Preparation method and application of sodium vanadium fluorophosphate composite positive electrode material
By using a hydrothermal and medium-high temperature calcination method to carbon-coat Na₃V₂O₂(PO₄)₂F, spherical sodium vanadium fluorophosphate composite cathode materials were prepared, which solved the problems of low specific capacity and poor electrochemical performance of sodium fluorophosphate batteries and improved the conductivity and rate performance of the material.
Patent Information
- Application Number
- CN202211253461.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-13
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2042-10-13
AI Technical Summary
Existing sodium fluorophosphate cathode materials have low specific capacity and poor electrochemical performance, especially prone to polarization at high rates.
Carbon coating of Na₃V₂O₂(PO₄)₂F was carried out using a hydrothermal + medium-high temperature calcination method. The carbon source Ketjen black and the surfactant polyethylene glycol were ultrasonically pretreated, mixed and reacted in a hydrothermal reactor, and then calcined to prepare spherical sodium vanadium fluoride phosphate composite cathode material.
It significantly improves the conductivity and rate performance of the cathode material, reduces the material particle size and increases the specific surface area, thereby enhancing the electrochemical performance of sodium-ion batteries, especially significantly improving cycle performance at high rates.
Smart Images

Figure CN115583644B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of battery cathode materials, and particularly relates to a method for preparing and applying a sodium vanadium fluoride phosphate composite cathode material. Background Technology
[0002] In recent years, sodium-ion batteries have attracted widespread attention due to their significant advantages in cost and resources. Sodium and lithium belong to the same group and share many similar properties. Furthermore, sodium is widely distributed in nature, with abundant untapped resources in the Earth's crust and seawater, making sodium-ion batteries more advantageous than lithium in terms of both resource reserves and price.
[0003] However, sodium-ion batteries have lower energy density and cycle stability than lithium-ion batteries. In the selection of cathode materials for sodium-ion batteries, like lithium-ion batteries, reversible charging and discharging of batteries are achieved through the insertion and extraction of ions. This requires the cathode material to have a stable ionic framework and structural stability so that ions can be quickly inserted and extracted.
[0004] Current research on cathode materials for sodium-ion batteries mainly falls into four categories: layered metal oxides, tunnel-structured oxides, Prussian blue materials, and polyanionic materials. Currently, research on polyanionic cathode materials primarily includes Na3V2(PO4)3, fluorophosphates (Na3V2O2x(PO4)2F3-2x, Na2MPO4F), etc. Due to their large polyanionic groups, these materials exhibit low electronic conductivity and are prone to polarization at high rates, resulting in low specific capacity and poor electrochemical performance. However, carbon coating, metal ion doping, and the creation of porous structures can improve the conductivity of these materials, thereby significantly enhancing their electrochemical performance.
[0005] There has been considerable research on coating methods for cathode materials of fluorophosphate batteries. Commonly studied electrochemical performance characteristics include: first discharge specific capacity and discharge specific capacity at different rates. However, the cathode performance of fluorophosphate batteries still needs continuous improvement. Summary of the Invention
[0006] To address the problems of low specific capacity and poor electrochemical performance in existing fluorophosphate batteries, this invention provides a method for preparing a spherical sodium vanadium fluorophosphate composite cathode material.
[0007] The technical solution of the present invention is as follows: A method for preparing a sodium vanadium fluorophosphate composite cathode material, comprising the following steps:
[0008] S1. According to the theoretical yield of Na3V2O2(PO4)2F, weigh the carbon source and mix it with the surfactant. Sonic pretreatment is performed to make the carbon source evenly dispersed in the surfactant.
[0009] S2. Dissolve the vanadium source, fluorine source, sodium source, phosphate, and reducing agent in an appropriate amount of ultrapure water solvent in proportion, pretreat under water bath heating conditions, and continue stirring until a clear blue solution is obtained.
[0010] S3. After mixing the carbon source and surfactant mixture from step S1 with the blue clear solution from step S2, transfer the mixture to a hydrothermal reactor for hydrothermal reaction.
[0011] After the reactants in step S4 and S3 are naturally cooled to room temperature, the resulting reactor liquid is centrifuged, washed with water and alcohol, and then dried to obtain a precursor. Then, it is calcined under inert gas protection to obtain solid particles of composite cathode material.
[0012] The surfactant is polyethylene glycol, the carbon source is Ketjen black, the vanadium source is ammonium metavanadate, the fluorine source and sodium source are both sodium fluoride, the phosphate is ammonium dihydrogen phosphate, and the reducing agent is oxalic acid.
[0013] Furthermore, in step S3, the temperature in the hydrothermal reactor is 160–200°C, and the reaction time is 6–10 h; in step S4, the calcination temperature is 300–500°C, and the calcination time is 2–6 h.
[0014] Furthermore, in step S1, the mass ratio of Ketjen black to Na3V2O2(PO4)2F is 3wt% to 10wt%, the ultrasonic power is 500W to 1000W, and the ultrasonic treatment time is 2 to 6 hours.
[0015] Furthermore, in step S2, the ratio of ammonium metavanadate, sodium fluoride, ammonium dihydrogen phosphate, and oxalic acid is 2:3:2:3, and the water bath temperature is 75℃~90℃.
[0016] Furthermore, in step S3, the device is cleaned 2-5 times with deionized water and ethanol respectively, and the inert gas atmosphere is argon or nitrogen.
[0017] Preferably, in step S1, the mass ratio of Ketjen black to Na3V2O2(PO4)2F is 3wt%, and the mixture is pretreated under 800W ultrasound for 3 hours; in step S2, the mixture is heated in an 80°C water bath and stirred until a clear blue solution is obtained; in step S3, the hydrothermal reaction temperature is 180°C and the reaction is carried out for 4 hours; in step S4, the mixture is calcined at 400°C for 4 hours under an argon atmosphere.
[0018] Preferably, in step S1, the mass ratio of Ketjen black to Na3V2O2(PO4)2F is 6wt%, and the mixture is pretreated under ultrasonic treatment at 800W for 3 hours; in step S2, the mixture is heated in a water bath at 80°C and stirred until a clear blue solution is obtained; in step S3, the hydrothermal reaction temperature is 180°C and the reaction is carried out for 4 hours; in step S4, the mixture is calcined at 400°C for 4 hours under an argon atmosphere.
[0019] Preferably, in step S1, the mass ratio of Ketjen black to Na3V2O2(PO4)2F is 9wt%, and the mixture is pretreated under 800W ultrasound for 3 hours; in step S2, the mixture is heated in an 80°C water bath and stirred until a clear blue solution is obtained; in step S3, the hydrothermal reaction temperature is 180°C and the reaction is carried out for 4 hours; in step S4, the mixture is calcined at 400°C for 4 hours under an argon atmosphere.
[0020] The present invention also provides a sodium vanadium fluoride phosphate composite cathode material, which is prepared by the above method.
[0021] The aforementioned sodium vanadium fluoride phosphate composite cathode material can be used in sodium-ion batteries.
[0022] The advantages of this invention are as follows: The carbon source Ketjenblack and the surfactant are first pretreated with polyethylene glycol via ultrasonic treatment. The remaining vanadium source, fluorine source, sodium source, phosphate, and reducing agent are preheated. The two pretreated components are then mixed and subjected to hydrothermal and medium-high temperature calcination to obtain a sodium-ion cathode material with increased specific surface area and reduced particle size. This results in a composite cathode material with more Ketjenblack doping, significantly improving the conductivity and rate performance of the cathode material. Furthermore, the preparation method is simple and minimizes material waste. In particular, the 6% Ketjenblack-doped sodium-ion cathode material shows a significant improvement in rate and cycle performance. Attached Figure Description
[0023] Figure 1 A flowchart for the preparation and synthesis of Na3V2O2(PO4)2F / C composite materials;
[0024] Figure 2 The first charge-discharge diagrams are shown for NVOPF and KB carbon-coated NVOPF with different percentage contents at different rates of 0.1C, 0.5C, 1C, 2C, and 5C.
[0025] Figure 3 The graph shows the cycle performance test results of coin cells with composite electrodes corresponding to NVOPF composite materials with different KB contents. Detailed Implementation
[0026] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0027] This invention mainly employs a hydrothermal + medium-high temperature calcination method to carbon-coat Na3V2O2(PO4)2F. The specific preparation process is as follows:
[0028] S1. According to the theoretical yield of Na3V2O2(PO4)2F, weigh the carbon source and mix it with the surfactant, and use ultrasound to make the carbon source evenly dispersed in the surfactant.
[0029] S2. Dissolve the vanadium source, fluorine source, sodium source, phosphate, and reducing agent in an appropriate amount of ultrapure water solvent in sequence according to the proportion, and stir continuously under water bath heating until a clear blue solution is obtained.
[0030] S3. The mixture of carbon source and surfactant from step S1 is mixed with the blue clear solution from step S2 and then transferred to a hydrothermal reactor for hydrothermal reaction.
[0031] After the reactants in steps S4 and S3 are naturally cooled to room temperature, the resulting reactor liquid is centrifuged, washed with water and alcohol, and then dried to obtain a precursor. The precursor is then calcined under inert gas protection to obtain solid particles of the composite cathode material.
[0032] The surfactant mentioned in step S1 is polyethylene glycol (PEG), the carbon source is Ketjen black (KB), the mass ratio of KB to Na3V2O2(PO4)2F is 3wt% to 10wt%, the ultrasonic power is 500W to 1000W, and the ultrasonic treatment time is 2 to 6 hours.
[0033] In step S2, the vanadium source is ammonium metavanadate (NH4VO3), the fluorine source and sodium source are both sodium fluoride (NaF), the phosphate is ammonium dihydrogen phosphate (NH4H2PO4), and the reducing agent is oxalic acid. The ratio of NH4VO3, NaF, NH4H2PO4 and oxalic acid is 2:3:2:3, and the water bath temperature is 75℃~90℃.
[0034] In step S3, the temperature in the hydrothermal reactor is 160–200°C, and the reaction time is 6–10 h.
[0035] In step S4, the sample is cleaned 2-5 times with deionized water and ethanol respectively; the inert gas atmosphere is argon or nitrogen, the calcination temperature is 300-500℃, and the calcination time is 2-6h.
[0036] In the preparation method of the present invention, materials other than carbon source KB are preheated at 80°C to reduce the generation of side reactions, prevent excessive temperature difference, improve material utilization, and reduce costs.
[0037] KB is first ultrasonically dispersed in PEG solvent because PEG, as a nonionic surfactant, has excellent water solubility and stability and is not easily affected by acids and alkalis. The large number of oxygen atoms in the PEG molecule can combine with the free hydroxyl groups of other material surface particles through hydrogen bonds, coating the particle surface and preventing particle aggregation. After subsequent calcination, PEG is slowly removed, leaving fine pores, which can increase the specific surface area of the synthesized material and reduce the particle size, allowing the final synthesized material to be doped with more KB, thereby improving the conductivity of the material and improving the rate performance. Ultrasonication is used to better mix and disperse PEG and KB and enhance their emulsification effect.
[0038] The preparation process of the present invention is illustrated below through several specific examples.
[0039] Example 1
[0040] Taking the preparation of 0.01 mol of Na3V2O2(PO4)2F carbon-coated composite cathode material (hereinafter referred to as NVOPF / C) as an example, the preparation method is as follows:
[0041] S1. Weigh 0.2259g of KB into an appropriate amount of PEG at a mass ratio of 3% of KB, and sonicate at 800W for 3 hours.
[0042] S2. Weigh 2.3396g of ammonium metavanadate, 1.2597g of sodium fluoride, 2.3006g of ammonium dihydrogen phosphate, and 2.7009g of oxalic acid into an appropriate amount of ultrapure water solvent according to the ratio of n(ammonium metavanadate):n(sodium fluoride):n(ammonium dihydrogen phosphate):n(oxalic acid) = 2:3:2:3. Heat the mixture in an 80°C water bath and stir until a clear blue solution is obtained.
[0043] S3. Mix the KB solution from step S1 with the clear blue solution from step S2 and transfer it to a polytetrafluoroethylene-lined reactor. Set the hydrothermal reaction temperature to 180°C and react for 4 hours.
[0044] After the reactants in step S4 and S3 are naturally cooled to room temperature, the resulting liquid is centrifuged, washed with water and ethanol three times each, and then dried to obtain the precursor. The precursor is then calcined in a tube furnace with argon gas at 400°C for 4 hours to obtain solid particles of NVOPF / C material.
[0045] S5. Using the above-mentioned NVOPF / C solid particles as the positive electrode active material, add a slurry (PVDF dissolved in NMP to prepare a slurry), conductive agent, binder and other substances, use aluminum foil as the current collector to make a positive electrode sheet; and combine it with sodium sheet to form a 2032 type coin cell and conduct performance tests.
[0046] Example 2
[0047] The preparation method of NVOPF / C composite cathode material is as follows:
[0048] S1. Weigh 0.4518g of KB into an appropriate amount of PEG at a mass ratio of 6% of KB, and sonicate at 800W for 3 hours.
[0049] S2. Weigh 2.3396g of ammonium metavanadate, 1.2597g of sodium fluoride, 2.3006g of ammonium dihydrogen phosphate, and 2.7009g of oxalic acid into an appropriate amount of ultrapure water solvent according to the ratio of n(ammonium metavanadate):n(sodium fluoride):n(ammonium dihydrogen phosphate):n(oxalic acid) = 2:3:2:3. Heat the mixture in an 80°C water bath and stir until a clear blue solution is obtained.
[0050] S3. Mix the KB solution from step S1 with the clear blue solution from step S2 and transfer the mixture to a reaction vessel. Set the hydrothermal reaction temperature to 180°C and react for 4 hours.
[0051] After the reactants in step S4 and S3 are naturally cooled to room temperature, the resulting liquid is centrifuged, washed with water and ethanol three times each, and then dried to obtain the precursor. The precursor is then calcined in a tube furnace with argon gas at 400°C for 4 hours to obtain solid particles of NVOPF / C material.
[0052] S5. Using the above-mentioned NVOPF / C solid particles as the positive electrode active material, add a slurry (PVDF dissolved in NMP to prepare a slurry), conductive agent, binder and other substances, use aluminum foil as the current collector to make a positive electrode sheet; and combine it with sodium sheet to form a 2032 type coin cell and conduct performance tests.
[0053] Example 3
[0054] The preparation method of NVOPF / C composite cathode material is as follows:
[0055] S1. Weigh 0.4518g of KB into an appropriate amount of PEG at a mass ratio of 6% of KB, and sonicate at 800W for 3 hours.
[0056] S2. Weigh 2.3396g of ammonium metavanadate, 1.2597g of sodium fluoride, 2.3006g of ammonium dihydrogen phosphate, and 2.7009g of oxalic acid into an appropriate amount of ultrapure water solvent according to the ratio of n(ammonium metavanadate):n(sodium fluoride):n(ammonium dihydrogen phosphate):n(oxalic acid) = 2:3:2:3. Heat the mixture in an 80°C water bath and stir until a clear blue solution is obtained.
[0057] S3. Mix the KB solution from step S1 with the clear blue solution from step S2 and transfer the mixture to a reaction vessel. Set the hydrothermal reaction temperature to 180°C and react for 4 hours.
[0058] After the reactants in step S4 and S3 are naturally cooled to room temperature, the resulting liquid is centrifuged, washed with water and ethanol three times each, and then dried to obtain the precursor. The precursor is then calcined in a tube furnace with argon gas at 400°C for 4 hours to obtain solid particles of NVOPF / C material.
[0059] S5. Using the above-mentioned NVOPF / C solid particles as the positive electrode active material, add a slurry (PVDF dissolved in NMP to prepare a slurry), conductive agent, binder and other substances, use aluminum foil as the current collector to make a positive electrode sheet; and combine it with sodium sheet to form a 2032 type coin cell and conduct performance tests.
[0060] Comparative Example 1
[0061] The preparation method of NVOPF / C cathode material is as follows:
[0062] S1. Weigh 2.3396g of ammonium metavanadate, 1.2597g of sodium fluoride, 2.3006g of ammonium dihydrogen phosphate, and 2.7009g of oxalic acid into an appropriate amount of ultrapure water solvent according to the ratio of n(ammonium metavanadate):n(sodium fluoride):n(ammonium dihydrogen phosphate):n(oxalic acid) = 2:3:2:3. Heat the mixture in an 80°C water bath and stir until a clear blue solution is obtained.
[0063] S2. Transfer the clear blue solution from step S1 to the reaction vessel, set the hydrothermal reaction temperature to 180℃, and react for 4 hours.
[0064] After the reactants in step S3 and S2 are naturally cooled to room temperature, the resulting liquid is centrifuged, washed with water and ethanol three times each, and then dried to obtain the precursor. The precursor is then calcined in a tube furnace with argon gas at 400°C for 4 hours to obtain solid particles of NVOPF / C material.
[0065] S4. Using the above-mentioned NVOPF / C solid particles as the positive electrode active material, add a slurry (PVDF dissolved in NMP to prepare a slurry), conductive agent, binder and other substances, use aluminum foil as the current collector to make a positive electrode sheet; and combine it with sodium sheet to form a 2032 type coin cell and conduct performance tests.
[0066] Figure 2 The first charge-discharge diagrams are shown for NVOPF and KB carbon-coated NVOPF with different percentage contents at different rates of 0.1C, 0.5C, 1C, 2C, and 5C. Figure 3 The graph shows the cycle performance test results of coin cells with composite electrodes corresponding to NVOPF composite materials with different KB contents.
[0067] The theoretical specific capacity of Na3V2O2(PO4)2F polyanion is 130 mA·h / g. Analysis of the above test results shows that, compared to the NVOPF cathode material without KB carbon coating in Comparative Example 1, the NVOPF / C with KB carbon coating exhibits improved conductivity and thus a higher initial charge / discharge rate. Figure 2 The NVOPF / C material in Example 1 (KB content 3%) achieved a first discharge specific capacity of 120 mAh·g at 0.1C. -1 Around 118 mAh / g, the initial discharge specific capacity decreased with increasing KB content. For 6% and 9% NVOPF / C materials, the initial discharge specific capacity was [not specified]. -1 This is related to the decrease in the proportion of the active material NVOPF. However, with the increase in carbon content, the conductivity of the material is also significantly improved, and the rate performance of the material under high current is significantly enhanced.
[0068] Figure 3 Among them, Example 2 (KB content of 6%) showed the best cycling performance and the most significant improvement in rate performance, with a specific discharge capacity of up to 154 mAh·g at 0.1C after 10 cycles. -1 The specific discharge capacity after 10 cycles at 0.2C, 0.5C, and 1C reached 140 mAh·g, respectively. -1 133mAh·g -1 115mAh·g -1 When the discharge rate returns from 1C to 0.1C, the discharge specific capacity also recovers to 154 mAh·g. -1 Its rate performance is excellent, but when the KB content exceeds 6%, the rate performance decreases significantly.
[0069] The rate cycling performance of Examples 1 (3% KB carbon coating) and 3 (9% KB carbon coating) was slightly less than 6%, but still close to 140 mAh·g at 0.1C. -1 It is around 108 mAh / g, which is better than most sodium-ion batteries and far exceeds the 108 mAh / g of Comparative Example 1. -1 This demonstrates that the NVOPF / C preparation method of the present invention can significantly improve the electrical conductivity of NVOPF materials.
[0070] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-described technical content to create equivalent embodiments without departing from the scope of the present invention. Any simple modifications, equivalent changes, and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.
Claims
1. A method for preparing a sodium vanadium fluoride phosphate composite cathode material, characterized in that, Includes the following steps: S1. According to the theoretical yield of Na3V2O2(PO4)2F, weigh the carbon source and mix it with the surfactant. Sonic pretreatment is performed to make the carbon source evenly dispersed in the surfactant. S2. Dissolve the vanadium source, fluorine source, sodium source, phosphate, and reducing agent in an appropriate amount of ultrapure water solvent in proportion, pretreat under water bath heating conditions, and continue stirring until a clear blue solution is obtained. S3. The mixture of carbon source and surfactant from step S1 is mixed with the blue clear solution from step S2 and then transferred to a hydrothermal reactor for hydrothermal reaction. After the reactants in step S4 and S3 are naturally cooled to room temperature, the resulting reactor liquid is centrifuged, washed with water and alcohol, and then dried to obtain a precursor. Then, it is calcined under inert gas protection to obtain solid particles of composite cathode material. The surfactant is polyethylene glycol, the carbon source is Ketjen black, the vanadium source is ammonium metavanadate, the fluorine source and sodium source are both sodium fluoride, the phosphate is ammonium dihydrogen phosphate, and the reducing agent is oxalic acid.
2. The preparation method of the sodium vanadium fluorophosphate composite cathode material according to claim 1, characterized in that, In step S3, the temperature in the hydrothermal reactor is 160–200℃, and the reaction time is 6–10 h; in step S4, the calcination temperature is 300–500℃, and the calcination time is 2–6 h.
3. The method for preparing the sodium vanadium fluorophosphate composite cathode material according to claim 2, characterized in that: In step S1, the mass ratio of Ketjen black to Na3V2O2(PO4)2F is 3wt% to 10wt%, the ultrasonic power is 500W to 1000W, and the ultrasonic treatment time is 2 to 6 hours.
4. The preparation method of the sodium vanadium fluorophosphate composite cathode material according to claim 2, characterized in that, In step S2, the ratio of ammonium metavanadate, sodium fluoride, ammonium dihydrogen phosphate, and oxalic acid is 2:3:2:3, and the water bath temperature is 75℃~90℃.
5. The method for preparing the sodium vanadium fluoride phosphate composite cathode material according to claim 1, characterized in that, In step S3, the device is cleaned 2 to 5 times with deionized water and ethanol respectively, and the inert gas atmosphere is argon or nitrogen.
6. The method for preparing the sodium vanadium fluorophosphate composite cathode material according to any one of claims 1 to 5, characterized in that, In step S1, the mass ratio of Ketjen black to Na3V2O2(PO4)2F is 3wt%, and the mixture is pretreated under 800W ultrasound for 3h; in step S2, the mixture is heated in an 80℃ water bath and stirred until a clear blue solution is obtained; in step S3, the hydrothermal reaction temperature is 180℃ and the reaction is carried out for 4h; in step S4, the mixture is calcined at 400℃ for 4h under an argon atmosphere.
7. The method for preparing the sodium vanadium fluorophosphate composite cathode material according to any one of claims 1 to 5, characterized in that, In step S1, the mass ratio of Ketjen black to Na3V2O2(PO4)2F is 6wt%, and the mixture is pretreated under 800W ultrasound for 3h; in step S2, the mixture is heated in an 80℃ water bath and stirred until a clear blue solution is obtained; in step S3, the hydrothermal reaction temperature is 180℃ and the reaction is carried out for 4h; in step S4, the mixture is calcined at 400℃ for 4h under an argon atmosphere.
8. The method for preparing the sodium vanadium fluorophosphate composite cathode material according to any one of claims 1 to 5, characterized in that, In step S1, the mass ratio of Ketjen black to Na3V2O2(PO4)2F is 9wt%, and the mixture is pretreated under 800W ultrasound for 3h; in step S2, the mixture is heated in an 80℃ water bath and stirred until a clear blue solution is obtained; in step S3, the hydrothermal reaction temperature is 180℃ and the reaction is carried out for 4h; in step S4, the mixture is calcined at 400℃ for 4h under an argon atmosphere.
9. A sodium vanadium fluoride phosphate composite cathode material, characterized in that, It is made using the method described in any one of claims 1 to 8.
10. An application of a sodium vanadium fluoride phosphate composite cathode material in sodium-ion batteries, characterized in that, A sodium vanadium fluorophosphate composite cathode material prepared by the method described in any one of claims 1 to 8.
Citation Information
Patent Citations
Carbon nanotube / lithium iron phosphate composite positive electrode material and in situ preparation method thereof
CN101714627A
Nanosheet flower-shaped sodium vanadium oxyfluoride phosphate electrode material and preparation method and application thereof
CN113036114A