Micro-nano island-shaped carbonate film, preparation method and perovskite solar cell

By using micro/nano-island carbonate films as interface modification layers in perovskite solar cells, the stress-strain state of the perovskite active layer is adjusted, solving the problems of film cracking and delamination at the interface of perovskite solar cells, and improving efficiency and stability.

CN115498112BActive Publication Date: 2026-11-20BEIJING INST OF TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211209041.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-30
Publication Date
2026-11-20
Estimated Expiration
2042-09-30

AI Technical Summary

Technical Problem

Existing perovskite solar cells suffer from problems such as thin film cracking and device delamination at the interface in terms of stress-strain regulation, resulting in insufficient stability. Currently, there is a lack of effective inorganic materials to achieve controllable stress-strain regulation at the interface.

Method used

Micro-nano island-shaped carbonate films are used as interface modification layers. By utilizing the high thermal expansion coefficient and nano-island structure of alkali metal carbonates, the stress-strain state of the perovskite active layer is adjusted through the annealing and cooling process, releasing the residual stress at the interface and forming a discontinuous island-shaped nanostructure to regulate the stress-strain state.

Benefits of technology

Effectively regulating the stress-strain state of the device interface and perovskite active layer reduces non-radiative recombination energy loss at the interface, suppresses ion migration and active layer decomposition, and improves the efficiency and stability of perovskite solar cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115498112B_ABST
    Figure CN115498112B_ABST
Patent Text Reader

Abstract

The application relates to a micro-nano island-shaped carbonate film, a preparation method and a perovskite solar cell, and belongs to the technical field of perovskite solar cells. The carbonate is an alkali metal carbonate with a thermal expansion coefficient of 10*10 ‑5 K ‑1 ~40*10 ‑5 K ‑1 , the nano island-shaped structure has a diameter of 100nm to 3000nm, and the thickness of the film is 0.5nm to 10nm. The film is prepared by adopting a solution method or a thermal physical evaporation method, controlling conditions to make the alkali metal carbonate discontinuously grow, and forming an island-shaped structure in an annealing stage. By virtue of the advantage that the thermal expansion coefficient of the alkali metal carbonate layer is higher than that of the perovskite active layer, the stress and strain behaviors of the perovskite active layer body phase can be adjusted to change the perovskite active layer from the original tensile state to a compression state through uneven deformation in the annealing cooling process. Further, the discontinuous island-shaped nano structure formed at the interface provides a deformation space and can release the concentrated residual stress and strain at the interface.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a micro / nano island-shaped carbonate thin film, its preparation method, and a perovskite solar cell, belonging to the field of perovskite solar cell technology. Background Technology

[0002] Perovskite solar cells have seen their photoelectric conversion efficiency increase dramatically from 3.8% to 25.7% in just over a decade, while tandem cells with silicon have surpassed the Shockley-Queisser limit, achieving a maximum conversion efficiency exceeding 29%. Despite the significant advantages of perovskite solar cells in photoelectric conversion efficiency, their stability remains a serious challenge.

[0003] Stress-strain engineering of perovskite solar cells has proven to have a significant impact on their photothermal stability, as it involves a comprehensive regulatory mechanism related to compositional heterogeneity, microstructure deformation, defect formation, electronic structure optimization, and ion migration barriers. Stress-strain induced lattice distortion in perovskite materials affects interatomic bonding, defect formation energy, and ion migration activation energy, leading to accelerated film degradation. At the interfaces of multilayer stacked device structures, stress-strain concentration is highly likely. Due to the thermal expansion coefficient mismatch between the charge transport layer and the perovskite, as well as relatively weak van der Waals forces, overloaded stress-strain can cause film rupture and premature delamination and separation of the device interface. These mechanical delaminations generate more exposed surface and point defects, providing channels for water and oxygen intrusion and sites for ion migration, thereby accelerating structural decomposition and device degradation. Therefore, controllable stress-strain modulation at the interface is crucial for improving the stability of perovskite solar cells.

[0004] To date, studies have shown that lattice strain in perovskite polycrystalline materials can be modulated through small atom / molecular doping, chemical crosslinking additives, and optimized annealing processes. These methods primarily focus on the stress-strain effect in the bulk. Furthermore, organic salts or polymers with specific functional groups are widely used in interface engineering to passivate defects and optimize optoelectronic performance. However, organic materials exhibit instability to the external environment (instability to water, oxygen, and light) and weak chemical interactions. Inappropriate selection of organic materials can even accelerate ion migration and halogen aggregation at the interface. Some studies have reported that Cs₂CO₃ can be used as a defect passivation layer or transport layer in solar cells to reduce non-radiative convergence losses and improve device conversion efficiency. However, no related technical solutions for achieving controllable stress-strain modulation at the interface using inorganic materials have been reported to date. Summary of the Invention

[0005] In view of this, the present invention aims to provide a micro / nano-island carbonate thin film, a preparation method thereof, and a perovskite solar cell. Utilizing the advantage that the alkali metal carbonate layer has a higher coefficient of thermal expansion than the perovskite active layer, the stress-strain behavior of the perovskite active layer bulk phase can be adjusted by non-uniform deformation during the annealing and cooling process, thereby changing it from a tensile state to a compressive state. Furthermore, the discontinuous island-like nanostructures formed at the interface provide deformation space, which can release the residual stress and strain concentrated at the interface.

[0006] To achieve the above objectives, the technical solution of the present invention is as follows:

[0007] A micro / nano-island-like carbonate film, wherein the carbonate has a coefficient of thermal expansion of 10 × 10⁻⁶. -5 K -1 ~40×10 - 5 K -1 The alkali metal carbonate has a micro / nano island structure with a diameter of 100 nm to 3000 nm and a film thickness of 0.5 nm to 10 nm.

[0008] Preferably, the diameter of the carbonate nanoisland structure is 500 nm to 1000 nm.

[0009] Preferably, the coefficient of thermal expansion of the carbonate is 20 × 10⁻⁶. -5 K -1 ~30×10 -5 K -1 .

[0010] Preferably, the carbonate is Li2CO3, Na2CO3, K2CO3, Rb2CO3 or Cs2CO3.

[0011] A method for preparing the micro / nano-island carbonate film according to the present invention, the method comprising the following steps:

[0012] molar concentration of 10 -6 mol / mL~10 -2 A mol / mL aqueous solution of alkali metal carbonate was spin-coated onto a substrate at a speed of 3000 rpm to 6000 rpm and annealed at 100℃ to 200℃ for 1 min to 15 min in an air annealing atmosphere to obtain a nano-island carbonate film on the substrate.

[0013] Alternatively, an alkali metal carbonate film can be deposited on the substrate using thermal evaporation, with a deposition vacuum degree of less than 1×10⁻⁶. -4 Pa, then annealed at 100℃~200℃ for 1min~5min, with a heating rate of 50℃ / s~200℃ / s, in a nitrogen atmosphere, to obtain a nano-island carbonate film on the substrate.

[0014] A perovskite solar cell includes a hole transport layer, a perovskite active layer, and an electron transport layer. The present invention describes a micro / nano-island carbonate film as an interface modification layer located on one or both sides of the perovskite active layer.

[0015] Preferably, when the interface modification layer is located between the hole transport layer and the perovskite active layer, the thickness is 8 nm to 10 nm; when the interface modification layer is located between the electron transport layer and the perovskite active layer, the thickness is 2 nm to 3 nm.

[0016] Preferably, the coefficient of thermal expansion of the perovskite active layer is 2 × 10⁻⁶. -5 K -1 ~8×10 -5 K -1 .

[0017] Preferably, the perovskite active layer is an ABX3 perovskite crystal, wherein A is one or more of formamidinium, methylamine, guanidine, cesium, rubidium, and potassium, B is one or more of a transition metal and a group IV to VI element, and X is one or more of a halide ion, such as iodide ion, chloride ion, bromide ion, or thiocyanate ion, and the thickness of the perovskite light-absorbing layer is 100 nm to 1000 nm.

[0018] Preferably, the hole transport layer material is 2,2',7,7'-tetratetra(N,N-p-methoxyaniline)-9,9'-spirodifluorene (Spiro-MeOTAD), methoxytriphenylamine-fluoroformamidinium (OMeTPAFA), poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] (PTAA), poly(3,4-ethylenedioxythiophene):poly(styrenesulfonate) (PEDOT:PSS), poly- 3-Hexylthiophene (P3HT), cuprous thiocyanate (CuSCN), nickel oxide, triphenylamine with a triphenylene core (H101), 3,4-ethylenedioxythiophene-methoxytriphenylamine (EDOT-OMeTPA), N-(4-aniline)carbazole-spirobisfluorene (CzPAF-SBF), poly[bis(4-phenyl)(4-butylphenyl)amine] (Poly-TPD) or polythiophene; thickness 50nm~300nm.

[0019] Preferably, the electron transport layer material is any one of imide compounds, quinone compounds, fullerenes and their derivatives, metal oxides and their doped oxides of Cd, Zn, In, Pb, Mo, W, Sb, Bi, Cu, Hg, Ti, Ag, Mn, Fe, V, Sn, Zr, Sr, Ga, Nb, Mg, Si and Cr, and lithium fluoride (LiF) and calcium fluoride (CaF2), and the thickness of the electron transport layer is 10 nm to 100 nm.

[0020] Preferably, the perovskite solar cell further includes a substrate and a counter electrode. The substrate is indium tin oxide conductive glass (ITO), fluorine-doped tin oxide conductive glass (FTO), indium tin oxide polyethylene naphthalate (PEN), or indium tin oxide polyethylene terephthalate (PET). The counter electrode layer material is platinum, gold, copper, silver, aluminum, chromium metal, or an alloy containing the aforementioned metals, and the thickness of the counter electrode layer is 80 nm to 500 nm.

[0021] Beneficial effects

[0022] This invention provides a micro / nano-island-shaped carbonate film, wherein the carbonate exhibits a high coefficient of thermal expansion, high melting and boiling points, high decomposition temperature, and easy solubility in water. The film's nano-island structure allows for the release of residual interfacial stress between the transport layer and the perovskite active layer, while simultaneously regulating the intrinsic stress of the active layer during the annealing and cooling process.

[0023] This invention provides a method for preparing micro / nano-island carbonate films. The method employs a solution method or a thermophysical evaporation method, and controls the conditions to allow alkali metal carbonates to grow discontinuously, forming island structures during the annealing stage. This results in the preparation of alkali metal carbonate layers with controllable thickness and different diameters of island-shaped nanostructures.

[0024] This invention provides a perovskite solar cell. By using an interface modification layer with a micro / nano-island carbonate thin film structure on one or both sides of the perovskite active layer, the high thermal expansion coefficient and nano-island structure of the interface modification material can effectively regulate the stress-strain state of the device interface and the perovskite active layer. It also satisfies the functions of regulating interface carrier dynamics, reducing non-radiative recombination energy loss at the interface, and suppressing interface ion migration and active layer decomposition. This can improve the efficiency and stability of the perovskite solar cell and has good application value for the industrialization of perovskite solar cells. Attached Figure Description

[0025] Figure 1 This is a diagram of the micro-island nanostructure of the alkali metal carbonate interface layer described in Example 1.

[0026] Figure 2 The stress-strain evolution diagram of the perovskite active layer before and after the insertion of the interface modification layer in Example 1 is shown.

[0027] Figure 3 The graph shows the conversion efficiency of the perovskite solar cell described in Example 1. Detailed Implementation

[0028] The present invention will be further described in detail below with reference to specific embodiments.

[0029] In the following embodiments or comparative examples:

[0030] (1) In perovskite solar cells:

[0031] The transparent electrode conductive substrate is characterized in that the substrate is indium tin oxide conductive glass (ITO), fluorine-doped tin oxide conductive glass (FTO), indium tin oxide polyethylene naphthalate (PEN), or indium tin oxide polyethylene terephthalate (PET).

[0032] The electron transport layer and hole transport layer are prepared by any one of the following methods: spin coating, blade coating, spray coating, screen printing, sputtering, vapor deposition, atomic layer deposition, and chemical vapor deposition.

[0033] The electron transport layer includes, but is not limited to, imide compounds, quinone compounds, fullerenes and their derivatives, metal oxides and their doped oxides of Cd, Zn, In, Pb, Mo, W, Sb, Bi, Cu, Hg, Ti, Ag, Mn, Fe, V, Sn, Zr, Sr, Ga, Nb, Mg, Si and Cr, as well as any one of lithium fluoride (LiF) and calcium fluoride (CaF2), and the thickness of the electron transport layer is 10 nm to 100 nm.

[0034] Hole transport layers include, but are not limited to, 2,2',7,7'-tetra(N,N-p-methoxyaniline)-9,9'-spirobifluorene (Spiro-MeOTAD), methoxytriphenylamine-fluoroformamidinium (OMeTPAFA), poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] (PTAA), poly(3,4-ethylenedioxythiophene):poly(styrene sulfonate) (PEDOT:PSS), poly-3-hexylthiophene (P3HT), cuprous thiocyanate (CuSCN), nickel oxide (Nickel Oxide), triphenylamine with a triphenylene core (H101), 3,4-ethylenedioxythiophene-methoxytriphenylamine (EDOT-OMeTPA), N-(4-aniline)carbazole-spirobifluorene (CzPAF-SBF), poly[bis(4-phenyl)(4-butylphenyl)amine] (Poly-TPD), and polythiophene.

[0035] Specifically, the perovskite light-absorbing layer material is ABX3 perovskite crystal, wherein A is any one or more of formamidinium, methylamine, guanidine, cesium, rubidium, and potassium alkali metals; B is any one or more of transition metals and group IV to VI elements; and X is any one or more of halide ions, iodide ions, chloride ions, bromide ions, or thiocyanate ions. The thickness of the perovskite light-absorbing layer is 100 nm to 1000 nm. The perovskite layer is prepared by any one of the following methods: suspension coating, spray coating, vapor deposition, blade coating, groove coating, flexographic printing, screen printing, and inkjet printing.

[0036] Specifically, the material of the counter electrode layer includes, but is not limited to, platinum, gold, copper, silver, aluminum, chromium metals or alloys containing such metals, and the counter electrode is prepared by magnetron sputtering, vacuum evaporation or electron beam evaporation, and the thickness of the counter electrode layer is 80 nm to 500 nm.

[0037] Example 1: Perovskite solar cell based on electron transport layer / Rb2CO3 interface modification layer

[0038] Step 1: The conductive ITO substrate is washed sequentially with distilled water, acetone, ethanol and isopropanol, and then treated with ultraviolet ozone for 30 minutes.

[0039] Step 2: Prepare a SnO2 electron transport layer on an ITO substrate. To prepare the electron transport layer, mix SnO2 and water at a volume ratio of 1:4, shake for 1 min to ensure homogeneity, and then filter through a 0.22 μm pore size filter membrane to obtain a SnO2 solution. Drop the SnO2 solution onto a conductive substrate, spin-coat at 3000 rpm for 30 s, and then anneal on a hot plate at 150 °C for 30 min to obtain the electron transport layer.

[0040] Step 3: Spin-coat the interface modification layer on the SnO2 electron transport layer. Mix 5 mg of alkali metal carbonate with 1 mL of deionized water, shake and swirl to prepare a clear carbonate aqueous solution. Spin-coat the solution onto the electron transport layer at 4000 rpm and anneal at 100 °C for 5 min in an air atmosphere to obtain the alkali metal carbonate interface modification layer.

[0041] Step 4: Two-step preparation of perovskite thin films. 691.5 mg PbI₂ (1.5 M) mixed with 20 mg CsI was dissolved in a mixed solvent of 900 mL N,N-dimethylformamide and 100 mL dimethyl sulfoxide. This solution was spin-coated onto the Rb₂CO₃ interface layer at 2500 rpm and annealed at 70 °C in a nitrogen glove box for 1 minute. A mixed organic cation solution was prepared by dissolving 90 mg methyl iodomethyl, 9 mg chloromethylamine, 8.35 mg bromomethylamine, and 18.8 mg methyl iodomethylamine in 1 mL isopropanol. This mixed organic cation solution was spin-coated onto the PbI₂ film at 2900 rpm for 30 s, and then annealed in air at 150 °C for 15 min to obtain the perovskite active layer.

[0042] Step 5: Add 72.3 mg of Spiro-OMeTAD to 1 ml of chlorobenzene solvent, along with 17.5 μL of Li-TFSI solution and 29 μL of 4-tert-butylpyridine as additives to prepare a Spiro-OMeTAD solution. Stir at room temperature for 6 h until completely dissolved. Filter the solution through a 0.22 μm pore size filter to obtain the Spiro-OMeTAD hole transport layer solution. Drop 15 μL of Spiro-OMeTAD solution onto the perovskite active layer and spin-coat at 3000 rpm for 30 s to prepare the hole transport layer.

[0043] Step 6: Place the battery prepared according to the above steps into a mask, and then place it together in a metal boat in a vacuum evaporation machine. Add an appropriate amount of gold as the evaporation material. Turn on the evaporation machine. When the vacuum degree is below 1.0 × 10⁻⁶... -4 Evaporation begins at Pa and stops when the evaporation thickness reaches 100 nm, thus preparing a gold electrode.

[0044] The scanning electron microscope results of the interface modification layer are as follows: Figure 1 As shown, Rb2CO3 is distributed in a micro-nano island structure with a diameter of 500 nm to 1000 nm.

[0045] The stress-strain results of the perovskite active layer before and after the insertion of the interface modification layer are as follows: Figure 2 As shown, the results indicate that the stress state of the perovskite active layer before the insertion of the interface modification layer is tensile, while the stress state after the insertion of the interface modification layer is compressive.

[0046] The resulting perovskite solar cell device was tested under standard simulated sunlight AM 1.5G (100mW / cm²). 2 Irradiation was performed under [a specific irradiation method], and a current-voltage scan was conducted using a Keithley 2400. The results are as follows: Figure 3 As shown, compared with perovskite solar cells without an interface modification layer, the energy absorption of the 30 perovskite solar cells prepared by the method described in this embodiment is significantly improved, and the statistical conversion efficiency increases from an average of 19% to 22%. Furthermore, the devices with Rb2CO3 interface treatment also exhibit excellent stability, with the cells maintaining 95% of their initial efficiency even after 2500 hours of continuous operation at the maximum power point.

[0047] Example 2: Perovskite solar cell based on hole transport layer / Rb2CO3 interface modification layer

[0048] Step 1: The conductive ITO substrate is washed sequentially with distilled water, acetone, ethanol and isopropanol, and then treated with ultraviolet ozone for 30 minutes.

[0049] Step 2: Prepare a SnO2 electron transport layer on an ITO substrate. To prepare the electron transport layer, mix SnO2 and water at a volume ratio of 1:4, shake for 1 min to ensure homogeneity, and then filter through a 0.22 μm pore size filter membrane to obtain a SnO2 solution. Drop the SnO2 solution onto a conductive substrate, spin-coat at 3000 rpm for 30 s, and then anneal on a hot plate at 150 °C for 30 min to obtain the electron transport layer.

[0050] Step 3: A two-step method was used to prepare the perovskite thin film. 691.5 mg PbI₂ (1.5 M) mixed with 20 mg CsI was dissolved in a mixed solvent of 900 mL N,N-dimethylformamide and 100 mL dimethyl sulfoxide. This solution was spin-coated onto the Rb₂CO₃ interface layer at 2500 rpm and annealed at 70 °C in a nitrogen glove box for 1 minute. A mixed organic cation solution was prepared by dissolving 90 mg methyl iodide, 9 mg chloromethylamine, 8.35 mg bromomethylamine, and 18.8 mg methyl iodide in 1 mL isopropanol. This mixed organic cation solution was spin-coated onto the PbI₂ film at 2900 rpm for 30 s, and then annealed in air at 150 °C for 15 min to obtain the perovskite active layer.

[0051] Step 4: Place the prepared substrate from the above steps into a completely perforated mask, and then place it together in a metal boat inside a vacuum evaporation machine. Add an appropriate amount of Rb₂CO₃ solid powder as the evaporation raw material. Turn on the evaporation machine. When the vacuum level is below 1.0 × 10⁻⁶... -4 Evaporation begins at Pa and stops when the evaporation thickness reaches 5 nm. After removal, it is quickly annealed for 5 min on a hot stage at 100 °C in a nitrogen glove box to prepare an alkali metal carbonate interface layer.

[0052] Step 5: Add 72.3 mg of Spiro-OMeTAD to 1 mL of chlorobenzene solvent, along with 17.5 μL of Li-TFSI solution and 29 μL of 4-tert-butylpyridine as additives to prepare a Spiro-OMeTAD solution. Stir at room temperature for 6 h until completely dissolved. Filter the solution through a 0.22 μm pore size filter to obtain the Spiro-OMeTAD hole transport layer solution. Drop 15 μL of Spiro-OMeTAD solution onto the perovskite layer and spin-coat at 3000 rpm for 30 s to prepare the hole transport layer.

[0053] Step 6: Place the prepared substrate from the above steps into a mask, and then place it together in a metal boat in a vacuum evaporation machine. Add an appropriate amount of gold as the evaporation material. Turn on the evaporation machine. When the vacuum level is below 1.0 × 10⁻⁶... -4 Evaporation begins at Pa and stops when the evaporation thickness reaches 100 nm, thus preparing a gold electrode.

[0054] Scanning electron microscopy results of the interface modification layer show that Rb2CO3 is distributed in a micro-nano island structure with a diameter of 500 nm to 1000 nm.

[0055] The stress-strain results of the perovskite active layer before and after the insertion of the interface modification layer show that the stress state of the perovskite active layer before the insertion of the interface modification layer is tensile, and the stress state after the insertion of the interface modification layer is compressive.

[0056] The resulting perovskite solar cell device was tested under standard simulated sunlight AM 1.5G (100mW / cm²). 2 Irradiation was performed under [a specific irradiation method], and current-voltage scanning tests were conducted using a Keithley 2400. The results showed that, compared to perovskite solar cells without an interface modification layer, the energy absorption of the 30 perovskite solar cells prepared by the method described in this embodiment was significantly improved, with the statistical conversion efficiency increasing from an average of 20% to 21.7%. Furthermore, the devices with the Rb₂CO₃ interface treatment also exhibited excellent stability.

[0057] In summary, the invention includes, but is not limited to, the above embodiments. Any equivalent substitutions or partial improvements made under the spirit and principles of this invention shall be considered to be within the protection scope of this invention.

Claims

1. A perovskite solar cell, characterized in that: It includes a hole transport layer, a perovskite active layer and an electron transport layer, with micro-nano island-shaped carbonate films serving as interface modification layers located on one or both sides of the perovskite active layer. The micro-nano island-shaped carbonate has a thermal expansion coefficient of 10 × 10⁻⁶. -5 K -1 ~40×10 -5 K -1 The alkali metal carbonate has a micro / nano island structure with a diameter of 100 nm to 3000 nm and a film thickness of 0.5 nm to 10 nm. The coefficient of thermal expansion of the perovskite active layer is 2×10⁻⁶. -5 K -1 ~8×10 -5 K -1 ; The carbonate is Li2CO3, Na2CO3, K2CO3, Rb2CO3 or Cs2CO3.

2. The perovskite solar cell as described in claim 1, characterized in that: The diameter of the carbonate nanoisland structure is 500 nm to 1000 nm.

3. A perovskite solar cell as described in claim 1, characterized in that: The coefficient of thermal expansion of the carbonate is 20 × 10⁻⁶. -5 K -1 ~30×10 -5 K -1 .

4. A perovskite solar cell as described in claim 1, characterized in that: The aforementioned micro / nano-island carbonate film is prepared by the following method, the steps of which include: molar concentration of 10 -6 mol / mL~10 -2 A mol / mL aqueous solution of alkali metal carbonate was spin-coated onto a substrate at a speed of 3000 rpm to 6000 rpm and annealed at 100℃ to 200℃ for 1 min to 15 min in an air atmosphere to obtain a micro-nano island-like carbonate film on the substrate. Alternatively, an alkali metal carbonate film can be deposited on the substrate using thermal evaporation, with a deposition vacuum degree of less than 1×10⁻⁶. 4 Pa, then annealed at 100℃~200℃ for 1min~5min, with a heating rate of 50℃ / s~200℃ / s, in a nitrogen atmosphere, to obtain a micro-nano island-like carbonate film on the substrate.

5. A perovskite solar cell as described in claim 1, characterized in that: When the interface modification layer is located between the hole transport layer and the perovskite active layer, the thickness is 8nm~10nm; when the interface modification layer is located between the electron transport layer and the perovskite active layer, the thickness is 2nm~3nm.

6. A perovskite solar cell as described in claim 1, characterized in that: The perovskite active layer is an ABX3 perovskite crystal, wherein A is one or more of formamidine, methylamine, guanidine, cesium, rubidium and potassium, B is one or more of transition metals and group IV to VI elements, and X is one or more of halide ions, iodide ions, chloride ions, bromide ions or thiocyanate ions, and the thickness of the perovskite active layer is 100nm~1000nm. The hole transport layer material is 2,2',7,7'-tetratetra(N,N-p-methoxyaniline)-9,9'-spirobisfluorene, methoxytriphenylamine-fluoroformamidinium, poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine], poly(3,4-ethylenedioxythiophene):poly(styrene sulfonate), poly-3-hexylthiophene, cuprous thiocyanate, nickel oxide, triphenylamine with a triphenylene core, 3,4-ethylenedioxythiophene-methoxytriphenylamine, N-(4-aniline)carbazole-spirobisfluorene, or poly[bis(4-phenyl)(4-butylphenyl)amine]; the thickness of the hole transport layer is 50 nm to 300 nm. The electron transport layer material is any one of imide compounds, quinone compounds, fullerenes and their derivatives, metal oxides and doped oxides of Cd, Zn, In, Pb, Mo, W, Sb, Bi, Cu, Hg, Ti, Ag, Mn, Fe, V, Sn, Zr, Sr, Ga, Nb, Mg, Si and Cr, and lithium fluoride and calcium fluoride; the thickness of the electron transport layer is 10 nm to 100 nm.

7. A perovskite solar cell as described in claim 1, characterized in that: The perovskite solar cell further includes a substrate and a counter electrode. The substrate is indium tin oxide conductive glass, fluorine-doped tin oxide conductive glass, indium tin oxide polyethylene naphthalate, or indium tin oxide polyterephthalate. The counter electrode layer material is platinum, gold, copper, silver, aluminum, chromium metal, or an alloy containing the aforementioned metals. The thickness of the counter electrode layer is 80 nm to 500 nm.

Citation Information

Patent Citations

  • High-performance perovskite solar cell and preparation method for same

    CN105826477A

  • Preparation method and solar cell of perovskite thin film

    CN113745405A