Molded body of composite resin with adjusted decomposition rate and method for manufacturing the same
By dispersing natural fibers in the main resin and covering them with a hydrolytic coating resin, the problem of insufficient mechanical strength and decomposition rate of biodegradable plastics in humid environments is solved, achieving high elastic modulus and high biodegradability.
Patent Information
- Application Number
- CN202210427785.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-04-30
- Filing Date
- 2022-04-22
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2042-04-22
AI Technical Summary
Existing biodegradable plastics have shortcomings in terms of mechanical strength and decomposition rate, especially in environments with few microorganisms where the decomposition rate is slow. They are also prone to hydrolysis and rigidity degradation during use, which limits their application range.
The method of manufacturing composite resin molded articles involves dispersing multiple natural fibers in the main resin, the surface of which contains microorganisms or enzymes, and covering them with a hydrolyzable coating resin to control the specific surface area of the fiber defibering sites and promote biodegradation in humid environments.
It achieves high elastic modulus and high biodegradability while maintaining high rigidity, making it suitable for humid environments and solving the problems of insufficient mechanical strength and decomposition rate in existing technologies.
Smart Images

Figure CN115260716B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a composite resin molded article with excellent mechanical properties and a biodegradation rate regulated in humid environments, and a method for manufacturing the same. Background Technology
[0002] Polyethylene (PE), polypropylene (PP), polystyrene (PS), and polyvinyl chloride (PVC), known as "general-purpose plastics," are not only very inexpensive but also easy to mold. Compared to metals or ceramics, they are only a fraction of the weight, making them lightweight. Therefore, general-purpose plastics are frequently used as materials for bags, various packaging materials, containers, sheets, and many other everyday consumer goods. They are also commonly used in automotive parts, electrical components, and other industrial parts, as well as in daily necessities and general merchandise.
[0003] As a result, the amount of plastic waste after use is increasing year by year. Because it is a substance that is not easily decomposed, it accumulates in the natural environment, causing environmental damage and pollution. In recent years, as one of the solutions to these problems, biodegradable plastics that decompose into water and carbon dioxide in the natural environment have been proposed, with the expectation that they will be widely used to replace general-purpose plastics that use petroleum-based raw materials.
[0004] However, compared to general-purpose plastics, biodegradable plastics have drawbacks such as insufficient mechanical strength. Therefore, the current situation is that biodegradable plastics do not possess the sufficient properties required for materials used in mechanical products such as automobiles, as well as various industrial products, including electrical / electronic / information products, thus limiting their application scope. Furthermore, biodegradable plastics are often prone to decomposition, leading to hydrolysis and rigidity degradation during use.
[0005] On the other hand, the biodegradation rate of discarded biodegradable plastics has a significant impact on the environment. In marine environments with few microorganisms, complete decomposition takes a long time, and biodegradability and other properties cannot be fully utilized. To address this issue, various methods have been proposed to accelerate the decomposition of biodegradable plastics after disposal.
[0006] For example, methods for coating or incorporating microorganisms with enzyme activity that decomposes biodegradable plastics have been disclosed (e.g., see Patent Document 1); and methods for pre-encapsulating microorganisms in biodegradable plastics (e.g., see Patent Document 2).
[0007] Existing technical documents
[0008] Patent documents
[0009] Patent Document 1: Japanese Patent Application Publication No. 2013-209587
[0010] Patent Document 2: Japanese Patent Application Publication No. 2020-520794 Summary of the Invention
[0011] One aspect of the present invention relates to a composite resin molded body comprising: a main resin and a plurality of natural fibers dispersed in the main resin, each of the plurality of natural fibers containing microorganisms or enzymes, wherein when the composite resin molded body is set to 100% by mass, the content of the plurality of natural fibers containing microorganisms or enzymes is 10% by mass or more and 99% by mass or less, at least one of the plurality of natural fibers is exposed on the surface of the composite resin molded body, and at least a portion of the surface of at least one of the plurality of natural fibers is coated with a hydrolyzable coating resin.
[0012] One aspect of the present invention relates to a method for manufacturing a composite resin molded article, comprising: a step of preparing microorganisms or enzymes, natural fibers, a hydrolyzable coating resin, and a main resin; a step of containing microorganisms or enzymes in the natural fibers; a step of melt-blending the natural fibers containing microorganisms or enzymes together with the coating resin, wherein the natural fibers containing microorganisms or enzymes are defibered from the ends along the fiber length direction to expand the surface area of the defibered portion at the ends; and a step of molding the coated natural fibers, on which at least a portion of the surface of the natural fibers is coated with the coating resin, together with the main resin into a composite resin molded article. Attached Figure Description
[0013] Figure 1 This is a schematic cross-sectional view showing the cross-sectional structure of the composite resin molded body according to Embodiment 1.
[0014] Figure 2 This is a schematic cross-sectional view showing the cross-sectional structure of the natural fibers that form the constituent components of the composite resin molded body according to Embodiment 1.
[0015] Figure 3 This is a schematic cross-sectional view showing the cross-sectional structure of a composite resin molded body containing natural fibers with defiberization sites according to Embodiment 1.
[0016] Figure 4 This is a schematic diagram of the manufacturing process of the composite resin molded body involved in Embodiment 1.
[0017] Figure 5 This is a diagram showing the composition and measurement results of the composite resin molded articles in the embodiments and comparative examples of the implementation.
[0018] Explanation of reference numerals in the attached figures
[0019] 1. Main agent resin
[0020] 2. Natural fibers
[0021] 3 Coating resin
[0022] 4. Microorganisms or enzymes
[0023] 5. Surface of the molded body
[0024] 10 Composite resin molded body. Detailed Implementation
[0025] In the method described in Patent Document 1, since microorganisms are directly mixed into biodegradable plastics, the material is limited to biodegradable plastics that can be molded at temperatures where microorganisms can survive. On the other hand, in the method described in Patent Document 2, in order to release the microorganism C microcapsules, the molded body must be physically destroyed, resulting in a problem that the rigidity of the molded body decreases as the content of microcapsules increases.
[0026] In order to solve the above-mentioned existing problems, the object of the present invention is to provide a composite resin molded body that maintains high rigidity during use and promotes biodegradation in humid environments such as oceans and soil after disposal.
[0027] The composite resin molded body involved in the first method contains: a main resin and a plurality of natural fibers dispersed in the main resin, each of the plurality of natural fibers containing microorganisms or enzymes, and when the composite resin molded body is set to 100% by mass, the content of the plurality of natural fibers containing microorganisms or enzymes is 10% by mass or more and 99% by mass or less, at least one of the plurality of natural fibers is exposed on the surface of the composite resin molded body, and at least a portion of the surface of at least one of the plurality of natural fibers is coated with a hydrolyzable coating resin.
[0028] Regarding the composite resin molded body involved in Method 2, in Method 1 above, the moisture content of the multiple natural fibers can be 5% or more by means of the method specified in ASTM D 1909.
[0029] Regarding the composite resin molded body involved in the third method, in the first or second method mentioned above, the main resin can be a biodegradable resin containing any substance selected from polyhydroxy acids, polyhydroxyalkanoates, polyalkylene dicarboxylates, and modified starches.
[0030] Regarding the composite resin molded body involved in the fourth method, in any of the methods 1 to 3 above, the melting point of the coated resin can be above the melting point of the main resin and below the carbonization temperature of the plurality of natural fibers.
[0031] Regarding the composite resin molded body involved in the fifth method, in any of the methods 1 to 4 above, the plurality of natural fibers may include fibers and microorganisms or enzymes supported on the surface of the fibers.
[0032] Regarding the composite resin molded body involved in the sixth method, in any of the methods 1 to 5 above, the plurality of natural fibers can be cellulose-based.
[0033] Regarding the composite resin molded body involved in the seventh method, in any of the methods described in the first to sixth methods above, at least one of the plurality of natural fibers may have a defibering portion at the end in the fiber length direction.
[0034] The method for manufacturing a composite resin molded body according to the eighth method includes: a step of preparing microorganisms or enzymes, natural fibers, a hydrolyzable coating resin, and a main resin; a step of containing microorganisms or enzymes in the natural fibers; a step of melt-blending the natural fibers containing microorganisms or enzymes with the coating resin, and a step of defiring the natural fibers from the ends along the fiber length direction to expand the surface area of the defiring portion at the ends; and a step of molding the coated natural fibers, whose surface at least a portion is coated with the coating resin, with the main resin after blending the coated natural fibers with the main resin.
[0035] Regarding the manufacturing method of the composite resin molded body involved in the above-mentioned ninth method, in the step of molding the composite resin molded body in the above-mentioned eighth method, the molding temperature can be set to a temperature of 125% or less of the melting point of the coated resin.
[0036] According to one aspect of the present invention, a composite resin molded article can achieve, compared with a single resin, a composite resin molded article that, in addition to high elastic modulus, also allows for controlled biodegradation rate in humid environments.
[0037] Hereinafter, the composite resin molded article and its manufacturing method according to the embodiments will be described with reference to the accompanying drawings. It should be noted that in the following description, the same symbols will be used to refer to the same components and descriptions will be omitted as appropriate.
[0038] (Implementation Method 1)
[0039] Figure 1 This is a schematic cross-sectional view showing the cross-sectional structure of the composite resin molded body 10 according to Embodiment 1. Figure 2 This is a schematic cross-sectional view showing the cross-sectional structure of natural fibers that are constituent components of the composite resin molded body 10 according to Embodiment 1.
[0040] The composite resin molded article 10 according to Embodiment 1 comprises a melt blend of a main resin 1 and natural fibers 2, wherein the natural fibers 2 are coated with a coating resin 3 and contain microorganisms or enzymes 4. Regarding the composite resin molded article 10, as... Figure 1As shown in the schematic cross-sectional view, natural fibers 2 containing microorganisms or enzymes 4 are dispersed in the main resin 1 and coated with the coating resin 3.
[0041] According to this composite resin molded body 10, at least one natural fiber 2 is exposed on the surface 5 of the molded body, and the natural fibers 2 have joints with each other. Therefore, in addition to high elastic modulus, it also has high water absorption. In a humid environment, if the coating resin 3 hydrolyzes due to water absorption by the natural fibers 2, the microorganisms or enzymes 4 carried on the natural fibers 2 are released, promoting the decomposition of the main resin 1. Therefore, a composite resin molded body 10 that maintains high rigidity during use and has excellent biodegradability in humid environments such as the ocean or soil after disposal can be achieved.
[0042] The components constituting the composite resin molded body are described below.
[0043] <Main Resin>
[0044] In this embodiment, the main agent resin 1 is preferably a biodegradable plastic comprising any substance selected from polyhydroxy acids, polyhydroxyalkanoates, polyalkylene dicarboxylate, and modified starches. Furthermore, to ensure good moldability, a thermoplastic resin is preferred, and the above-mentioned resins can be used alone or in combination of two or more. It should be noted that the main agent resin 1 is not limited to the above-mentioned materials as long as it is biodegradable.
[0045] In this embodiment, "biodegradable plastic" refers to "a resin that, when used, has the same function as existing petroleum-derived resins, and after use, is ultimately decomposed into water and carbon dioxide by microorganisms in the soil and ocean." Specific examples include: polyhydroxybutyrate, polyhydroxyvalerate, and other polyhydroxyalkanoates; polylactic acid, polyglycolic acid, polycaprolactone, and other polyhydroxy acids; polybutylene terephthalate, polyethylene succinate, polybutylene succinate, and other polyalkylene dicarboxylate esters; and modified starch, etc. As polyester resins, in addition to homopolymers of polyester monomers, they also include copolymers of polyester monomers such as poly(3-hydroxybutyrate-co-3-hydroxyvalerate), and copolymers of polyester monomers with other comonomers. These polyester resins can be used alone or in combination of two or more.
[0046] <Natural Fibers>
[0047] Next, the natural fiber 2 will be explained. The primary purpose of adding the natural fiber 2 (hereinafter sometimes simply referred to as "fiber") contained in the composite resin molded body 10 of this embodiment is to minimize the environmental impact when the composite resin molded body 10 is discarded after use, by allowing the coated resin 3 to come into contact with water and hydrolyze through water absorption in soil or ocean. For this purpose, it is preferable that the natural fiber 2 has high water absorption, and the moisture content of the natural fiber 2 is preferably 5% or more according to the method specified in ASTM D 1909. Specifically, it is preferable to use pulp, cellulose, cellulose nanofibers, lignocellulose, lignocellulose nanofibers, cotton, silk, or hemp, etc.
[0048] The second objective of adding natural fiber 2 is to improve mechanical properties and enhance dimensional stability due to a decrease in the coefficient of linear expansion. For this purpose, it is preferable that the elastic modulus of natural fiber 2 is higher than that of the main resin 1. Examples of suitable natural fibers include: pulp, cellulose, cellulose nanofibers, lignocellulose, lignocellulose nanofibers, cotton, silk, wool, or hemp. Furthermore, among these, cellulose-based fibers are particularly preferred from the viewpoints of ease of handling, high elastic modulus, and low coefficient of linear expansion. It should be noted that natural fiber 2 is not limited to the materials mentioned above, as long as it improves mechanical properties and has water absorption.
[0049] When the natural fiber 2 contains microorganisms or enzyme 4, and the composite resin molded body 10 is set to 100% by mass, the content of the natural fiber 2 containing microorganisms or enzyme 4 in the composite resin molded body 10 is preferably 10% by mass or more and 99% by mass or less. If the content of the natural fiber 2 containing microorganisms or enzyme 4 is less than 10% by mass, the natural fibers 2 are unlikely to have joints with each other inside the composite resin molded body 10, and therefore do not have sufficient water absorption. On the other hand, if the content of the natural fiber 2 containing microorganisms or enzyme 4 is greater than 99% by mass, the proportion of the main resin 1 and the coating resin 3 becomes smaller, and therefore the effect of bonding the natural fibers 2 together disappears, resulting in poor moldability.
[0050] The manner in which the natural fibers 2 are incorporated into the composite resin molded body 10 will be explained. When the interface between the natural fibers 2 and the coating resin 3 is large, the hydrolysis of the coating resin 3 is promoted when the natural fibers 2 absorb water; therefore, a high specific surface area of the natural fibers 2 is preferable. On the other hand, to improve the water absorption of the composite resin molded body 10, it is preferable that the natural fibers 2 are exposed on the surface of the composite resin molded body 10. By exposing the natural fibers 2 on the surface of the composite resin molded body 10, the natural fibers 2 absorb water from the exposed portion, and through the capillary effect of the fibers constituting the natural fibers, water is absorbed into the interior of the composite resin molded body 10. When the specific surface area of the natural fibers 2 exposed on the surface of the composite resin molded body is small, the water absorption becomes high. This is because when the specific surface area of the natural fibers 2 exposed on the surface is large, the water repellency becomes high due to the effect of the fine irregularities. Furthermore, as... Figure 3 As shown, by having a defibering portion at the end of the natural fiber 2, the specific surface area of the defibering portion increases, and the number of joints between the natural fibers 2 increases. Thus, the water absorption rate can be increased through the joints of the natural fibers 2 in a humid environment.
[0051] The central portion of the undefused natural fiber 2, with its small specific surface area, has less entanglement with the main resin 1 and, depending on the molding conditions, is easily exposed on the surface of the composite resin molded body. Conversely, the front end portion of the defused natural fiber 2 has more entanglement with the main resin 1 and enters the interior along with the main resin 1. Thus, a composite resin molded body 10 can be obtained in which the central portion of the natural fiber 2, excluding the two ends, is exposed on the surface.
[0052] As the front-end defibering section, it is preferably 5% to 50% of the overall fiber length L of the natural fiber 2. When the defibering section is less than 5% of the overall fiber length L, the specific surface area is small, and therefore, no increase in elastic modulus is observed. When it is longer than 50%, the defibering section with a large aspect ratio is exposed on the surface of the composite resin molded body, resulting in poor water absorption.
[0053] Next, the characteristics of natural fiber 2 will be explained. Regarding the types of main resin 1 and natural fiber 2, as described above, if natural fiber 2 is too soft relative to main resin 1, i.e., has a low elastic modulus, the overall elastic modulus of the composite resin molded body 10 will decrease, resulting in reduced strength. On the other hand, if natural fiber 2 is too hard relative to main resin 1, i.e., has a high elastic modulus, the shock wave generated during impact cannot propagate and is absorbed at the interface between main resin 1 and natural fiber 2. Therefore, cracks are easily generated near this interface, resulting in reduced impact resistance. Therefore, regarding the relationship between the elastic moduli of main resin 1 and natural fiber 2, it is preferable that the elastic modulus of natural fiber 2 is higher and the difference is as small as possible. Regarding the optimal relationship, calculations based on simulation results show that the difference in elastic modulus between main resin 1 and natural fiber 2 is preferably within 20 GPa.
[0054] In addition, for the purpose of improving the adhesion to the main resin 1 and the coating resin 3 or the dispersibility in the composite resin molded body 10, these natural fibers 2 are sometimes surface treated. However, if the water absorption of the natural fibers 2 is impaired due to the surface treatment, it is preferable not to perform surface treatment in advance.
[0055] <Additives>
[0056] Additives may be used as needed to improve the affinity between the main resin 1 and the natural fiber 2. It should be noted that any commonly used additives may be used.
[0057] <Coating Resin>
[0058] Next, the coating resin 3 will be described. In this embodiment, the coating resin 3 serves the following purpose: to protect the microorganisms or enzymes 4 carried on the natural fibers 2 during the use of the composite resin molded body 10, preventing contact with the main resin 1. After the composite resin molded body 10 is discarded, in order to promote biodegradation in a humid environment, the coating resin 3 must be decomposed to release the microorganisms or enzymes 4 carried on the natural fibers 2. Therefore, a hydrolyzable resin that decomposes in an environment with humidity of 50% or higher is preferred. Examples include polyester resins such as polylactic acid, polybutylene terephthalate, and polycarbonate. Furthermore, to ensure good moldability, a thermoplastic resin is preferred; the above-mentioned resins can be used alone or in combination of two or more. It should be noted that the coating resin 3 is not limited to the materials mentioned above as long as it has hydrolytic properties.
[0059] Furthermore, the coating resin 3 maintains a state in which it coats at least a portion of the surface of the natural fiber 2 within the composite resin molded body 10. Therefore, the melting point of the coating resin 3 is preferably within the range of above the melting point of the main resin 1 and below the carbonization temperature of the natural fiber 2. If the melting point of the coating resin 3 is above the melting point of the main resin 1, it will not melt during the molding of the composite resin molded body 10; if it is below the carbonization temperature of the natural fiber 2, it can coat the natural fiber 2 without causing it to deteriorate.
[0060] The state of the coating resin 3 in the composite resin molded body 10 is described. By controlling the coating rate of the natural fiber 2, the coating resin 3 can slow down the release of microorganisms or enzymes 4 carried on the natural fiber 2, thereby controlling the decomposition rate.
[0061] <Microorganisms or enzymes>
[0062] Next, the microorganism or enzyme 4 will be described. The microorganism or enzyme 4 in the present embodiment is intended to accelerate the decomposition of the composite resin molded article 10 in a humid environment. The microorganism or enzyme 4 in the present embodiment varies depending on the base resin 1, and specific examples include: microorganisms of the genus Amycolatopsis as polylactic acid degrading agents and polybutylene succinate degrading agents, microorganisms of the genus Streptomyces, microorganisms of the genus Pseudomonas such as Pseudomonas lemoignei, microorganisms of the genus Alcaligenes such as Alcaligenes paradoxus as poly-3-hydroxybutyrate degrading agents, microorganisms of the genus Pseudomonas such as Pseudomonas stutzeri, Pseudomonas aeruginosa, and Pseudomonas vesicularis, microorganisms of the genus Alcaligenes, microorganisms of the genus Acinetobacter, and microorganisms of the genus Xanthomonas as degrading agents for polyethers such as polyethylene glycol.
[0063] Examples of the enzyme in the present embodiment include various enzymes extracted from the aforementioned microorganisms. Specifically, examples of the enzyme for decomposing polylactic acid include Proteinase K; examples of the enzyme for decomposing polyvinyl alcohol include polyvinyl alcohol dehydrogenase, polyvinyl alcohol oxidase, and secondary alcohol oxidase; examples of the enzyme for decomposing poly-3-hydroxybutyrate include PHB depolymerase; and examples of the enzyme for decomposing polyurethane include cholesterol esterase, Chitopearl cholesterol esterase, and urease. The aforementioned microorganisms or enzymes may be used alone or in combination of two or more. It should be noted that the materials are not limited to those described above as long as they have degradability for the base resin 1.
[0064] <Method for Producing Composite Resin Molded Article>
[0065] Next, the method for producing the composite resin molded article 10 will be described. Figure 4 is a flowchart illustrating the production process of the composite resin molded article 10 in the present embodiment.
[0066] (1) The surface of the natural fiber 2 is loaded with the microorganism or enzyme 4 in advance. Examples of the method for loading the microorganism or enzyme 4 include physical adsorption by dry blending, an impregnation method of natural fibers using a dispersion solvent, a crosslinking method, an entrapment method, and the like. The loading method is not limited to the above methods as long as it is a method capable of retaining the microorganism or enzyme 4 on the surface of the natural fiber 2.
[0067] (2) The natural fibers 2 and the coating resin 3 are charged into a melt-kneading treatment apparatus, and melt-kneaded in the apparatus. As a result, the coating resin 3 is melted, and the natural fibers 2 are dispersed in the molten coating resin 3. In addition, the shearing action of the apparatus promotes the defibration of the aggregated masses of the natural fibers 2, so that the natural fibers 2 can be finely dispersed in the coating resin 3. By adjusting the shearing conditions at this time, as Figure 3 shown, the ends of the natural fibers 2 are defibrated to obtain defibrated portions.
[0068] Traditionally, when compounding fibers with resins, fibers obtained by pre-defibrillating the fibers through pretreatments such as wet dispersion are used. However, if natural fibers are defibrillated in the solvent used for wet dispersion, the fibers swell due to the solvent. Therefore, in order for the natural fibers to fully absorb water and swell in the composite resin molded article, the solvent in the natural fibers must be dried before compounding with the main resin. Furthermore, defibrillation using wet dispersion is easier than defibrillation in molten main resin, thus preventing the defibrillation of only the ends and the entire natural fiber from being defibrillated. Additionally, there are problems such as increased processing steps and decreased productivity due to pretreatment.
[0069] In contrast, in the manufacturing process of the composite resin molded body 10 in this embodiment, a pretreatment based on wet dispersion aimed at defibrating the natural fibers is not performed. Instead, it is melt-blended together with the coating resin 3 (a completely dry process). In this process, the natural fibers 2 are not wet-dispersed, thereby suppressing the swelling of the natural fibers 2 during the manufacturing process and increasing the water absorption rate of the natural fibers 2 in the composite resin molded body 10. Drying the natural fibers 2 beforehand or during blending can further improve the water absorption rate of the composite resin molded body 10 in humid environments. In addition, as described above, by providing defibrating portions to the natural fibers 2, there are more contact points between the fibers inside the composite resin molded body 10, which can increase the water absorption rate of the composite resin molded body 10 through the contact points between the fibers.
[0070] To produce the natural fiber 2 of this embodiment using a completely dry process, it is preferable to apply high shear stress during mixing. Specific mixing methods include single-screw mixers, twin-screw mixers, roll mixers, Banbury mixers, and combinations thereof. From the viewpoint of easy application of high shear stress and high production capacity, continuous twin-screw mixers and continuous roll mixers are particularly preferred. Any mixing method capable of applying high shear stress may also be used, other than those described above.
[0071] (3) The composite resin composition of natural fiber 2 extruded from the melt-blending device and coating resin 3 is pulverized by a cutting machine or a pulverizer, thereby obtaining natural fiber 2 whose surface is at least partially coated by the coating resin 3 in this embodiment. Specific methods include granulators, ball mills, roller mills, hammer mills, universal pulverizers, jet mills, and combinations thereof. Any cutting or pulverizing method other than those described above can be used as long as it can maintain the state in which at least a portion of the natural fiber 2 is coated by the coating resin 3.
[0072] (4) After dry mixing the main resin 1 and the natural fiber 2 coated with the coated resin 3, the mixture is kneaded and then injection molded to produce an injection-molded article as a composite resin molded body 10. The molding temperature during injection molding is preferably below 125% of the melting point of the coated resin 3. If the molding temperature is above 125% of the melting point of the coated resin 3, the coated resin 3 will melt and disperse in the main resin 1 during molding.
[0073] The following describes each embodiment and comparative example from the experiments conducted by the inventors.
[0074] (Example 1)
[0075] In Example 1, a cellulose composite poly(3-hydroxybutyrate-co-3-hydroxyvalerate) (PHBV) resin molded article was manufactured by the following manufacturing method.
[0076] Softwood pulp (trade name: NBKPCelgar, manufactured by Mitsubishi Paper) was used as the starting material for natural fibers. PHBV depolymerizing enzyme was used, which was extracted from the culture medium of Streptomyces microorganisms. Softwood pulp and PHB depolymerizing enzyme were dry-mixed at a mass ratio of 90:10 and pulverized by a roller mill to obtain the enzyme-loaded cellulose filler.
[0077] Polylactic acid (Unitika trade name: TE-2000), used as the coating resin, and the aforementioned enzyme-carrying cellulose filler were weighed and dry-mixed at a mass ratio of 50:50. Then, melt-mixing was performed using a twin-screw extruder (Kurimoto Iron Works KRC kneader). The screws were set to medium shear type. The melt-mixing conditions were set as follows: material temperature 200°C, speed 50 min. -1 The composite resin composition discharged from the twin-screw mixer was thermally cut to produce cellulose composite polylactic acid resin granules.
[0078] The prepared cellulose-polylactic acid composite granules were pulverized using a wonder crusher (Osaka Chemical Manufacturing WC-3) to obtain cellulose fibers coated with polylactic acid resin. The pulverization conditions were set to a speed of 15,000 rpm.
[0079] Cellulose fibers coated with polylactic acid resin and PHBV (TianAn Biopolymer trade name: Y1000P) as the main resin were weighed and dry-mixed at a mass ratio of 50:50. Then, the mixture was melt-mixed using a twin-screw extruder (Kurimoto Iron Works KRC kneader). The screws were set to medium shear type. The melt-mixing conditions were set as follows: material temperature 180°C, speed 50 min. -1The composite resin composition discharged from the twin-screw mixer was thermally cut to produce cellulose composite PHBV resin granules with a mass ratio of main resin, enzyme-containing natural fiber, and coating resin of 50:25:25.
[0080] Then, test specimens of cellulose composite PHBV resin molded parts were produced using an injection molding machine (Nippon Seiko 180AD). The conditions for producing the test specimens were set as follows: main resin temperature 200°C, mold temperature 50°C, injection speed 100 mm / s, and holding pressure 100 Pa. The shape of the test specimens was modified according to the evaluation items described below.
[0081] (Evaluation of fiber absorbency)
[0082] The water absorption of fibers is evaluated by determining the moisture content of the fibers using the method specified in ASTM D 1909. Specifically, the weight of the fibers after drying at 80°C for 24 hours is measured and used as the baseline weight. Then, the weight of the fibers after maintaining a temperature of 20°C and a humidity of 65% for 24 hours is measured. The increase in weight from the baseline weight is taken as moisture, and the moisture content is calculated. A moisture content less than 5% is designated as "C", and a moisture content greater than 5% is designated as "B". The moisture content of coniferous pulp is 6.5%, and its evaluation is "B".
[0083] (End defibrillation of fibers)
[0084] The obtained cellulose composite PHBV resin molded body was impregnated in chloroform solvent to dissolve PHBV and polylactic acid. The shape of the remaining cellulose fibers was observed by SEM. The fiber ends were in a disintegrated state.
[0085] (Evaluation of the elastic modulus of composite resin molded articles)
[0086] A three-point bending test was conducted using a dumbbell-shaped test piece of JIS K7139 type A12 size. Here, as an evaluation method for the elastic modulus, values less than 200 MPa are designated as "C", and values greater than 200 MPa are designated as "B". The elastic modulus of this test piece was 259 MPa, and its evaluation was "B".
[0087] (Deterioration test of composite resin molded articles)
[0088] Using the obtained JIS K7139 Type A12 dumbbell-shaped test piece, a deterioration test was performed. The test piece was held at a temperature of 60°C and a humidity of 40% for 48 hours. The environment of 60°C corresponds to an accelerated test of about 50 times relative to a normal atmosphere at room temperature. Using the test piece after the deterioration test, a 3-point bending test was performed. As a deterioration evaluation method, a case where the reduction rate of the elastic modulus relative to that before the accelerated test is less than 10% is defined as "B", and a case where the reduction rate is 10% or more is defined as "C". The reduction rate of the elastic modulus of this test piece was 5%, and its evaluation was "B".
[0089] (Evaluation of biodegradability of composite resin molded article)
[0090] Using a rod-shaped test piece formed from the obtained cellulose composite resin molded article, a biodegradation test was performed. 50 g of a seeding source for compost (manufactured by Yawata Bussan, YK-11) was charged into a plastic container, and a rod-shaped test piece with a height of 20 mm, a width of 10 mm, and a thickness of 3 mm whose weight was measured in advance was embedded in the seeding source, held at a temperature of 58°C and a humidity of 50%, and the weight reduction after 2 months was evaluated. As an evaluation method for the biodegradation rate, a case where the value of weight reduction is 50% or more is evaluated as "A", a case where the value is 40% or more and less than 50% is evaluated as "B", and a case where the value is less than 40% is evaluated as "C". The biodegradation rate of this test piece was 42%, and its evaluation was "B".
[0091] (Example 2)
[0092] In Example 2, a cellulose composite PHBV resin molded article was produced in the same manner as in Example 1 under the same material conditions and process conditions except that the mass ratio of the base resin, the enzyme-containing natural fiber, and the coating resin was changed to 67.5:25:7.5. Regarding the evaluation, the same evaluations as in Example 1 were also performed.
[0093] (Comparative Example 1)
[0094] In Comparative Example 1, an uncoated enzyme-supported cellulose filler was used. A cellulose composite PHBV resin molded article was produced in the same manner as in Example 1 under the same material conditions and process conditions except that the mass ratio of the base resin to the enzyme-supported cellulose filler was changed to 25:75. Regarding the evaluation, the same evaluations as in Example 1 were also performed.
[0095] (Comparative Example 2)
[0096] In Comparative Example 2, natural fibers were not used. The polylactic acid resin to be coated was melt-blended with the enzyme at a mass ratio of 95:5. The mass ratio of the main resin and the enzyme-containing polylactic acid resin was changed to 50:50. All other material and process conditions were the same as in Example 1, and a PHBV composite resin molded article was prepared. The same evaluation as in Example 1 was also performed.
[0097] (Comparative Example 3)
[0098] In Comparative Example 3, PET fibers with a diameter of 20 μm and a length of 100 μm were used instead of coniferous pulp to prepare enzyme-carrying PET fibers. All other material and process conditions were the same as in Example 1, and PHBV composite resin molded articles were prepared. The same evaluation as in Example 1 was also performed.
[0099] (Comparative Example 4)
[0100] In Comparative Example 4, polylactic acid resin was used instead of PHBV resin as the main resin, and the process conditions were otherwise the same as in Example 1, resulting in a polylactic acid composite resin molded article. The same evaluation as in Example 1 was also performed.
[0101] (Comparative Example 5)
[0102] In Comparative Example 5, PHBV resin was used as the raw material without the use of natural fibers, coating resin, and enzymes. All other process conditions were the same as in Example 1, and a PHBV resin molded article was produced. The same evaluation as in Example 1 was also performed.
[0103] The composition and measurement results of the composite resin molded articles from Examples 1, 2, and Comparative Examples 1-5 are shown below. Figure 5 .
[0104] according to Figure 5 It is evident that in Examples 1 and 2, where the enzymes supported on natural fibers were protected by the coating resin, the elastic modulus reached over 200 MPa, and rigidity degradation was suppressed in a low-humidity environment of 40% compared to Comparative Example 2. The biodegradation rate was also promoted compared to Comparative Example 5. In the biodegradation evaluation, Example 2, with a smaller proportion of coating resin compared to Example 1, showed a higher biodegradation rate.
[0105] As described above, it has been confirmed that by compounding natural fibers with enzymes on their surface, at least a portion of the fiber surface is coated with a hydrolyzable resin, and the fibers are exposed on the surface of the composite resin molded body, and the natural fibers have a high water absorption rate, a composite resin with high elastic modulus, high durability, and high biodegradability can be obtained.
[0106] For Comparative Example 1, which was made without using a coating resin, the elastic modulus was improved compared to Comparative Example 5 due to the composite of natural fibers. However, during molding, the enzyme was not protected by the coating resin, and the thermal damage to the enzyme was significant during mixing and molding. Therefore, the biodegradation rate was lower than that of Comparative Example 3, and it was rated as "C".
[0107] In Comparative Example 2, which was made without the use of natural fibers, the elastic modulus was improved by the composite of polylactic acid resin. However, since natural fibers were not used to absorb water into the composite resin mold, the hydrolysis of polylactic acid resin did not occur, and the biodegradation rate was lower than that of Comparative Example 5, and it was rated as "C".
[0108] Comparative Example 3, which uses PET fiber instead of coniferous pulp, has a low moisture content and no water absorption. Therefore, in the biodegradability evaluation, the hydrolysis of polylactic acid resin did not occur, and the biodegradation rate was lower than that of Comparative Example 5, and the evaluation was "C".
[0109] In Comparative Example 4, which used polylactic acid resin instead of PHBV resin as the main resin, hydrolysis of the main resin occurred during the degradation test, resulting in a decrease in the elastic modulus, and the evaluation was "C". In the biodegradability evaluation, the polylactic acid resin as the main resin had a lower biodegradation rate compared to the PHBV resin, and therefore, the biodegradability rate was also lower, resulting in an evaluation of "C".
[0110] Based on the above evaluation, it has been confirmed that by using absorbent natural fibers and biodegradable plastics, loading enzymes onto the surface of the natural fibers, coating at least a portion of the fiber surface with a hydrolyzable coating resin, and exposing the fibers on the surface of the composite resin molded body, it is possible to obtain a composite resin molded body with high elastic modulus, high durability, and high biodegradability.
[0111] It should be noted that this disclosure includes situations where any of the above-described various implementation methods and / or embodiments are appropriately combined to achieve the effects of each implementation method and / or embodiment.
[0112] Industrial availability
[0113] The composite resin molded articles according to the present invention provide composite resin molded articles with controllable mechanical strength and biodegradation rate compared to existing biodegradable plastics. Through the present invention, the properties of the main resin are improved, and therefore it can be used as a substitute for general-purpose plastics derived from petroleum. Therefore, the environmental burden of various industrial products or consumer goods made from general-purpose plastics derived from petroleum can be significantly reduced. Furthermore, it can be used in packaging materials, daily necessities, appliance frames, building materials, etc.
Claims
1. A composite resin molded article, comprising: Main agent resin, and Multiple natural fibers dispersed in the main resin. Each of the aforementioned natural fibers contains microorganisms or enzymes. When the composite resin molded body is set to 100% by mass, the content of the plurality of natural fibers containing the microorganisms or enzymes is 10% by mass or more and 99% by mass or less. At least one of the plurality of natural fibers is exposed on the surface of the composite resin molded body. At least a portion of the surface of at least one of the plurality of natural fibers is coated with a hydrolyzable coating resin. The main resin is a biodegradable resin containing polyhydroxyalkanoates.
2. The composite resin molded article according to claim 1, wherein, The moisture content of the plurality of natural fibers is greater than 5% by means of the method specified in ASTM D 1909.
3. The composite resin molded article according to claim 1 or 2, wherein, The melting point of the coating resin is above the melting point of the main resin and below the carbonization temperature of the plurality of natural fibers.
4. The composite resin molded article according to claim 1 or 2, wherein, Each of the plurality of natural fibers comprises a fiber and the microorganisms or enzymes supported on the surface of the fiber.
5. The composite resin molded article according to claim 1 or 2, wherein, The aforementioned natural fibers are cellulose-based.
6. The composite resin molded article according to claim 1 or 2, wherein, At least one of the plurality of natural fibers has a defibering portion at the end in the fiber length direction.
7. A method for manufacturing a composite resin molded article, the method comprising: The steps for preparing microorganisms or enzymes, natural fibers, hydrolyzable coating resins, and main resins; The step of making the natural fiber contain the microorganisms or enzymes; The coating resin melt-blending step involves melting and blending the natural fiber containing the microorganisms or enzymes together with the coating resin, and then unwinding the natural fiber containing the microorganisms or enzymes from the end along the fiber length direction to expand the surface area of the unwinding portion at the end. as well as The step of molding a composite resin molded body by mixing coated natural fibers, whose surface at least a portion is coated with the coating resin, together with the main resin. The main resin is a biodegradable resin containing polyhydroxyalkanoates.
8. The method for manufacturing a composite resin molded article according to claim 7, wherein, In the step of molding the composite resin molded body, the molding temperature is set to a temperature below 125% of the melting point of the coated resin.
Citation Information
Patent Citations
Biodegradable plastic product with controlled decomposition rate and method for manufacturing the same
JP2013209587A
Method for preparing biodegradable capsules and the resulting capsules
JP2020520794A
Cellulose composite resin and method for production thereof
CN110857351A
Aliphatic polyester resin composition and molded body
JP2019034987A