A method for preparing front and back glass glaze of film forming substrate

By employing stepwise sintering of glass enamel layers at different sintering temperatures, the problems of glass enamel layer adhesion damage and low processing efficiency on the front and back sides of the film-forming substrate are solved, achieving efficient and high-quality glass enamel layer preparation suitable for LTCC substrates.

CN115527865BActive Publication Date: 2026-11-24EAST CHINA INST OF OPTOELECTRONICS INTEGRATEDDEVICE
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202211188583.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-28
Publication Date
2026-11-24
Estimated Expiration
2042-09-28

AI Technical Summary

Technical Problem

Existing technologies suffer from problems such as glass glaze layer adhesion loss, low processing efficiency, difficulty in controlling sintering quality, and unsuitability for LTCC substrates during the preparation of glass glaze on the front and back sides of the film-forming substrate.

Method used

First and second glass enamel layers with different sintering temperatures are used. The sintering temperature of the first glass enamel layer is higher than that of the second glass enamel layer. By screen printing and step-by-step sintering, adhesion between glass enamel layers and substrate deformation are avoided.

Benefits of technology

It improves processing efficiency, ensures sintering quality, and is suitable for LTCC substrates, avoiding glass enamel layer adhesion damage and substrate bending deformation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115527865B_ABST
    Figure CN115527865B_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing anti-adhesion glass enamel on the front and back sides of a film-forming substrate, comprising the following steps: printing a first glass enamel layer on one side of the film-forming substrate, and placing the film-forming substrate with the printed first glass enamel layer facing upwards on a placement device; transferring the film-forming substrate to a drying oven for drying, and then transferring it to a sintering furnace for sintering; removing the sintered film-forming substrate, printing a second glass enamel layer on the other side of the film-forming substrate, and placing the film-forming substrate with the printed second glass enamel layer facing upwards on a placement device; transferring the film-forming substrate to a drying oven for drying, and then transferring it to a sintering furnace for sintering. The sintering temperature of the first glass enamel layer is higher than that of the second glass enamel layer, preventing defects in the first glass enamel layer due to molten contact and adhesion, and eliminating the need to use hard objects to support the substrate to prevent substrate bending and deformation. This invention significantly improves the sintering efficiency and quality of the glass enamel on the front and back sides of the film-forming substrate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of hybrid integrated circuit manufacturing technology, and specifically to a method for preparing anti-adhesion glass glaze on the front and back sides of a film-forming substrate. Background Technology

[0002] To meet the miniaturization requirements of hybrid integrated circuits, wiring needs to be applied to both sides of the film-forming substrate during layout design to improve integration density. Simultaneously, glass enamel encapsulation is required for the wiring on both sides of the film-forming substrate. Existing fabrication methods use the same type of glass enamel for printing and sintering the glass enamel on both sides of the film-forming substrate, as follows: 1) Preparation of the first glass glaze layer: The first glass glaze layer is printed on the front (or back) of the film-forming substrate using conventional screen printing technology. The substrate with the printed glass glaze side facing up is then neatly placed on a placement device, transferred to a drying oven for drying, and then transferred to a sintering furnace for sintering. The drying and sintering temperatures are determined according to the actual technical requirements of the glass glaze slurry.

[0003] 2) Preparation of the second glass enamel layer: After completing the preparation of the first glass enamel layer, the other side of the film-forming substrate is printed with a second glass enamel layer using conventional screen printing technology. The substrate is then neatly placed on a placement device with the enamel-printed side facing upwards, at which point the prepared first glass enamel layer is in contact with the placement device. It is then transferred to a drying oven for drying, and then to a sintering furnace for sintering. The drying and sintering temperatures are determined according to the actual technical requirements of the glass enamel slurry.

[0004] The problem with this method is that when the film-forming substrate is visually inspected, it is found that the first glass glaze pattern in contact with the placement device is damaged. The reason is that the first glass glaze layer and the second glass glaze layer are made of the same material. Therefore, when the second glass glaze layer is sintered and melted, the first glass glaze layer also melts. At this time, the first glass glaze layer is in contact with the placement device, which causes the glass glaze at the contact point to be stuck off by the placement device.

[0005] 2. An improvement is made to the existing method described above, which is as follows: 1) Preparation of the first glass glaze layer: Same as the above-mentioned original technology! 2) Preparation of the second glass glaze layer: The printing and drying process is the same as the original technology! However, an improvement is taken before sintering. At this time, the corner of one side of the substrate with the first glass glaze layer that has been sintered is padded with a ceramic substrate (or other high-temperature resistant material). In this way, only one side of the substrate is in contact with the padding material and the other side edge of the substrate is in contact with the placement device, while the pattern of the first glass glaze layer is not in contact with the placement device, thereby preventing the first glass glaze layer from being smeared or damaged by the placement device.

[0006] However, this method still has problems: ①Low processing efficiency: When the second layer of glass glaze is sintered, the corners of the substrate with the first layer of glass glaze already sintered need to be padded with hard objects, which takes a lot of time to arrange. ② The sintering quality is difficult to control: First, the padding material is placed manually, which cannot guarantee that the padding material will not come into contact with the pattern of the first glass enamel layer; second, during the rotation process, it is impossible to guarantee that there will be no shaking, and the film-forming substrate and the padding material will be displaced; third, during the sintering process, the vibration of the conveyor belt rotation will also cause the substrate and the hard object to be displaced from each other, which will easily lead to contact with the surface of the substrate with the first glass enamel layer that has been sintered, causing the first glass enamel layer to be stuck off when the second glass enamel layer is sintered. ③LTCC (Low Temperature Co-fired Ceramic) substrates are not applicable: When the substrate material is LTCC or similar, it is not possible to use a hard object to support the substrate, because the sintering temperature of the glass glaze will cause the substrate to soften. If this method is used, the substrate will bend and deform after the glass glaze is sintered. Summary of the Invention

[0007] To address the aforementioned technical problems, this invention provides a method for preparing anti-adhesion glass glaze on the front and back sides of a film-forming substrate.

[0008] The present invention adopts the following technical solution: A method for preparing anti-sticking glass glaze on the front and back sides of a film-forming substrate, characterized by comprising the following steps: S1. Print a first glass glaze layer on one side of the film-forming substrate using a first glass glaze, and place the film-forming substrate with the side printed with the first glass glaze layer facing upwards on the placement device; S2. The film-forming substrate is transferred to a drying oven for drying, and then transferred to a sintering oven for sintering at the sintering temperature corresponding to the first glass glaze. S3. Take out the sintered film-forming substrate, print the second glass glaze layer on the other side of the film-forming substrate using the second glass glaze, and place the side of the film-forming substrate with the printed second glass glaze layer facing up on the placement device. S4. The film-forming substrate is transferred to a drying oven for drying, and then transferred to a sintering oven for sintering at the sintering temperature corresponding to the second glass glaze. The sintering temperature of the first glass glaze layer is higher than that of the second glass glaze layer.

[0009] Furthermore, the film-forming substrate is fabricated by screen printing first and second glass enamel layers.

[0010] Furthermore, the difference between the sintering temperature of the first glass glaze layer and the sintering temperature of the second glass glaze layer is 50℃±10℃.

[0011] Compared with existing technologies, the present invention has the following advantages: 1. High processing efficiency: The first glass glaze layer is printed and sintered using a material with a higher sintering temperature, while the second glass glaze layer is printed and sintered using a material with a lower sintering temperature. This way, when the second glass glaze layer is sintered, the substrate with the first glass glaze layer already sintered can be placed directly on the placement device. Because the sintering temperature of the second glass glaze layer will not cause the first glass glaze layer to melt and become stuck or damaged, a lot of substrate placement time is saved. 2. Good sintering quality: When sintering the second glass glaze layer, the sintering temperature is insufficient to melt the first glass glaze layer, so the sintering quality of the first glass glaze layer will not be affected. At the same time, the second glass glaze layer is sintered according to its sintering temperature, and its quality is also guaranteed. 3. Applicable to LTCC substrates: By adopting the technical solution of this invention, such flexible substrates can be directly placed on the placement device. The surface of the placement device is horizontal, and there is no need to set up additional support points between the upper and lower substrates, so that the substrates will not bend. This ensures both the sintering quality of the glass glaze and the shape quality of the flexible substrate.

[0012] This solution significantly improves the sintering efficiency and quality of glass glaze on both the front and back sides of the film-forming substrate. Attached Figure Description

[0013] Figure 1 This is a schematic diagram of the film-forming substrate structure prepared using the present invention. Detailed Implementation

[0014] To make the present invention clearer, the following description, in conjunction with the accompanying drawings, further illustrates a method for preparing anti-adhesion glass glaze on the front and back sides of a film-forming substrate. The specific embodiments described herein are for illustrative purposes only and are not intended to limit the scope of the invention.

[0015] like Figure 1 As shown, a method for preparing anti-adhesion coatings for glass glazes on both sides of a film-forming substrate is applied to a film-forming substrate with double-sided glass glaze. It includes the following steps: S1. The front side of the film-forming substrate 1 is printed with conventional screen printing technology using the first glass enamel to form the first glass enamel layer 2, and the surface of the first glass enamel layer 2 printed on the film-forming substrate 1 is placed flat on the placement device with the surface facing up. The placement device is existing technology. S2. The film-forming substrate 1 is transferred to a drying oven for drying, and then transferred to a sintering oven for sintering at the sintering temperature corresponding to the first glass glaze. S3. Take out the sintered film-forming substrate 1, and use conventional screen printing technology to print the second glass glaze layer 3 on the reverse side of the film-forming substrate using the second glass glaze. Place the film-forming substrate 1 with the surface of the printed second glass glaze layer 3 facing up on the placement device. S4. The film-forming substrate 1 is transferred to a drying oven for drying, and then transferred to a sintering oven for sintering at the sintering temperature corresponding to the second glass glaze. The glass enamel materials and their usage parameters for the first and second glass enamel layers are all existing technologies, and the sintering temperature of the first glass enamel layer is higher than that of the second glass enamel layer. The glass enamel material for the first glass enamel layer is the I4337 type glass enamel material from Xi'an Hongxing Company, with a sintering temperature of 550℃; the glass enamel material for the second glass enamel layer is the 7137 type glass enamel material from DuPont Company, with a sintering temperature of 500℃. The difference between the sintering temperatures of the first and second glass enamel layers is 50℃±10℃, which sets a certain temperature difference margin to prevent the first glass enamel layer from melting due to furnace temperature fluctuations.

[0016] Microscopic visual inspection of the glass enamel layer of the film-forming substrate prepared by the present method and the original method revealed that the glass enamel surface of the front and back of the film-forming substrate prepared by the present method was bright and dense, without surface contamination or defects, while the glass enamel layer of the film-forming substrate prepared by the original method showed surface contamination and defects.

[0017] The above embodiments of the present invention are merely examples for clearly illustrating the present invention and are not intended to limit the implementation of the present invention. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively describe all embodiments here. However, obvious variations or modifications derived from the essential spirit of the present invention still fall within the protection scope of the present invention.

Claims

1. A method for preparing a glass glaze anti-adhesion coating on the front and back sides of a film-forming substrate, wherein the film-forming substrate is used for hybrid integrated circuits, and wiring and glass glaze encapsulation are performed on the front and back sides of the film-forming substrate, characterized in that... Includes the following steps: S1. Print a first glass glaze layer on one side of the film-forming substrate using a first glass glaze, and place the film-forming substrate with the side printed with the first glass glaze layer facing upwards on the placement device; S2. The film-forming substrate is transferred to a drying oven for drying, and then transferred to a sintering oven for sintering at the sintering temperature corresponding to the first glass glaze. S3. Take out the sintered film-forming substrate, print the second glass glaze layer on the other side of the film-forming substrate using the second glass glaze, and place the side of the film-forming substrate with the printed second glass glaze layer facing up on the placement device. S4. The film-forming substrate is transferred to a drying oven for drying, and then transferred to a sintering oven for sintering at the sintering temperature corresponding to the second glass glaze. The sintering temperature of the first glass glaze layer is higher than that of the second glass glaze layer, and the difference between the sintering temperatures of the first and second glass glaze layers is 50℃ ± 10℃.

2. The method for preparing anti-adhesion glass glaze on the front and back sides of a film-forming substrate according to claim 1, characterized in that: The film-forming substrate is formed by screen printing the first and second glass enamel layers.

Citation Information

Patent Citations

  • Double-sided decorative ceramic plate and preparation method thereof

    CN111152334A