Method for preparing a magnetic fluid and display device
By preparing storage containers and delaying emulsification structures in magnetic flowing liquids, the problems of bubbles and foams when magnetic flowing liquids come into contact with transparent liquids are solved, improving the movement flexibility and service life of magnetic flowing liquids, and enhancing their aesthetic appeal.
Patent Information
- Application Number
- CN202211302836.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-24
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-10-24
AI Technical Summary
When magnetic flowing liquids come into contact with transparent liquids, bubbles and foams are easily generated, which leads to a shortened service life and reduced operational flexibility. Furthermore, the addition of emulsifiers can affect the aesthetics and maneuverability.
By preparing a storage container, inserting a magnetic flow structure and a flow medium, a delayed emulsification structure is formed. The emulsification phenomenon is prevented by assembling with an anti-emulsification substance and an amphiphilic active material, thereby enhancing the movement flexibility and service life of the magnetic flow structure.
It effectively slows down the emulsification between the magnetic flowing liquid and the transparent liquid, improves the flexibility of movement and service life, and also enhances the aesthetics.
Smart Images

Figure CN115602433B_ABST
Abstract
Description
TECHNICAL FIELD
[0001] The present application relates to the technical field of magnetic fluid, in particular to a preparation method of magnetic fluid and a display device. BACKGROUND
[0002] Magnetic fluid, also known as magnetic liquid, ferromagnetic fluid or magnetic liquid, is a new type of functional material, which has both the fluidity of liquid and the magnetism of solid magnetic material. It is a stable colloidal liquid formed by mixing magnetic solid particles with a diameter of nanometer level (below 10 nanometers), base liquid (also called medium) and surfactant. The fluid has no magnetic attraction in static state, but shows magnetism when subjected to an external magnetic field. At present, magnetic fluid can be applied in more and more fields, such as sound, clock and metronome, and the quality requirements for magnetic fluid are also higher and higher.
[0003] However, during the use of most magnetic fluid display devices, the liquid has a certain air solubility rate, and the magnetic fluid and the transparent liquid are in long-term contact. When the magnetic fluid is shaken or shaken by a magnet, a large number of air bubbles or foams containing the magnetic fluid will appear at the interface of the two incompatible liquids. If the shaking time is prolonged, emulsification and foams containing the magnetic fluid will occur at the same time, which will shorten the service life of the magnetic fluid and reduce the operation flexibility and rapidity of restoration. If an emulsifier is added, the magnetic fluid and the transparent liquid will become turbid, which will seriously affect the ornamental and movement flexibility of the magnetic fluid. SUMMARY
[0004] The main purpose of the present application is to provide a preparation method of magnetic fluid, which aims to delay the emulsification phenomenon between two media and improve the movement flexibility of the magnetic fluid.
[0005] The above problems solved by the present application are realized by the following technical solutions:
[0006] A preparation method of magnetic fluid, comprising the following steps:
[0007] Preparation of a storage container;
[0008] Placing a flow medium into the interior of the storage container;
[0009] Preparation of a magnetic flow structure; and placing the magnetic fluid into the interior of the storage container, so that the magnetic flow structure flows in the flow medium; and the magnetic flow structure is insoluble in the flow medium;
[0010] The anti-emulsifying substance is assembled with the amphiphilic active material to form a delayed emulsification structure; the delayed emulsification structure is placed in the storage container, so that the delayed emulsification solid is arranged on the surface of the magnetic flow structure.
[0011] Preferably, the magnetic flow structure comprises a magnetic flow body; the magnetic flow body is selected from an aqueous magnetic flow body or an oily magnetic flow body; the flow medium is selected from an oily liquid or an aqueous liquid.
[0012] Preferably, when the magnetic flow body is selected from an aqueous magnetic flow body, the step of preparing the magnetic flow structure comprises:
[0013] After removing oxygen in the first mixed solution by bubbling N2 in the mixed solution of Fe3+ and Fe2+ at a molar ratio of 4:3, NaOH solution is added to the first mixed solution to adjust the pH value of the first mixed solution to 7.5, the first mixed solution is heated to 80-85℃ and stirred at constant temperature for 30-38min, the solid is filtered and screened, and the nano Fe3O4 is obtained by washing;
[0014] The nano Fe3O4 is added to polyethylene glycol, stirred by a stirrer for 19-19.5h, washed repeatedly with deionized water and anhydrous ethanol until the washing liquid is neutral, then deionized water is used to make the concentration of nano Fe3O4 0.095-0.099g / ml, and then ultrasonic treatment is performed for 37-39min to form an aqueous magnetic flow body;
[0015] Or, when the magnetic flow body is selected from an oily magnetic flow body, the step of preparing the magnetic flow structure comprises:
[0016] The magnetite particles are dispersed in an oil-based dispersion medium to form an oil-based magnetic fluid in the presence of a surfactant; wherein the surfactant is selected from one of oleic acid, stearic acid or lauric acid.
[0017] Preferably, the magnetic flow structure further comprises a chameleon pearl material and a magnetic flow body; the step of preparing the magnetic flow structure comprises:
[0018] The magnetic flow body is placed in a first dissolving medium in a first dissolving container to form a second mixed solution;
[0019] The chameleon pearl material is prepared;
[0020] The chameleon pearl material is placed in the second mixed solution and stirred uniformly at a temperature of 40-80 degrees, so that the chameleon pearl material is arranged on the surface of different magnetic flow bodies.
[0021] Preferably, the step of preparing the chameleon pearl material comprises:
[0022] mixing and stirring the carrier, the oil-soluble carbon black, the diffusing agent and the silicone powder in a mass ratio of (96-97) : (0.2-0.4) : (1.3-1.7) : (0.5-0.7) to obtain a first material;
[0023] uniformly stirring the color-changing pearl luster powder and the first material in a mass ratio of 1:99 to obtain the color-changing pearl luster material.
[0024] Preferably, the step of assembling the anti-emulsification substance and the amphiphilic active material to form the delayed emulsification structure comprises:
[0025] placing the anti-emulsification substance and the amphiphilic active material into a third dissolving medium and uniformly stirring at a temperature of 40-80 degrees to arrange the amphiphilic active material on the surface of the anti-emulsification substance.
[0026] Preferably, the anti-emulsification substance is selected from inorganic powder materials; and the step of preparing the anti-emulsification substance comprises the following steps:
[0027] placing the inorganic powder into a second dissolving medium to form a third mixture, adding an adjusting substance to the third mixture to form a fourth mixture, heating the fourth mixture to a first preset temperature and maintaining the first preset temperature for a first preset time;
[0028] cooling to room temperature and centrifuging to obtain the inorganic powder material.
[0029] Preferably, the amphiphilic active material is selected from carboxylate amphiphilic active materials.
[0030] Preferably, a magnetic fluid display device uses the preparation method of the magnetic fluid according to any one of the preceding aspects; the magnetic fluid display device comprises a storage container, a flowing medium, a magnetic flowing structure and a delayed emulsification structure; the storage container is provided with a placing cavity, the flowing medium is placed in the placing cavity, the magnetic flowing structure is arranged in the flowing medium and is insoluble in the flowing medium, and the delayed emulsification structure comprises an anti-emulsification substance and an amphiphilic active material, the amphiphilic active material is arranged on the surface of the anti-emulsification substance, and the amphiphilic active material is used to be adsorbed and connected with the flowing medium and the magnetic flowing structure.
[0031] Preferably, the magnetic flowing structure comprises a magnetic flowing body and a color-changing pearl luster material, and the color-changing pearl luster material is arranged on the surface of the magnetic flowing body.
[0032] Beneficial Effects: The technical solution of this invention first prepares a storage container, enabling the display device to move within a relatively independent space; then, a flowing medium is placed inside the storage container; next, a magnetic flow structure is prepared; and the magnetic fluid is placed inside the storage container, allowing the magnetic flow structure to flow in the flowing medium; the magnetic flow structure is insoluble in the flowing medium, thus enabling it to move within the medium and improving its flexibility; finally, a delayed emulsification structure is prepared by assembling an anti-emulsification substance and an amphiphilic active material, and then placed in the storage container, so that the delayed emulsification solids are placed on the surface of the magnetic flow structure. This allows the delayed emulsification solids to puncture bubbles or foam generated by the magnetic flow structure during its movement, achieving an anti-foaming effect. Furthermore, the delayed emulsification solids can at least partially isolate the magnetic flow structure from the flowing medium, thus delaying emulsification between the two media, improving the flexibility of the magnetic fluid's movement, extending the lifespan of the magnetic flow structure, and solving the aesthetic defects caused by foam at the interface between substances. Attached Figure Description
[0033] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on the structures shown in these drawings without creative effort.
[0034] Figure 1 This is a flowchart of an embodiment of a method for preparing a magnetic fluid according to the present invention.
[0035] Figure 2 This is a schematic diagram of an embodiment of a magnetic fluid display device according to the present invention.
[0036] Figure 3 This is a schematic diagram of a delayed emulsification structure according to an embodiment of a magnetic fluid display device of the present invention.
[0037] Explanation of icon numbers:
[0038] Reference Name Reference Name 1 Storage container 2 Flowing medium 3 Magnetic fluid 4 Delayed emulsification structure 41 First amphiphilic active agent 42 Anti-emulsifying substance 43 Second amphiphilic active agent
[0039] The above is a corresponding explanation of the attached diagram. Detailed Implementation
[0040] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0041] It should be noted that if the embodiments of the present invention involve directional indications (such as up, down, left, right, front, back, etc.), the directional indications are only used to explain the relative positional relationship and movement of the components in a specific posture. If the specific posture changes, the directional indications will also change accordingly.
[0042] Furthermore, if the embodiments of this invention involve descriptions such as "first" or "second," these descriptions are for descriptive purposes only and should not be construed as indicating or implying their relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined with "first" or "second" may explicitly or implicitly include at least one of those features. Additionally, the use of "and / or" or "and / or" throughout the text includes three parallel solutions. For example, "A and / or B" includes solution A, solution B, or a solution where both A and B are satisfied simultaneously. Furthermore, the technical solutions of the various embodiments can be combined with each other, but this must be based on the ability of those skilled in the art to implement them. When the combination of technical solutions is contradictory or impossible to implement, it should be considered that such a combination of technical solutions does not exist and is not within the scope of protection claimed by this invention.
[0043] This invention proposes a method for preparing magnetic fluid.
[0044] like Figure 1 As shown, in one embodiment of the present invention, the method for preparing the magnetic fluid includes the following steps:
[0045] S1. Prepare storage containers;
[0046] S2. Place the flowing medium into the storage container;
[0047] S3. Prepare a magnetic flow structure; and place the magnetic fluid into the interior of the storage container so that the magnetic flow structure flows in the flow medium; and the magnetic flow structure is insoluble in the flow medium.
[0048] S4. Assemble the antiemulsifying substance and the amphiphilic active material to form a delayed emulsification structure; place the delayed emulsification structure into the storage container so that the delayed emulsification solid is disposed on the surface of the magnet flow structure.
[0049] The technical solution of this invention first prepares a storage container, enabling the display device to move within a relatively independent space; then, a flowing medium is placed inside the storage container; next, a magnetic flow structure is prepared; and the magnetic fluid is placed inside the storage container, allowing the magnetic flow structure to flow in the flowing medium; the magnetic flow structure is insoluble in the flowing medium, thus enabling it to move within the medium and improving its flexibility; finally, a delayed emulsification structure is prepared by assembling an anti-emulsification substance and an amphiphilic active material, and then placed in the storage container, so that the delayed emulsification solids are placed on the surface of the magnetic flow structure. This allows the delayed emulsification solids to puncture any bubbles or foam generated by the magnetic flow structure during its movement, achieving an anti-foaming effect. Furthermore, the delayed emulsification solids can at least partially isolate the magnetic flow structure from the flowing medium, thus delaying emulsification between the two media, improving the flexibility of the magnetic fluid's movement, extending the lifespan of the magnetic flow structure, and solving the aesthetic defects caused by foam at the interface between substances.
[0050] Specifically, in some embodiments, in S1, the step of preparing the storage container includes the following steps:
[0051] The lid and container body of the storage container are obtained by using a thermoforming machine and left to stand for a first preset time to prepare the storage container.
[0052] The storage container is pre-cleaned, including dust removal, sterilization, and drying. This results in a cleaner storage container, preventing damage from other substances to the flow medium, magnetic flow structure, and delayed emulsion structure, thus improving safety during use.
[0053] Specifically, in some embodiments, the magnetic flow structure includes a magnetic fluid; the magnetic fluid is selected as an aqueous magnetic fluid or an oily magnetic fluid; the flow medium is selected as an oily liquid or an aqueous liquid, wherein the oily liquid is selected as one of hydrocarbon oil, fluorinated oil, fluorinated hydrocarbon oil, chlorinated hydrocarbon oil, glycerol ester or methacrylic anhydride oil; wherein the aqueous liquid is selected as water.
[0054] In some embodiments, when the magnetic flow structure includes an aqueous magnetic fluid, the flow medium is an oily liquid; in other embodiments, when the magnetic flow structure includes an oily magnetic fluid, the flow medium is an aqueous liquid. This structure can prevent the magnetic flow structure and the flow medium from dissolving into each other, thus avoiding affecting the smoothness of movement, thereby ensuring movement flexibility and improving viewing performance.
[0055] Specifically, in some embodiments, when the magnetic fluid is an aqueous magnetic fluid, in step S3, the step of preparing the magnetic flow structure includes:
[0056] After passing N2 into a mixed solution of Fe3+ and Fe2+ with a molar ratio of 4:3 to remove oxygen from the first mixture, NaOH solution is added to the first mixture to adjust the pH value to 7.5. The first mixture is heated to 80-85℃ and stirred for 30-38 minutes. The solid is filtered out and washed to obtain nano Fe3O4.
[0057] The nano-Fe3O4 was added to polyethylene glycol and stirred for 19-19.5 hours. The solution was then repeatedly washed with deionized water and anhydrous ethanol until neutral. The volume was then adjusted with deionized water to a concentration of 0.095-0.099 g / ml for the nano-Fe3O4. Finally, the solution was ultrasonically treated for 37-39 minutes to form an aqueous magnetic fluid. This yielded a colorless aqueous magnetic fluid.
[0058] Specifically, in some embodiments, when the magnetic fluid is an oil-based magnetic fluid, in step S3, the step of preparing the magnetic flow structure includes:
[0059] In the presence of a surfactant, magnetite particles are dispersed in an oil-based dispersion medium to prepare an oil-based magnetic fluid; wherein the surfactant is selected from oleic acid, stearic acid, or lauric acid. The magnetite particles are hydrophilically treated using a surfactant or epoxy resin to create an oleophilic layer, and then subjected to corona treatment to impart non-magnetic properties to the magnetite particles and a hydrophilic layer to the metal component. This yields a colorless, oily magnetic fluid.
[0060] Specifically, in some embodiments, the magnetic flow structure further includes a chameleon pearl material and a magnetic fluid; the step of preparing the magnetic flow structure includes:
[0061] The magnetic fluid is placed into a first dissolving medium in a first dissolving container to form a second mixture; wherein, the first dissolving medium may be a water-based dissolving medium.
[0062] Prepare the chameleon pearl light material;
[0063] The chameleon atomizing material is placed in the second mixture and stirred evenly at a temperature of 40-80 degrees Celsius, so that the chameleon atomizing material is disposed on the surface of different magnetic fluids. Through stirring and at a suitable temperature, the chameleon atomizing material can be disposed at the interface between the magnetic fluids, so that the magnetic fluids can display different colors, thereby making the movement state of the magnetic fluids more clearly observable and improving the flexibility of use.
[0064] Specifically, in some embodiments, the step of preparing the chameleon aurora material includes:
[0065] The carrier, oil-soluble carbon black, dispersant, and silicone powder are uniformly mixed and stirred in a mass ratio of (96-97):(0.2-0.4):(1.3-1.7):(0.5-0.7) to obtain the first material; wherein, the carrier can be an aqueous carrier.
[0066] The color-changing pearlescent powder with a mass ratio of 1:99 is uniformly stirred with the first material to obtain the chameleon pearlescent material.
[0067] Specifically, in some embodiments, the antiemulsifying agent is selected from inorganic powder materials; in S4, the step of preparing the antiemulsifying agent includes the following:
[0068] Inorganic powder is placed in a second dissolving medium to form a third mixture, and a conditioning substance is added to the third mixture to form a fourth mixture; the fourth mixture is heated to a first preset temperature and maintained for a first preset time;
[0069] The inorganic powder material is obtained by cooling it to room temperature and centrifuging it.
[0070] In some embodiments, when titanium dioxide powder is selected as the inorganic powder material, 100g of titanium dioxide powder is added to 500ml of water, and 15g of lecithin is added at the same time. The mixture is placed in a 1000ml three-necked flask, then heated to 90°C, maintained at that temperature for 120min, cooled to room temperature (20-45°C), and then centrifuged.
[0071] In some other embodiments, when zinc oxide powder is selected as the inorganic powder material, 100g of zinc oxide powder is added to 500ml of water, and 17.5g of cocamidopropyl betaine is added at the same time. The mixture is then added to a 1000ml three-necked flask, and the flask is placed in an ultrasonic bath for 30min (the temperature of the liquid will rise if it is placed in an ultrasonic bath for a long time). Then, it is cooled to room temperature (20-45 degrees Celsius) and centrifuged.
[0072] In another embodiment, when zinc oxide powder is selected as the inorganic powder material, 100g of zinc oxide powder, 500ml of water and 10g of sodium oleocarboxylate are placed in a 1000ml three-necked flask, placed in an ultrasonic bath for 45min, and then cooled to room temperature before centrifugation.
[0073] Specifically, in some embodiments, in step S4, the step of assembling the antiemulsifying substance with the amphiphilic active material to form a delayed emulsification structure includes:
[0074] The antiemulsifying substance and the amphiphilic active material are placed in a third dissolving medium and stirred evenly at a temperature of 40-80 degrees Celsius, so that the amphiphilic active material is deposited on the surface of the antiemulsifying substance. This allows the emulsification-retarding structure to simultaneously possess amphiphilic functionality.
[0075] Specifically, in some embodiments, the amphiphilic active material is selected from carboxylate amphiphilic active materials.
[0076] This invention also proposes a magnetic fluid display device, which utilizes a method for preparing the magnetic fluid. The specific details of this method are described in the above embodiments. Since this magnetic fluid display device employs all the technical solutions of the above embodiments, it possesses at least all the beneficial effects brought about by the technical solutions of the above embodiments, which will not be elaborated upon here. For example, Figure 2 As shown,
[0077] The magnetic fluid display device includes a storage container 1, a flow medium 2, a magnetic flow structure 3, and a delayed emulsification structure 4. The storage container 1 has a placement cavity, and the flow medium 2 is placed inside the placement cavity. The magnetic flow structure 3 is disposed inside the flow medium 2 and is insoluble in the flow medium 2. The delayed emulsification structure 4 includes an anti-emulsification substance 42 and an amphiphilic active material. The amphiphilic active material is disposed on the surface of the anti-emulsification substance 42 and is used to adsorb and connect with the flow medium 2 and the magnetic flow structure 3.
[0078] Specifically, in some implementations, such as Figure 3 As shown, the amphiphilic active material includes a first amphiphilic surfactant 41 and a second amphiphilic surfactant 43; the first amphiphilic surfactant 41 and the second amphiphilic surfactant 43 are respectively disposed on both sides of the antiemulsifying material 42.
[0079] Specifically, in some embodiments, the magnetic flow structure includes a magnetic fluid; the magnetic fluid is selected as an aqueous magnetic fluid or an oily magnetic fluid; the flow medium is selected as an oily liquid or an aqueous liquid, wherein the oily liquid is selected as one of hydrocarbon oil, fluorinated oil, fluorinated hydrocarbon oil, chlorinated hydrocarbon oil, glycerol ester or methacrylic anhydride oil; wherein the aqueous liquid is selected as an aqueous liquid.
[0080] Specifically, in some embodiments, when the magnetic flow structure includes an aqueous magnetic fluid, the flow medium is an oily liquid; in other embodiments, when the magnetic flow structure includes an oily magnetic fluid, the flow medium is an aqueous liquid.
[0081] Specifically, in some other embodiments, the magnetic flow structure further includes a chameleon atomizing material and a magnetic fluid, wherein the chameleon atomizing material is disposed on the surface of the magnetic fluid.
[0082] The above description is merely a preferred embodiment of the present invention and does not limit the patent scope of the present invention. Any equivalent structural transformations made using the contents of the present invention's specification and drawings under the inventive concept of the present invention, or direct / indirect applications in other related technical fields, are included within the patent protection scope of the present invention.
Claims
1. A method for preparing a magnetic fluid, characterized in that, Includes the following steps: Prepare storage containers; The flowing medium is placed inside the storage container; A magnetic flow structure is prepared; and the magnetic flow structure is placed inside the storage container to allow the magnetic flow structure to flow in the flow medium; and the magnetic flow structure is insoluble in the flow medium. An antiemulsifying agent and an amphiphilic active material are assembled to form a delayed emulsification structure; the delayed emulsification structure is placed in the storage container so that the delayed emulsification structure is disposed on the surface of the magnetic flow structure; wherein, the antiemulsifying agent is an inorganic powder material; the amphiphilic active material is a carboxylate amphiphilic active material; The step of assembling the antiemulsifying substance with the amphiphilic active material to form a delayed emulsification structure includes: The antiemulsifying substance and the amphiphilic active material are placed in a third dissolving medium and stirred evenly at a temperature of 40-80 degrees Celsius, so that the amphiphilic active material is disposed on the surface of the antiemulsifying substance. The magnetic flow structure further includes a chameleon pearl light material and a magnetic fluid; the step of preparing the magnetic flow structure includes: The magnetic fluid is placed into the first dissolving medium in the first dissolving container to form a second mixture; Preparation of the chameleon pearl light material; The chameleon atomized material is placed into the second mixture and stirred evenly at a temperature of 40-80 degrees Celsius, so that the chameleon atomized material is disposed on the surface of different magnetic fluids; The step of preparing the chameleon aurora material includes: The carrier, oil-soluble carbon black, dispersant and silicone powder in a mass ratio of (96-97):(0.2-0.4):(1.3-1.7):(0.5-0.7) are uniformly mixed and stirred to obtain the first material; The color-changing pearlescent powder at a mass ratio of 1:99 is uniformly stirred with the first material to obtain the chameleon pearlescent material.
2. The method for preparing a magnetic fluid according to claim 1, characterized in that, The magnetic flow structure includes a magnetic fluid; the magnetic fluid is selected as an aqueous magnetic fluid or an oily magnetic fluid; the flow medium is selected as an oily liquid or an aqueous liquid.
3. The method for preparing a magnetic fluid according to claim 2, characterized in that, When the magnetic fluid is an aqueous magnetic fluid, the step of preparing the magnetic flow structure includes: After passing N2 into a mixed solution of Fe3+ and Fe2+ with a molar ratio of 4:3 to remove oxygen from the first mixture, NaOH solution is added to the first mixture to adjust the pH value to 7.
5. The first mixture is heated to 80-85℃ and stirred for 30-38 minutes. The solid is filtered out and washed to obtain nano Fe3O4. The nano-Fe3O4 was added to polyethylene glycol and stirred with a stirrer for 19-19.5 h. The mixture was then repeatedly washed with deionized water and anhydrous ethanol until the washing solution was neutral. The volume was then adjusted with deionized water to a concentration of 0.095-0.099 g / ml. Finally, the mixture was ultrasonically treated for 37-39 min to form an aqueous magnetic fluid. Alternatively, when the magnetic fluid is an oil-based magnetic fluid, the step of preparing the magnetic flow structure includes: In the presence of a surfactant, magnetite particles are dispersed in an oil-based dispersion medium to prepare an oil-based magnetic fluid; wherein the surfactant is selected from oleic acid, stearic acid, or lauric acid.
4. The method for preparing a magnetic fluid according to claim 1, characterized in that, The steps for preparing the antiemulsifier include the following: Inorganic powder is placed in a second dissolving medium to form a third mixture, and a conditioning substance is added to the third mixture to form a fourth mixture; the fourth mixture is heated to a first preset temperature and maintained for a first preset time; The inorganic powder material is obtained by cooling it to room temperature and centrifuging it.
5. A magnetic fluid display device, characterized in that, The method for preparing the magnetic fluid according to any one of claims 1-4; the display device of the magnetic fluid includes a storage container, a flow medium, a magnetic flow structure, and a delayed emulsification structure; the storage container has a placement cavity, and the flow medium is placed inside the placement cavity; the magnetic flow structure is disposed inside the flow medium, and the magnetic flow structure is insoluble in the flow medium; the delayed emulsification structure includes an anti-emulsification substance and an amphiphilic active material, the amphiphilic active material is disposed on the surface of the anti-emulsification substance, and the amphiphilic active material is used for adsorption and connection with the flow medium and the magnetic flow structure.
6. A magnetic fluid display device according to claim 5, characterized in that, The magnetic flow structure includes a magnetic fluid and a chameleon atomizing material, wherein the chameleon atomizing material is disposed on the surface of the magnetic fluid.
Citation Information
Patent Citations
Processing technology of magnetic fluid and magnetic fluid display device thereof
CN114464441A