Portable wireless intelligent sensor based on black phosphorus-based composite material for determining 6,7-dihydroxycoumarin

By modifying a screen-printed electrode with a composite material of black phosphorus and nanodiamond, a portable wireless smart sensor was constructed, which solved the problems of long detection time and high cost of 6,7-dihydroxycoumarin in the prior art, and achieved detection effect with high sensitivity and fast response.

CN115201290BActive Publication Date: 2026-11-24HAINAN NORMAL UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202210283034.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-22
Publication Date
2026-11-24
Estimated Expiration
2042-03-22

AI Technical Summary

Technical Problem

Existing electrochemical detection methods for 6,7-dihydroxycoumarin suffer from problems such as long detection time, high cost, and complex operation, and lack the high sensitivity and rapid response capability of portable wireless intelligent sensors.

Method used

A screen-printed electrode (SPE) based on a black phosphorus (BP) and nanodiamond (ND) composite material is used to form an ND@BP composite material through a simple preparation method. This material is used to construct a portable wireless smart sensor for electrochemical detection via a smartphone or computer connection.

Benefits of technology

It achieves high sensitivity and fast response capability of portable wireless smart sensor, with significant detection effect, low cost and simple operation, and is suitable for rapid detection of 6,7-dihydroxycoumarin.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115201290B_ABST
    Figure CN115201290B_ABST
Patent Text Reader

Abstract

This invention designs a portable wireless intelligent sensor based on a black phosphorus / nanodiamond composite material for the determination of 6,7-dihydroxycoumarin. A portable wireless intelligent sensor modified with a composite material (ND@BP) was prepared by combining black phosphorus and nanodiamond, and this sensor was used for the detection of 6,7-dihydroxycoumarin (6,7-DHC). The main steps include: (1) preparation of a thin layer of black phosphorus (BP); (2) preparation of the ND@BP composite material; (3) preparation of the modified electrode: using a drop-coating method, in a glove box filled with N2, the ND@BP composite material was drop-coated onto the surface of a screen-printed electrode (SPE), and then naturally dried to prepare the ND@BP / SPE electrode; (4) preparation of the portable wireless intelligent sensor: using a portable workstation connected to a smartphone or computer via Bluetooth, the constructed sensor was used for the detection of 6,7-DHC, and the sensor was applied to the detection of actual drugs containing 6,7-DHC. This invention has a simple process, low manufacturing cost, is portable, highly sensitive, intelligent, and has significant measurement effects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of portable wireless intelligent sensor fabrication, and relates to a portable wireless intelligent sensor based on a two-dimensional black phosphorus (BP) and nanodiamond (ND) composite material modified screen-printed electrode (SPE) for the determination of 6,7-dihydroxycoumarin (6,7-DHC). Background Technology

[0002] Coumarins are a general term for o-hydroxycinnamic acid lactones with benzo-α-pyranone as the basic skeleton. Most coumarin compounds are characterized by oxygen functional groups linked at the 6 and 7 positions. Therefore, 6,7-DHC is one of the coumarin derivatives, widely found in various plants such as artemisia and lemon. It has attracted attention due to its strong antioxidant properties and has been widely used in the medical field. However, research on the electrochemical applications of 6,7-DHC is limited. The methods for determining 6,7-DHC mainly focus on liquid chromatography detection. Although this method can detect 6,7-DHC, it still has some shortcomings in terms of detection time, cost, and operation. Therefore, the development of a rapid detection method for 6,7-DHC is imperative. BP is a novel two-dimensional nanomaterial with unique physical and structural properties, such as large specific surface area, high thermal stability, low cytotoxicity, and biocompatibility. It is widely used in biosensing, photothermal therapy, drug delivery, and other fields. However, black phosphorus exhibits excellent biodegradability, readily degrading into PxOy in oxygen- and water-containing environments. To improve the environmental stability of BP, prevent degradation, or enhance functionality, many reports primarily focus on adding protective agents or modifying its surface. Nitrogen oxides (NDs) are a unique class of carbon nanoparticles, attracting increasing attention due to their excellent electronic properties, wide electrochemical potential window, low dielectric constant, excellent biocompatibility, and chemical stability, and are frequently used in the construction of electrochemical and biosensors. The core component of electrochemical detection is the modified electrode; ND@BP composite modified electrodes combine the advantages of both NDs and BPs, exhibiting excellent electrochemical performance. Electrochemical testing methods offer advantages such as compact equipment, small sample volume, and simple operation. For the detection of 6,7-DHC, they offer advantages such as low operating environment requirements and diverse modification materials. Portable wireless intelligent sensors, on the other hand, are characterized by simple preparation, portability, wireless operation, speed, high sensitivity, easy modification, good stability, wide detection range, and the ability to detect anytime, anywhere. In addition, the rise of electronic products such as smartphones and computers has driven the rapid development of biosensors. With the increasing analytical requirements in research and practical applications, high sensitivity, selectivity, and fast response speed remain the demands for portable wireless smart sensors. Summary of the Invention

[0003] In view of this, the present invention provides a new method for determining 6,7-DHC. The portable wireless smart sensor provided by the present invention is simple to prepare, low in cost, and effective. During the electrochemical testing process, it has a high effective surface area and analytical detection performance.

[0004] This invention provides an ND@BP composite material, which exhibits excellent stability.

[0005] Preferably, the effective surface area of ​​the ND@BP composite material is 0.181 cm². 2 ; Preferably, the ND@BP composite material has a thin sheet-like structure and a relatively uniform morphology.

[0006] This invention provides the fabrication of the portable wireless smart sensor described in the above technical solution, comprising the following steps: (1) Mix and stir BPNPs and NMP, then sonicate in an ice bath for 5 minutes and centrifuge; (2) Based on step 1, mix thin-layer BP with ND and sonicate for 4 hours, then let stand in a 4 ℃ refrigerator for 24 hours to obtain ND@BP composite material; (3) Based on step 2, drop-coat the ND@BP composite material onto the surface of SPE in a glove box and air dry to prepare ND@BP / SPE electrode; (4) Use a portable workstation to connect with a smartphone or computer via Bluetooth to the modified electrode obtained in step (3) for the detection of 6,7-DHC, and apply the sensor to the detection of actual drugs containing 6,7-DHC; (5) Air dry the electrode obtained in step (4) at room temperature and construct a three-electrode system for electrochemical testing.

[0007] Preferably, the concentration of the nano ND is 1.0 mg / mL, and the BP solution is generally a thin-layer BP dispersion; the ND@BP composite material is made by mixing ND and BP at a volume ratio of 1:1, ultrasonically treating, and then standing in a refrigerator at 4°C for 24 hours.

[0008] Preferably, the ND@BP composite material modified electrode is prepared in a glove box filled with N2.

[0009] Preferably, the detection concentration of 6,7-DHC is 1.0 × 10⁻⁶. -4 mol / L.

[0010] Preferably, the portable wireless smart sensor is connected to a smartphone or computer via Bluetooth using a portable workstation.

[0011] This invention provides a portable wireless smart sensor based on black phosphorus (BP) and nanodiamond (ND) composite for determining 6,7-dihydroxycoumarin (6,7-DHC) as described in the above technical solution, or the application of the modified electrode prepared as described in the above technical solution in portable wireless smart sensor materials.

[0012] The portable wireless smart sensor provided by this invention utilizes a portable electrochemical workstation to wirelessly connect to smartphones or computers via Bluetooth. The composite material provided by this invention is composed of ND and BP, possessing a large effective area and combining the performance characteristics of both, effectively improving the conductivity and effective area of ​​the portable wireless smart sensor. Results from the embodiments show that the ND@BP composite material modified electrode provided by this invention has an effective area of ​​0.181 cm² at a potassium ferricyanide concentration of 1.0 mmol / L. 2 . Attached Figure Description

[0013] Figure 1 Scanning electron microscope (SEM) and transmission electron microscope (TEM) images of the ND@BP composite material prepared in Example 1.

[0014] Figure 2 Cyclic voltammetry curves of different modified electrodes prepared for test example 1 in a mixed electrolyte of 1.0 mmol / L K3[Fe(CN)6] and 0.5 mol / L KCl.

[0015] Figure 3 Cyclic voltammetry curves of the modified electrode ND@BP / SPE of Test Example 1 at different scan rates in a mixed electrolyte of 1.0 mmol / L K3[Fe(CN)6] and 0.5 mol / L KCl.

[0016] Figure 4 The redox peak current and υ of the ND@BP / SPE modified electrode prepared in Example 1 at different scan rates were tested. 1 / 2 The linear relationship.

[0017] Figure 5 The concentration optimization diagram is shown for test example 1ND.

[0018] Figure 6 Cyclic voltammetry curves of different modified electrodes in 0.1 mmol / L phosphate buffer (PBS) were used to test Example 1.

[0019] Figure 7 Cyclic voltammetry curves of the ND@BP / SPE modified electrode prepared for test example 1 in PBS at different pH values.

[0020] Figure 8The DPV curve of the ND@BP / SPE modified electrode in Test Example 2 is shown in 0.1 mol / L 6,7-DHC. Detailed Implementation

[0021] This invention provides a portable wireless smart sensor based on a black phosphorus (BP) / nanodiamond (ND) composite material for the determination of 6,7-dihydroxycoumarin (6,7-DHC). The portable wireless smart sensor provided by this invention has a simple, easy-to-operate, and low-cost preparation method, and exhibits significant detection performance when used for the determination of 6,7-dihydroxycoumarin.

[0022] The effective area of ​​the ND@BP / SPE provided by this invention is 0.181 cm². 2 .

[0023] Preferably, the ND@B composite material has a thin sheet-like structure and a relatively uniform morphology.

[0024] This invention provides the fabrication of the portable wireless smart sensor described in the above technical solution, comprising the following steps: First, BPNPs and NMP are mixed and stirred, then sonicated in an ice bath for 5 minutes and centrifuged. Thin-layer BP is mixed with ND and sonicated for 4 hours, then allowed to stand in a 4 ℃ refrigerator to obtain ND@BP composite material. In a glove box, ND@BP composite material is drop-coated onto the surface of SPE and air-dried to prepare ND@BP / SPE electrode.

[0025] In this invention, the concentration of the nano ND is 1.0 mg / mL, and the BP solution is generally a thin-layer BP dispersion; the ND@BP composite material is made by mixing ND and BP at a volume ratio of 1:1, ultrasonically treating, and then standing in a refrigerator at 4°C for 24 hours.

[0026] The preferred method for preparing the ND@BP composite material modified electrode is to perform the preparation in a glove box filled with N2. Preferably, the drop-coated ND@BP composite material undergoes post-treatment to obtain the ND@BP / SPE modified electrode. In this invention, the post-treatment is preferably performed by drying at room temperature in a glove box filled with N2. The ND@BP composite material has the characteristics of large specific surface area and high conductivity.

[0027] In this invention, the modified electrode is refrigerated in a refrigerator at around 4°C when not in use, and there are no special requirements for refrigeration time and temperature.

[0028] In this invention, a specific process for modifying the modified electrode as described above is provided, which mainly includes: optimization of ND concentration.

[0029] In this invention, the concentration of ND is 0.5 mg / mL, 1.0 mg / mL, 1.5 mg / mL, 2.0 mg / mL, and more preferably 1.0 mg / mL.

[0030] After obtaining the modified electrode, the present invention preferably dries the modified electrode at room temperature in a glove box to obtain the ND@BP / SPE working electrode. In the present invention, the reference electrode is preferably a saturated calomel electrode, and the counter electrode is preferably a platinum wire electrode; the present invention has no special requirements on the thickness of the drop coating and the specific implementation process of the coating, and conventional drop coating thickness and operation known to those skilled in the art can be used; in the present invention, there are no specific requirements on the drying time, and air drying is sufficient.

[0031] To further illustrate the present invention, the technical solutions provided by the present invention will be described in detail below with reference to the embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0032] Example 1 First, BPNPs and NMP are mixed and stirred, then sonicated in an ice bath for 5 minutes and centrifuged. Thin-layer BP is mixed with ND and sonicated for 4 hours, then immediately placed in a 4 ℃ refrigerator and left to stand for 24 hours to obtain ND@BP composite material.

[0033] Figure 1 For the characterization of different modified materials by scanning electron microscopy and transmission electron microscopy, Figure 1 In the figure, A represents the scanning electron microscope characterization of the ND@BP composite material with a scale bar of 100 nm. It can be concluded that the ND@BP composite material prepared in this embodiment has a thin sheet-like structure and a relatively uniform morphology. Figure 1 In the image, B is a transmission electron microscope image of the ND@BP composite material at a scale bar of 10 nm. It can be observed that ND is uniformly distributed on the BP surface and the size of ND is less than 10 nm.

[0034] Example 2 In a glove box filled with N2, the ND@BP composite material was drop-coated onto the surface of the SPE and allowed to air dry. The resulting modified electrode is the ND@BP / SPE. Other modified electrodes (BP / SPE) and SPEs modified with different concentrations of ND (ND / SPE) were prepared using the drop-coating method. All electrodes were stored at approximately 4°C when not in use. A portable workstation was used to connect to a smartphone or computer via Bluetooth for the detection of 6,7-DHC.

[0035] Test Example 1 The ND / SPE, BP / SPE, and ND@BP / SPE electrodes prepared in Example 2 were used as working electrodes, a saturated calomel electrode as a reference electrode, and a platinum wire as a counter electrode. The three electrodes were placed in a mixed electrolyte of 1.0 mmol / L K3[Fe(CN)6] and 0.5 mol / L KCl and the electrochemical performance was tested by cyclic voltammetry.

[0036] Figure 2 Cyclic voltammetry curves of the ND / SPE, BP / SPE, and ND@BP / SPE electrodes prepared in Example 2 at 100 mV / s in a mixed electrolyte of 1 mmol / L K3[Fe(CN)6] and 0.5 mol / L KCl are shown below. Figure 2 As shown, compared with the bare SPE (curve a), the peak current increased significantly after nano-ND was drop-coated onto the SPE (curve b). This is mainly because ND has good conductivity, which promotes the Fe... 3+ with Fe 2+ Electron transfer rate between the electrolyte and the electrode. After BP was drop-coated onto SPE (curve c), the peak current signal further increased, indicating that BP has stronger conductivity. When ND@BP was modified onto SPE (curve d), the peak current signal further increased, indicating that the conductivity of the ND@BP composite material was further improved after modification, providing a faster channel for electron transfer. From Figure 2 It can be seen that the redox peak current of ND@BP / SPE is the largest compared to that of other modified electrodes.

[0037] Figure 3 Cyclic voltammetry curves of the ND@BP / SPE electrode prepared in Example 2 at different scan rates in a mixed electrolyte of 1 mmol / L K3[Fe(CN)6] and 0.5 mol / L KCl were obtained. Figure 3 It can be seen that as the scan rate increases, the redox peak potential shifts to the positive and negative directions, respectively, and the redox peak current also gradually increases with the increase of the scan rate.

[0038] Figure 4 The redox peak current and υ of the ND@BP / SPE modified electrode prepared in Example 2 at different scan rates 1 / 2 The linear relationship, from Figure 4 It can be seen that the redox peak current and υ 1 / 2 A good linear relationship is formed.

[0039] Figure 5The diagram shows the concentration optimization corresponding to ND as described in Example 2. Dispersions with concentrations of 0.5 mg / mL, 1.0 mg / mL, 1.5 mg / mL, and 2.0 mg / mL were prepared, and 15 μL of each was uniformly coated onto the SPE surface and air-dried at room temperature to obtain four ND / SPE electrodes. The electrochemical performance of the four electrodes was tested using cyclic voltammetry in an electrolyte containing 1.0 mmol / L K3[Fe(CN)6] and 0.5 mol / L KCl at a scan rate of 100 mV / s.

[0040] Figure 6 The following are cyclic voltammograms of different modified electrodes in 0.1 mmol / L PBS in Example 2. Figure 7 In the SPE (curve a), a pair of reversible redox peaks appear. In the ND / SPE (curve b), the redox peak current is larger than that in curve a, indicating that ND has good conductivity. In the BP / SPE (curve c), the oxidation peak further increases, while the reduction peak changes little, indicating that the conductivity of BP is stronger than that of ND. In the ND@BP / SPE (curve d), the oxidation peak continues to increase, while the reduction peak does not change significantly, indicating that the synergistic effect of ND and BP is very obvious.

[0041] Figure 7 The graph shows the pH change of ND@BP / SPE in Example 2. It can be seen from the graph that the redox peak potentials gradually shift towards the negative direction as the pH increases. This indicates that the redox peak current is largest at pH 3.0.

[0042] Test Example 3 The ND@BP / SPE electrode prepared in Example 2 was used as the working electrode, the saturated calomel electrode as the reference electrode, and the platinum wire as the counter electrode. The three electrodes were placed in a mixed electrolyte of 10.0 mmol / L K3[Fe(CN)6] and 0.1 mol / L KCl and the electrocatalytic performance was tested by differential pulse voltammetry (DPV).

[0043] Figure 8 The DPV diagrams for the modified electrode ND@BP / SPE in Example 2 at different concentrations of 6,7-DHC are shown. With the addition of 6,7-DHC, the reduction peak current gradually increases, while the oxidation peak current gradually decreases until it disappears. When the concentration of 6,7-DHC ranges from 0.01 to 450 µmol / L, the reduction peak current shows a good linear relationship with the 6,7-DHC concentration, and the detection limit is 0.0033 μmol / L (3σ), indicating that the ND@BP composite material has high electrocatalytic activity for 6,7-DHC.

[0044] Although the above embodiments have provided a detailed description of the present invention, they are only some embodiments of the present invention, and not all embodiments. Other embodiments can be obtained based on these embodiments without creative effort, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A method for preparing an ND@BP / SPE electrode, characterized in that, Specifically, the following steps are included: (1) Mix and stir the multilayer nanosheets BPNPs and NMP, then sonicate in an ice bath for 5 minutes, and then centrifuge; (2) Based on step (1), thin-layer BP and nanodiamond are mixed at a volume ratio of 1:1 and ultrasonicated for 4 hours, and then placed in a 4°C refrigerator for 24 hours to obtain ND@BP composite material; The concentration of the nanodiamond is 1.0 mg / mL; (3) Based on step (2), in a glove box filled with N2, the ND@BP composite material is drop-coated onto the surface of the screen-printed electrode SPE and air-dried to obtain the ND@BP / SPE electrode.

2. An ND@BP / SPE electrode prepared by the method described in claim 1.

3. The application of an ND@BP / SPE electrode prepared by the method described in claim 1 in the preparation of a portable wireless smart sensor.

4. A portable wireless smart sensor, characterized in that, This includes the ND@BP / SPE electrode prepared by the method described in claim 1.

5. A method of making a portable wireless smart sensor as claimed in claim 4, wherein, Specifically, the following steps are included: The ND@BP / SPE electrode prepared by the method described in claim 1 was air-dried at room temperature and a three-electrode system was constructed. The system was then connected to a smartphone or computer via Bluetooth using a portable workstation.

6. The application of a portable wireless smart sensor as described in claim 4 in the detection of 6,7-DHC.

Citation Information

Patent Citations

  • Preparation method for black phosphorus quantum dot-graphene nanosheet three dimensional composite

    CN105217611A

  • Electrochemical sensing analysis method for simply and quickly detecting OTA (ochratoxin A) in food

    CN108181371A

  • Preparation and application of nanocrystalline graphite / boron-doped diamond composite material

    CN112899640A