Laminated package substrate structure and method of making the same
By pre-forming windows in the insulating layer and using a composite insulating layer, the problems of fiberglass cloth breakage and exposure during lamination are solved, the thickness uniformity and filling capacity of the insulating layer are improved, and the stability and reliability of the encapsulation substrate are enhanced.
Patent Information
- Application Number
- CN202211131854.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-16
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2042-09-16
AI Technical Summary
In the prior art, the insulating layer using fiberglass cloth is prone to breakage or exposure during the lamination process, resulting in uneven insulating layer thickness and insufficient filling capacity, which affects the stability and reliability of the packaging substrate.
Openings corresponding to the conductive posts are pre-formed in the insulation layer, and a composite insulation layer containing fiberglass cloth and pure resin layer is formed by pre-pressing to avoid direct impact of the conductive posts on the fiberglass cloth, thus ensuring the uniformity of the insulation layer thickness and the filling capacity.
It improves the thickness control and filling capacity of the insulating layer, prevents fiberglass cloth exposure, reduces the surface roughness of the insulating layer, and enhances the stability and yield of the packaging substrate.
Smart Images

Figure CN115513067B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of semiconductor packaging technology, and in particular to the structure of a lamination packaging substrate and its fabrication method. Background Technology
[0002] With the rapid development of electronic technology, the performance requirements of electronic products are becoming increasingly demanding, leading to more complex electronic components and circuit board substrates. Simultaneously, the size requirements for electronic products are shrinking and thinning. This makes the integration, miniaturization, and multifunctionality of electronic components and circuit board substrates an inevitable trend. This necessitates smaller linewidths, line spacings, and vias / pillars on the circuit board, which serves as the carrier of components. Furthermore, the transmission of high-frequency signals and the requirement for signal integrity place higher demands on the impedance design of the circuit board, requiring corresponding circuit patterns with less side etching, fewer defects, and better integrity.
[0003] In existing technologies, lamination typically involves stacking an insulating layer of a certain thickness on the conductive pillars before lamination. The resulting insulating layer also requires grinding to expose the conductive pillars connecting the upper and lower circuit layers and to control the thickness of the insulating layer. If a pure resin film such as ABF or RCF is used as the insulating layer, it is prone to breakage due to the lack of fiberglass support, and the thickness control of the insulating layer after lamination becomes poor. Using a PP prepreg containing fiberglass as the insulating layer results in lower filling capacity, higher surface roughness of the thinned insulating layer, and exposure of the fiberglass. Summary of the Invention
[0004] In view of this, the purpose of this application is to propose a press-fit packaging substrate structure and a method for manufacturing the same.
[0005] To achieve the above objectives, this application provides a method for fabricating a lamination and packaging substrate structure, comprising the following steps:
[0006] (a) Prepare a temporary support plate;
[0007] (b) A first conductive post is formed on the surface of the temporary support plate;
[0008] (c) Forming a first insulating layer having a first opening, wherein the first insulating layer comprises fiberglass cloth;
[0009] (d) A first insulating layer is laminated on the first conductive post, such that the first conductive post passes through the first window and is embedded in the first insulating layer;
[0010] (e) A second conductive post and a first circuit layer are formed on the upper surface of the first insulating layer, wherein the second conductive post is electrically connected to the first conductive post;
[0011] (f) A second insulating layer having a second window is laminated on the first circuit layer and the second conductive post, such that the second conductive post is embedded in the second insulating layer through the second window, wherein the second insulating layer has fiberglass cloth.
[0012] (g) A second circuit layer is formed on the upper surface of the second insulating layer, wherein the second circuit layer is electrically connected to the first circuit layer through the second conductive post;
[0013] (h) Remove the temporary support plate and form a third circuit layer on the lower surface of the first insulating layer, wherein the third circuit layer is electrically connected to the first circuit layer through the first conductive post.
[0014] This application embodiment also provides a press-fit packaging substrate structure, including: a first insulating layer having a first opening, a first conductive post embedded in the first opening, a second insulating layer having a second opening on the first insulating layer, a first circuit layer embedded in the second insulating layer and a second conductive post embedded in the second opening, a second circuit layer on the second insulating layer, and a third circuit layer below the first insulating layer.
[0015] The first insulating layer and the second insulating layer are made of fiberglass cloth, the first circuit layer and the third circuit layer are electrically connected through a first conductive post, and the first circuit layer and the second circuit layer are electrically connected through a second conductive post.
[0016] Therefore, the lamination and packaging substrate structure and its preparation method provided in this application, by pre-forming windows corresponding to the conductive pillars within the insulating layer containing fiberglass cloth, allows the conductive pillars to pass through the insulating layer via the windows. This prevents unevenness caused by the conductive pillars forcibly passing through the insulating layer during lamination, prevents fiberglass cloth exposure, reduces the surface roughness of the thinned insulating layer, improves packaging stability, and increases yield. Furthermore, by pre-pressing the dielectric layer containing fiberglass cloth and the pure resin layer without fiberglass cloth to form the insulating layer, the thickness control capability of the insulating layer after lamination can be improved, as well as the filling capacity of the insulating layer. At the same time, it prevents excessive surface roughness of the thinned insulating layer and exposure of the fiberglass cloth. Attached Figure Description
[0017] To more clearly illustrate the technical solutions in this application or related technologies, the drawings used in the description of the embodiments or related technologies will be briefly introduced below. Obviously, the drawings described below are only embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0018] Figure 1 This is a schematic diagram of the cross-sectional structure of a laminated structure in the prior art;
[0019] Figure 2 This is another cross-sectional schematic diagram of a laminated structure in the prior art;
[0020] Figure 3 This is a cross-sectional schematic diagram of the lamination and packaging substrate structure according to an embodiment of this application;
[0021] Figure 4 This is another cross-sectional schematic diagram of the lamination and packaging substrate structure according to an embodiment of this application;
[0022] Figures 5a to 5n for Figure 3 and Figure 4 A cross-sectional schematic diagram of the intermediate structure in each step of the fabrication method of the lamination and packaging substrate structure. Detailed Implementation
[0023] To make the objectives, technical solutions, and advantages of this application clearer, the following detailed description is provided in conjunction with specific embodiments and the accompanying drawings.
[0024] It should be noted that, unless otherwise defined, the technical or scientific terms used in the embodiments of this application should have the ordinary meaning understood by one of ordinary skill in the art to which this application pertains. The terms "first," "second," and similar terms used in the embodiments of this application do not indicate any order, quantity, or importance, but are merely used to distinguish different components. Terms such as "comprising" or "including" mean that the element or object preceding the word encompasses the elements or objects listed after the word and their equivalents, without excluding other elements or objects. Terms such as "connected" or "linked" are not limited to physical or mechanical connections, but can include electrical connections, whether direct or indirect. Terms such as "upper," "lower," "left," and "right" are only used to indicate relative positional relationships; when the absolute position of the described object changes, the relative positional relationship may also change accordingly.
[0025] Figures 1-2 A schematic diagram of the cross-sectional structure of a laminated structure in the prior art is shown.
[0026] like Figure 1 As shown, during lamination, the insulating material is pressed between the protruding conductive posts, and then thinning and other processes are performed to expose the conductive posts. For example... Figure 2 As shown, when conventional PP prepreg containing fiberglass cloth is used as the insulating layer, the fiberglass cloth in the insulating layer will be pushed to the top of the insulating layer. After subsequent thinning treatment, it is easy to be exposed or broken. It will also lead to uneven thickness of the insulating layer and insufficient filling performance for the side of the conduction post, thus affecting the stability and reliability of the press-fit packaging substrate structure.
[0027] Figure 3 A cross-sectional schematic diagram of the press-fit packaging substrate structure according to an embodiment of this application is shown.
[0028] like Figure 3 As shown, the lamination and packaging substrate structure provided in this application embodiment may include: a first insulating layer 110 with a first window, a first conductive post 120 embedded in the first window, a second insulating layer 160 with a second window on the first insulating layer 110, a first circuit layer 140 embedded in the second insulating layer 160 and a second conductive post 150 embedded in the second window, a second circuit layer 170 on the second insulating layer 160, and a third circuit layer 130 below the first insulating layer 110, wherein the first insulating layer 110 has fiberglass cloth 111, and the second insulating layer 160 has fiberglass cloth 161. The first circuit layer 140 and the third circuit layer 130 are electrically connected through the first conductive post 120, and the first circuit layer 140 and the second circuit layer 170 are electrically connected through the second conductive post 150.
[0029] In some embodiments, the first insulating layer 110 is formed by laminating a first dielectric layer and a second dielectric layer, with the second dielectric layer close to the third circuit layer 130. The first dielectric layer can be a PP prepreg with fiberglass cloth in its center. The second dielectric layer is a pure resin layer without fiberglass cloth. In this way, the fiberglass cloth structure in the first insulating layer 110 obtained after lamination is close to the lower surface of the first insulating layer 110, the pure resin layer is close to the first circuit layer 140, and the PP prepreg is close to the third circuit layer 130, which can further improve the uniformity of the thickness of the first insulating layer 110.
[0030] In some embodiments, the material of the second dielectric layer may be a thin-film pure resin layer, such as an ABF film or an RCF film.
[0031] In some embodiments, the second insulating layer 160 has the same structure as the first insulating layer 110. That is, the second insulating layer 160 has a second opening corresponding to the second conductive post 150, and the second insulating layer 160 has fiberglass cloth 161.
[0032] In some embodiments, the second insulating layer 160 is formed by laminating a third dielectric layer and a fourth dielectric layer, with the fourth dielectric layer close to the first circuit layer 140. The third dielectric layer has a fiberglass cloth in its middle portion, which, after lamination, is close to the lower surface of the second insulating layer 160. The material and structure of the third dielectric layer can be the same as the first dielectric layer, and the material and structure of the fourth dielectric layer can be the same as the second dielectric layer; further details are omitted here.
[0033] In some embodiments, the surface of the first circuit layer 140 is covered by the fiberglass cloth 111 of the first insulating layer 110.
[0034] In some embodiments, multiple first conductive posts 120 and second conductive posts 150 may be provided, and they may be metal conductive posts, such as copper posts. A first metal seed layer 131 may be applied to the lower surface of the first insulating layer 110; a second metal seed layer 141 may be applied to the upper surface of the first insulating layer 110. In some embodiments, a third metal seed layer 171 may be applied to the upper surface of the second insulating layer 160.
[0035] In some embodiments, such as Figure 4 As shown, the substrate may further include a first solder mask 181 disposed on the upper surface of the second circuit layer 170 and a second solder mask 182 disposed on the lower surface of the third circuit layer 130. The first solder mask 181 and the second solder mask 182 provide insulation to the laminated package substrate structure. Pads (not shown) may be provided on the first solder mask 181 at positions corresponding to the second circuit layer 170 for electrical connection or testing. Pads may be provided on the second solder mask 182 at positions corresponding to the third circuit layer 130 for electrical connection or testing.
[0036] In some embodiments, a protective layer (not shown) may also be included, disposed on the upper surface of the pads. The protective layer prevents pad oxidation and enhances substrate reliability. Protective layer materials include chemically stable metals such as nickel-palladium-gold, nickel-gold, tin, and silver, or mechanically insulating solder films.
[0037] Reference Figures 5a to 5n , showed Figure 3 and Figure 4 The method for fabricating a lamination and packaging substrate structure.
[0038] The fabrication method of the lamination and packaging substrate structure includes the following steps: preparing a temporary carrier board 10 - step (a), such as Figure 5a As shown. Typically, the temporary carrier board can be a core board with a separable copper foil layer, which facilitates subsequent removal of the temporary carrier board. Specifically, the temporary carrier board may include a core layer 101, a first metal layer 102, a second metal layer 103, an etch barrier layer 104, and a first metal seed layer 131. The first metal layer 102 and the second metal layer 103 are typically copper layers, which can be physically bonded and separated. The etch barrier layer 104 protects the circuitry and copper pillars of the final laminated packaging substrate from damage caused by excessive etching. Typically, the etch barrier layer is made of nickel. Typically, the first metal seed layer 131 is made of copper with a thickness of 1-3 μm, serving as a conductive basis for subsequent electroplating.
[0039] Next, a first conductive post 120 is formed on the surface of the temporary support plate – step (b), as follows: Figure 5b As shown. Typically, this step may include the following sub-steps:
[0040] A photoresist material is applied to the surface of the first metal seed layer 131 of the temporary support plate. This photoresist material can typically be applied by lamination or coating.
[0041] The photoresist material is processed to fabricate the first conductive pillar 120 pattern, forming the first photoresist layer 191, as shown below. Figure 5c As shown. The first conductive pillar window 1911 is usually formed by exposure and development, thus creating the first conductive pillar pattern.
[0042] A first conductive post 120 is formed within the first conductive post window 1911. The first conductive post 120 is typically formed by electroplating. The material of the first conductive post 120 can be copper, i.e., a first conductive copper post. The thickness of the first conductive copper post can be defined according to actual needs, and is usually less than the thickness of the first photoresist layer 191 to facilitate the fabrication of the first conductive post 120. One or more first conductive posts 120 can be used, and usually multiple posts are used.
[0043] After removing the first photoresist layer 191, we obtain Figure 5b The structure shown. The first photoresist layer 191 can usually be removed by peeling or etching.
[0044] Then, a first insulating layer 110 with a first opening 112 is formed, the first opening 112 corresponding to and adapted to the first conductive post 120 - step (c), as follows. Figure 5d As shown. Typically, the first insulating layer 110 has a reinforcing structure, such as fiberglass cloth 111, to ensure that the final laminated encapsulation substrate structure has sufficient support strength and to prevent cracking of the insulating layer after removal of the carrier plate during the laminated encapsulation substrate fabrication process. This step typically includes the following sub-steps:
[0045] Prepare the first dielectric layer 113 and the second dielectric layer 114, such as Figure 5e The first dielectric layer 113 can be made of PP prepreg, which includes fiberglass cloth 111. Typically, the fiberglass cloth can be located in the center of the prepreg to improve its strength. The second dielectric layer 114 can be made of pure resin, such as ABF film or RCF film. The upper and lower surfaces of the pure resin layer can each have a first release film 115 and a second release film 116.
[0046] Remove the second release film 116 from the side of the second dielectric layer 114 closest to the first dielectric layer 113, and apply a third release film 117 to the side of the first dielectric layer 113 furthest from the second dielectric layer 114. Pre-press the second dielectric layer 114 onto the surface of the first dielectric layer 113 so that the fiberglass cloth 111 is close to the lower surface of the first insulating layer 110. Figure 5fPre-compression can be completed on traditional presses, vacuum laminators, or high-speed presses. After pre-compression, the fiberglass cloth 111 is positioned close to the lower surface of the first insulating layer 110. This avoids damage to the fiberglass cloth when the first insulating layer 110 is subsequently thinned.
[0047] A window is made at the position corresponding to the first conductive post 120 to form a first window 112, thereby obtaining the first insulating layer 110. Figure 5d As shown. Before opening the window, the first release film 115 and the third release film 117 can be removed. In this way, by pre-forming the first window 112 on the first insulating layer 110, it can be avoided that when the first insulating layer 110 is subsequently laminated directly onto the first conductive post 120, the first conductive post 120 directly impacts the first insulating layer 110, causing damage such as... Figure 2 The method shown above, by placing the fiberglass cloth on top of the insulating layer (e.g., the first insulating layer 110), avoids the performance degradation of the insulating layer (e.g., the first insulating layer 110) and can prevent the fiberglass cloth from breaking and being exposed during subsequent thinning processes, as well as avoid problems such as uneven thickness of the insulating layer (e.g., the first insulating layer 110). It also improves the support strength of the insulating layer (e.g., the first insulating layer 110), facilitates the subsequent fabrication of conductive pillars and circuit layers, improves the reliability of the substrate, and thus improves the overall yield of the press-fit packaging substrate structure.
[0048] In some embodiments, the height of the first insulating layer 110 is greater than the height of the first conductive post 120, which is beneficial for controlling the flushness between the upper surfaces of the first insulating layer 110 and the first conductive post 120. For example, it is convenient to make the upper surface of the first conductive post 120 flush with the upper surface of the first insulating layer 110 through subsequent thinning processes to expose the upper surface of the first conductive post 120.
[0049] Next, a first insulating layer 110 is laminated onto the first conductive post 120 – step (d), as follows: Figure 5g Typically, this step includes the following sub-steps:
[0050] A first insulating layer 110 is laminated onto the first conductive post 120 by pre-pressing a second dielectric layer 114 onto the surface of the first dielectric layer 113.
[0051] The first insulating layer 110 is thinned so that its upper surface is flush with the upper surface of the first conductive post 120, thus exposing the upper surface of the first conductive post 120. Since the first conductive post 120 passes through the first opening 112 in the first insulating layer 110, it will not push up the fiberglass cloth, thus preventing the fiberglass cloth from being exposed, and also preventing unevenness of the first insulating layer 110 and reduction of the surface roughness of the first insulating layer 110 after thinning. At the same time, it can avoid damage to the surface of the first conductive post 120 caused by thinning.
[0052] Then, a second conductive post 150 and a first circuit layer 140 are formed on the upper surface of the first insulating layer 110 – step (e), as follows. Figure 5h This step typically includes the following sub-steps:
[0053] A second metal seed layer 141 is formed on the surface of the first insulating layer 110. Typically, the second metal seed layer 141 can be a copper layer, which can be formed by copper melting or copper sputtering.
[0054] A second photoresist layer 192 is fabricated on the surface of the second metal seed layer 141. The photoresist material can be applied by lamination or coating; and the photoresist material is exposed and developed to fabricate a first circuit layer pattern 1921 and a second conduction post pattern 1922, thus forming the second photoresist layer 192. Figure 5i .
[0055] A second conductive post 150 and a first circuit layer 140 are formed within the second conductive post pattern 1922 and the first circuit layer pattern 1921, respectively, and the second photoresist layer 192 is removed, as shown. Figure 5i The first circuit layer 140 can be formed by electroplating, and its thickness can be defined according to actual needs, usually being less than the thickness of the second photoresist layer 192. The second photoresist layer 192 can typically be removed by a stripping process. The second conductive post 150 can be formed by a separate process involving exposure, development, electroplating, and stripping.
[0056] Next, a second insulating layer 160 is formed. The preparation method of the second insulating layer 160 can be the same as that of the first insulating layer 110. The second insulating layer 160 may have a second opening corresponding to the second conductive post 150 to further improve the overall performance of the lamination packaging substrate structure. It is understood that the preparation of the second insulating layer 160 may include the following sub-steps:
[0057] Prepare a third dielectric layer and a fourth dielectric layer. The third dielectric layer has a fiberglass cloth 161 in the middle. The materials of the third dielectric layer and the fourth dielectric layer can be the same as the materials of the first dielectric layer 113 and the second dielectric layer 114, which will not be described in detail here.
[0058] A fourth dielectric layer is pre-pressed onto the surface of the third dielectric layer so that the fiberglass cloth 161 is close to the lower surface of the second insulating layer 160.
[0059] A window is made at the position corresponding to the second conductive post 150 to form a second window.
[0060] Then, a second insulating layer 160 is laminated onto the upper surface of the first circuit layer 140 and the second conductive post 150 – step (f), as follows. Figure 5j .
[0061] The second insulating layer 160 is thinned so that its upper surface is flush with the upper surface of the second conductive post 150, thus exposing the upper surface of the second conductive post 150. Since the second conductive post 150 passes through the second opening in the second insulating layer 160, it does not push up the fiberglass cloth, thus preventing the fiberglass cloth from being exposed, avoiding unevenness in the second insulating layer 160 and reducing the surface roughness of the second insulating layer 160 after thinning, and simultaneously avoiding damage to the surface of the second conductive post 150 caused by thinning.
[0062] Next, a third photoresist layer 193 is applied to the upper surface of the second insulating layer 160, a second circuit layer pattern 1931 is formed in the third photoresist layer 193, a second circuit layer 170 is formed within the second circuit layer pattern 1931, and the third photoresist layer 193 is removed – step (g), as follows. Figure 5k As shown. The second circuit layer 170 is electrically connected to the first circuit layer 140 via a second conductive post 150; this step typically includes the following sub-steps:
[0063] A third metal seed layer 171 is formed on the surface of the second insulating layer 160. Typically, the third metal seed layer 171 can be a copper layer, which can be formed by copper melting or copper sputtering.
[0064] A third photoresist layer 193 is fabricated on the surface of the third metal seed layer 171. The photoresist material can be applied by lamination or coating; and the photoresist material is exposed and developed to create a second circuit layer pattern 1931, forming the third photoresist layer 193. Figure 5k .
[0065] A second circuit layer 170 is formed within the second circuit layer pattern 1931, and the third photoresist layer 193 is removed, as follows. Figure 5l The second circuit layer 170 can be formed by electroplating, and its thickness can be defined according to actual needs, typically being less than the thickness of the third photoresist layer 193. The third photoresist layer 193 can usually be removed using methods such as film stripping. Figure 5k .
[0066] Then, remove the temporary support plate, such as Figure 5m As shown. This step typically includes the following sub-steps:
[0067] The first and second metal layers are separated to separate the carrier plate from the substrate. This separation is typically achieved by tearing off the first and second metal layers.
[0068] The first metal layer on the lower surface of the carrier plate is usually removed by etching.
[0069] Removing the etch barrier layer typically involves etching with specific chemicals, such as nickel etching solution.
[0070] Next, a third wiring layer 130 is formed on the lower surface of the first insulating layer 110 – step (h). The third wiring layer 130 is electrically connected to the first wiring layer 140 via a first conductive post 120. Typically, this step may include the following sub-steps:
[0071] A fourth photoresist layer 194 is fabricated on the surface of the first metal seed layer 131. The photoresist material can be applied by lamination or coating; and the photoresist material is exposed and developed to create a third circuit layer pattern 1941, forming the fourth photoresist layer 194. Figure 5n .
[0072] A third circuit layer 130 is formed within the third circuit layer pattern 1941, and the fourth photoresist layer 194 is removed, as follows. Figure 3 The third circuit layer 130 can be formed by electroplating, and its thickness can be defined according to actual needs, usually being less than the thickness of the fourth photoresist layer 194. The fourth photoresist layer 194 can typically be removed using methods such as film stripping.
[0073] Then, a first solder mask layer 181 and a second solder mask layer 182 can be formed on the surfaces of the third circuit layer 130 and the second circuit layer 170, respectively, such as Figure 4 As shown. The first solder mask 181 and the second solder mask 182 can make the press-fit package substrate structure insulating. The first solder mask 181 can be provided with pads (not shown) at the position corresponding to the second circuit layer 170 for electrical connection or testing. The second solder mask 182 can be provided with pads (not shown) at the position corresponding to the third circuit layer 130 for electrical connection or testing.
[0074] Next, protective layers (not shown) can be formed on the surfaces of the first solder resist layer 181 and the second solder resist layer 182, respectively. Specifically, these layers can be disposed on the upper surface of the solder pads. By setting the protective layer, the solder pads can be prevented from oxidizing, thereby enhancing the reliability of the substrate. The protective layer materials include chemically stable metals such as nickel-palladium-gold, nickel-gold, tin, and silver, or mechanically protective solder films.
[0075] The lamination packaging substrate structure and its fabrication method provided in this application pre-press conventional PP prepreg and pure resin film (ABF or RCF) and then open windows at the corresponding copper pillar positions to laminate and fabricate the insulating layer. This can improve the thickness uniformity and filling capacity of the insulating layer, and make the surface roughness of the insulating layer smaller, which is conducive to the fabrication of fine lines. It can also prevent the fiberglass cloth from being exposed, and make the thickness control of the insulating layer after lamination better and the filling capacity of the insulating layer stronger.
[0076] Those skilled in the art should understand that the discussion of any of the above embodiments is merely exemplary and is not intended to imply that the scope of this application (including the claims) is limited to these examples; within the framework of this application, the technical features of the above embodiments or different embodiments can also be combined, the steps can be implemented in any order, and there are many other variations of different aspects of the embodiments of this application as described above, which are not provided in the details for the sake of brevity.
[0077] Additionally, to simplify the description and discussion, and to avoid obscuring the embodiments of this application, the well-known power / ground connections to integrated circuit (IC) chips and other components may or may not be shown in the provided drawings. Furthermore, the apparatus may be shown in block diagram form to avoid obscuring the embodiments of this application, and this also takes into account the fact that the details of the implementation of these block diagram apparatuses are highly dependent on the platform on which the embodiments of this application will be implemented (i.e., these details should be fully understood by those skilled in the art). While specific details (e.g., circuits) have been set forth to describe exemplary embodiments of this application, it will be apparent to those skilled in the art that the embodiments of this application can be implemented without these specific details or with variations thereof. Therefore, these descriptions should be considered illustrative rather than restrictive.
[0078] Although this application has been described in conjunction with specific embodiments thereof, many substitutions, modifications, and variations of these embodiments will be apparent to those skilled in the art from the foregoing description. For example, other memory architectures (e.g., dynamic RAM (DRAM)) may be used with the embodiments discussed.
[0079] The embodiments of this application are intended to cover all such substitutions, modifications, and variations that fall within the broad scope of the appended claims. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the embodiments of this application should be included within the protection scope of this application.
Claims
1. A method for fabricating a press-fit packaging substrate structure, characterized in that, Includes the following steps: (a) Prepare a temporary support plate; (b) A first conductive post is formed on the surface of the temporary support plate; (c) Forming a first insulating layer having a first opening, wherein the first insulating layer comprises fiberglass cloth; (d) A first insulating layer is laminated on the first conductive post, such that the first conductive post passes through the first window and is embedded in the first insulating layer; The height of the first insulating layer is greater than the height of the first conductive post; the first insulating layer is thinned to expose the first conductive post on the first insulating layer; (e) A second conductive post and a first circuit layer are formed on the upper surface of the first insulating layer, wherein the second conductive post is electrically connected to the first conductive post; (f) A second insulating layer having a second window is laminated on the first circuit layer and the second conductive post, such that the second conductive post is embedded in the second insulating layer through the second window, wherein the second insulating layer has fiberglass cloth. (g) A second circuit layer is formed on the upper surface of the second insulating layer, wherein the second circuit layer is electrically connected to the first circuit layer through the second conductive post; (h) Remove the temporary support plate and form a third circuit layer on the lower surface of the first insulating layer, wherein the third circuit layer is electrically connected to the first circuit layer through the first conductive post; step (c) further includes: The first insulating layer is formed by pre-pressing a second dielectric layer onto the surface of a first dielectric layer, wherein the fiberglass cloth is located in the middle of the first dielectric layer so that the fiberglass cloth is close to the lower surface of the first insulating layer; the first dielectric layer is a PP prepreg; the second dielectric layer is a pure resin layer without fiberglass cloth. A window is made in the first insulating layer at the position corresponding to the first conductive post to form the first window.
2. The manufacturing method according to claim 1, characterized in that, Step (f) also includes: The second insulating layer is formed by pre-pressing a fourth dielectric layer onto the surface of a third dielectric layer, wherein the fiberglass cloth is located in the middle of the third dielectric layer, so that the fiberglass cloth is close to the lower surface of the second insulating layer. A second window is formed by making a window at the position of the second insulating layer corresponding to the position of the second conductive post.
3. The manufacturing method according to claim 1, characterized in that, The height of the second insulating layer is greater than the height of the second conductive post.
4. The manufacturing method according to claim 3, characterized in that, Step (d) further includes thinning the second insulating layer to expose the upper surface of the second conductive post on the second insulating layer.
5. The manufacturing method according to claim 2, characterized in that, The fourth dielectric layer is a pure resin layer without fiberglass cloth.
6. The manufacturing method according to claim 1, characterized in that, A fiberglass cloth covering the first circuit layer with the second insulating layer.
7. The manufacturing method according to claim 1, characterized in that, It also includes forming a first solder resist layer and a second solder resist layer on the surfaces of the third circuit layer and the second circuit layer, respectively.
8. A press-fit packaging substrate structure, characterized in that, include: A first insulating layer having a first opening, a first conductive post embedded in the first opening, a second insulating layer having a second opening on the first insulating layer, a first circuit layer embedded in the second insulating layer and a second conductive post embedded in the second opening, a second circuit layer on the second insulating layer, and a third circuit layer below the first insulating layer. The first and second insulating layers are made of fiberglass cloth. The first circuit layer and the third circuit layer are electrically connected through a first conductive post, and the first circuit layer and the second circuit layer are electrically connected through a second conductive post. The first insulating layer is formed by pressing a first dielectric layer and a second dielectric layer together. The fiberglass cloth is located in the middle of the first dielectric layer and is close to the lower surface of the first insulating layer. The second dielectric layer is close to the first circuit layer, and the first dielectric layer is close to the third circuit layer. The first dielectric layer is a PP semi-cured sheet. The second dielectric layer is a pure resin layer without fiberglass cloth.
9. The press-fit packaging substrate structure according to claim 8, characterized in that, The second insulating layer is formed by laminating a third dielectric layer and a fourth dielectric layer. The third dielectric layer has a fiberglass cloth in the middle, which is close to the lower surface of the second insulating layer. The fourth dielectric layer is close to the second circuit layer, and the third dielectric layer is close to the first circuit layer.
10. The press-fit packaging substrate structure according to claim 9, characterized in that, The fourth dielectric layer is a pure resin layer without fiberglass cloth.
11. The press-fit packaging substrate structure according to claim 8, characterized in that, A fiberglass cloth covering the first circuit layer with the second insulating layer.
12. The press-fit packaging substrate structure according to claim 8, characterized in that, It also includes a first solder mask layer on the upper surface of the second circuit layer and a second solder mask layer on the lower surface of the third circuit layer.
Citation Information
Patent Citations
Electric packaging part and manufacture method thereof
CN106158808A
Circuit board and manufacturing method thereof
CN112201652A