A method for pyrolyzing electronic waste plastics to co-produce phenolic chemicals and CO2 adsorption carbon materials

By mixing electronic waste plastics with alkaline salt solutions for rapid pyrolysis, high-value phenolic compounds and CO2 adsorption carbon materials are generated, which solves the problem of difficult resource utilization of electronic waste plastics in the existing technology and achieves efficient resource disposal. and environmental protection.

CN115322076BActive Publication Date: 2024-10-22NORTH CHINA ELECTRIC POWER UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210995704.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-18
Publication Date
2024-10-22
Estimated Expiration
2042-08-18

AI Technical Summary

Technical Problem

The existing technology makes it difficult to effectively utilize electronic waste plastics, especially the efficient preparation of high-value phenolic compounds and CO2 adsorption carbon materials, and the difficulty of separation and purification. It cannot effectively solve the resource utilization and environmental pollution problems of electronic waste plastics.

Method used

By mixing electronic waste plastics with alkaline salt solutions of different concentrations, rapid pyrolysis is performed under anaerobic conditions to generate high-value phenolic chemicals and CO2 adsorption carbon materials, and the alkaline salt solution is used to promote the formation of carbonate bonds and iso- The propyl bond is broken to increase the yield of phenolic compounds, and the coke is activated by alkaline salt solution to form an efficient CO2 adsorption material.

Benefits of technology

It achieves efficient disposal and resource utilization of electronic waste plastics, improves the yield and CO2 adsorption performance of phenolic compounds, reduces the difficulty and economic cost of separation and purification, solves the problem of environmental pollution, and helps achieve the "double carbon" goal. .

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention belongs to the field of organic solid waste utilization, and specifically relates to a method for pyrolyzing electronic waste plastics to produce phenolic chemicals and CO 2 Method for adsorbing carbon materials. According to the method provided by the present invention, waste electronic plastics are used as raw materials, alkaline salt solutions of different concentrations are prepared, the waste electronic plastics and the alkaline salt solution are mixed according to a certain solid-liquid ratio, the mixture is rapidly pyrolyzed under anaerobic conditions, the obtained pyrolysis gas is condensed to obtain high-value phenolic chemicals, the solid product is washed and dried, and CO is obtained. 2 The alkaline salt solution involved in the method of the present invention has the advantages of wide sources, economical and easy to obtain, etc. It can not only promote the decomposition of electronic waste plastics to generate phenol and isopropenylphenol, but also act as a chemical activator, so that the obtained solid product has a developed pore structure and a high specific surface area, which can be used as an excellent CO 2 Adsorption carbon materials can achieve efficient disposal and resource utilization of electronic waste plastics.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of organic solid waste utilization, and specifically relates to a method for pyrolyzing electronic waste plastics to co-produce phenolic chemicals and CO2 adsorption carbon materials. Background Art

[0002] As the amount of scrapped electronic equipment such as household appliances and communication equipment continues to increase, the output of electronic waste plastics has also increased year by year. Specifically, the global output of electronic waste plastics reached 10.72 million tons in 2019, and it is expected to reach 14.94 million tons by 2030. Therefore, how to make high-value and reasonable use of these electronic waste plastics will become an urgent problem to be solved in the resource recovery of waste electronic and electrical products.

[0003] Pyrolysis is a thermochemical recycling technology that can quickly degrade electronic waste plastics and convert them into a variety of energy and chemical platform products. It has great potential in replacing traditional fossil resources. Studies have found that the pyrolysis of electronic waste plastics follows a free radical reaction mechanism, and a variety of high-value phenolic compounds can be formed through random cleavage of molecular chains. For example, phenol and isopropenylphenol can be used as intermediates in the fields of chemical industry, medicine and pesticides. However, the types of phenolic compounds obtained by pyrolysis are complex and the content is low, which makes separation and purification difficult and difficult to use as chemical raw materials. In order to selectively obtain the target phenolic compounds, it is necessary to control the pyrolysis process of electronic waste plastics in a directional manner (such as adding catalysts) to promote or inhibit certain specific reactions, thereby improving the selectivity and yield of the target phenolic compounds. However, at this stage, research on the preparation of phenolic chemicals by catalytic pyrolysis of electronic waste plastics is still limited.

[0004] In addition to phenolic compounds, electronic waste plastics also produce 20-30wt% of solid products (coke) during the pyrolysis process. These cokes are formed by cross-linking of volatiles produced by pyrolysis of electronic waste plastics. They have a developed pore structure, a high specific surface area and good thermochemical stability, and have great application prospects in the field of CO2 adsorption. With the rapid development of modern industry, large-scale emissions of greenhouse gases such as CO2 have led to global warming. Therefore, using electronic waste plastics as raw materials to prepare CO2 adsorption carbon materials can not only turn waste into treasure, but also solve environmental pollution problems.

[0005] Therefore, there is an urgent need to invent a clean and efficient pyrolysis method for waste electronic plastics, which can not only obtain high-yield target phenolic chemicals, but also obtain carbon materials with good CO2 adsorption performance, thereby realizing the clean disposal and resource utilization of organic solid waste, and helping to achieve the "dual carbon" goal. Summary of the invention

[0006] The purpose of the present invention is to overcome the deficiencies of the prior art and to provide a method for pyrolyzing electronic waste plastics to co-produce phenolic chemicals and CO2 adsorption carbon materials.

[0007] The method of the present invention is specifically as follows:

[0008] According to the method provided by the present invention, electronic waste plastics are used as raw materials, alkaline salt solutions of different concentrations are prepared, the electronic waste plastics and the alkaline salt solution are mixed according to a certain solid-liquid ratio, the mixture is rapidly pyrolyzed under anaerobic conditions, the obtained pyrolysis gas is condensed to obtain high-value phenolic chemicals, and the solid product is washed and dried to obtain CO2 adsorption carbon material.

[0009] Preferably, the electronic waste plastic includes at least one of polysulfone resin, phenolic resin or polycarbonate.

[0010] Preferably, the alkaline salt solution includes sodium carbonate solution, potassium carbonate solution, sodium bicarbonate solution, potassium bicarbonate solution, sodium formate solution or potassium formate solution.

[0011] Preferably, the concentration of the alkaline salt solution is 0.25-2 mol / L.

[0012] Preferably, the electronic waste plastic is placed in an alkaline salt solution with a solid-liquid ratio of 1:5 to 1:30 g / mL.

[0013] Preferably, the anaerobic condition is to maintain the reaction system under an inert anaerobic protective gas environment.

[0014] Preferably, the pyrolysis temperature is 450-650° C., and the pyrolysis time is 5-20 min.

[0015] The beneficial effects of the present invention are:

[0016] The present invention directly conducts rapid pyrolysis after mixing and contacting electronic waste plastics with an alkaline salt solution, and co-produces phenolic chemicals and CO2 adsorption carbon materials, thereby realizing efficient disposal and resource utilization of electronic waste plastics. The alkaline salt solution used has the advantages of wide sources, economical and easy to obtain. Under high temperature, the hydroxide ions ionized by the alkaline salt solution can effectively promote the breakage of carbonate bonds and isopropylidene bonds in electronic waste plastics, generate a large amount of phenol and isopropenylphenol, and the content of other products is very low, reducing the difficulty and economic cost of subsequent separation and purification. In addition, the alkaline salt solution can also be used as a chemical activator to make the coke have a developed pore structure and a high specific surface area, thereby obtaining an excellent CO2 adsorption carbon material. DETAILED DESCRIPTION

[0017] The present invention provides a method for pyrolyzing electronic waste plastics to co-produce phenolic chemicals and CO2 adsorption carbon materials. The present invention is further described below in conjunction with specific embodiments. It should be understood that the following specific embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention.

[0018] The calculation method of the liquid product yield in the following examples is as follows:

[0019] Liquid product yield = (mass of the collected liquid product (minus the mass of water in the alkaline salt solution) ÷ mass of the raw material) × 100%.

[0020] In the following examples, the contents of phenol and isopropenylphenol were quantitatively analyzed by gas chromatography / mass spectrometry coupled with an external standard method, and the calculation method of the yields of phenol and isopropenylphenol was as follows:

[0021] Yield of phenol = (mass of phenol / mass of raw material) × 100%;

[0022] Yield of isopropenylphenol=(mass of isopropenylphenol÷mass of raw material)×100%.

[0023] Solid product yield = (mass of the collected solid product (minus the mass of the salt in the weakly alkaline salt solution) / mass of the raw material) × 100%.

[0024] In the following examples, the CO2 adsorption capacity of the solid product was tested by a thermogravimetric analyzer.

[0025] The percentages in the following examples are by mass unless otherwise specified.

[0026] Example 1

[0027] Take 1g of polysulfone resin as raw material, put it into 0.25mol / L sodium carbonate solution with a solid-liquid ratio of 1:10g / mL, and quickly pyrolyze the uniformly mixed sample at 650℃ under nitrogen atmosphere for 10min. The yield of the liquid product obtained is 58.74%. The contents of phenol and isopropenylphenol are detected by gas chromatography / mass spectrometry, and the calculated yields are 23.47% and 18.56%, respectively; the yield of the solid product obtained is 13.59%, and the adsorption amount of CO2 detected by thermogravimetric analyzer is 1.58mmol / g.

[0028] Example 2

[0029] Take 1g of polysulfone resin as raw material, put it into 0.5mol / L potassium carbonate solution with a solid-liquid ratio of 1:30g / mL, and quickly pyrolyze the uniformly mixed sample at 600℃ under nitrogen atmosphere for 5min. The yield of the liquid product obtained is 62.36%. The contents of phenol and isopropenylphenol are detected by gas chromatography / mass spectrometry, and the calculated yields are 27.54% and 21.17%, respectively; the yield of the solid product obtained is 13.34%, and the adsorption amount of CO2 detected by thermogravimetric analyzer is 1.62mmol / g.

[0030] Example 3

[0031] Take 1g of polysulfone resin as raw material, put it into 0.75mol / L sodium bicarbonate solution with a solid-liquid ratio of 1:20g / mL, and quickly pyrolyze the uniformly mixed sample at 600℃ under nitrogen atmosphere for 10min. The yield of the liquid product obtained is 66.07%. The contents of phenol and isopropenylphenol are detected by gas chromatography / mass spectrometry, and the calculated yields are 30.53% and 26.12%, respectively; the yield of the solid product obtained is 12.89%, and the adsorption amount of CO2 detected by thermogravimetric analyzer is 1.68mmol / g.

[0032] Example 4

[0033] Take 1g of polysulfone resin as raw material, put it into 1mol / L potassium bicarbonate solution with a solid-liquid ratio of 1:5g / mL, and quickly pyrolyze the uniformly mixed sample at 550℃ under nitrogen atmosphere for 20min. The yield of the liquid product obtained is 64.52%. The contents of phenol and isopropenylphenol are detected by gas chromatography / mass spectrometry, and the calculated yields are 27.54% and 22.74%, respectively; the yield of the solid product obtained is 12.78%, and the adsorption amount of CO2 detected by thermogravimetric analyzer is 1.72mmol / g.

[0034] Example 5

[0035] Take 1g of polysulfone resin as raw material, put it into 1.5mol / L sodium formate solution with a solid-liquid ratio of 1:20g / mL, and quickly pyrolyze the uniformly mixed sample at 450℃ under nitrogen atmosphere for 15min. The yield of the liquid product obtained is 51.06%. The contents of phenol and isopropenylphenol are detected by gas chromatography / mass spectrometry, and the calculated yields are 18.75% and 14.98%, respectively; the yield of the solid product obtained is 14.74%, and the adsorption amount of CO2 detected by thermogravimetric analyzer is 1.26mmol / g.

[0036] Example 6

[0037] Take 1g of polysulfone resin as raw material, put it into 2mol / L potassium formate solution with a solid-liquid ratio of 1:5g / mL, and quickly pyrolyze the uniformly mixed sample at 500℃ under nitrogen atmosphere for 20min. The yield of the liquid product obtained is 54.82%. The contents of phenol and isopropenylphenol are detected by gas chromatography / mass spectrometry, and the calculated yields are 20.75% and 15.24%, respectively; the yield of the solid product obtained is 14.18%, and the adsorption amount of CO2 detected by thermogravimetric analyzer is 1.51mmol / g.

[0038] Example 7

[0039] Take 1g of phenolic resin as raw material, put it into 2mol / L sodium carbonate solution with a solid-liquid ratio of 1:20g / mL, and quickly pyrolyze the uniformly mixed sample at 450℃ under nitrogen atmosphere for 10min. The yield of the liquid product obtained is 52.41%. The contents of phenol and isopropenylphenol are detected by gas chromatography / mass spectrometry, and the calculated yields are 21.36% and 18.66%, respectively; the yield of the solid product obtained is 14.95%, and the adsorption amount of CO2 detected by thermogravimetric analyzer is 1.37mmol / g.

[0040] Example 8

[0041] Take 1g of phenolic resin as raw material, put it into 1.5mol / L potassium carbonate solution with a solid-liquid ratio of 1:30g / mL, and quickly pyrolyze the uniformly mixed sample at 500℃ under nitrogen atmosphere for 10min. The yield of the liquid product obtained is 56.42%. The contents of phenol and isopropenylphenol are detected by gas chromatography / mass spectrometry, and the calculated yields are 21.65% and 16.41%, respectively; the yield of the solid product obtained is 14.67%, and the adsorption amount of CO2 detected by thermogravimetric analyzer is 1.47mmol / g.

[0042] Example 9

[0043] Take 1g of phenolic resin as raw material, put it into 1mol / L sodium bicarbonate solution with a solid-liquid ratio of 1:10g / mL, and quickly pyrolyze the uniformly mixed sample at 600℃ under nitrogen atmosphere for 20min. The yield of the liquid product obtained is 67.26%. The contents of phenol and isopropenylphenol are detected by gas chromatography / mass spectrometry, and the calculated yields are 29.13% and 26.65%, respectively; the yield of the solid product obtained is 12.89%, and the adsorption amount of CO2 detected by thermogravimetric analyzer is 1.71mmol / g.

[0044] Example 10

[0045] Take 1g of phenolic resin as raw material, put it into 0.75mol / L potassium bicarbonate solution with a solid-liquid ratio of 1:5g / mL, and quickly pyrolyze the uniformly mixed sample at 550℃ under nitrogen atmosphere for 15min. The yield of the liquid product obtained is 62.41%. The contents of phenol and isopropenylphenol are detected by gas chromatography / mass spectrometry, and the calculated yields are 27.32% and 21.23%, respectively; the yield of the solid product obtained is 13.23%, and the adsorption amount of CO2 detected by thermogravimetric analyzer is 1.64mmol / g.

[0046] Embodiment 11

[0047] Take 1g of phenolic resin as raw material, put it into 0.5mol / L sodium formate solution with a solid-liquid ratio of 1:15g / mL, and quickly pyrolyze the uniformly mixed sample at 600℃ under nitrogen atmosphere for 5min. The yield of the liquid product obtained is 60.06%. The contents of phenol and isopropenylphenol are detected by gas chromatography / mass spectrometry, and the calculated yields are 24.51% and 21.82%, respectively; the yield of the solid product obtained is 13.44%, and the adsorption amount of CO2 detected by thermogravimetric analyzer is 1.62mmol / g.

[0048] Example 12

[0049] Take 1g of phenolic resin as raw material, put it into 0.25mol / L potassium formate solution with a solid-liquid ratio of 1:10g / mL, and quickly pyrolyze the uniformly mixed sample at 650℃ under nitrogen atmosphere for 15min. The yield of the liquid product obtained is 57.22%. The contents of phenol and isopropenylphenol are detected by gas chromatography / mass spectrometry, and the calculated yields are 22.94% and 18.54%, respectively; the yield of the solid product obtained is 12.68%, and the adsorption amount of CO2 detected by thermogravimetric analyzer is 1.55mmol / g.

[0050] Example 13

[0051] 1 g of polycarbonate was taken as raw material and placed in a 0.5 mol / L sodium carbonate solution with a solid-liquid ratio of 1:5 g / mL. The uniformly mixed sample was rapidly pyrolyzed at 500°C under a nitrogen atmosphere for 20 min. The yield of the liquid product obtained was 56.33%. The contents of phenol and isopropenylphenol were detected by gas chromatography / mass spectrometry, and the calculated yields were 22.35% and 18.01%, respectively. The yield of the solid product obtained was 13.86%, and the adsorption amount of CO2 detected by thermogravimetric analyzer was 1.50 mmol / g.

[0052] Embodiment 14

[0053] Take 1g of polycarbonate as raw material, put it into 1mol / L sodium carbonate solution with a solid-liquid ratio of 1:10g / mL, and quickly pyrolyze the uniformly mixed sample at 600℃ under nitrogen atmosphere for 10min. The yield of the liquid product obtained is 71.43%. The contents of phenol and isopropenylphenol are detected by gas chromatography / mass spectrometry, and the calculated yields are 33.77% and 28.83%, respectively; the yield of the solid product obtained is 12.64%, and the adsorption amount of CO2 detected by thermogravimetric analyzer is 1.75mmol / g.

[0054] Embodiment 15

[0055] 1 g of polycarbonate was taken as raw material and placed in a 0.25 mol / L potassium carbonate solution with a solid-liquid ratio of 1:10 g / mL. The uniformly mixed sample was rapidly pyrolyzed at 650°C under a nitrogen atmosphere for 10 min. The yield of the liquid product obtained was 59.34%. The contents of phenol and isopropenylphenol were detected by gas chromatography / mass spectrometry, and the calculated yields were 24.32% and 20.65%, respectively. The yield of the solid product obtained was 12.87%, and the adsorption amount of CO2 detected by thermogravimetric analyzer was 1.54 mmol / g.

[0056] Example 16

[0057] 1 g of polycarbonate was taken as raw material and placed in a 1.5 mol / L potassium carbonate solution with a solid-liquid ratio of 1:20 g / mL. The uniformly mixed sample was rapidly pyrolyzed at 450°C under a nitrogen atmosphere for 15 min. The yield of the liquid product obtained was 53.85%. The contents of phenol and isopropenylphenol were detected by gas chromatography / mass spectrometry, and the calculated yields were 19.77% and 15.04%, respectively. The yield of the solid product obtained was 14.26%, and the adsorption amount of CO2 detected by thermogravimetric analyzer was 1.36 mmol / g.

[0058] Embodiment 17

[0059] 1 g of polycarbonate was taken as raw material and placed in a 2 mol / L sodium bicarbonate solution with a solid-liquid ratio of 1:30 g / mL. The uniformly mixed sample was rapidly pyrolyzed at 600°C under a nitrogen atmosphere for 5 min. The yield of the liquid product obtained was 65.43%. The contents of phenol and isopropenylphenol were detected by gas chromatography / mass spectrometry, and the calculated yields were 29.25% and 25.42%, respectively. The yield of the solid product obtained was 12.54%, and the CO2 adsorption amount detected by thermogravimetric analyzer was 1.70 mmol / g.

[0060] Embodiment 18

[0061] Take 1g of polycarbonate as raw material, put it into 1mol / L sodium bicarbonate solution with a solid-liquid ratio of 1:10g / mL, and quickly pyrolyze the uniformly mixed sample at 550℃ under nitrogen atmosphere for 20min. The yield of the obtained liquid product is 61.24%. The contents of phenol and isopropenylphenol are detected by gas chromatography / mass spectrometry, and the calculated yields are 27.42% and 23.44%, respectively; the yield of the obtained solid product is 12.98%, and the adsorption amount of CO2 detected by thermogravimetric analyzer is 1.67mmol / g.

[0062] Embodiment 19

[0063] 1 g of polycarbonate was taken as raw material and placed in 0.5 mol / L potassium bicarbonate solution with a solid-liquid ratio of 1:10 g / mL. The uniformly mixed sample was rapidly pyrolyzed at 650°C under a nitrogen atmosphere for 10 min. The yield of the liquid product obtained was 60.48%. The contents of phenol and isopropenylphenol were detected by gas chromatography / mass spectrometry, and the calculated yields were 26.58% and 22.98%, respectively. The yield of the solid product obtained was 11.88%, and the adsorption amount of CO2 detected by thermogravimetric analyzer was 1.62 mmol / g.

[0064] Embodiment 20

[0065] Take 1g of polycarbonate as raw material, put it into 2mol / L potassium bicarbonate solution with a solid-liquid ratio of 1:5g / mL, and quickly pyrolyze the uniformly mixed sample at 600℃ under nitrogen atmosphere for 15min. The yield of the liquid product obtained is 64.87%. The contents of phenol and isopropenylphenol are detected by gas chromatography / mass spectrometry, and the calculated yields are 28.21% and 24.24%, respectively; the yield of the solid product obtained is 11.07%, and the adsorption amount of CO2 detected by thermogravimetric analyzer is 1.73mmol / g.

[0066] Embodiment 21

[0067] 1 g of polycarbonate was taken as raw material and placed in 0.75 mol / L sodium formate solution with a solid-liquid ratio of 1:20 g / mL. The uniformly mixed sample was rapidly pyrolyzed at 500°C under a nitrogen atmosphere for 5 min. The yield of the liquid product obtained was 56.63%. The contents of phenol and isopropenylphenol were detected by gas chromatography / mass spectrometry, and the calculated yields were 23.54% and 18.47%, respectively. The yield of the solid product obtained was 14.67%, and the adsorption amount of CO2 detected by thermogravimetric analyzer was 1.49 mmol / g.

[0068] Embodiment 22

[0069] Take 1g of polycarbonate as raw material and put it into 1mol / L sodium formate solution with a solid-liquid ratio of 1:10g / mL. The evenly mixed sample is rapidly pyrolyzed at 600℃ under a nitrogen atmosphere for 10min. The yield of the liquid product obtained is 62.87%. The contents of phenol and isopropenylphenol are detected by gas chromatography / mass spectrometry, and the calculated yields are 27.32% and 22.66%, respectively; the yield of the solid product obtained is 13.88%, and the adsorption amount of CO2 detected by thermogravimetric analyzer is 1.66mmol / g.

[0070] Embodiment 23

[0071] Take 1g of polycarbonate as raw material, put it into 1mol / L potassium formate solution with a solid-liquid ratio of 1:30g / mL, and quickly pyrolyze the uniformly mixed sample at 550℃ under nitrogen atmosphere for 20min. The yield of the liquid product obtained is 60.24%. The contents of phenol and isopropenylphenol are detected by gas chromatography / mass spectrometry, and the calculated yields are 25.19% and 20.05%, respectively; the yield of the solid product obtained is 14.33%, and the adsorption amount of CO2 detected by thermogravimetric analyzer is 1.53mmol / g.

[0072] Embodiment 24

[0073] 1 g of polycarbonate was taken as raw material and placed in 2 mol / L potassium formate solution with a solid-liquid ratio of 1:10 g / mL. The uniformly mixed sample was rapidly pyrolyzed at 450°C under a nitrogen atmosphere for 10 min. The yield of the liquid product obtained was 52.41%. The contents of phenol and isopropenylphenol were detected by gas chromatography / mass spectrometry, and the calculated yields were 19.78% and 15.63%, respectively. The yield of the solid product obtained was 14.56%, and the adsorption amount of CO2 detected by thermogravimetric analyzer was 1.29 mmol / g.

[0074] Embodiment 25

[0075] Take 0.5g of polysulfone resin and 0.5g of phenolic resin as a mixed raw material, put them into 0.5mol / L sodium carbonate solution with a solid-liquid ratio of 1:20g / mL, and rapidly pyrolyze the uniformly mixed sample at 600°C under a nitrogen atmosphere for 10min. The yield of the obtained liquid product is 58.54%. The contents of phenol and isopropenylphenol are detected by gas chromatography / mass spectrometry, and the calculated yields are 24.21% and 20.23%, respectively; the yield of the obtained solid product is 13.21%, and the adsorption amount of CO2 detected by thermogravimetric analyzer is 1.65mmol / g.

[0076] Embodiment 26

[0077] Take 0.5g of phenolic resin and 0.5g of polycarbonate as a mixed raw material, put them into 1mol / L potassium carbonate solution with a solid-liquid ratio of 1:10g / mL, and rapidly pyrolyze the uniformly mixed sample at 650°C under a nitrogen atmosphere for 15min. The yield of the obtained liquid product is 62.87%. The contents of phenol and isopropenylphenol are detected by gas chromatography / mass spectrometry, and the calculated yields are 26.75% and 21.90%, respectively; the yield of the obtained solid product is 12.80%, and the adsorption amount of CO2 detected by thermogravimetric analyzer is 1.71mmol / g.

[0078] Embodiment 27

[0079] 0.5 g of polycarbonate and 0.5 g of polysulfone resin were taken as mixed raw materials and placed in 1.5 mol / L sodium bicarbonate solution with a solid-liquid ratio of 1:10 g / mL. The uniformly mixed sample was rapidly pyrolyzed at 550°C under a nitrogen atmosphere for 15 min. The yield of the obtained liquid product was 64.86%. The contents of phenol and isopropenylphenol were detected by gas chromatography / mass spectrometry, and the calculated yields were 28.08% and 25.41%, respectively. The yield of the obtained solid product was 12.85%, and the adsorption amount of CO2 detected by thermogravimetric analyzer was 1.69 mmol / g.

[0080] Embodiment 28

[0081] 0.4 g of polysulfone resin, 0.3 g of phenolic resin and 0.3 g of polycarbonate were taken as mixed raw materials and placed in 0.75 mol / L potassium bicarbonate solution with a solid-liquid ratio of 1:5 g / mL. The uniformly mixed sample was rapidly pyrolyzed at 500°C under a nitrogen atmosphere for 10 min. The yield of the obtained liquid product was 56.07%. The contents of phenol and isopropenylphenol were detected by gas chromatography / mass spectrometry, and the calculated yields were 21.40% and 16.87%, respectively. The yield of the obtained solid product was 13.72%, and the adsorption amount of CO2 detected by thermogravimetric analyzer was 1.61 mmol / g.

[0082] Embodiment 29

[0083] 0.3g of polysulfone resin, 0.4g of phenolic resin and 0.3g of polycarbonate were taken as mixed raw materials and placed in 2mol / L sodium formate solution with a solid-liquid ratio of 1:30g / mL. The uniformly mixed sample was rapidly pyrolyzed at 600°C under a nitrogen atmosphere for 20min. The yield of the obtained liquid product was 66.75%. The contents of phenol and isopropenylphenol were detected by gas chromatography / mass spectrometry, and the calculated yields were 29.23% and 25.21%, respectively. The yield of the obtained solid product was 12.45%, and the adsorption amount of CO2 detected by thermogravimetric analyzer was 1.72mmol / g.

[0084] Embodiment 30

[0085] 0.3g of polysulfone resin, 0.3g of phenolic resin and 0.4g of polycarbonate were taken as mixed raw materials and placed in 1mol / L potassium formate solution with a solid-liquid ratio of 1:10g / mL. The uniformly mixed sample was rapidly pyrolyzed at 550°C under a nitrogen atmosphere for 10min. The yield of the obtained liquid product was 56.60%. The contents of phenol and isopropenylphenol were detected by gas chromatography / mass spectrometry, and the calculated yields were 23.01% and 19.33%, respectively. The yield of the obtained solid product was 13.52%, and the adsorption amount of CO2 detected by thermogravimetric analyzer was 1.63mmol / g.

[0086] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of the present invention.

Claims

1. A method for pyrolyzing electronic waste plastics to co-produce phenolic chemicals and CO2 adsorption carbon materials, characterized in that: The electronic waste plastics are mixed with an alkaline salt solution in a certain solid-liquid ratio, the mixture is rapidly pyrolyzed under anaerobic conditions, the obtained pyrolysis gas is condensed to obtain phenol and isopropenylphenol, and the solid product is washed and dried to obtain a CO2 adsorption carbon material; wherein the electronic waste plastics include at least one of polysulfone resin, phenolic resin or polycarbonate; the pyrolysis time is 5 to 20 min; the concentration of the alkaline salt solution is 0.25 to 2 mol / L; the solid-liquid ratio is 1:5 to 1:30 g / mL; and the pyrolysis temperature is 450 to 650°C.

2. A method for pyrolyzing electronic waste plastics to co-produce phenolic chemicals and CO2 adsorption carbon materials according to claim 1, wherein: The alkaline salt solution includes sodium carbonate solution, potassium carbonate solution, sodium bicarbonate solution, potassium bicarbonate solution, sodium formate solution or potassium formate solution.