wherein the thickness of the AlN-containing film is 300 nm or more and 10,000 nm or less, and the oxygen concentration of the AlN-containing film is 10. 18 cm -3 Above and 10 21 cm -3 Hereinafter, the hydrogen concentration of the AlN-containing film is 10. 16 cm -3 Above and 2×10 17 cm -3 the following.
[0019] Furthermore, one aspect of the present invention relates to a semiconductor element comprising the aforementioned nitride semiconductor substrate.
[0020] Furthermore, one aspect of the present invention relates to a method for manufacturing a nitride semiconductor substrate, comprising: a preparation step of preparing a substrate; a film formation step of forming an AlN film having a thickness of 100 nm or more and 900 nm or less on the substrate; and an annealing step of annealing the AlN film formed in the film formation step at a temperature of 1500 °C or higher, wherein at least one of the film formation step and the annealing step is performed multiple times, and the through dislocation density of the formed AlN film is 2 × 10⁻⁶. 8 cm -2 the following.
[0021] Invention Effects
[0022] According to the present invention, high-quality nitride semiconductor substrates and the like can be realized. Attached Figure Description
[0023] Figure 1 This is a diagram illustrating a configuration example of a nitride semiconductor substrate according to the first embodiment.
[0024] Figure 2 This is a diagram illustrating a configuration example of a nitride semiconductor substrate according to the second embodiment.
[0025] Figure 3 This is a diagram illustrating a configuration example of a nitride semiconductor substrate according to the third embodiment.
[0026] Figure 4 This is a schematic diagram illustrating an example of the configuration of a sputtering apparatus according to an embodiment.
[0027] Figure 5 This is a flowchart illustrating an example of a method for manufacturing a nitride semiconductor substrate according to the first embodiment.
[0028] Figure 6 This is a flowchart illustrating an example of a method for manufacturing a nitride semiconductor substrate according to the second embodiment.
[0029] Figure 7 This is a flowchart illustrating an example of a method for manufacturing a nitride semiconductor substrate according to the third embodiment.
[0030] Figure 8 This is a diagram illustrating an example of a table showing the crystallinity of a nitride semiconductor substrate according to an embodiment.
[0031] Figure 9A This is a diagram showing a planar TEM image of the nitride semiconductor substrate according to the embodiment.
[0032] Figure 9B This is another example of a table showing the crystallinity of a nitride semiconductor substrate involved in an embodiment.
[0033] Figure 9C This is a TEM image showing a cross-sectional view of the nitride semiconductor substrate according to the embodiment.
[0034] Figure 10 This is a graph showing the analysis results of the impurity concentration of the nitride semiconductor substrate involved in the embodiment.
[0035] Figure 11 This is another example of a table showing the crystallinity of a nitride semiconductor substrate involved in an embodiment.
[0036] Figure 12 This is a schematic diagram illustrating an example of temperature changes in the manufacturing method of the second example.
[0037] Figure 13 This is another example of a table showing the crystallinity of a nitride semiconductor substrate involved in an embodiment.
[0038] Figure 14 This is a schematic diagram illustrating another example of temperature changes in the manufacturing method of Example 2.
[0039] Figure 15 This is another example of a table showing the crystallinity of a nitride semiconductor substrate involved in an embodiment.
[0040] Figure 16 This is a schematic diagram illustrating another example of temperature changes in the manufacturing method of Example 2.
[0041] Figure 17 This is a figure showing other examples of the analysis results of the impurity concentration of the nitride semiconductor substrate involved in the embodiments.
[0042] Figure 18 This is a graph showing the relationship between the film thickness, annealing time, and through dislocation density of the AlN-containing film involved in the embodiment.
[0043] Figure 19 This is a schematic diagram of the stacked structure of the ultraviolet light-emitting element involved in the implementation method. Detailed Implementation
[0044] Hereinafter, embodiments of the present invention will be described in detail with reference to the accompanying drawings.
[0045] Furthermore, the embodiments described below are all examples, either general or specific. The numerical values, shapes, materials, constituent elements, the arrangement and connection methods of the constituent elements, steps, and the order of steps shown in the following embodiments are examples and are not intended to limit the scope of the present invention.
[0046] Furthermore, the figures are schematic diagrams and need not be strictly illustrated. In addition, in the figures, the same symbols are used to mark the same components, and sometimes repeated explanations are omitted or simplified.
[0047] Furthermore, in the following embodiments, the terms "above" and "below" do not refer to the absolute spatial direction of upward (vertical above) and downward (vertical below). In addition, the terms "above" and "below" apply not only to the case where two constituent elements are arranged with a gap between them and other constituent elements exist between them, but also to the case where two constituent elements are arranged closely together and in contact with each other.
[0048] In the following descriptions, aluminum may sometimes be represented as Al, gallium as Ga, indium as In, nitrogen as N, aluminum nitride as AlN, aluminum gallium nitride as AlGaN, aluminum gallium indium nitride as AlGaInN, aluminum boron nitride as BAlN, aluminum gallium boron nitride as BAlGaN, and scandium aluminum magnesium oxide as ScAlMgO4.
[0049] (Implementation Method)
[0050] [The structure of nitride semiconductor substrates]
[0051] First, adopt Figure 1 , 2 Section 3 will describe the configuration examples of the first example of the nitride semiconductor substrate 11, the second example of the nitride semiconductor substrate 21, and the third example of the nitride semiconductor substrate 31 involved in this embodiment.
[0052] Figure 1 This is a diagram illustrating a configuration example of the nitride semiconductor substrate 11 according to the first example of this embodiment. Figure 2 This is a diagram illustrating a configuration example of the nitride semiconductor substrate 21 in the second example according to this embodiment. Figure 3 This is a diagram illustrating a configuration example of the nitride semiconductor substrate 31 in the third example according to this embodiment.
[0053] The first example's nitride semiconductor substrate 11 includes a substrate 2 and an AlN-containing film 100. The second example's nitride semiconductor substrate 21 includes a substrate 2 and an AlN-containing film 200. The third example's nitride semiconductor substrate 31 includes a substrate 2 and an AlN-containing film 300. The AlN-containing film 100, AlN-containing film 200, and AlN-containing film 300 are films containing AlN, such as AlGaN. In the first to third examples of the embodiments, films made of AlN are described.
[0054] Substrate 2 is, for example, a substrate made of sapphire. The material constituting substrate 2 is not limited to sapphire; substrate 2 can be any substrate made of one of sapphire, silicon carbide, and ScAlMgO4. Furthermore, substrate 2 in the first, second, and third examples can also be made of different materials.
[0055] AlN-containing films 100, 200, and 300 are thin films disposed above the substrate 2. Furthermore, in the first example, the AlN-containing film 100 is composed of a first AlN film 10. In the second example, the AlN-containing film 200 is composed of a first AlN film 10 and a second AlN film 20. In the third example, the AlN-containing film 300 is composed of a first AlN film 10, a second AlN film 20, and a third AlN film 30.
[0056] The first AlN film 10, the second AlN film 20, and the third AlN film 30 are hexagonal crystals, thin films composed of aggregates of grains. The first AlN film 10, the second AlN film 20, and the third AlN film 30 can be made from AlN, Al... x Ga y In 1-x-y N(0.5≤x≤1, 0≤y≤0.5, x+y≤1) and B z Al w Ga 1-z-w One of the following compositions is selected from N (0≤z≤0.5, 0.5≤w≤1, z+w≤1). That is, the first AlN film 10, the second AlN film 20, and the third AlN film 30 can also be AlN, AlGaN, AlGaInN, BAlN, or BAlGaN.
[0057] Furthermore, when the first AlN film 10, the second AlN film 20, and the third AlN film 30 are composed of Al x Ga y In 1-x-y When N is used, the number of Al elements is more than 50% compared to the combined number of Al, Ga, and In. Furthermore, when the first AlN film 10, the second AlN film 20, and the third AlN film 30 are composed of B... z Al w Ga 1-z-w When N is used, the number of elements in Al is more than 50% compared to the total number of elements in B, Al and Ga.
[0058] Furthermore, the first AlN film 10, the second AlN film 20, and the third AlN film 30 can be composed of the same material or they can be composed of different materials.
[0059] The thickness of AlN-containing films 100, 200, and 300 is 10,000 nm or less. The thickness of AlN-containing films 100, 200, and 300 can also be 300 nm or more. Furthermore, the thickness of AlN-containing films 100, 200, and 300 is more preferably 450 nm or more and 3,000 nm or less, and even more preferably 600 nm or more and 2,000 nm or less.
[0060] [Method and apparatus for manufacturing nitride semiconductor substrates]
[0061] Next, the manufacturing apparatus and manufacturing method for the nitride semiconductor substrate 11 in the first example, the nitride semiconductor substrate 21 in the second example, and the nitride semiconductor substrate 31 in the third example will be described. The manufacturing apparatus can be used in the first, second, and third examples.
[0062] Furthermore, the nitride semiconductor substrate 11 of the first example can be manufactured by the manufacturing method of the first example, the nitride semiconductor substrate 21 of the second example can be manufactured by the manufacturing method of the second example, and the nitride semiconductor substrate 31 of the third example can be manufactured by the manufacturing method of the third example.
[0063] <Manufacturing Method of Example 1>
[0064] First, the manufacturing method of the first example of the nitride semiconductor substrate 11 used to manufacture the first example will be described.
[0065] Figure 4 This is a schematic diagram illustrating a configuration example of the sputtering apparatus 1000 according to this embodiment. Figure 5 This is a flowchart illustrating an example of a method for manufacturing a nitride semiconductor substrate 11 according to the first embodiment of this invention.
[0066] First of all, Figure 4 The configuration example of the sputtering apparatus 1000 shown will be described. As shown in the figure, the sputtering apparatus 1000 includes a chamber 110, an intake pipe 101, an exhaust pipe 102, a valve 103, an exhaust pump 104, a substrate support plate 105, a permanent magnet 108, and a high-voltage power supply 109.
[0067] The chamber 110 is a generally sealed room in which the substrate 2 and the target 107, which is the raw material for the first AlN film 10, are held opposite each other, and the gas pressure and temperature inside the chamber 110 can be arbitrarily set. Hereinafter, the gas pressure inside the chamber 110 during sputtering will be referred to as the sputtering pressure.
[0068] The suction tube 101 is used to introduce an externally supplied inert gas into the interior of the chamber 110. The inert gas can be helium (He), nitrogen (N2), argon (Ar), etc. The suction tube 101 can also supply multiple gases simultaneously from a single suction tube.
[0069] Alternatively, the chamber 110 may be configured with multiple suction tubes 101 connected to it. Furthermore, gases other than inert gases may be introduced through the suction tubes 101. Examples of gases other than inert gases include hydrogen (H2), oxygen (O2), and ammonia (NH3). The suction tubes 101 may also be equipped with a mechanism for precisely controlling the flow rate of the supplied gas.
[0070] The exhaust pipe 102 is used to exhaust the gas inside the chamber 110 to the outside.
[0071] Valve 103 regulates the exhaust flow rate of exhaust pipe 102.
[0072] The exhaust pump 104 is a pump used to exhaust gas inside the chamber 110 to the outside via the exhaust pipe 102 and the valve 103.
[0073] The substrate tray 105 holds the substrate 2 in the state of a wafer substrate. Furthermore, the substrate tray 105 can also hold multiple substrates 2 that are simultaneously deposited with films. The substrate tray 105 has a heating mechanism and can also heat and hold the substrate 2 in a range of 500°C or higher and 650°C or lower, for example, at 600°C.
[0074] The substrate support 105 may also have a mechanism that allows arbitrary control of the angle of the substrate 2 estimated from the target 107. The substrate may also be rotated or revolved during sputtering.
[0075] The target 107 is held on the target holder. Furthermore, the target holder can hold various targets 107 made of different materials, and can also be switched to be the target 107 to be sputtered. In this case, a configuration is formed that can continuously sputter various different materials while maintaining the chamber 110 in a high vacuum state.
[0076] Furthermore, it can be configured to simultaneously sputter multiple different materials. The target 107 may be, for example, a circle with a diameter of 10 cm. The target 107 may also be rectangular or other shapes.
[0077] A high-voltage power supply 109 applies a high-frequency voltage between the substrate 2 and the target 107. The high-frequency voltage is, for example, an RF (Radio Frequency) voltage. The RF voltage component of the high-frequency voltage plasmas the gas supplied from the suction pipe 101 between the substrate 2 and the target 107.
[0078] The plasma-entrained gas impacts the target 107 through an electric field formed by a DC voltage component applied by a self-biased voltage or an external power supply, ejecting atoms from the surface of the target 107 (sputtering). The ejected atoms fly toward the substrate 2 and attach according to the kinetic energy imparted by sputtering.
[0079] As a result, a film made from the target 107 or a film formed from a compound of the material constituting the target 107 and the gas supplied from the suction pipe 101 is formed on the substrate 2. The voltage of the high-frequency voltage can be, for example, 0V or higher and 5000V or lower, and the frequency of the high-frequency voltage can be 13.56MHz. The DC voltage component can be set to 0V or higher and 2000V or lower.
[0080] Furthermore, in Figure 4 The sputtering apparatus 1000 shows an example of so-called RF sputtering using a high-frequency voltage, but DC sputtering using a direct current voltage is also possible. Furthermore, a voltage can be applied in a pulsed manner with a certain time amplitude. In DC sputtering, the target 107 needs to be made of a conductive material.
[0081] A permanent magnet 108 forms a magnetic field to confine electrons in the plasma to the vicinity of the target 107. This increases the plasma density near the target 107, thereby increasing the sputtering rate. Furthermore, by keeping the plasma away from the substrate 2, the crystal quality of the first AlN film 10 can be prevented from deteriorating due to the irradiation of the substrate 2 with electrons or charged particles.
[0082] Furthermore, the sputtering apparatus 1000 may not include the permanent magnet 108. The permanent magnet 108 can be moved arbitrarily during sputtering. Cooling water is used to cool the target 107 and the vicinity of the permanent magnet 108 to suppress the temperature rise of the target 107.
[0083] In addition, Figure 4 In the sputtering apparatus 1000, an example of an upper sputtering type (or face-down type) configuration in which the substrate 2 is disposed opposite each other on the upper side of the target 107 has been described. However, it is not limited to this. A lower sputtering type (face-up type) in which the substrate 2 is disposed opposite each other on the lower side of the target 107 can also be used, as well as a side sputtering type (side-mounted type) in which the substrate 2 is disposed opposite each other on the side of the target 107 can also be used.
[0084] Figure 4 In this case, the distance between the substrate 2 and the target 107 is, for example, 14 cm.
[0085] Next, adopt Figure 5 The flowchart illustrates the manufacturing method of the nitride semiconductor substrate 11.
[0086] like Figure 5 As shown, the manufacturing method of the nitride semiconductor substrate 11 has, in a broad sense, steps S21, S22, S23 and S24.
[0087] Step S21 is a preparation step for preparing substrate 2. Specifically, in step S21, substrate 2 is prepared on substrate holder 105 within sputtering apparatus 1000. As described above, substrate 2 is, for example, a sapphire substrate. The sapphire substrate may, for example, have a surface that is inclined at 0.1° or more and 1.0° or less from the (0001) surface relative to the [1-100] direction (m-axis direction) or the [11-20] direction (a-axis direction) of sapphire.
[0088] The surface of the sapphire substrate can be formed with a single atomic layer or a stepped structure consisting of a single molecular layer. The back side of the sapphire substrate can also be ground into an optical mirror finish or subjected to a roughening process.
[0089] A layer formed of AlN or a material other than AlN can be deposited on the back side of the sapphire substrate. The substrate tray 105 can, for example, be configured to hold four or more 2-inch wafer substrates. The substrate tray 105 can also be configured to hold substrates of a size of 2 inches or larger.
[0090] As a pre-process stage of the first process S21, the following processes may also be performed.
[0091] First, the substrate 2 is placed on Figure 4 Although not shown in the diagram, the loading and locking chamber is located adjacent to and grounded to the chamber 110 and can be independently subjected to atmospheric release and vacuum exhaust. After the loading and locking chamber is evacuated to a sufficiently high vacuum, the substrate 2 is transferred from the loading and locking chamber to the sputtering chamber under vacuum. Alternatively, the substrate 2 can be placed on the substrate support plate 105 inside the chamber 110.
[0092] Therefore, when the substrate 2 is placed on the substrate holder 105, since the chamber 110 is not exposed to the atmosphere, a high vacuum level can always be maintained inside the chamber 110. Consequently, the crystal quality of the sputtered AlN film can be stably controlled. Before transferring the substrate 2 into the chamber 110, it is preferable to reduce the pressure inside the loading and locking chamber to, for example, 1 × 10⁻⁶. -4 Below Pa.
[0093] In the second step S22, the film-forming material, namely the target 107, is prepared within the sputtering apparatus 1000. Alternatively, the preparation step may include the first step S21 and the second step S22. The target 107 is, for example, a sintered body of AlN.
[0094] In steps S21 and S22, after the substrate 2 and target 107 are arranged, and before sputtering film deposition begins in step S23, it is preferable to allow sufficient time to evacuate the chamber 110 and reduce the pressure in the chamber 110. Furthermore, at this time, it is preferable to reduce the pressure in the chamber 110 while maintaining the temperature of the substrate 2 at the same temperature as during sputtering film deposition or at a higher temperature.
[0095] This reduces the residual gas concentration within chamber 110, thus stabilizing the crystallinity of the sputtered AlN film. Furthermore, by simultaneously heating the substrate 2 and vacuum-venting chamber 110, moisture adsorbed on the surface of the substrate 2 can be effectively removed before the substrate 2 is placed inside chamber 110. Therefore, the crystallinity of the sputtered AlN film can be stabilized. Before starting the third step S23, it is preferable to reduce the pressure inside chamber 110 to, for example, 6 × 10⁻⁶. -5 Below Pa.
[0096] Step S23 is the film formation process for forming an AlN film (first AlN film 10). Specifically, in step S23, the first AlN film 10 containing the target material is formed on the substrate 2 by sputtering the target 107 at a sputtering pressure of less than 0.5 Pa. Step S23 is also referred to as sputtering process.
[0097] More specifically, the sputtering pressure of chamber 110 is adjusted by the flow rate of gas supplied from the suction pipe, the exhaust speed of exhaust pump 104, and the opening degree of valve 103 to achieve a desired pressure of less than 0.5 Pa. The heating mechanism of substrate support plate 105 can maintain the surface temperature of substrate 2 in a temperature range of approximately 500°C to 650°C, for example, approximately 600°C.
[0098] An inert gas, such as nitrogen, is supplied from the intake pipe 101. The nitrogen flow rate is, for example, 10 sccm (Standard Cubic Centimeter per Minute) or more and 100 sccm or less. The unit sccm is a standardized unit at 0°C and 1 atmosphere.
[0099] The high-frequency voltage of the high-voltage power supply 109 is several hundred volts, and the frequency of the high-frequency voltage is, for example, 13.56 MHz. The power supplied from the high-voltage power supply 109 to the target 107 is, for example, more than 200 W and less than 1000 W. The sputtering time can be determined based on the desired film thickness of the first AlN film 10 to be formed and the power supplied to the target.
[0100] Furthermore, before the formation of the first AlN film 10 on the substrate 2, a process can be performed to generate plasma between the target 107 and the shield with a shield disposed between the substrate 2 and the target 107, and to sputter the target 107.
[0101] Thus, by sputtering the target 107 in a state where the atoms sputtered from the target 107 are blocked by the shield and do not reach the substrate 2, impurities attached to the surface of the target 107 can be removed.
[0102] After sufficient time has been spent sputtering the surface of the target 107, the shield disposed between the substrate 2 and the target 107 can be removed, and the formation of the first AlN film 10 on the substrate 2 can begin. This allows for stable control of the crystal quality of the subsequently sputtered first AlN film 10.
[0103] The thickness of the first AlN film 10 provided in the nitride semiconductor substrate 11 in the first example can be, for example, 300 nm or more and 1200 nm or less. Furthermore, in order to suppress the introduction of cracks accompanying the annealing process (described later) into the first AlN film 10, a greater thickness of the first AlN film 10 can reduce the sputtering pressure of the chamber 110. For example, the sputtering pressure of the chamber 110 can be 0.05 Pa or less.
[0104] Furthermore, more specifically, when the sputtering pressure of chamber 110 is set to P (Pa) or less and the film thickness of the nitride layer is set to T (nm) or less in order to suppress cracking, the group of (P, T) can also satisfy at least one of (0.05, 640), (0.1, 480), and (0.2, 320). Alternatively, the sputtering pressure P and the film thickness T of the nitride layer can also be selected in a manner that includes the following ranges.
[0105] In other words, it is also possible to obtain (1.1)P≤31117×T -2.06 Choose from the range contained in either (1.1) or (1.2) where 300≤T≤640 and (1.2)P≤0.05 and T≥640.
[0106] It is preferable if the group of (P, T) satisfies at least one of (0.05, 560) and (0.1, 400). In this case, when the sputtering pressure and film thickness are values other than those mentioned above, the sputtering pressure P and the film thickness T of the nitride layer can also be selected in such a way that they are included in the following ranges.
[0107] In other words, it can also be derived from (2.1) P≤1436×T -1.61 Choose from the range contained in either (2.1) or (2.2) where 300≤T≤560 and (2.2)P≤0.05 and T≥560.
[0108] It is preferable if the group of (P, T) satisfies at least one of (0.03, 850), (0.05, 480), and (0.1, 320). In this case, when the sputtering pressure and film thickness are values other than those mentioned above, they can also be selected such that the sputtering pressure P and the film thickness T of the nitride layer are included in the following ranges.
[0109] In other words, it can also be derived from (3.1) P≤76.6×T -1.17 The range to be selected is either (3.1) or (3.2) where 300≤T≤850, or P≤0.03 and T≥850. The range of P and T values is ±10% of the above range.
[0110] Step S24 is an annealing process in which the AlN film (first AlN film 10) formed in the film-forming process (step S23) is annealed at a temperature of 1500°C or higher. Specifically, in step S24, the substrate 2 on which the first AlN film 10 is formed is heat-treated at a temperature of 1500°C or higher, more preferably 1650°C or higher and 1750°C or lower. Step S24 is also referred to as annealing treatment.
[0111] More specifically, firstly, the substrate 2, on which the first AlN film 10 has been formed in step 3 S23, is placed inside the annealing apparatus. The annealing apparatus can be any apparatus capable of performing annealing; it can be a different apparatus from the sputtering apparatus 1000, or it can be the sputtering apparatus 1000 itself. The arrangement of the substrate 2 inside the annealing apparatus is as follows.
[0112] In other words, an airtight state is formed by covering the main surface of the first AlN film 10 with a cover member, which is used to prevent the components of the material constituting the first AlN film 10 from dissociating from the main surface of the first AlN film 10. Here, "dissociation" refers to the separation and shedding of the components (nitrogen, aluminum, gallium, indium, boron, etc.) of the first AlN film 10 from its main surface, including sublimation, evaporation, and diffusion. Furthermore, the "main surface" of the first AlN film 10 (or substrate 2) refers to the surface of the side on which other materials are stacked (formed) when they are laminated (or formed) on it.
[0113] Furthermore, when the cover component is not installed between the film-forming process (step 3 S23) and the annealing process (step 4 S24), the substrate 2 with the first AlN film 10 formed is exposed to the atmosphere.
[0114] Next, in order to remove impurities from inside the annealing apparatus, after venting the apparatus to create a vacuum, gas replacement is performed by introducing an inert gas or a mixed gas. Then, while maintaining the first AlN film 10 in the aforementioned airtight state, the temperature of the substrate 2 on which the first AlN film 10 is formed is increased. The rate at which the temperature is increased is called the heating rate. The heating rate can be, for example, 18.9°C per minute.
[0115] When the temperature of the substrate 2 on which the first AlN film 10 is formed reaches, for example, a predetermined temperature (e.g., above 1650°C and below 1750°C), the first AlN film 10 is annealed by holding the temperature of the substrate 2 on which the first AlN film 10 is formed at the predetermined temperature for a predetermined time. The temperature of the substrate 2 on which the first AlN film 10 is formed during annealing is called the annealing temperature, and the time held at the annealing temperature is called the annealing time.
[0116] To reduce the through dislocation density of the first AlN film 10 after annealing, annealing can be performed at a higher annealing temperature. The annealing temperature is more preferably 1700°C or higher and 1750°C or lower, and even more preferably 1725°C or higher and 1750°C or lower.
[0117] Annealing time can be, for example, 3 hours or more but less than 12 hours. Furthermore, to reduce the through dislocation density of the first AlN film 10, the thicker the first AlN film 10, the longer the annealing time can be. However, when the annealing temperature is too high or the annealing time is too long, the surface flatness of the first AlN film 10 after annealing may sometimes decrease. To reduce the through dislocation density without compromising the surface flatness of the first AlN film 10, the annealing temperature can be increased and the annealing time extended within a range that does not compromise surface flatness.
[0118] After the substrate 2 with the first AlN film 10 formed is held at the annealing temperature for the specified annealing time, the temperature of the substrate 2 with the first AlN film 10 formed is lowered to below 100°C. Then, the substrate 2 with the first AlN film 10 formed is removed from the annealing apparatus. The rate at which the temperature is lowered is called the cooling rate. The cooling rate can be, for example, 1°C or more per minute and 100°C or less per minute. Furthermore, the cooling rate can be constant or it can vary over time.
[0119] At this time, the substrate 2 on which the first AlN film 10 is formed is annealed in an atmosphere of inert gases such as nitrogen, argon, and helium, or in a mixture of inert gases with added ammonia and carbon monoxide.
[0120] Furthermore, regarding the pressure of the inert gas or gas mixture within the annealing apparatus, a range of 0.1 atm to 10 atm (76 Torr to 7600 Torr) is considered suitable for achieving the desired annealing effect. However, depending on factors such as explosion-proof strength at high temperatures, a range of 0.5 atm to 2 atm can be established. In principle, a higher partial pressure of nitrogen in these gases can lead to suppression of the crystallinity and surface roughness of the first AlN film 10, but the gas pressure can also be set to around 1 atm. Here, the pressure units are: 1 atm = 101325 Pa (Pascal) = 760 Torr.
[0121] Such annealing can reduce the through dislocation density of the first AlN film 10 and improve its crystallinity.
[0122] Furthermore, the annealing apparatus is a heating container with a constant volume, and it only needs to have the function of controlling the substrate temperature at a temperature above 500°C and below 1800°C, and the function of controlling the pressure and flow rate of the inert gas and mixed gas introduced into the apparatus for displacement.
[0123] The annealing apparatus covers the substrate 2 with the first AlN film 10 deposited thereon, which is disposed within the apparatus, with a cover member. Alternatively, the cover member can be positioned upwards, and the substrate 2 with the first AlN film 10 deposited thereon can be disposed lying flat on it in such a way that the first AlN film 10 contacts the cover member. Furthermore, a mechanism for applying arbitrary pressure between the cover member and the substrate may be included. The annealing apparatus can also simultaneously heat-treat multiple substrates 2 with the first AlN film 10 deposited on them.
[0124] Next, the airtightness of step S24 will be explained.
[0125] The term "airtight state" refers to a state achievable within the annealing apparatus, where the main surface of the first AlN film 10 is covered by a cover component to prevent the components (nitrogen, aluminum, gallium, indium, etc.) of the first AlN film 10 from dissociating from its main surface. In other words, the airtight state physically suppresses the dissociation of the components of the first AlN film 10 from its main surface. In this state, a substantially non-flowing gas stagnation occurs between the cover component and the main surface of the first AlN film 10.
[0126] By annealing the nitride semiconductor substrate 11 under such a hermetically sealed condition, roughness of the main surface caused by the dissociation of the components of the first AlN film 10 from its main surface can be suppressed. Furthermore, annealing at higher temperatures can be performed, resulting in a nitride semiconductor substrate 11 with a flat surface and high-quality first AlN film 10.
[0127] Furthermore, the target 107 prepared in the second step S22 is not limited to a sintered body of AlN, but can also be Al, AlGaN, AlNGaIn, BAlN or BAlGaN.
[0128] Furthermore, the inert gas used in the sputtering of the third step S23 is not limited to nitrogen; it can also be argon, helium, or a mixture of nitrogen and argon / helium.
[0129] Furthermore, the airtight state during annealing is achieved with the aim of easily obtaining a flat nitride layer surface. Therefore, if the annealing conditions do not substantially result in roughness due to detachment from the surface, or if there is an intention to create an uneven structure on the surface of the first AlN film 10, the surface may not need to be covered.
[0130] <Manufacturing Method of Example 2>
[0131] Next, the manufacturing method of the second example of the nitride semiconductor substrate 21 used to make the second example will be described. Figure 6 This is a flowchart illustrating an example of a method for manufacturing a nitride semiconductor substrate 21 according to the second example of this embodiment.
[0132] like Figure 6As shown, the manufacturing method of the nitride semiconductor substrate 21 is generally classified into steps S31, S32, S33, S34, S35, and S36. Here, steps S31 and S32 are the same as steps S21 and S22 of the manufacturing method of the first example.
[0133] In the second example, step S33 is the film formation process for forming an AlN film (first AlN film 10). Specifically, in step S33, the first AlN film 10 containing the target material is formed on the substrate 2 by sputtering the target 107 at a sputtering pressure of less than 0.5 Pa. That is to say, step S33 is the first sputtering process.
[0134] More specifically, the sputtering pressure of chamber 110 is adjusted by the flow rate of gas supplied from the suction pipe, the exhaust speed of exhaust pump 104, and the opening degree of valve 103 to achieve a desired pressure of less than 0.5 Pa. The surface temperature of substrate 2 can be maintained in a temperature range of approximately 500°C to 650°C, for example, approximately 600°C, by means of the heating mechanism of substrate support plate 105.
[0135] Nitrogen gas, which is an inert gas, is supplied from the intake pipe 101. The flow rate of the nitrogen gas is, for example, 10 sccm or more and 100 sccm or less.
[0136] The high-frequency voltage of the high-voltage power supply 109 is several hundred volts, and the frequency of the high-frequency voltage is, for example, 13.56 MHz. The power supplied from the high-voltage power supply 109 to the target 107 is, for example, more than 200 W and less than 1000 W. The sputtering time can be determined based on the desired film thickness of the first AlN film 10 to be formed and the power supplied to the target.
[0137] Furthermore, before the formation of the first AlN film 10 on the substrate 2, a process can be provided in which plasma is generated between the target 107 and the shield while a shield is placed between the substrate 2 and the target 107, and the target 107 is sputtered.
[0138] Thus, by sputtering the target 107 in a state where atoms sputtered from the target 107 are blocked by the shield and do not reach the substrate 2, impurities attached to the surface of the target 107 can be removed. After sputtering the surface of the target 107 for a sufficient time, the shield disposed between the substrate 2 and the target 107 can be removed, and the formation of the first AlN film 10 on the substrate 2 can begin. As a result, the crystal quality of the first AlN film 10 formed by subsequent sputtering can be stably controlled.
[0139] The thickness of the first AlN film 10 provided in the nitride semiconductor substrate 11 in the second example can be, for example, 100 nm or more and 900 nm or less. Furthermore, the thickness of the first AlN film 10 provided in the nitride semiconductor substrate 11 in the second example is more preferably 150 nm or more and 750 nm or less, and even more preferably 200 nm or more and 600 nm or less.
[0140] Furthermore, in order to suppress the introduction of cracks accompanying the annealing process described later into the first AlN film 10, a greater thickness of the first AlN film 10 can reduce the sputtering pressure of the chamber 110. For example, the sputtering pressure of the chamber 110 can be 0.05 Pa or less.
[0141] Furthermore, more specifically, when the sputtering pressure of chamber 110 is set to P (Pa) or less and the film thickness of the nitride layer is set to T (nm) or less in order to suppress cracking, the group of (P, T) can also satisfy at least one of (0.05, 640), (0.1, 480), and (0.2, 320). Alternatively, the sputtering pressure P and the film thickness T of the nitride layer can also be selected in a manner that includes the following ranges.
[0142] In other words, it is also possible to obtain (1.1)P≤31117×T -2.06 Choose from the range contained in either (1.1) or (1.2) where 300≤T≤640 and (1.2)P≤0.05 and T≥640.
[0143] It is preferable if the group of (P, T) satisfies at least one of (0.05, 560) and (0.1, 400). In this case, when the sputtering pressure and film thickness are values other than those mentioned above, the sputtering pressure P and the film thickness T of the nitride layer can also be selected in such a way that they are included in the following ranges.
[0144] In other words, it can also be derived from (2.1) P≤1436×T -1.61 Choose from the range contained in either (2.1) or (2.2) where 300≤T≤560 and (2.2)P≤0.05 and T≥560.
[0145] It is preferable if the group of (P, T) satisfies at least one of (0.03, 850), (0.05, 480), and (0.1, 320). In this case, when the sputtering pressure and film thickness are values other than those mentioned above, they can also be selected such that the sputtering pressure P and the film thickness T of the nitride layer are included in the following ranges.
[0146] In other words, it can also be derived from (3.1) P≤76.6×T -1.17Choose from the range contained in either (3.1) or (3.2) where 300≤T≤850 and (3.2)P≤0.03 and T≥850.
[0147] Step S34 is an annealing process in which the AlN film (first AlN film 10) formed in the film-forming process (step S33) is annealed at a temperature of 1500°C or higher. Specifically, in step S34, the substrate 2 on which the first AlN film 10 is formed is annealed at a temperature of 1500°C or higher, more preferably 1650°C or higher and 1750°C or lower. In other words, step S34 is the first annealing process.
[0148] To explain more specifically, firstly, the substrate 2, on which the first AlN film 10 has been formed in step 3 S33, is placed inside the annealing apparatus. The arrangement of the substrate 2 inside the annealing apparatus is as follows.
[0149] In other words, similar to the first example, in the second example, an airtight state is also formed by covering the main surface of the first AlN film 10 with a cover member, which is used to suppress the dissociation of nitride semiconductor components from the main surface of the first AlN film 10.
[0150] Next, in order to remove impurities from inside the annealing apparatus, after venting the apparatus to create a vacuum, gas replacement is performed by introducing an inert gas or a mixed gas. Then, while maintaining the first AlN film 10 in the aforementioned airtight state, the temperature of the substrate 2 on which the first AlN film 10 is formed is increased. At this time, the heating rate can be, for example, 18.9°C per minute.
[0151] After the temperature of the substrate 2 on which the first AlN film 10 is formed reaches a predetermined temperature (e.g., above 1650°C and below 1750°C), the first AlN film 10 is annealed by maintaining the temperature of the substrate 2 on which the first AlN film 10 is formed for a predetermined time.
[0152] Furthermore, in the second example, the annealing temperature and annealing time used to reduce the through dislocation density of the first AlN film 10 are the same as those in step S24 of the first example.
[0153] Furthermore, in the second example, the pressure of the inert gas or mixed gas in the annealing apparatus can be set to be the same as that in the fourth step S24 of the first example.
[0154] Next, proceed with step 5 (S35) and step 6 (S36).
[0155] Step 5, S35, is the film formation process for forming the AlN film (the second AlN film 20). In other words, step 5, S35, is the same as step 3, S33, and step 5, S35, is the second sputtering process.
[0156] Step 6, S36, is an annealing process that anneals the AlN film (second AlN film 20) formed in the film-forming process (step 5, S35) at a temperature above 1500°C. In other words, step 6, S36, is the same as step 4, S34, and step 6, S36, is the second annealing treatment.
[0157] Therefore, in the manufacturing method described in the second example of this embodiment, the film-forming process and the annealing process are performed multiple times.
[0158] Here, we will briefly explain step 5, S35, focusing on its differences from step 3, S33.
[0159] In step S35, a second AlN film 20 is formed above the first AlN film 10, which has undergone annealing treatment in step S34. Specifically, in step S35, a second AlN film 20 containing the composition of the target material can be formed by sputtering the target 107 at a sputtering pressure of less than 0.5 Pa.
[0160] In step 5 S35, the steps until the mask is removed and the second AlN film 20 is formed on the first AlN film 10 are the same as in step 3 S33. However, the sputtering conditions such as the surface temperature of the substrate 2, sputtering pressure, RF power, type of supply gas, flow rate of supply gas, and target material can be the same as or different from those in step 3 S33 when forming the first AlN film 10. For example, the sputtering pressure when forming the second AlN film 20 can be set to be higher than that when forming the first AlN film 10.
[0161] The thickness of the second AlN film 20 is preferably 100 nm or more and 900 nm or less. Furthermore, the thickness of the second AlN film 20 is more preferably 150 nm or more and 750 nm or less, and even more preferably 200 nm or more and 600 nm or less. Moreover, the thicknesses of the first AlN film 10 and the second AlN film 20 may be the same or different. For example, the thickness of the second AlN film 20 may be greater than the thickness of the first AlN film 10.
[0162] Furthermore, in order to suppress the occurrence of cracks accompanying the annealing process in step 6 S36 into the first AlN film 10 and the second AlN film 20, the greater the film thickness of the first AlN film 10 and the second AlN film 20, the lower the sputtering pressure of the chamber 110 can be. For example, the sputtering pressure of the chamber 110 in steps 3 S33 and 5 S35 is preferably 0.05 Pa or less.
[0163] Next, the differences between step 6 S36 and step 4 S34 will be briefly explained.
[0164] In step S36, the substrate 2 on which the first AlN film 10 and the second AlN film 20 are formed is annealed at a temperature of 1500°C or higher, more preferably 1650°C or higher and 1750°C or lower.
[0165] In step S36, the steps until the annealing process begins are the same as in step S34. However, the annealing conditions, such as the heating rate, cooling rate, annealing temperature, and annealing time, may or may not be the same as those in step S34.
[0166] For example, the annealing time of the annealing process in step S36 can be longer than the annealing time of the annealing process in step S34. In addition, the annealing temperature of the annealing process in step S36 can be higher than the annealing temperature of the annealing process in step S34.
[0167] After the substrate 2, to which the first AlN film 10 and the second AlN film 20 are formed, has been held at the annealing temperature for the specified annealing time, the temperature of the substrate 2 to which the first AlN film 10 and the second AlN film 20 are formed is reduced to below 100°C, and it is removed from the annealing apparatus. The cooling rate can be, for example, 1°C or more and 100°C or less per minute. Furthermore, the cooling rate can be constant or it can vary over time.
[0168] Here, Non-Patent Document 1 will be described. For example, in the nitride semiconductor substrate of this document, a first AlN layer and a second AlN layer are formed on the substrate by manufacturing methods using Al and AlN targets, respectively. Therefore, in the nitride semiconductor substrate of this document, the polarity of the first AlN layer and the second AlN layer is reversed.
[0169] On the other hand, in this example, AlN was used as the target 107 in steps S33 and S35. Al can also be used as the target 107, but the material constituting the target 107 is preferably the same material in steps S33 and S35.
[0170] Therefore, in this example, the first AlN film 10 and the second AlN film 20 have the same polarity, having Al polarity. Furthermore, even in the nitride semiconductor substrate 21 in this example, multiple layers with different polarities are sometimes formed, but most of the first AlN film 10 and the second AlN film 20 have Al polarity, and the thickness of the layer with N polarity is less than 200 nm.
[0171] <Manufacturing Method of Example 3>
[0172] Next, the manufacturing method of the third example of the nitride semiconductor substrate 31 used to manufacture the third example will be described. Figure 7This is a flowchart illustrating an example of a method for manufacturing a nitride semiconductor substrate 31 according to the third example of this embodiment.
[0173] like Figure 7 As shown, the manufacturing method of the nitride semiconductor substrate 31, broadly categorized, includes steps S41, S42, S43, S44, S45, S46, S47, and S48. Here, steps S41 to S46 of the manufacturing method of the nitride semiconductor substrate 31 in the third example are the same as steps S31 to S36 of the manufacturing method of the nitride semiconductor substrate 21 in the second example.
[0174] Furthermore, step 7, S47, is the film-forming process for forming the AlN film (the third AlN film 30). In other words, step 7, S47, is the same as step 3, S43, and step 5, S45; step 7, S47, is the third sputtering process.
[0175] Step 8, S48, is an annealing process that anneals the AlN film (3rd AlN film 30) formed in the film-forming process (step 7, S47) at a temperature above 1500°C. In other words, step 8, S48, is the same as step 4, S44, and step 6, S46, and step 8, S48, is the third annealing treatment.
[0176] Therefore, in the manufacturing method described in the third example of this embodiment, the film-forming process and the annealing process are performed multiple times.
[0177] Here, we will briefly explain the 7th step S47, focusing on its difference from the 5th step S45 (i.e., the 5th step S35 in the 2nd example).
[0178] In step 7 S47, a third AlN film 30 is formed on top of the second AlN film 20, which has undergone annealing treatment in step 5 S45.
[0179] In step 7 S47, the steps until the mask is removed and the second AlN film 20 is formed are the same as in step 5 S45. However, the sputtering conditions such as the surface temperature of the substrate 2, sputtering pressure, RF power, type of supply gas, flow rate of supply gas, and target material can be the same as or different from those used when forming the first AlN film 10 and the second AlN film 20.
[0180] The thickness of the third AlN film 30 is preferably 100 nm or more and 900 nm or less. Furthermore, the thickness of the third AlN film 30 is more preferably 150 nm or more and 750 nm or less, and even more preferably 200 nm or more and 600 nm or less.
[0181] Furthermore, the thicknesses of the first AlN film 10, the second AlN film 20, and the third AlN film 30 can be the same or different. In addition, the film formation method can be sputtering, or other film formation methods such as MOVPE (Metal Organic Vapor Phase Epitaxy), or a combination thereof. Furthermore, different sputtering devices can be used for each film formation, and the film formation devices and annealing devices can be arranged in a production line during production.
[0182] Next, the 8th step S48 will be briefly explained, focusing on its differences from the 6th step S46 (i.e., the 6th step S36 in the 2nd example).
[0183] In step S48, the substrate 2 on which the first AlN film 10, the second AlN film 20 and the third AlN film 30 are formed is annealed at a temperature of 1500°C or higher, more preferably 1650°C or higher and 1750°C or lower.
[0184] In step S48, the steps until the annealing process begins are the same as in step S46. However, the annealing conditions, such as the heating rate, cooling rate, annealing temperature, and annealing time, can be the same as or different from those in steps S44 and S46.
[0185] After the substrate 2, to which the first AlN film 10, the second AlN film 20, and the third AlN film 30 have been formed, has been held at the annealing temperature for the specified annealing time, the temperature of the substrate 2 is reduced to below 100°C, and it is removed from the annealing apparatus. The cooling rate can, for example, be between 1°C and 100°C per minute. Furthermore, the cooling rate can be constant or it can vary over time.
[0186] Furthermore, Figure 7 Although not illustrated, a film-forming process and an annealing process can also be performed after step S48. For example, after step S48, a film-forming process and an annealing process can be performed more than once, but it is preferable to perform them four times or less to simplify the manufacturing process.
[0187] Furthermore, in this example, the first AlN film 10, the second AlN film 20, and the third AlN film 30 have the same polarity, being Al polarity. Moreover, even in the nitride semiconductor substrate 31 of this example, multiple layers with different polarities are sometimes formed, but most of the first AlN film 10, the second AlN film 20, and the third AlN film 30 are Al polarity, and the thickness of the N polarity layer is less than 200 nm.
[0188] In summary, the manufacturing method described in this embodiment includes a preparation step for preparing the substrate 2, a film formation step, and an annealing step. The film formation step, for example, involves forming an AlN film (first AlN film 10, second AlN film 20, and third AlN film 30) with a thickness of 100 nm or more and 900 nm or less on top of the substrate 2. The annealing step is a process of annealing the AlN film formed in the film formation step at a temperature of 1500°C or higher.
[0189] Furthermore, the film-forming process and the annealing process can be performed multiple times. That is, as shown in the manufacturing methods of Examples 2 and 3, the film-forming process can be performed multiple times, and the annealing process can also be performed multiple times. In addition, it is not limited to this; at least one of the film-forming process and the annealing process can be performed multiple times. That is, for example, one film-forming process can be performed and multiple annealing processes can be performed, or multiple film-forming processes can be performed and one annealing process can be performed.
[0190] [Evaluation of Nitride Semiconductor Substrates 1]
[0191] Next, the results of evaluating the through dislocation density of AlN-containing film 100, AlN-containing film 200, and AlN-containing film 300 by changing the manufacturing conditions in the manufacturing methods of the first, second, and third examples of this embodiment will be explained.
[0192] Figure 8 This is a diagram illustrating an example of a table showing the crystallinity of the nitride semiconductor substrates 11, 21, and 31 according to this embodiment. Furthermore, more specifically, Figure 8 The results of measurements of nitride semiconductor substrates 11, 21, and 31 using an X-ray diffractometer (XRD) are shown.
[0193] Figure 8 The sample substrates shown (substrate numbers) are substrates corresponding to the nitride semiconductor substrates 11, 21 and 31 involved in this embodiment. Figure 8 The diagram shows the full width at half maximum (WHM) of the X-ray diffraction rocking curves (XRC) of AlN-containing films 100, 200, and 300 relative to the film thickness, annealing temperature, and annealing time of the first AlN film 10, the second AlN film 20, and the third AlN film 30 involved in this embodiment. Specifically, the full width at half maximum (WHM) of the XRC for the (0002) plane and the full width at half maximum (WHM) of the XRC for the (10-12) plane of AlN-containing films 100, 200, and 300 are shown.
[0194] The crystallinity of AlN-containing films 100, 200, and 300 corresponds to the full width at half maximum (FWHM) of the diffraction peaks obtained by XRC measurements through the (0002) and (10-12) planes. A smaller FWHM indicates sharper diffraction peaks and better crystallinity. Furthermore, the unit of FWHM for XRC is arcsec (""), representing angles.
[0195] Furthermore, the surface states of AlN-containing films 100, 200, and 300 can be represented by flat, pits, and rough. Flat represents the surface with the highest flatness, rough represents the surface with roughness, and pits represents an intermediate state between flat and rough.
[0196] Figure 8 The sample substrates shown with substrate numbers correspond to nitride semiconductor substrates 11, 21, and 31 manufactured using the manufacturing method described in this embodiment. Hereinafter, the sample substrates with substrate numbers will be referred to by substrate numbers, for example, as substrate number A1.
[0197] Figure 8 In this case, the thickness of the second AlN film 20 is 0 nm, which means that after the first annealing treatment, the second annealing treatment was performed without forming the second AlN film 20 through the second sputtering treatment. Furthermore, between the first and second annealing treatments, the sample substrate was exposed to the atmosphere.
[0198] Similarly, the thickness of the third AlN film 30 is 0 nm, which means that the third annealing process was performed after the second annealing process without forming the third AlN film 30 by the third sputtering process. Furthermore, between the second annealing process and the third sputtering, the sample substrate was exposed to the atmosphere.
[0199] As described above, the sample with a film thickness of 0 nm for the second AlN film 20 and the third AlN film 30 was not formed by the second and third sputtering processes, and thus it is equivalent to the nitride semiconductor substrate 11 manufactured according to the manufacturing method of the first example of this embodiment.
[0200] Specifically, substrate numbers A1, A2, A3, B1, B2, B3, C1, C2, D1, and D2 correspond to nitride semiconductor substrate 11.
[0201] Furthermore, when the thickness of the second AlN film 20 is greater than 0 nm, the sample substrate is exposed to the atmosphere between the first annealing treatment and the second sputtering.
[0202] Therefore, as described above, the sample with a film thickness greater than 0 nm of the second AlN film 20 is equivalent to the nitride semiconductor substrate 21 manufactured according to the manufacturing method of the second example of this embodiment.
[0203] Specifically, substrate numbers F1, F2, F3, F4, G1, H1, H2 and H3 correspond to nitride semiconductor substrate 21.
[0204] Furthermore, substrate number F1 is a nitride semiconductor substrate used as a comparative example because the annealing temperature in the second annealing process is lower than 1500°C.
[0205] Furthermore, when the thickness of the third AlN film 30 is greater than 0 nm, the sample substrate is exposed to the atmosphere between the second annealing treatment and the third sputtering.
[0206] Therefore, as described above, the sample with a film thickness greater than 0 nm of the third AlN film 30 corresponds to the nitride semiconductor substrate 31 manufactured according to the manufacturing method of the third example of this embodiment.
[0207] Specifically, substrate numbers G2 and H4 correspond to nitride semiconductor substrate 31.
[0208] Here, the full width at half maximum (WHM) of the XRC values relative to the film thickness, annealing temperature, and annealing time of the first AlN film 10, the second AlN film 20, and the third AlN film 30 will be explained. From the following explanation, it will be stated that a smaller WHM of the XRC value for the (10-12) plane indicates higher crystallinity.
[0209] As shown in substrate numbers A1, A2 and A3, when the thickness of the first AlN film 10 is 480 nm, the crystallinity remains the same even when the annealing time is extended.
[0210] However, as shown in the substrate numbers A1, A2, A3, B1, B2, B3, C1 and C2, if the thickness of the first AlN film 10 is increased from 480 nm to 600 nm and 900 nm, the crystallinity is improved by extending the annealing time.
[0211] In other words, the greater the thickness of the first AlN film 10, the higher the crystallinity can be by extending the annealing time.
[0212] Furthermore, as shown in substrate numbers A1, G1, and G2, the greater the thickness of AlN film 100, AlN film 200, and AlN film 300, the higher the crystallinity is achieved by extending the annealing time.
[0213] Furthermore, the same tendency was confirmed even in substrate numbers B1, H1, and H4.
[0214] As described above, the AlN-containing films 100, 200, and 300 involved in this embodiment have a film thickness of 300 nm or more and 10,000 nm or less. That is, in this embodiment, the AlN-containing films 100, 200, and 300 can have sufficiently thick film thicknesses, and the nitride semiconductor substrates 11 and 21 involved in this embodiment have high crystallinity. In other words, high-quality nitride semiconductor substrates 11, 21, and 31 can be achieved. Furthermore, as... Figure 8 As shown, by annealing with sufficient annealing temperature and annealing time, higher quality nitride semiconductor substrates 11, 21 and 31 can be achieved.
[0215] Furthermore, as described above, as indicated by substrate numbers B1, B2, B3, C1, and C2, crystallinity is improved by extending the annealing time (i.e., performing one film-forming process and multiple annealing processes).
[0216] In other words, the nitride semiconductor substrate 11 manufactured by a manufacturing method that includes a preparation step, a film formation step, and an annealing step, and at least one of the film formation step and the annealing step is performed multiple times, exhibits high crystallinity. Therefore, by employing the manufacturing method according to this embodiment, high-quality crystallinity of the nitride semiconductor substrate 11 can be achieved.
[0217] Furthermore, as shown in substrate numbers D1 and H1, the thickness of the first AlN film 10 in substrate number D1 and the combined thickness of the first AlN film 10 and the second AlN film 20 in substrate number H1 are both 1200 nm, and the combined annealing time is also both 6 hours. However, the crystallinity of the nitride semiconductor substrate 21 (substrate number H1) manufactured using the manufacturing method of the second example is higher than the crystallinity of the nitride semiconductor substrate 11 (substrate number D1) manufactured using the manufacturing method of the first example.
[0218] Therefore, by employing the manufacturing method of the second example, which includes a preparation process, a film formation process, and an annealing process, and performs the film formation and annealing processes multiple times, the crystallinity of the nitride semiconductor substrate 21 can be further improved. In other words, by employing the manufacturing method according to this embodiment, a high-quality nitride semiconductor substrate 21 can be achieved. Furthermore, the occurrence of cracks can be effectively suppressed. In addition, the decrease in surface flatness can be effectively suppressed.
[0219] Furthermore, the same trend was also confirmed in substrate numbers D2 and H2.
[0220] Furthermore, as indicated by substrate numbers F1, F2, F3 and F4, the crystallinity is improved by increasing the annealing temperature of the first AlN film 10.
[0221] like Figure 8 As shown, the full width at half maximum (WWHM) of the XRC in the (10-12) planes of the AlN-containing film 100, AlN-containing film 200 and AlN-containing film 300 involved in this embodiment is less than 120 arcsec.
[0222] Therefore, the nitride semiconductor substrates 11, 21, and 31 involved in this embodiment have high crystallinity. In other words, high-quality nitride semiconductor substrates 11, 21, and 31 can be achieved.
[0223] In addition, the full width at half maximum (WHM) of the XRC in the (0002) plane of the AlN-containing film 100, AlN-containing film 200 and AlN-containing film 300 involved in this embodiment is 120 arcsec or less.
[0224] Therefore, the nitride semiconductor substrates 11, 21, and 31 involved in this embodiment have high crystallinity. In other words, high-quality nitride semiconductor substrates 11, 21, and 31 can be achieved.
[0225] Furthermore, the substrate 2 in this embodiment is made of sapphire, but it is not limited to this; it can also be a substrate made of silicon carbide, ScAlMgO4, etc. These materials constituting the substrate 2 have... Figure 8 The example illustrates high durability at such high temperatures. Therefore, the AlN-containing film 100, AlN-containing film 200, and AlN-containing film 300 stacked on the substrate 2 can be annealed at high temperatures. Thus, as shown... Figure 8 As shown, high-quality nitride semiconductor substrates 11, 21, and 31 can be achieved.
[0226] Furthermore, as described above, the first AlN film 10, the second AlN film 20, and the third AlN film 30 can be made of AlN, Al x Ga y In 1-x-y N and B z Al w Ga 1-z-w One of the components in N. In this embodiment, the first AlN film 10, the second AlN film 20, and the third AlN film 30 are made of AlN. Thus, as Figure 8 As shown, high-quality nitride semiconductor substrates 11, 21, and 31 can be achieved.
[0227] Here, images of the nitride semiconductor substrate 11 and nitride semiconductor substrate 21 as described in this embodiment, as observed by a scanning transmission electron microscope (STEM), will be explained.
[0228] Figure 9AThis is a diagram showing planar STEM images of the nitride semiconductor substrate 11 (substrate number D2) and the nitride semiconductor substrate 21 (substrate numbers H2 and H3) according to this embodiment. More specifically, Figure 9A (a) is a diagram showing the result of the planar STEM image of substrate number D2. Figure 9A (b) is a diagram showing the result of the planar STEM image of substrate number H2. Figure 9A (c) is a diagram showing the result of the planar STEM image of substrate number H3.
[0229] Figure 9A The values recorded together are the through dislocation densities of the nitride semiconductor substrate 11 and the nitride semiconductor substrate 21. The through dislocation density is a value derived by calculating the density of dark spots per unit area by counting the number of dark spots (dark spots correspond to through dislocations) appearing in the count image.
[0230] Figure 9B This is another example of a table showing the crystallinity of the nitride semiconductor substrates 11 and 21 according to this embodiment. Specifically, it is from... Figure 9A The planar STEM image shown yielded the values of the through dislocation densities of nitride semiconductor substrate 11 (substrate number D2) and nitride semiconductor substrate 21 (substrate numbers H2 and H3).
[0231] like Figure 9B As shown, in this embodiment, the through-dislocation densities of the AlN-containing film 100 of the nitride semiconductor substrate 11 and the AlN-containing film 200 of the nitride semiconductor substrate 21 are sufficiently concentrated at 2 × 10⁻⁶. 8 cm -2 More specifically, the through dislocation density of AlN-containing film 100 and AlN-containing film 200 is 1.5 × 10⁻⁶. 8 cm -2 To be more specific, it is 1×10 8 cm -2 the following.
[0232] In other words, the nitride semiconductor substrates 11 and 21 according to this embodiment include a substrate 2 and an AlN-containing film (AlN-containing film 100 and AlN-containing film 200) disposed above the substrate 2. The thickness of the AlN-containing film is less than 10000 nm, and the through dislocation density of the AlN-containing film is 2 × 10⁻⁶. 8 cm -2 the following.
[0233] Thus, by employing the manufacturing method described in this embodiment, the nitride semiconductor substrates 11 and 21 described in this embodiment can sufficiently reduce the through dislocation density and improve crystallinity. In other words, high-quality nitride semiconductor substrates 11 and 21 can be achieved.
[0234] Figure 9C This is a cross-sectional STEM image showing the nitride semiconductor substrate 21 (substrate number H2) according to this embodiment. For this analysis, an AlN film is formed on top of substrate number H2 using MOVPE. Figure 9C In the text, it is recorded as MOVPE-AlN.
[0235] Figure 9C (a) is a cross-sectional view of the interface from the sapphire substrate and the first AlN film 10 to the surface of the MOVPE-AlN. Figure 9C (b) and Figure 9C (c) is to Figure 9C (a) shows the magnified cross-sectional images of regions (b) and (c).
[0236] like Figure 9C As shown, the first AlN film 10 and the second AlN film 20 are mostly AlN films with Al polarity. However, near the interface between the first AlN film 10 and the substrate 2 within the first AlN film 10, and near the interface between the second AlN film 20 and the first AlN film 10 within the second AlN film 20, layers of AlN films with N polarity are formed. In this case, the thickness of the layers of AlN films with N polarity is less than 200 nm.
[0237] Two dark lines are observed in the cross-sectional STEM image at the interface between the second AlN film 20 and the first AlN film 10, and near the interface between the second AlN film 20 and the first AlN film 10 within the second AlN film 20. The region enclosed by these two dark lines is defined as the interface region. Alternatively, the polarity of the AlN film can be reversed using this interface region or the dark lines as boundaries, and the AlN film adjacent to the interface region can also possess Al polarity. Furthermore, in this embodiment, the interface region is... Figure 9C The N-polar region in the second AlN film 20 shown.
[0238] like Figure 9C As shown in (a), through dislocations that occur at the interface between the first AlN film 10 and the substrate 2 and propagate in the first AlN film 10 are bent or terminated in the interface region formed at the interface between the second AlN film 20 and the first AlN film 10, and no longer propagate to the second AlN film 20. Therefore, it is speculated that the aforementioned interface region may have the function of preventing the propagation of through dislocations and reducing the density of through dislocations reaching the outermost surface of the nitride semiconductor substrate 21.
[0239] Next, the distribution of impurity concentrations in nitride semiconductor substrates 11 and 21 will be described.
[0240] Figure 10 This is a graph showing the analysis results of the impurity concentration of the nitride semiconductor substrates 11 and 21 involved in this embodiment.
[0241] Furthermore, to be more specific, Figure 10 (a) is a graph showing the result for substrate number D2. Figure 10 (b) is a graph showing the result for substrate number H2. Figure 10 (c) is a graph showing the result for substrate number H3. Furthermore, Figure 10 Impurity concentration analysis was performed using SIMS (Secondary Ion Mass Spectrometry). Furthermore, for this analysis, AlN films were formed on substrates numbered D2, H2, and H3 using MOVPE. Figure 10 It is recorded as MOVPE-AlN.
[0242] also, Figure 10 The horizontal axis of the graph representing the impurity concentration distribution, i.e., the depth (μm), represents the distance from MOVPE-AlN toward substrate 2 in the direction of travel.
[0243] As described above, substrate number D2 is the nitride semiconductor substrate 11 of the first example, and substrate numbers H2 and H3 are the nitride semiconductor substrate 21 of the second example. Therefore, in substrate number D2, the AlN film 100 is composed of the first AlN film 10, and in substrate numbers H2 and H3, the AlN film 200 is composed of the first AlN film 10 and the second AlN film 20.
[0244] like Figure 10 As shown, the oxygen concentration of AlN-containing membrane 100 and AlN-containing membrane 200 is 10. 18 cm -3 Above and 10 21 cm -3 The following is more specific: the oxygen concentration is 10. 19 cm -3 Above and 10 21 cm -3 To be more specific, the following is for 10. 20 cm -3 Above and 10 21 cm -3 The following. Furthermore, the hydrogen concentration of AlN-containing film 100 and AlN-containing film 200 is 10. 16 cm -3 Above and 2×10 17 cm-3 The following is more specific: the hydrogen concentration is 10. 16 cm -3 Above and 10 17 cm -3 the following.
[0245] Furthermore, the oxygen and hydrogen concentrations do not need to fall within the aforementioned concentration range across the entire area containing the AlN film 100 and the AlN film 200. For example, the area where the oxygen and hydrogen concentrations fall within the aforementioned concentration range can also be a region exceeding a predetermined proportion across the entire area containing the AlN film 100 and the AlN film 200. This predetermined proportion could be, for example, 30%, 50%, or 70%. Additionally, the area where the oxygen and hydrogen concentrations fall within the aforementioned concentration range can also be a predetermined region based on the interface between the substrate 2 and the AlN film 100 or the AlN film 200. This predetermined region could, for example, extend from a position 100 nm away from the interface to a position 1000 nm away from the interface.
[0246] Furthermore, the AlN-containing film 200 has a first layer 201 and a second layer 202 that is different from the first layer 201.
[0247] Furthermore, layer 1, 201, is also an interface layer. Layer 1, 201 (interface layer) is a layer where the elemental concentration has a maximum value. For example, layer 1, 201 (interface layer) is a layer where the oxygen concentration, carbon concentration, and silicon (Si: silicon) concentration have maximum values. Furthermore, layer 1, 201 (interface layer) is a layer where at least one of the oxygen concentration, carbon (C) concentration, and silicon (Si: silicon) concentration has a maximum value. For example... Figure 10 As shown, the first layer 201 (interface layer) is located between the substrate 2 and the first layer 201. Furthermore, "between the substrate 2 and the first layer 201" means the interface between the AlN film 200 and the substrate 2, and the surface of the AlN film 200 on the opposite side of the substrate 2 (i.e., Figure 10 Between the AlN film 200 and the MOVPE-AlN interface.
[0248] In addition, the second layer 202 is the layer located around the first layer 201 (interface layer).
[0249] For example, in the first layer, 201. Figure 10 As shown, this is the region located at the interface between the first AlN film 10 and the second AlN film 20, with the thickness of the first layer 201 being more than 10 nm and less than 200 nm.
[0250] In addition, the second layer 202, for example, Figure 10 The region shown is located in the second AlN film 20, but it is not limited to this as long as it is a region different from the first layer 201.
[0251] like Figure 10 As shown, the elemental concentration of layer 1 201 is higher than that of layer 202. For example, the oxygen concentration of layer 1 201 is higher than that of layer 202. In other words, the oxygen concentration of layer 1 201 (interface layer) has a maximum value. In the nitride semiconductor substrate 21 of the second example, i.e., substrates H2 and H3, it is exposed to the atmosphere between the first annealing process and the second sputtering. The reason why the oxygen concentration of layer 1 201 is higher than that of layer 202 is believed to be due to atmospheric exposure, through which the oxygen concentration of layer 1 201 has a peak (maximum point).
[0252] In other words, as shown in this embodiment, the nitride semiconductor substrate that is inferred to have a region with a high elemental concentration (e.g., the first layer 201) compared to the surrounding region (e.g., the second layer 202) is a nitride semiconductor substrate 21 manufactured by the manufacturing method described in the second example.
[0253] By adopting the manufacturing method of the second example, the crystallinity of the nitride semiconductor substrate 21 can be further improved. Therefore, the element concentration (e.g., oxygen concentration) of the first layer 201 is higher than that of the second layer 202, which means that the crystallinity of the nitride semiconductor substrate 21 is high.
[0254] Furthermore, such as Figure 10 As shown, the silicon concentration of layer 1 201 is higher than that of layer 202, and the carbon concentration of layer 1 201 is higher than that of layer 202. Similarly, the reason for the higher silicon or carbon concentration of layer 1 201 than that of layer 202 is atmospheric exposure.
[0255] In this embodiment, the oxygen concentration or silicon concentration in the first layer 201 is more than twice that of the second layer 202. The same effect can be expected from this. Furthermore, the oxygen concentration or silicon concentration in the first layer 201 can be more than 1.5 times, or more than 1.2 times, compared to the second layer 202.
[0256] As described above, in the nitride semiconductor substrates 11 and 21 of this embodiment, the through dislocation density of the AlN-containing films (AlN-containing film 100 and AlN-containing film 200) is 2 × 10⁻⁶. 8 cm -2 Below, the full width at half maximum (WWHM) of the XRC in the (10-12) plane containing the AlN film is 120 arcsec or less. The full WWHM of the XRC in the (10-12) plane containing the AlN film is 90 arcsec or less in substrate numbers H2 and H3, and 80 arcsec or less in substrate number H2. Additionally, as... Figure 10 As shown, the oxygen concentration of the AlN-containing membrane is 10. 18 cm-3 Above and 10 21 cm -3 Below, the hydrogen concentration is 10. 16 cm -3 Above and 2×10 17 cm -3 the following.
[0257] Thus, the nitride semiconductor substrates 11 and 21 of this embodiment, with oxygen and hydrogen concentrations within the aforementioned ranges for the AlN film, exhibit very low through-dislocation density, very low full width at half maximum (FWHM) XRC, and high crystallinity. In other words, high-quality nitride semiconductor substrates 11 and 21 are achieved.
[0258] Furthermore, the nitride semiconductor substrates 11 and 21 according to this embodiment include a substrate 2 and an AlN-containing film (AlN-containing film 100 and AlN-containing film 200) disposed above the substrate 2. The thickness of the AlN-containing film is 300 nm or more and 10000 nm or less. Additionally, as... Figure 10 As shown, the oxygen concentration of the AlN-containing membrane is 10. 18 cm -3 Above and 10 21 cm -3 Below, the hydrogen concentration is 10. 16 cm -3 Above and 2×10 17 cm -3 the following.
[0259] As described above, by employing the manufacturing method of this embodiment, the AlN-containing film of the nitride semiconductor substrates 11 and 21 involved in this embodiment has a sufficiently thick film thickness and high crystallinity, thereby realizing high-quality nitride semiconductor substrates 11 and 21.
[0260] Furthermore, in this embodiment, the film thickness of AlN films 100, 200, and 300 is preferably less than 2000 nm. For example... Figure 8 As shown, the AlN films with the aforementioned thicknesses of 100, 200, and 300 exhibit high crystallinity. In other words, high-quality nitride semiconductor substrates 11, 21, and 31 can be achieved.
[0261] [Evaluation of Nitride Semiconductor Substrates 2]
[0262] Furthermore, here, the evaluation results of the crystallinity of the AlN-containing film 100 of the nitride semiconductor substrate 11 manufactured by changing the manufacturing conditions in the manufacturing method of the second example of this embodiment will be explained. In addition, in the [Evaluation 2 of nitride semiconductor substrate], the descriptions that are repeated with the [Evaluation 1 of nitride semiconductor substrate] are sometimes omitted or simplified.
[0263] Furthermore, compared to the nitride semiconductor substrates 11, 21, and 31 described in [Evaluation of Nitride Semiconductor Substrates 1], the nitride semiconductor substrate 11 described in [Evaluation of Nitride Semiconductor Substrates 2] mainly possesses the following two characteristics. Specifically, one of the two characteristics is that the second annealing process is performed without forming the second AlN film 20 through the second sputtering process. Another of the two characteristics is that the substrate 2, in which the first AlN film 10 (i.e., AlN film 100) is formed during the period between the first and second annealing processes, is not exposed to the atmosphere, but is kept in the chamber 110 or annealing apparatus at a specified temperature (T, described later). mid )Keep.
[0264] First, the effect of controlling the temperature of the substrate 2 on which the first AlN film 10 is formed during the period between the first annealing treatment and the second annealing treatment is analyzed using... Figure 11 and Figure 12 Please provide an explanation.
[0265] Figure 11 This is another example of a table showing the crystallinity of the nitride semiconductor substrate 11 according to this embodiment. Furthermore, more specifically, Figure 11 The results of XRD measurements of the nitride semiconductor substrate 11 are shown below. Furthermore, in the following description... Figure 13 and Figure 15 The results obtained by XRD are also shown in the diagram.
[0266] The crystallinity of the AlN film 100 corresponds to the full width at half maximum (WHaV) of the diffraction peaks obtained by XRC measurement of the (0002) and (10-12) planes. A smaller WHaV in XRC, indicating sharper diffraction peaks, signifies better crystallinity. Furthermore, the unit of WHaV in XRC is arcsec ("). Additionally, as discussed later... Figure 13 and Figure 15 The same applies to China.
[0267] Figure 11 The sample substrates shown with substrate numbers correspond to the nitride semiconductor substrate 11 manufactured using the manufacturing method according to this embodiment. Furthermore, in the following description... Figure 13 and Figure 15 The same applies to China.
[0268] In the following [Evaluation of Nitride Semiconductor Substrates 2], the sample substrates with substrate numbers, such as substrate number 51, will be described by substrate number.
[0269] also, Figure 12 This is a schematic diagram illustrating an example of temperature changes in the manufacturing method of Example 2. More specifically, Figure 12 The image shows the materials used in manufacturing. Figure 11 Temperature variation during the manufacturing method of the second example of the nitride semiconductor substrate 11 (substrate numbers 51-55) shown. Furthermore, Figure 12 The horizontal axis represents processing time, and the vertical axis represents processing temperature. Furthermore, as described later... Figure 14 and Figure 16 Similarly, the horizontal axis represents processing time, and the vertical axis represents processing temperature.
[0270] use Figure 12 The temperature changes in the annealing process (first annealing treatment (fourth step S34) and second annealing treatment (sixth step S36)) of the manufacturing method of substrates 51 to 55, namely the manufacturing method of Example 2, will be explained.
[0271] In the manufacturing method of substrates 51 to 55, i.e., the manufacturing method of Example 2, such as Figure 12 As shown, in the first annealing process (step S34), the substrate 2 on which the first AlN film 10 is formed is annealed at 1700°C for 3 hours. Additionally, the temperature of the substrate 2 on which the first AlN film 10 is formed is lowered to T. mid .
[0272] Furthermore, as mentioned above, no second AlN film 20 was formed during the second sputtering process.
[0273] Next, as Figure 12 As shown, in the second annealing process (step S36), the substrate 2 with the first AlN film 10 deposited thereon is annealed at 1700°C for 6 hours. Then, the substrate 2 with the first AlN film 10 deposited thereon is removed from the annealing apparatus. Substrates 51 to 55 are thus manufactured.
[0274] In other words, Figure 12 In the manufacturing method of the second example shown, during the period between the first annealing treatment and the second annealing treatment, the substrate 2 with the first AlN film 10 formed is not exposed to the atmosphere, but is heated in the chamber 110 or the annealing apparatus at a specified temperature, i.e., T. mid Keep.
[0275] like Figure 11 As shown, in substrates 51-55, the thickness of the first AlN film 10 is 784 nm or 793 nm, which are approximately the same. Substrates 51-55 are respectively distinguished by the specified temperature (T) during the period between the first and second annealing processes. mid Aside from this difference, they are manufactured using the same manufacturing method.
[0276] In addition, such as Figure 11As shown, T is arranged in the order of substrate numbers 51, 52, 53, 54, and 55. mid The value decreases. Additionally, as... Figure 11 As shown, there is a tendency for the full width at half maximum (FWHM) of the XRC on the (10-12) plane to decrease in the order of substrate numbers 51, 52, 53, 54 and 55, i.e., crystallinity increases in this order.
[0277] Based on the above, the specified temperature (T) during the temporary cessation of annealing between the first and second annealing processes is determined. mid The low crystallinity of the first AlN film 10 (i.e., the AlN-containing film 100) can improve the crystallinity of the first AlN film 10, thus achieving a high-quality nitride semiconductor substrate 11. Specifically, Figure 11 In the middle, in T mid At values of 400℃ and 150℃ (i.e., substrate numbers 54 and 55), a more suitable full width at half maximum (FWHM) of XRC was achieved. Maintaining the specified temperature (T...) mid The annealing time can be selected within a range of 0 seconds to 120 minutes. By thus reducing the temperature during the temporary halt annealing process in the annealing treatment, strain-induced through dislocations are generated based on the thermal expansion coefficients of sapphire and AlN. The movement of through dislocations is effective in reducing the density of through dislocations.
[0278] In addition, the impact on the combined processing time of the first and second annealing processes was assessed using... Figure 13 and Figure 14 Please provide an explanation.
[0279] Figure 13 This is another example of a table showing the crystallinity of the nitride semiconductor substrate 11 according to this embodiment.
[0280] also, Figure 14 This is a schematic diagram illustrating another example of temperature changes in the manufacturing method of Example 2. More specifically, Figure 14 (a) shows the method of manufacturing Figure 13 Temperature variation during the manufacturing process of the second example of the nitride semiconductor substrate 11 (substrate number 56) shown. Figure 14 (b) shows the method of manufacturing Figure 13 Temperature variation in the manufacturing method of the second example of the nitride semiconductor substrate 11 (substrate number 57) shown.
[0281] use Figure 14 The temperature changes in the annealing process (first annealing treatment (fourth step S34) and second annealing treatment (sixth step S36)) of the manufacturing method of substrates 56 and 57, i.e. the manufacturing method of Example 2, will be explained.
[0282] In the manufacturing method of substrates 56 and 57, i.e., the manufacturing method of Example 2, such as Figure 14 As shown, in the first annealing process (step S34), after the substrate 2 with the first AlN film 10 formed is annealed at 1650°C for 3 hours, it is then annealed at 1700°C for 3 hours. In addition, the temperature of the substrate 2 with the first AlN film 10 formed is reduced to 150°C.
[0283] Furthermore, in the manufacturing method of the second example in [Evaluation of Nitride Semiconductor Substrates 2], in Figure 6 In the second sputtering process (step S35), the second AlN film 20 was not formed.
[0284] Next, as Figure 14 As shown, in the second annealing process (step S36), the substrate 2 with the first AlN film 10 deposited thereon is annealed at 1700°C for a predetermined time. Then, the substrate 2 with the first AlN film 10 deposited thereon is removed from the annealing apparatus. Substrates 56 and 57 are thus manufactured.
[0285] like Figure 13 As shown, in substrates 56 and 57, the thickness of the first AlN film 10 is 784 nm or 793 nm, which are approximately the same. Substrates 56 and 57 are manufactured using the same manufacturing method, except for the annealing time in the second annealing process.
[0286] like Figure 14 As shown, the annealing times in the second annealing process for substrates 56 and 57 are 9 hours and 6 hours, respectively. Therefore, as Figure 13 As shown, the annealing times at 1700°C for substrates 56 and 57 are 12 hours and 9 hours, respectively. Additionally, as... Figure 13 As shown, there is a tendency for the full width at half maximum (FWHM) of the XRC on the (10-12) plane to increase in the order of substrate numbers 56 and 57. In other words, substrate number 57, which has a longer annealing time at 1700°C, has higher crystallinity compared to substrate number 56.
[0287] In addition, the effect of nitrogen flow rate in the first sputtering process was investigated using... Figure 15 and Figure 16 Please provide an explanation.
[0288] Figure 15 This is another example of a table showing the crystallinity of the nitride semiconductor substrate 11 according to this embodiment.
[0289] For use in manufacturing Figure 15 The manufacturing method of the second example of substrate numbers 58 to 60 shown will be described.
[0290] First, the first sputtering process for forming the first AlN film 10 will be described. Furthermore, Figure 15 The “N2 Flow (sccm) During SP” shown indicates the flow rate of nitrogen gas during the first sputtering process.
[0291] In the manufacturing method of the second example used to manufacture substrates 58-60, the flow rate of nitrogen in the first sputtering process is different for each of substrates 58-60. In substrate 58, the flow rate is constant at 24 sccm during the first sputtering process. In substrates 59 and 60, the flow rate is controlled to increase during the first sputtering process. More specifically, in substrate 59, the flow rate is increased from 19 sccm to 28 sccm, and in substrate 60, the flow rate is increased from 19 sccm to 32 sccm.
[0292] Next, refer to Figure 16 The annealing process (first annealing treatment (4th step S34) and second annealing treatment (6th step S36)) is described. Figure 16 This is a schematic diagram illustrating another example of temperature changes in the manufacturing method of Example 2. More specifically, Figure 16 The middle shows Figure 15 Temperature variation in the manufacturing method of the second example of manufacturing nitride semiconductor substrate 11 (substrate number 58-60) shown.
[0293] In the first annealing process (step S34), after the substrate 2 with the first AlN film 10 formed is annealed at 1650°C for 3 hours, it is then annealed at 1700°C for 3 hours. In addition, the temperature of the substrate 2 with the first AlN film 10 formed is reduced to 150°C.
[0294] Furthermore, as mentioned above, no second AlN film 20 was formed during the second sputtering process.
[0295] Next, as Figure 16 As shown, in the second annealing process (step 6 S36), the substrate 2 with the first AlN film 10 deposited thereon is annealed at 1700°C for 6 hours. Then, the substrate 2 with the first AlN film 10 deposited thereon is removed from the annealing apparatus. Substrates 58 to 60 are thus manufactured.
[0296] like Figure 15 As shown, in substrates 58 to 60, the thickness of the first AlN film 10 is 778 nm, 791 nm, or 798 nm, which are approximately the same. Substrates 58 to 60 are manufactured using the same manufacturing method, except for the aforementioned differences in flow rate.
[0297] like Figure 15As shown, compared to substrate number 58, there is a tendency for the full width at half maximum (WHM) of the XRC on the (10-12) facet of substrate numbers 59 and 60 to decrease, meaning that crystallinity is improved by increasing the aforementioned flow rate. Furthermore, compared to substrate number 59, crystallinity is improved by decreasing the full width at half maximum (WHM) of the XRC on the (10-12) facet of substrate number 60, meaning that crystallinity is improved by increasing the aforementioned flow rate to a value higher than 24 sccm.
[0298] Figure 17 These are figures illustrating other examples of analytical results regarding the impurity concentration of the nitride semiconductor substrate 11 according to this embodiment. More specifically, Figure 17 (a) is a graph showing the analysis results of the impurity concentration of the nitride semiconductor substrate 11 before the first annealing treatment. Figure 17 (b) is a graph showing the analysis results of the impurity concentration of the nitride semiconductor substrate 11 after the first annealing treatment.
[0299] Furthermore, regarding Figure 17 The nitride semiconductor substrate 11 used in the process has the same structure as the substrate number A1 mentioned above, except that the thickness of the first AlN film 10 (including the AlN film 100) is 320 nm, the annealing temperature in the first annealing process is 1700 °C and the annealing time is 3 hours.
[0300] like Figure 17 As shown in (a) and (b), the impurity concentration changes by performing the first annealing treatment. In particular, the hydrogen concentration changes more significantly compared to other elements. Furthermore, by performing the first annealing treatment, the hydrogen concentration of the first AlN film 10 (containing AlN film 100) reaches 10. 16 cm -3 Above and 2×10 17 cm -3 The following. (e.g.) Figure 17 As shown in (b), the region where the hydrogen concentration of the first AlN film 10 (containing AlN film 100) is within the aforementioned range is a region where the hydrogen concentration is at least a specified proportion (e.g., 50% here) or higher across the entire region containing AlN film 100. Furthermore, the oxygen concentration of the first AlN film 10 (containing AlN film 100) is 10. 18 cm -3 Above and 10 21 cm -3 the following.
[0301] In other words, Figure 17 The nitride semiconductor substrate 11 used in the process includes a substrate 2 and an AlN-containing film 100 disposed above the substrate 2. The AlN-containing film 100 has a thickness of 300 nm or more and 10,000 nm or less. Additionally, as... Figure 17As shown, the oxygen concentration of the AlN-containing membrane 100 is 10. 18 cm -3 Above and 10 21 cm -3 Below, the hydrogen concentration is 10. 16 cm -3 Above and 2×10 17 cm -3 the following.
[0302] As described above, by employing the manufacturing method of this embodiment, the AlN-containing film 100 of the nitride semiconductor substrate 11, which serves as a substrate for semiconductor elements, has a sufficiently thick film thickness and high crystallinity, thereby achieving a high-quality nitride semiconductor substrate 11.
[0303] [Evaluation of Nitride Semiconductor Substrates 3]
[0304] Furthermore, here, the evaluation results of the crystallinity of the AlN-containing film 100 of the nitride semiconductor substrate 11 manufactured by changing the manufacturing conditions in the manufacturing method of the first example of this embodiment will be explained. In addition, in the [Evaluation 3 of nitride semiconductor substrate], the descriptions that are repeated with the [Evaluation 1 of nitride semiconductor substrate] are sometimes omitted or simplified.
[0305] In [Evaluation of Nitride Semiconductor Substrate 3], the evaluation mainly focuses on nitride semiconductor substrate 11, which has the same structure as substrate number A1 except for the following two points. Specifically, the two points are that the thickness of the first AlN film 10 (including AlN film 100) is 100, 200, 300, 400, 500, 600, 700, 1000 or 1100 nm, and the annealing temperature in the first annealing process is 1700 °C and the annealing time is 1, 3, 6, 9 or 12 hours.
[0306] Figure 18 This is a graph showing the relationship between the film thickness, annealing time, and through dislocation density of the AlN-containing film 100 involved in this embodiment. (See figure) Figure 18 As shown, substrates 2 with AlN films 100 having a thickness of 100, 200, 300, 400, 500, 600, 700, 1000 or 1100 nm were annealed for 1, 3, 6, 9 or 12 hours respectively, thereby manufacturing multiple nitride semiconductor substrates 11.
[0307] Furthermore, the through dislocation densities of each of the multiple nitride semiconductor substrates 11 are calculated. Moreover, the through dislocation densities can be calculated from the full width at half maximum (WHM) of the XRC values of the (0002) and (10-12) planes.
[0308] The longer the annealing time, the lower the through dislocation density. Furthermore, the thicker the AlN film (100), the lower the through dislocation density. However, if... Figure 18 As shown, if the thickness of the AlN film 100 exceeds the specified thickness, the through dislocation density increases. In other words, if the thickness of the AlN film 100 exceeds the upper limit, the through dislocation density deteriorates. This is because if the thickness of the AlN film 100 increases, the half-width of the XRC of the (0002) plane increases, that is, the axial rocking of the c-axis of the grain increases.
[0309] In addition, such as Figure 18 As shown, when the thickness of the AlN film 100 is 2000 nm or less, more specifically 1500 nm or less, and even more specifically 1000 nm or less, the through dislocation density can be sufficiently reduced, indicating that the crystallinity of the nitride semiconductor substrate 11 according to this embodiment can be improved. In other words, a high-quality nitride semiconductor substrate 11 can be achieved. Figure 18 When the thickness of the AlN film 100 is between 500 nm and 1500 nm, it can be read as a value that allows the through dislocation density to be between 2 × 10⁻⁶. 8 cm -2 the following.
[0310] [Semiconductor Components]
[0311] Furthermore, here, a semiconductor device incorporating the nitride semiconductor substrates 11, 21, and 31 according to this embodiment will be described. The semiconductor device may be, for example, a high electron mobility transistor (HEMT), but here it is an ultraviolet light-emitting device. In particular, it can be used as a deep ultraviolet LED with a wavelength of 200 nm or more and 280 nm or less.
[0312] Reference Figure 19 The configuration of the ultraviolet light emitting element 400 according to this embodiment will be described.
[0313] Figure 19 This is a schematic diagram of the stacked structure of the ultraviolet light emitting element 400 involved in this embodiment.
[0314] As an example, the ultraviolet light-emitting element 400 comprises a nitride semiconductor substrate 11, a planarization layer 3, a buffer layer 4, an electron injection layer 5, a light-emitting layer 6, an electron blocking layer 7, a hole injection layer 8, and an electrode contact layer 9, which are formed sequentially.
[0315] The planarization layer 3 is made of AlN, but is not limited to it. For example, the planarization layer 3 can also be AlN, AlGaN, or AlGaInN. The planarization layer 3 is used to planarize the surface of the nitride semiconductor substrate 11. In addition, the planarization layer 3 also serves to integrate the lattice constant.
[0316] Furthermore, buffer layer 4 is made of AlGaN, but is not limited to this. Like planarization layer 3, buffer layer 4 can also be made of AlN, AlGaN, or AlGaInN. Buffer layer 4, like planarization layer 3, functions as a layer for integrating the lattice constant.
[0317] Furthermore, the electron injection layer 5 is made of n-AlGaN, but is not limited to this. Similar to the planarization layer 3 and the buffer layer 4, it can also be AlN, AlGaN, or AlGaInN, for example. In addition, for the purpose of performing the electron injection function, the electron injection layer 5 is preferably an n-type semiconductor.
[0318] Furthermore, the electron injection layer 5 can also function as an electron transport layer. To function as an n-type semiconductor, the electron injection layer 5 can be made of doping materials such as Si (silicon), Ge (germanium), Sn (tin), O (oxygen), S (sulfur), Se (selenium), or Te (tellurium), but Si is used in this embodiment.
[0319] Furthermore, the light-emitting layer 6 can be an MQW (Multiple Quantum Well) layer formed by multiple AlGaN layers with different Al compositions. MQW refers to a structure of multiple quantum wells formed by overlapping multiple quantum wells.
[0320] The light-emitting layer 6 injects electrons and holes from the electron injection layer 5 and the hole injection layer 8. In the light-emitting layer 6, electrons and holes recombine to emit light. That is, the larger the energy difference between the conduction band and the valence band of the light-emitting layer 6, i.e., the larger the band gap, the shorter the wavelength of light emitted.
[0321] AlGaN can have its own band gap, ranging from 3.4 eV (GaN) to 6.0 eV (AlN), because the composition ratio of Al and Ga can be controlled. Since this region is the ultraviolet emission region, AlGaN is suitable as a light-emitting material for ultraviolet light-emitting devices.
[0322] The electron blocking layer 7 is made of AlN, but is not limited to it. Similar to the planarization layer 3, buffer layer 4, and electron injection layer 5, it can also be made of AlN, AlGaN, or AlGaInN, for example. The electron blocking layer 7 prevents electrons injected from the electron injection layer 5 from leaking from the light-emitting layer 6 towards the hole injection layer 8. Therefore, the electron blocking layer 7 functions effectively by being made of a material with a larger band gap than the light-emitting layer 6.
[0323] The electron blocking layer 7 can also be a structure in which multiple materials with different band gaps are stacked. The electron blocking layer 7 can also be a structure in which the band gap varies continuously relative to the stacking direction. For p-type semiconductorization, the electron blocking layer 7 can also be doped with elements other than Al, Ga, In, and N as impurities.
[0324] The hole injection layer 8 is p-AlGaN, but is not limited to this. Like the planarization layer 3, buffer layer 4, electron injection layer 5, and electron blocking layer 7, the hole injection layer 8 can also be AlN, AlGaN, or AlGaInN. This hole injection layer 8 has the function of injecting holes into the light-emitting layer, and can also have the function of transporting holes. Furthermore, for p-type semiconductorization, the hole injection layer 8 can be doped with Mg (magnesium), Be (beryllium), C (carbon), or Zn (zinc), but Mg is used in this embodiment.
[0325] The electrode contact layer 9 uses p-AlGaN with added doping material compared to the hole injection layer 8, but is not limited to this. Like the planarization layer 3, buffer layer 4, electron injection layer 5, electron blocking layer 7, and hole injection layer 8, the electrode contact layer 9 can also be made of AlN, AlGaN, or AlGaInN, for example. The electrode contact layer 9 is connected to the electrode supplying holes.
[0326] As described above, the nitride semiconductor substrate 11 of this embodiment has high crystallinity, thus enabling the semiconductor element of this embodiment to exhibit high performance. For example, when the semiconductor element is an ultraviolet light-emitting element 400, since the decrease in light-emitting performance caused by through dislocations and the like in the nitride semiconductor substrate 11 can be suppressed, the ultraviolet light-emitting element 400 has high luminous efficiency. Furthermore, the same effect can be obtained even when nitride semiconductor substrates 21 and 31 are used.
[0327] Thus, by incorporating the nitride semiconductor substrates 11, 21, and 31 of this embodiment into the semiconductor element, a semiconductor element with high characteristics can be realized.
[0328] (other)
[0329] The above describes the nitride semiconductor substrate and the like involved in the embodiments, but the present invention is not limited to the above embodiments.
[0330] For example, in this embodiment, AlN-containing films 100, 200, and 300 were formed by sputtering, but the method is not limited to this. For example, MOVPE, hydride vapor phase epitaxy (HVPE), molecular beam epitaxy (MBE), etc., can also be used.
[0331] Furthermore, the present invention also includes various modifications conceived by those skilled in the art to the above embodiments, or any combination of constituent elements and functions in the embodiments without departing from the spirit of the present invention.
[0332] Industrial availability
[0333] This invention can be used as a high-quality nitride semiconductor substrate, as an ultraviolet light emitting element, and other optical semiconductor devices.
[0334] Symbol Explanation
[0335] 2: Substrate
[0336] 3: Planarization layer
[0337] 4: Buffer layer
[0338] 5: Electron injection layer
[0339] 6: Emissive layer
[0340] 7: Electron blocking layer
[0341] 8: Hole injection layer
[0342] 9: Electrode contact layer
[0343] 10: First AlN film
[0344] 11, 21, 31: Nitride semiconductor substrates
[0345] 20: Second AlN film
[0346] 30: Third AlN film
[0347] 100, 200, 300: AlN-containing film
[0348] 101: Inhalation tube
[0349] 102: Exhaust pipe
[0350] 103: Valves
[0351] 104: Exhaust pump
[0352] 105: Substrate pallet
[0353] 107: Target
[0354] 108: Permanent magnet
[0355] 109: High-voltage power supply
[0356] 110: Chamber
[0357] 400: Ultraviolet light emitting element
[0358] 1000: Sputtering device
[0359] S21, S31, S41: First process
[0360] S22, S32, S42: Second process
[0361] S23, S33, S43: Third process
[0362] S24, S34, S44: Fourth process
[0363] S35, S45: Fifth process
[0364] S36, S46: Step 6
[0365] S47: Step 7
[0366] S48: 8th process
Claims
1. A nitride semiconductor substrate comprising: substrate, and An AlN-containing film is disposed above the substrate; The thickness of the AlN-containing film is less than 10000 nm. The interconnected dislocation density of the AlN-containing film is 1.5 × 10⁻⁶. 8 cm -2 the following, The full width at half maximum (WHM) of the X-ray diffraction rocking curve in the (10-12) plane of the AlN film is less than 120 arcsec. The substrate is composed of one of sapphire, silicon carbide, and ScAlMgO4. The AlN-containing film has a first AlN film disposed above the substrate and a second AlN film disposed above the first AlN film. The thickness of the first AlN film is greater than 100 nm and less than 900 nm. The thickness of the second AlN film is greater than 100 nm and less than 900 nm.
2. The nitride semiconductor substrate according to claim 1, wherein, The oxygen concentration of the AlN-containing membrane is 10. 18 cm -3 Above and 10 21 cm -3 the following, The hydrogen concentration of the AlN-containing membrane is 10. 16 cm -3 Above and 2×10 17 cm -3 the following.
3. The nitride semiconductor substrate according to claim 1, wherein, The density of the through dislocations is 1.0 × 10⁻⁶. 8 cm -2 the following.
4. The nitride semiconductor substrate according to claim 1, wherein, The AlN-containing film contains at least one interface layer with a maximum element concentration between itself and the substrate.
5. The nitride semiconductor substrate according to claim 4, wherein, The thickness of the interface layer is greater than 10 nm and less than 200 nm. In the interface layer, the oxygen or silicon concentration is more than twice as high as that in the layers surrounding the interface layer.
6. The nitride semiconductor substrate according to claim 1, wherein, The AlN-containing membrane is composed of AlN and Al x Ga y In 1-x-y N and B z Al w Ga 1-z-w One composition of N, wherein 0.5≤x≤1, 0≤y≤0.5, x+y≤1, 0≤z≤0.5, 0.5≤w≤1, and z+w≤1 are the conditions for the composition ratio.
7. The nitride semiconductor substrate according to any one of claims 1 to 6, wherein, The thickness of the AlN-containing film is less than 2000 nm.
8. A semiconductor device comprising a nitride semiconductor substrate according to any one of claims 1 to 7.
9. A method for manufacturing a nitride semiconductor substrate, comprising: Preparation steps for preparing the substrate. The film formation process of forming an AlN film with a thickness of 100 nm or more and 900 nm or less on the substrate, and An annealing process that anneals the AlN film formed in the film-forming process at a temperature above 1500°C. At least one of the film-forming process and the annealing process is performed multiple times. The through dislocation density of the AlN-containing film having the AlN film is 1.5 × 10⁻⁶. 8 cm -2 the following, The full width at half maximum (WHM) of the X-ray diffraction rocking curve in the (10-12) plane of the AlN-containing film having the AlN film is less than 120 arcsec. In the annealing process, the AlN film, which has been formed in the film-forming process, is annealed in an airtight state with the main surface of the AlN film covered by a cover member. The cover member is used to suppress the dissociation of the components of the material constituting the AlN film. In the film-forming process, the AlN film is formed by sputtering. In the annealing process, the AlN film is annealed at a temperature above 1500°C and below 1750°C. Between the multiple annealing processes, the substrate is held at a temperature lower than the temperature at which the AlN film is annealed.
Citation Information
Patent Citations
Nitride semiconductor substrate manufacturing method, nitride semiconductor substrate and heating device of the same
JP2017055116A
Method of producing periodic table group 13 metal nitride semiconductor crystal and periodic table group 13 metal nitride semiconductor crystal produced by this production method
US20140294713A1