Epitaxial gan on diamond substrate and method of making same
By using a combination of diamond substrate, graphene, and aluminum nitride layer in GaN-based microwave power devices, the reliability and stability issues caused by heat accumulation in the devices are solved, achieving efficient heat dissipation and long-life device performance.
Patent Information
- Application Number
- CN202211063665.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-31
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-08-31
AI Technical Summary
GaN-based microwave power devices suffer from heat accumulation during the miniaturization and power increase process, leading to reliability and stability issues. Heat dissipation has become a major bottleneck restricting their further development.
Using diamond as the substrate material, combined with single or multiple layers of graphene and aluminum nitride, the high thermal conductivity of CVD diamond and the lattice matching of graphene improve thermal mismatch and crystal quality, and gallium nitride thin films are epitaxially grown.
It effectively improves the heat dissipation capacity of the device, reduces the temperature by more than 100°C, increases the power density by three times, extends the device life, and improves the quality of the gallium nitride layer and the stability of the device.
Smart Images

Figure CN115377196B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of power device technology, and in particular to an epitaxial GaN with diamond substrate and its preparation method. Background Technology
[0002] Existing silicon power devices have reached their theoretical limits, while gallium nitride (GaN) materials, as third-generation semiconductor materials, have superior fundamental parameters and greater potential for development. GaN power devices are suitable for high-frequency, high-temperature, and high-efficiency applications, effectively reducing system size, increasing power density, and ultimately lowering system costs.
[0003] However, with continuous improvements in the design and fabrication of GaN power devices, their theoretical output power is increasing, their frequency is rising, and their size is shrinking. Yet, under these conditions of miniaturization and power increase, the reliability and stability of GaN-based microwave power devices face serious challenges. The primary reason is that as power density increases, the heat accumulation effect in the active region of the GaN chip rapidly increases, leading to a rapid deterioration of various performance indicators and preventing the full realization of their high-power advantages. Therefore, heat dissipation has become one of the main problems restricting the further development and widespread application of GaN-based power devices.
[0004] The study found that diamond wafers are generally made of polycrystalline diamond. Polycrystalline diamond often has some drawbacks that are difficult to solve with current processing technology. During grinding or polishing, due to the polycrystalline structure, some tiny grains will fall off under stress, causing nanoscale pits on the diamond surface. If aluminum nitride is sputtered directly, it will cause serious deterioration of the quality of aluminum nitride and the formation of pits on the surface of aluminum nitride, which will seriously affect the subsequent epitaxy of gallium nitride. Summary of the Invention
[0005] This application is made in view of the above-mentioned problems, and its purpose is to provide a solution to the problems of high defect density, tensile or compressive stress, lattice mismatch and thermal mismatch, poor thermal conductivity, unstable operation and short life in gallium nitride devices.
[0006] To achieve the above objectives, this application provides an epitaxial GaN with a diamond substrate, comprising a diamond substrate, a single or multiple graphene layers disposed on the diamond substrate, an aluminum nitride layer sputtered on the graphene layers, and a gallium nitride thin film epitaxially grown on the aluminum nitride; wherein the diamond is single-crystal diamond or polycrystalline diamond.
[0007] Therefore, this application utilizes CVD diamond with a thermal conductivity as high as 2000W / mK, which can quickly dissipate the heat generated by the device, cool the device in a timely manner, maintain stable operation of the device, and extend the device life.
[0008] By introducing single-layer or multi-layer graphene, the shedding of some fine grains caused by grinding and polishing the surface of polycrystalline diamond can be reduced, thus reducing the formation of nanoscale pits on the diamond surface and greatly improving the adverse effects of these pits on aluminum nitride growth. It can also eliminate lattice and thermal mismatches between diamond and aluminum nitride, and eliminate tensile or compressive stresses in the crystal, greatly improving the crystal quality of sputtered aluminum nitride. At the same time, since the lattice constants of aluminum nitride and gallium nitride are very close, the quality of the epitaxial gallium nitride layer is also greatly improved.
[0009] Diamond is the substance with the highest thermal conductivity in nature, with a thermal conductivity value five times that of copper. Currently, the thermal conductivity of synthetic diamond can reach over 2000 W / mK, and the linear thermal expansion coefficient of diamond can be as low as 1.2 ppm / K. Diamond is composed of simple carbon atoms forming a regular tetrahedron, which is an ideal molecular structure for efficient heat transfer.
[0010] Diamond conducts heat rapidly in both the horizontal and vertical directions, possessing not only excellent thermal conductivity but also excellent heat dissipation capabilities, resulting in uniform heat distribution and timely heat dissipation from the chip. Furthermore, it exhibits superior mechanical, acoustic, optical, electrical, and chemical properties, giving it a significant advantage in addressing heat dissipation challenges in high-power optoelectronic devices.
[0011] Therefore, when diamond is used as the substrate material in GaN-based devices, due to diamond's excellent thermal conductivity, the heat generated in the device source region can be quickly dissipated, cooling the device. The device temperature can be reduced by 100°C or even higher, while the device power density can be increased by more than three times.
[0012] In any embodiment, the thickness of the diamond is 100-300 micrometers.
[0013] In any embodiment, the thickness of the aluminum nitride layer is 20-200 nm.
[0014] In any embodiment, the thickness of the gallium nitride film is 150-250 nm.
[0015] A method using CVD diamond with a thermal conductivity as high as 2000 W / mK can rapidly dissipate the heat generated by the device, cool the device in a timely manner, maintain stable operation, and extend the device life. Introducing single-layer or multi-layer graphene can greatly improve the adverse effects of pits on aluminum nitride growth, eliminate lattice mismatch and thermal mismatch between diamond and aluminum nitride, eliminate tensile or compressive stress in the crystal, and greatly improve the crystal quality of sputtered aluminum nitride, thus improving the overall quality of aluminum nitride.
[0016] The second aspect of this application provides a method for preparing epitaxial GaN on a diamond substrate, the steps of which are as follows: Step 1: Preparation of polycrystalline diamond substrate A) The processed silicon wafer is placed in MPCVD (microwave plasma chemical vapor deposition), the cavity is evacuated, hydrogen gas is then introduced, the microwave power supply is turned on, and methane gas is introduced. The methane is decomposed, and polycrystalline diamond is gradually grown on the surface of the silicon wafer. B) After growth is complete, the sample is removed from the cavity and ground and polished. After polishing, the silicon bonded to the polycrystalline diamond is removed by chemical etching, and finally a self-supporting substrate of polycrystalline diamond is formed. Step 2: Preparation of single or multiple graphene layers A) A layer of PMMA solution is uniformly spin-coated onto the surface of multilayer or single-layer graphene grown on copper foil, and then dried. B) After drying, place it in a copper-corroding solution for at least half an hour. C) After etching, place the substrate in pure deionized water and then transfer the PMMA / graphene film to the surface of the polycrystalline diamond substrate; coat the graphene with PMMA to prevent damage during subsequent transfer.
[0017] D) After the transfer is completed, the polycrystalline diamond is dried to ensure that the graphene layer adheres tightly to the surface of the polycrystalline diamond substrate; then the polycrystalline diamond substrate is placed in an acetone solution and heated in a water bath to completely dissolve the PMMA. E) The polycrystalline diamond is then dried in a drying oven to form a single or multiple layer of graphene on the surface of the polycrystalline diamond.
[0018] Step 3: Sputtering aluminum nitride layer A) Place the diamond substrate with the transferred graphene into a magnetron sputtering apparatus and perform vacuuming; B) Introduce nitrogen and argon gas while heating the sample. Once the temperature is reached, perform sputtering. C) The sputtering time is 5-40 minutes, and the thickness of the aluminum nitride film is between 20-200 nanometers to complete the sputtering of the aluminum nitride layer; Step 4: Fabrication of gallium nitride epitaxial layer The sample after magnetron sputtering aluminum nitride was taken out in a high-cleanliness environment and then placed in an MOCVD device. The reaction temperature was set to 1000-1100℃ and the gas pressure in the reaction chamber was 15-25 Torr. Ammonia and gallium source gas were introduced into the reaction chamber to epitaxially form a high-quality gallium nitride thin film with a thickness of 150-250 nanometers on the surface of aluminum nitride.
[0019] A method for preparing epitaxial GaN on a diamond substrate, comprising the following steps: Step 1: Prepare single-crystal diamond, which has a thickness of 300-500 micrometers and a surface roughness of less than 2 nanometers; Step 2: Transfer of single or multiple graphene layers A) A layer of PMMA solution is uniformly spin-coated onto the surface of multilayer or single-layer graphene grown on copper foil, and then dried. B) After drying, place it in a copper-corroding solution for at least half an hour. C) After etching, place the substrate in pure deionized water and then transfer the PMMA / graphene film to the surface of the single-crystal diamond substrate; coat the graphene with PMMA to prevent damage during subsequent transfer.
[0020] D) After the transfer is completed, the single crystal diamond is dried to ensure that the graphene layer adheres tightly to the surface of the single crystal diamond substrate; then the single crystal diamond substrate is placed in an acetone solution and heated in a water bath to completely dissolve the PMMA. E) The single-crystal diamond is then dried in a drying oven to form a single layer or multiple layers of graphene on the surface of the single-crystal diamond.
[0021] Step 3: Sputtering aluminum nitride layer A) Place the single-crystal diamond substrate with the transferred graphene into a magnetron sputtering device and perform vacuuming; B) Introduce nitrogen and argon gas while heating the sample. Once the temperature is reached, perform sputtering. C) The sputtering time is 5-40 minutes, and the thickness of the aluminum nitride film is between 20-200 nanometers to complete the sputtering of the aluminum nitride layer; Step 4: Fabrication of gallium nitride epitaxial layer The sample after magnetron sputtering aluminum nitride was taken out in a high-cleanliness environment and then placed in an MOCVD device. The reaction temperature was set to 1000-1100℃ and the gas pressure in the reaction chamber was 15-25 Torr. Ammonia and gallium source gas were introduced into the reaction chamber to epitaxially form a high-quality gallium nitride thin film with a thickness of 150-250 nanometers on the surface of aluminum nitride.
[0022] When processing diamond, the surface roughness of polycrystalline diamond must be below 1 nanometer, and the grain size must be around 50 micrometers. For sputtering aluminum nitride, the substrate sample needs to be heated to 1000°C to produce high-quality aluminum nitride.
[0023] In some embodiments, step A) involves pre-treating the silicon wafer by sequentially sonicating it with hydrofluoric acid, alcohol, and acetone for 2-5 minutes, then placing it in a diamond micron powder solution and sonicating it for half an hour, followed by sequentially sonicating it with alcohol and deionized water for 2-5 minutes.
[0024] In some embodiments, the growth time in step A) is 30-60 hours, and the diamond thickness is 100-300 micrometers.
[0025] In some embodiments, the diamond micron powder in step A) has a particle size of 15-25 micrometers, preferably 20 micrometers.
[0026] In some embodiments, step two (D) involves water bath heating at a temperature of 50-70°C for a duration of no less than five hours.
[0027] In some embodiments, in step two (E), the polycrystalline diamond is dried in a drying oven at a temperature of 80-100°C.
[0028] In some embodiments, in step three (A), the vacuum level in the cavity is reduced to less than 0.1 mTorr, and then nitrogen and argon are introduced to clean the vacuum cavity.
[0029] In some embodiments, the heating rate in step three (B) is no higher than 20°C per minute, with a preferred heating rate of 10-20°C per minute, heating the sample to 700-1000°C. After the temperature is reached, formal sputtering is performed. During sputtering, the gas pressure is controlled at 3-6 mTorr, the power of the RF power supply is 150-250 watts, and the target material is pure aluminum.
[0030] In some embodiments, in step four, ammonia gas with a flow rate of 2000-2400 sccm and gallium source gas with a flow rate of 30-50 sccm are introduced into the reaction chamber.
[0031] The beneficial effects of this invention are: 1. Traditional gallium nitride (GaN) devices use silicon, silicon carbide, or sapphire as substrate materials. These devices often generate significant heat during operation. However, due to the limited thermal conductivity of silicon and silicon carbide, this heat cannot be dissipated quickly, leading to decreased power density, reduced lifespan, and even device failure. CVD diamond, on the other hand, boasts a thermal conductivity as high as 2000 W / mK, enabling rapid heat dissipation, timely cooling, stable operation, and extended device lifespan.
[0032] 2. During the grinding and polishing process, due to its own structure, some small grains may fall off the surface of polycrystalline diamond, forming nanoscale pits on the surface of polycrystalline diamond. This is detrimental to the subsequent growth of aluminum nitride layers. By introducing single or multiple layers of graphene, the adverse effects of these pits on aluminum nitride growth can be greatly mitigated.
[0033] 3. The lattice and thermal mismatch between single-crystal or polycrystalline diamond and aluminum nitride is significant. Directly growing aluminum nitride on the diamond surface often results in poor aluminum nitride quality, high defect density in the crystal, and the presence of tensile or compressive stress, which is also detrimental to subsequent epitaxial gallium nitride layers. By introducing graphene intercalation, the lattice and thermal mismatch between diamond and aluminum nitride can be eliminated, as well as the tensile or compressive stress in the crystal, greatly improving the crystal quality of sputtered aluminum nitride.
[0034] 4. The quality of aluminum nitride was improved by introducing a graphene layer. Similarly, since the lattice constants of aluminum nitride and gallium nitride are very close, the quality of the epitaxial gallium nitride layer was also greatly improved. Attached Figure Description
[0035] Figure 1 This is a structural diagram of an epitaxial GaN with a diamond substrate; Figure 2 This is an HRXRD pattern of aluminum nitride sputtered in epitaxial GaN with a diamond substrate; Figure 3 This is an AFM image of aluminum nitride sputtered in an epitaxial GaN substrate with diamond as the substrate; Figure 4 This is a SEM image of aluminum nitride sputtered in epitaxial GaN with a diamond substrate; Figure 5 This is a SEM image of diamond in epitaxial GaN with a diamond substrate; Figure 6 This is an AFM image of diamond in epitaxial GaN with a diamond substrate. Detailed Implementation
[0036] The following detailed description, with appropriate reference to the accompanying drawings, discloses an embodiment of a method for preparing epitaxial GaN on a diamond substrate according to this application. However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repetitive descriptions of practically identical structures may be omitted. This is to avoid unnecessarily lengthy descriptions and to facilitate understanding by those skilled in the art. Furthermore, the accompanying drawings and the following description are provided for the purpose of enabling those skilled in the art to fully understand this application and are not intended to limit the subject matter of the claims.
[0037] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values of 1 and 2 are listed, and if maximum range values of 3, 4, and 5 are listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0038] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.
[0039] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions.
[0040] Unless otherwise specified, all steps in this application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the mention that the method may also include step (c) indicates that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.
[0041] Unless otherwise specified, the terms "comprising" and "including" as used in this application can be open-ended or closed-ended. For example, "comprising" and "including" can mean that other components not listed may also be included, or that only the listed components may be included.
[0042] Unless otherwise specified, the term "or" is inclusive in this application. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, the condition "A or B" is satisfied by any of the following conditions: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0043] The embodiments described below illustrate embodiments of this application. These embodiments are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.
[0044] Example 1 A method for preparing epitaxial GaN on a diamond substrate, comprising the following steps: Step 1: Prepare a polycrystalline diamond substrate or directly use single-crystal diamond. A) Pre-treat the silicon wafer by sequentially sonicating it with hydrofluoric acid, alcohol, and acetone for 2 minutes each, then placing it in a diamond micron powder solution and sonicating it for half an hour, followed by sequentially sonicating it with alcohol and deionized water for 3 minutes each.
[0045] B) The processed silicon wafer is placed in an MPCVD chamber, the chamber is evacuated, and then hydrogen gas is introduced. The microwave power supply is turned on, initiating a glow discharge within the chamber and creating a plasma environment. Methane gas is then introduced, causing it to decompose and deposit on the silicon wafer surface. Simultaneously, hydrogen ions etch the sp2 carbon, gradually growing polycrystalline diamond on the silicon wafer surface. The growth time is not fixed and can be adjusted according to the desired diamond thickness. In this experiment, the growth time was 30 hours, and the diamond thickness was 100 micrometers.
[0046] C) After growth, the sample is removed from the chamber and ground and polished to achieve a surface roughness of approximately 1 nanometer. After polishing, the silicon substrate bonded to the diamond is removed by chemical etching, ultimately forming a self-supporting substrate from the prepared diamond.
[0047] The diamond used in the following steps is either single-crystal diamond or polycrystalline diamond.
[0048] Step 2: Preparation of single or multiple graphene layers.
[0049] A) A layer of PMMA solution is uniformly spin-coated onto the surface of multilayer or single-layer graphene grown on copper foil, and then dried. B) After drying, place it in a copper-corroding solution for half an hour to completely corrode the copper foil. C) After etching, place the film in pure deionized water and then transfer the PMMA / graphene film to the surface of the diamond substrate. D) After the transfer is complete, the diamond is dried to ensure a tight bond between the graphene layer and the diamond substrate surface. The diamond substrate is then placed in an acetone solution and heated in a water bath at 50°C. This step aims to completely dissolve the PMMA covering the graphene surface in the acetone, thus exposing the graphene film on the diamond surface. The water bath heating lasts for 5 hours to ensure complete dissolution of the PMMA.
[0050] E) The diamond is then dried in a drying oven at 80°C to complete the preparation of single-layer or multi-layer graphene.
[0051] Step 3: Sputter aluminum nitride layer.
[0052] A) Place the diamond substrate with the transferred graphene into a magnetron sputtering device and evacuate it to a vacuum level below 0.1 mTorr. Then, purge the vacuum chamber with nitrogen and argon.
[0053] B) After cleaning, nitrogen and argon gases are introduced while the sample is heated at a rate not exceeding 10°C per minute to 700°C. Once the temperature is reached, the gas pressure is adjusted to 15 mTorr, and pre-sputtering is performed for ten minutes. Afterward, the sample baffle is opened for the formal sputtering. During sputtering, the gas pressure is controlled at 3 mTorr, the RF power supply is 150 watts, and the target material is pure aluminum.
[0054] C) The sputtering time is 5 minutes, and the thickness of the aluminum nitride film is between 20 nanometers, to complete the preparation of the sputtered aluminum nitride layer.
[0055] Step 4: Fabrication of gallium nitride epitaxial layer The sample after magnetron sputtering aluminum nitride was removed under a high-cleanliness environment and then placed in an MOCVD apparatus. The reaction temperature was set to 1000℃ and the gas pressure in the reaction chamber was 15 Torr. Ammonia gas at a flow rate of 2000 sccm and gallium source gas at a flow rate of 30 sccm were introduced into the reaction chamber to epitaxially deposit a high-quality gallium nitride thin film on the aluminum nitride surface. The thickness of the film was 150 nanometers, and the specific thickness could be adjusted according to the epitaxial time.
[0056] Example 2 A method for preparing epitaxial GaN on a diamond substrate, comprising the following steps: Step 1: Prepare a polycrystalline diamond substrate or directly use single-crystal diamond. A) Pre-treat the silicon wafer by sequentially sonicating it with hydrofluoric acid, alcohol, and acetone for 3 minutes each, then placing it in a diamond micron powder solution and sonicating it for half an hour, followed by sequentially sonicating it with alcohol and deionized water for 4 minutes each.
[0057] B) The processed silicon wafer is placed in an MPCVD chamber, the chamber is evacuated, and then hydrogen gas is introduced. The microwave power supply is turned on, initiating a glow discharge within the chamber and creating a plasma environment. Methane gas is then introduced, causing it to decompose and deposit on the silicon wafer surface. Simultaneously, hydrogen ions etch the sp2 carbon, gradually growing polycrystalline diamond on the silicon wafer surface. The growth time is not fixed and can be adjusted according to the desired diamond thickness. In this experiment, the growth time was 40 hours, and the diamond thickness was 200 micrometers.
[0058] C) After growth, the sample is removed from the chamber and ground and polished to achieve a surface roughness of approximately 1 nanometer. After polishing, the silicon substrate bonded to the diamond is removed by chemical etching, ultimately forming a self-supporting substrate from the prepared diamond.
[0059] The diamond used in the following steps is either single-crystal diamond or polycrystalline diamond.
[0060] Step 2: Preparation of single or multiple graphene layers.
[0061] A) A layer of PMMA solution is uniformly spin-coated onto the surface of multilayer or single-layer graphene grown on copper foil, and then dried. B) After drying, place it in a copper-corroding solution for half an hour or even longer until the copper foil is completely corroded away. C) After etching, place the film in pure deionized water and then transfer the PMMA / graphene film to the surface of the diamond substrate. D) After the transfer is complete, the diamond is dried to ensure a tight bond between the graphene layer and the diamond substrate surface. The diamond substrate is then placed in an acetone solution and heated in a water bath at 60°C. The purpose of this step is to completely dissolve the PMMA covering the graphene surface in the acetone, thereby exposing the graphene film on the diamond surface. The water bath heating time should be no less than five hours to ensure complete dissolution of the PMMA.
[0062] E) The diamond is then dried in a drying oven at 90°C to complete the preparation of single-layer or multi-layer graphene.
[0063] Step 3: Sputter aluminum nitride layer.
[0064] A) Place the diamond substrate with the transferred graphene into a magnetron sputtering device and evacuate it to a vacuum level below 0.1 mTorr. Then, purge the vacuum chamber with nitrogen and argon.
[0065] B) After cleaning, nitrogen and argon gases are introduced while the sample is heated at a rate not exceeding 15°C per minute to 800°C. Once the temperature is reached, the gas pressure is adjusted to 18 mTorr, and pre-sputtering is performed for ten minutes. Afterward, the sample baffle is opened for the formal sputtering. During sputtering, the gas pressure is controlled at 5 mTorr, the RF power supply is 200 watts, and the target material is pure aluminum.
[0066] C) The sputtering time is 20 minutes, and the thickness of the aluminum nitride film is between 100 nanometers, to complete the preparation of the sputtered aluminum nitride layer.
[0067] Step 4: Fabrication of gallium nitride epitaxial layer The sample after magnetron sputtering aluminum nitride was removed under a high-cleanliness environment and then placed in an MOCVD apparatus. The reaction temperature was set to 1080℃ and the gas pressure in the reaction chamber was 20 Torr. Ammonia gas was introduced into the reaction chamber at a flow rate of 2200 sccm, and the film thickness was 200 nanometers. The specific thickness could be adjusted according to the epitaxial growth time.
[0068] Example 3 A method for preparing epitaxial GaN on a diamond substrate, comprising the following steps: Step 1: Prepare a polycrystalline diamond substrate or directly use single-crystal diamond. A) Pre-treat the silicon wafer by sequentially sonicating it with hydrofluoric acid, alcohol, and acetone for 5 minutes each, then placing it in a diamond micron powder solution and sonicating it for half an hour, followed by sequentially sonicating it with alcohol and deionized water for 5 minutes each.
[0069] B) The processed silicon wafer is placed in an MPCVD chamber, the chamber is evacuated, and then hydrogen gas is introduced. The microwave power supply is turned on, initiating a glow discharge within the chamber and creating a plasma environment. Methane gas is then introduced, causing it to decompose and deposit on the silicon wafer surface. Simultaneously, hydrogen ions etch the sp2 carbon, gradually growing polycrystalline diamond on the silicon wafer surface. The growth time is not fixed and can be adjusted according to the desired diamond thickness. In this experiment, the growth time was 60 hours, and the diamond thickness was 300 micrometers.
[0070] C) After growth, the sample is removed from the chamber and ground and polished to achieve a surface roughness of approximately 1 nanometer. After polishing, the silicon substrate bonded to the diamond is removed by chemical etching, ultimately forming a self-supporting substrate from the prepared diamond.
[0071] The diamond used in the following steps is either single-crystal diamond or polycrystalline diamond.
[0072] Step 2: Preparation of single or multiple graphene layers.
[0073] A) A layer of PMMA solution is uniformly spin-coated onto the surface of multilayer or single-layer graphene grown on copper foil, and then dried. B) After drying, place it in a copper-corroding solution for half an hour or even longer until the copper foil is completely corroded away. C) After etching, place the film in pure deionized water and then transfer the PMMA / graphene film to the surface of the diamond substrate. D) After the transfer is complete, the diamond is dried to ensure a tight bond between the graphene layer and the diamond substrate surface. The diamond substrate is then placed in an acetone solution and heated in a water bath at 70°C. The purpose of this step is to completely dissolve the PMMA covering the graphene surface in the acetone, thereby exposing the graphene film on the diamond surface. The water bath heating time should be no less than five hours to ensure complete dissolution of the PMMA.
[0074] E) The diamond is then dried in a drying oven at 100°C to complete the preparation of single-layer or multi-layer graphene.
[0075] Step 3: Sputter aluminum nitride layer.
[0076] A) Place the diamond substrate with the transferred graphene into a magnetron sputtering device and evacuate it to a vacuum level below 0.1 mTorr. Then, purge the vacuum chamber with nitrogen and argon.
[0077] B) After cleaning, nitrogen and argon gases are introduced while the sample is heated at a rate not exceeding 20°C per minute to 1000°C. Once the temperature is reached, the gas pressure is adjusted to 20 mTorr, and pre-sputtering is performed for ten minutes. Afterward, the sample baffle is opened for the formal sputtering. During sputtering, the gas pressure is controlled at 5 mTorr, the RF power supply is 250 watts, and the target material is pure aluminum.
[0078] C) The sputtering time is 40 minutes, and the thickness of the aluminum nitride film is between 200 nanometers, to complete the preparation of the sputtered aluminum nitride layer.
[0079] Step 4: Fabrication of gallium nitride epitaxial layer The sample after magnetron sputtering aluminum nitride was removed under a high-cleanliness environment and then placed in an MOCVD apparatus. The reaction temperature was set to 1100℃ and the gas pressure in the reaction chamber was 25 Torr. Ammonia gas at a flow rate of 2400 sccm and gallium source gas at a flow rate of 50 sccm were introduced into the reaction chamber to epitaxially deposit a high-quality gallium nitride thin film on the aluminum nitride surface. The thickness of the film was 250 nanometers, and the specific thickness could be adjusted according to the epitaxial time.
[0080] The single-crystal diamond is either commercially available or obtained using existing preparation methods to meet the requirements of this application.
[0081] The test results at each stage are as follows: Figure 1-6 . Figure 2 By introducing a graphene layer, the quality of aluminum nitride was significantly improved, and the full width at half maximum (FWHM) of the XRD rocking curve decreased from 6 to about 2.85. Figure 3 The roughness of sputtered aluminum nitride is very low, less than one nanometer. Figure 4 The sputtered aluminum nitride surface is very uniform and has a very high degree of flatness.
[0082] It should be noted that this application is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this application are included in the technical scope of this application. Furthermore, various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing by combining some of the constituent elements of the embodiments, without departing from the spirit of this application, are also included in the scope of this application.
Claims
1. A method for producing diamond substrate epitaxial GaN, characterized by, Includes the following steps: Step 1: Preparation of polycrystalline diamond substrate A) The processed silicon wafer is placed in an MPCVD chamber, the chamber is evacuated, hydrogen gas is then introduced, the microwave power supply is turned on, and methane gas is introduced to gradually grow polycrystalline diamond on the surface of the silicon wafer. B) After growth is complete, the sample is removed from the chamber and ground and polished; After polishing, the silicon bonded to the diamond is removed by chemical etching, ultimately forming a self-supporting diamond substrate. Step 2: Preparation of single or multiple graphene layers A) A layer of PMMA solution is uniformly spin-coated onto the surface of multilayer or single-layer graphene grown on copper foil, and then dried. B) After drying, place it in a copper-corroding solution for at least half an hour. C) After etching, place the film in pure deionized water and then transfer the PMMA / graphene film to the surface of the diamond substrate. D) After the transfer is completed, the diamond is dried; then the diamond substrate is placed in an acetone solution and heated in a water bath at 50-70°C for no less than five hours to completely dissolve the PMMA. E) The diamond is then dried in a drying oven to form a single or multiple layer of graphene on the diamond surface. The single or multiple layer of graphene is used to improve the adverse effect of nanoscale pits formed on the surface of the polycrystalline diamond substrate due to grain shedding on the growth of the aluminum nitride layer. Step 3: Sputtering aluminum nitride layer A) Place the diamond substrate with the transferred graphene into a magnetron sputtering device and perform vacuuming; B) Introduce nitrogen and argon gas while heating the sample. Sputter the sample after the temperature reaches 800-1000℃. C) The sputtering time is 5-40 minutes, and the thickness of the aluminum nitride layer is between 20-200 nanometers to complete the sputtering of the aluminum nitride layer; Step 4: Fabrication of gallium nitride epitaxial layer The sample after magnetron sputtering aluminum nitride was taken out in a high-cleanliness environment and then placed in an MOCVD device. The reaction temperature was set to 1000-1100℃ and the gas pressure to 15-25 Torr. Ammonia gas with a flow rate of 2000-2400 sccm and gallium source gas with a flow rate of 30-50 sccm were introduced into the reaction chamber to epitaxially form a high-quality gallium nitride thin film with a thickness of 150-250 nanometers on the surface of aluminum nitride.
2. The production method according to claim 1, characterized by, In step A), the silicon wafer is pretreated by sequentially sonicating it with hydrofluoric acid, alcohol, and acetone for 2-5 minutes, then placing it in a diamond micro powder solution and sonicating it for half an hour, followed by sequentially sonicating it with alcohol and deionized water for 2-5 minutes.
3. The preparation method according to claim 1, characterized in that, In step A), the growth time is 30-60 hours and the diamond thickness is 100-300 micrometers.
4. The preparation method according to claim 1, characterized in that, In step two (E), the temperature at which the diamond is dried in the drying oven is 80-100℃.
5. The preparation method according to claim 1, characterized in that, In step three (A), a vacuum is drawn to reduce the vacuum level in the cavity to below 0.1 mTorr, and then nitrogen and argon are introduced to clean the vacuum cavity.
6. The preparation method according to claim 1, characterized in that, In step three (B), the gas pressure is controlled during sputtering, the power of the RF power supply is 150-250 watts, and the target material is pure aluminum.
7. The epitaxial GaN on a diamond substrate obtained by the preparation method according to any one of claims 1-6, characterized in that, include: The polycrystalline diamond substrate comprises a single or multiple graphene layer disposed on the polycrystalline diamond substrate, an aluminum nitride layer sputtered on the graphene layer, and a gallium nitride thin film epitaxially grown on the aluminum nitride; the surface roughness of the polycrystalline diamond substrate is less than 1 nanometer, and the single or multiple graphene layers are used to mitigate the adverse effects of nanoscale pits formed on the surface of the polycrystalline diamond substrate due to grain shedding on the growth of the aluminum nitride layer; the thickness of the aluminum nitride layer is 20-200 nanometers; and the thickness of the gallium nitride thin film is 150-250 nanometers.
Citation Information
Patent Citations
GaN / AlGaN heterojunction material based on monocrystalline diamond substrate and preparation method of GaN / AlGaN heterojunction material
CN110828291A