An optical chip substrate structure and a method of manufacturing the same
By adding a Si3N4 waveguide layer between Si and LN thin films, silicon nitride waveguides were fabricated using low-pressure chemical vapor deposition, solving the etching problem of lithium niobate thin films, realizing the integration of silicon-based photonic chips and LN optical chips, reducing losses and improving chip performance.
Patent Information
- Application Number
- CN202211247027.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-12
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2042-10-12
AI Technical Summary
In the existing technology, lithium niobate thin films are difficult to etch when preparing electro-optic modulators, with low etching efficiency and insufficient verticality of the etched sidewalls, which limits the performance improvement of silicon-based optoelectronic chips.
A Si3N4 waveguide layer is added between the Si thin film and the LN thin film, and a silicon nitride waveguide is prepared by low-pressure chemical vapor deposition to avoid direct etching of the lithium niobate thin film. Chip fabrication is then carried out in conjunction with mature silicon-based optoelectronic processes.
This technology enables heterogeneous integration of silicon-based photonic chips and LN optical chips, reducing propagation loss, simplifying the fabrication process, and improving the overall performance of the chip.
Smart Images

Figure CN115685600B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of chip technology, and in particular to an optical chip substrate structure and its fabrication method. Background Technology
[0002] With the increasing demand for higher communication speeds, silicon-on-insulator (SOI) based optoelectronic chips have gradually gained attention from the industry. Currently, SOI-based optoelectronic chips have been commercialized and are very mature in the fabrication of various passive and active devices. However, SOI has inherent disadvantages in optical applications. Because silicon is a centrosymmetric crystal and does not exhibit electro-optic effects, modulators fabricated using the plasma dispersion effect suffer from high losses and low extinction ratios, limiting further improvements in the performance of silicon-based optoelectronic chips.
[0003] In recent years, lithium niobate thin films have attracted widespread attention due to their great application potential in the fabrication of high-performance electro-optic modulators. However, the fabrication of electro-optic modulators with lithium niobate thin films still faces challenges such as difficult etching of lithium niobate materials, low etching efficiency, and insufficient verticality of the etching sidewalls. Summary of the Invention
[0004] This invention achieves heterogeneous integration of silicon-based photonic chips and LN optical chip substrate structures by adding a Si3N4 waveguide layer between Si and LN thin films. At the same time, it avoids the use of immature LN etching processes and utilizes mature silicon-based optoelectronic device libraries and mature processing technologies for large-scale chip fabrication, which is more conducive to the large-scale fabrication of high-quality hybrid photonic chips.
[0005] To address the aforementioned technical problems, this application discloses an optical chip substrate structure, comprising a substrate structure, a piezoelectric thin film layer, a waveguide layer, and a silicon thin film layer stacked sequentially.
[0006] The waveguide layer includes waveguides and isolation structures arranged alternately along a first direction; the first direction is a direction perpendicular to the axis of the substrate structure.
[0007] The waveguide is made of silicon nitride; the piezoelectric thin film layer is made of lithium niobate.
[0008] Optionally, the width of the waveguide can range from 0.5 to 5 micrometers;
[0009] The width of the isolation structure is greater than 10 micrometers.
[0010] Optionally, the difference between the thickness of the isolation structure and the thickness of the waveguide is greater than zero and less than or equal to 300 nanometers.
[0011] Optionally, an isolation layer is provided between the waveguide layer and the silicon thin film layer;
[0012] The material of the isolation layer is the same as that of the isolation structure.
[0013] Optionally, the thickness of the isolation layer can range from 0 to 300 nanometers.
[0014] Optionally, the substrate structure includes a stacked support substrate and a low-refractive-index layer.
[0015] Optionally, the material of the support substrate is any one of silicon, silicon oxide, sapphire, diamond, aluminum nitride, quartz, gallium nitride, and silicon carbide;
[0016] The material of this low-refractive-index layer includes silicon dioxide.
[0017] Optionally, the thickness of the piezoelectric thin film layer ranges from 200 to 1000 nanometers;
[0018] The thickness of the silicon thin film layer ranges from 100 to 500 nanometers.
[0019] Optionally, the material of the isolation structure includes silicon dioxide;
[0020] The material of this silicon thin film layer includes monocrystalline silicon.
[0021] On the other hand, this application also discloses a method for preparing the above-mentioned optical chip substrate structure, which includes:
[0022] Provide a silicon-on-insulator (SOI) substrate on an insulating substrate;
[0023] The surface of the silicon substrate on the insulating substrate is oxidized to obtain an SOI substrate with an oxide layer on the surface.
[0024] The oxide layer is patterned to obtain a patterned SOI substrate; the surface of the patterned SOI substrate has multiple spaced grooves.
[0025] Waveguides were deposited in the multiple spaced grooves using low-pressure chemical vapor deposition; the waveguide material included silicon nitride.
[0026] Provide a piezoelectric thin film structure;
[0027] The piezoelectric thin film layer of the piezoelectric thin film structure is bonded to the waveguide of the SOI substrate to obtain the bonded structure; the material of the piezoelectric thin film layer is lithium niobate.
[0028] The silicon layer and silicon dioxide layer away from the waveguide in the SOI substrate are removed to obtain the optical chip substrate structure.
[0029] Optionally, the bonding vacuum during this bonding process should be less than 10. -3 millibar;
[0030] The bonding temperature is greater than 50℃.
[0031] Optionally, methods for removing the silicon and silicon dioxide layers in the SOI substrate that are far from the waveguide include mechanical polishing and selective chemical removal.
[0032] Optionally, the piezoelectric thin film structure includes a support substrate, a low refractive index layer and a piezoelectric thin film layer stacked sequentially.
[0033] When the material of the supporting substrate is silicon, before bonding the piezoelectric thin film layer of the piezoelectric thin film structure to the waveguide of the SOI substrate to obtain the bonded structure, the process further includes:
[0034] A barrier layer is deposited on the supporting substrate of the piezoelectric thin film;
[0035] The silicon layer and silicon dioxide layer away from the waveguide in the SOI substrate are removed to obtain the optical chip substrate structure, including:
[0036] Remove the silicon layer in the SOI substrate that is far from the waveguide;
[0037] The silicon dioxide layer and the blocking layer in the SOI substrate far from the waveguide were removed by selective removal of chemical reagents to obtain the optical chip substrate structure.
[0038] By adopting the above technical solution, the optical chip substrate structure provided in this application has the following beneficial effects:
[0039] The optical chip substrate structure provided in this application includes a substrate structure, a piezoelectric thin film layer, a waveguide layer, and a silicon thin film layer stacked sequentially. The waveguide layer includes waveguides and isolation structures arranged alternately along a first direction, which is perpendicular to the axis of the substrate structure. The waveguide material includes silicon nitride, and the piezoelectric thin film layer material is lithium niobate. This piezoelectric thin film layer and waveguide composite structure provided in this application has the advantage of low propagation loss because the waveguide can be deposited using low-pressure chemical vapor deposition. It also avoids direct etching of the lithium niobate thin film layer, further reducing loss. Furthermore, the optical chip substrate structure provided in this application forms a silicon thin film layer on top of the composite waveguide, which can be used to fabricate silicon waveguide passive devices, thus forming a structure containing three optical materials. The lithium niobate thin film layer can be used to fabricate electro-optic modulators and nonlinear devices, and the silicon waveguide layer can be used to fabricate passive devices. This achieves single-platform integration of silicon photonic chips, lithium niobate photonic chips, and silicon nitride photonic devices, demonstrating excellent application prospects. Attached Figure Description
[0040] To more clearly illustrate the technical solutions in the embodiments of this application, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0041] Figure 1 This is a schematic diagram of an optional optical chip substrate structure according to this application;
[0042] Figure 2 This is a schematic diagram of another optional optical chip substrate structure in this application;
[0043] Figure 3 This is a schematic diagram of the fabrication process for an optional optical chip substrate structure according to this application.
[0044] The following is supplementary explanation of the attached figures:
[0045] 1-Substrate structure; 11-Supporting substrate; 12-Low refractive index layer; 2-Piezoelectric thin film layer; 3-Waveguide layer; 31-Waveguide; 32-Isolation structure; 4-Silicon thin film layer; 5-Barrier layer; 6-Oxide layer. Detailed Implementation
[0046] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of this application, and not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of this application without creative effort are within the scope of protection of this application.
[0047] The term "an embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of this application. In the description of this application, it should be understood that the terms "upper," "lower," "top," "bottom," etc., indicating orientation or positional relationships based on the orientation or positional relationships shown in the accompanying drawings, are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of this application. Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of that feature. Moreover, the terms "first," "second," etc., are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence. It should be understood that such data can be interchanged where appropriate so that the embodiments of this application described herein can be implemented in orders other than those illustrated or described herein.
[0048] For the purposes of the detailed description below, it should be understood that the invention may take various alternative variations and sequences of steps unless expressly stated otherwise. Furthermore, except in any operational instance, or otherwise indicated, all figures representing the amounts of ingredients used, for example, in the specification and claims, should be understood to be modified in all cases by the term “about.” Therefore, unless indicated to the contrary, the numerical parameters set forth in the following specification and appended claims are approximations varying with the desired performance to be obtained according to the invention. It is not at all an attempt to limit the application of the doctrine of equivalents to the scope of the claims; each numerical parameter should be interpreted at least according to the number of significant figures reported and by applying ordinary rounding techniques.
[0049] Although the numerical ranges and parameters illustrating the broad scope of the invention are approximate, the values listed in the specific examples are reported as precisely as possible. However, any numerical value inherently contains some error that is necessarily caused by the standard deviation found in their respective test measurements.
[0050] When a numerical range is disclosed herein, the range is considered continuous and includes the minimum and maximum values of the range, as well as every value between the minimum and maximum values. Furthermore, when the range refers to an integer, it includes every integer between the minimum and maximum values of the range. Additionally, when multiple ranges are provided to describe a feature or characteristic, the ranges may be combined. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges to which they are included. For example, a specified range from “1 to 10” should be considered to include any and all subranges between the minimum value 1 and the maximum value 10. Exemplary subranges of the range 1 to 10 include, but are not limited to, 1 to 6.1, 3.5 to 7.8, 5.5 to 10, etc.
[0051] Lithium niobate thin films possess excellent optoelectronic properties, but when applied to electro-optic modulators, they often require etching to form the strip-shaped waveguide 31 in the desired waveguide layer 3. However, etching lithium niobate films is challenging, resulting in low etching line perpendicularity and high propagation loss in the formed devices. Combining lithium niobate with silicon-based optoelectronic chips is a promising approach to improving optoelectronic chip technology. This not only allows for the fabrication of electro-optic modulators for signal processing using the electro-optic modulation characteristics of lithium niobate, but also enables large-scale, low-cost chip fabrication using mature silicon-based optoelectronic chip processes and device libraries. For further information, please refer to... Figure 1 , Figure 1 This is a schematic diagram of an optional optical chip substrate structure according to this application. One aspect of this application discloses an optical chip substrate structure comprising a substrate structure 1, a piezoelectric thin film layer 2, a waveguide layer 3, and a silicon thin film layer 4, stacked sequentially. The waveguide layer 3 includes waveguides 31 and isolation structures 32 alternately arranged along a first direction; the first direction is perpendicular to the axis of the substrate structure 1; the waveguide 31 is made of silicon nitride; and the piezoelectric thin film layer 2 is made of lithium niobate.
[0052] In this embodiment, the first direction can be Figure 1In the x-axis direction. The optical chip substrate structure provided in this application utilizes silicon nitride to form a strip waveguide 31, and combines it with a lithium niobate thin film layer to form a composite waveguide 31, thereby avoiding the etching of the lithium niobate thin film. Moreover, in the prior art, due to the limited temperature resistance of lithium niobate thin film materials, waveguide 31 materials can generally only be grown using plasma-enhanced chemical vapor deposition (PECVD) or reactive magnetron sputtering, resulting in high waveguide 31 losses. In contrast, the silicon nitride waveguide 31 provided in this application can be deposited using low-pressure chemical vapor deposition, further reducing losses. Furthermore, the optical chip substrate structure provided in this application forms a silicon thin film layer 4 on top of the composite waveguide 31, which can be used to fabricate passive devices of the silicon waveguide 31, thus forming a structure containing three optical materials. The lithium niobate thin film layer can be used to fabricate electro-optic modulators and nonlinear devices, and the silicon waveguide 31 layer can be used to fabricate passive devices, thereby realizing the single-platform integration of silicon photonic chips, lithium niobate photonic chips, and silicon nitride photonic devices, which has excellent application prospects.
[0053] In one feasible embodiment, the width of waveguide 31 is in the range of 0.5 to 5 micrometers; the width of the isolation structure 32 is greater than 10 micrometers; that is, the spacing between adjacent waveguides 31 is greater than 10 micrometers.
[0054] In one feasible embodiment, the thickness of the isolation structure 32 is equal to the thickness of the waveguide 31; in another feasible embodiment, the thickness of the isolation structure 32 is greater than the thickness of the waveguide 31, but the difference is less than or equal to 300 nanometers, thereby effectively ensuring the flatness of the surface of the waveguide layer 3. During the fabrication process, the waveguide layer 3 is bonded to the piezoelectric thin film layer 2.
[0055] In one possible embodiment, see [reference] Figure 2 , Figure 2 This is a schematic diagram of another optional optical chip substrate structure of this application. The substrate structure 1 includes a stacked support substrate 11 and a low refractive index layer 12.
[0056] In one feasible embodiment, the material of the support substrate 11 is any one of silicon, silicon oxide, sapphire, diamond, aluminum nitride, quartz, gallium nitride, and silicon carbide; the material of the low refractive index layer 12 includes silicon dioxide.
[0057] In one feasible embodiment, the thickness of the piezoelectric thin film layer 2 is in the range of 200 to 1000 nanometers; and the thickness of the silicon thin film layer 4 is in the range of 100 to 500 nanometers.
[0058] Optionally, the thickness of the low refractive index layer 12 ranges from 0.5 to 10 micrometers.
[0059] In one feasible embodiment, the material of the isolation structure 32 includes silicon dioxide; the material of the silicon thin film layer 4 includes monocrystalline silicon.
[0060] In one feasible embodiment, in order to improve the flexibility of the fabrication method and to prevent the elements in the silicon thin film layer 4 and the waveguide layer 3 from diffusing into each other, an isolation layer is provided between the waveguide layer 3 and the silicon thin film layer 4; the material of the isolation layer is the same as the material of the isolation structure 32.
[0061] In one feasible embodiment, the thickness of the isolation layer ranges from 0 to 300 nanometers.
[0062] On the other hand, see Figure 3 , Figure 3 This is a schematic diagram illustrating the fabrication process of an optional optical chip substrate structure according to this application. This application also discloses a method for fabricating the aforementioned optical chip substrate structure, which includes the following steps:
[0063] 1) Provide a silicon-on-insulator (SOI) substrate on an insulating substrate, see [reference]. Figure 3 The structure shown in Figure (a) is an SOI substrate comprising a first silicon layer, a silicon dioxide layer, and a second silicon layer stacked sequentially.
[0064] 2) The surface of the silicon substrate on the insulating substrate is oxidized to obtain an SOI substrate with an oxide layer 6 on the surface. (See reference...) Figure 3 The structure shown in Figure (b) involves oxidizing the second silicon layer of the SOI substrate to form an oxide layer 6 of a predetermined thickness on the surface of the second silicon layer.
[0065] 3) The oxide layer 6 is patterned to obtain a patterned SOI substrate; the surface of the patterned SOI substrate has multiple spaced grooves, see [reference]. Figure 3 The structure shown in Figure (c) can be formed by etching the oxide layer 6 to create a strip-shaped through hole of a preset width, which can then be used to form a groove in conjunction with the underlying structure.
[0066] 4) Waveguide 31 is deposited in the multiple spaced grooves using low-pressure chemical vapor deposition; the material of waveguide 31 includes silicon nitride.
[0067] Optionally, step 4) can be specifically described as: depositing a silicon nitride thin film layer 4 (e.g., using low-pressure chemical vapor deposition) on the surface with grooves. Figure 3 The structure shown in Figure (d) is then subjected to planarization treatment to obtain the structure shown in Figure (d). Figure 3The structure shown in Figure (e) is an example of this method of growing silicon nitride thin film layer 4 using high-temperature low-pressure chemical vapor deposition, which results in waveguide 31 with low optical loss.
[0068] Optionally, in step 3) above, the groove in the patterned SOI substrate can be a through-hole structure penetrating the oxide layer 6, or it can be a groove structure located in the oxide layer 6, which can be formed according to different etching conditions. When the oxide layer 6 is a groove structure, there is an isolation layer (at the bottom of the groove structure of the oxide layer 6) between the subsequent waveguide 31 and the silicon thin film layer 4. The material of this isolation layer is the same as the material of the isolation structure 32.
[0069] In one feasible embodiment, the thickness of the isolation layer ranges from 0 to 300 nanometers.
[0070] 5) Provide a piezoelectric thin film structure, such as Figure 3 The structure shown in Figure (f) is as follows.
[0071] Optionally, the piezoelectric thin film structure includes a support substrate 11, a low refractive index layer 12, and a piezoelectric thin film layer 2 stacked sequentially.
[0072] In one feasible embodiment, the material of the support substrate 11 is any one of silicon, silicon oxide, sapphire, diamond, aluminum nitride, quartz, gallium nitride, and silicon carbide; the material of the low refractive index layer 12 includes silicon dioxide.
[0073] In this embodiment, the material of the piezoelectric thin film layer 2 is lithium niobate.
[0074] Optionally, the deposition method of the low refractive index layer 12 can be any one of thermal oxidation, PECVD, low pressure chemical vapor deposition (LPCVD), and magnetron sputtering.
[0075] Optionally, the thickness of the low-refractive-index layer 12 ranges from 0.5 to 10 micrometers.
[0076] In one feasible embodiment, when the material of the supporting substrate 11 is silicon, after step 5), the method further includes: depositing a barrier layer 5 on the supporting substrate 11 of the piezoelectric thin film, such as... Figure 3 The structure shown in Figure (g) is described below; step 7) below includes: removing the silicon layer in the SOI substrate away from waveguide 31 to obtain the structure shown in Figure (g); Figure 3 The structure shown in Figure (i) is described; the silicon dioxide layer and the blocking layer 5 in the SOI substrate, which are far from the waveguide 31, are removed using a chemical reagent selective removal method to obtain the optical chip substrate structure, as shown in Figure (i). Figure 3 The structure shown in Figure (j) is as follows.
[0077] To simplify the subsequent removal steps, in this embodiment, the material of the barrier layer 5 is silicon dioxide.
[0078] 6) The piezoelectric thin film layer 2 of the piezoelectric thin film structure is bonded to the waveguide 31 of the SOI substrate to obtain the bonded structure, as shown below. Figure 3 The structure shown in Figure (h) is as follows.
[0079] In one feasible embodiment, during the bonding process in step 6), the bonding vacuum should be less than 10. -3 Millibars; bonding temperature greater than 50°C. The aim is to reduce the probability of bonding voids between waveguide layer 3 and the upper piezoelectric thin film layer 2.
[0080] 7) Remove the silicon layer and silicon dioxide layer in the SOI substrate that are far from the waveguide 31 to obtain the optical chip substrate structure.
[0081] In one feasible embodiment, the method for removing the silicon layer and silicon dioxide layer in the SOI substrate away from the waveguide 31 includes mechanical polishing and selective chemical removal.
[0082] The method for fabricating the optical chip substrate structure provided in this application has the following advantages: The method of growing a silicon nitride thin film layer 4 using high-temperature, low-pressure chemical vapor deposition results in a waveguide 31 with low optical loss. The fabricated waveguide 31 is then transferred to a lithium niobate thin film substrate, simultaneously achieving the fabrication of the loaded strip waveguide 31 and heterogeneous integration of the silicon thin film and the lithium niobate thin film. After bonding, only the silicon waveguide 31 needs to be processed to form the optical chip substrate structure, simplifying subsequent processing. After bonding, the processing interface is on the SOI substrate and the thermally oxidized layer formed thereon, not at the bonding interface between the lithium niobate thin film layer and the waveguide 31, avoiding detachment due to insufficient bonding strength and the detachment of the top-layer processed waveguide 31.
[0083] To better understand the technical solution of this application, the following are some specific embodiments.
[0084] Example 1
[0085] See Figure 3 An SOI substrate is provided, and the surface of a silicon substrate on the insulating substrate is oxidized to obtain an SOI substrate with an oxide layer 6 on the surface; the oxide layer 6 is patterned to obtain a patterned SOI substrate; the surface of the patterned SOI substrate has multiple spaced grooves; waveguides 31 are deposited in the multiple spaced grooves using low-pressure chemical vapor deposition; the material of the waveguides 31 includes silicon nitride; the grooves are through-hole structures penetrating the oxide layer 6.
[0086] A piezoelectric thin film structure is provided, comprising a support substrate 11, a low refractive index layer 12, and a piezoelectric thin film layer 2 stacked sequentially; wherein the support substrate 11 is made of silicon, the low refractive index layer 12 is made of silicon dioxide, and the piezoelectric thin film layer 2 is made of lithium niobate; the piezoelectric thin film layer 2 of the piezoelectric thin film structure is bonded to the waveguide 31 of the SOI substrate to obtain the bonded structure; the silicon layer and silicon dioxide layer in the SOI substrate that are far from the waveguide 31 are removed to obtain the optical chip substrate structure.
[0087] Example 2
[0088] An SOI substrate is provided, and the surface of a silicon substrate on the insulating substrate is oxidized to obtain an SOI substrate with an oxide layer 6 on the surface. (See reference) Figure 3 The oxide layer 6 is patterned to obtain a patterned SOI substrate. The surface of the patterned SOI substrate has multiple spaced grooves. Waveguides 31 are deposited in the multiple spaced grooves using low-pressure chemical vapor deposition. The material of the waveguides 31 includes silicon nitride. The grooves are groove structures located in the oxide layer 6, which can isolate the thin film layer 4 from the waveguide layer 3, thereby preventing the elements in the silicon thin film layer 4 and the waveguide layer 3 from diffusing into each other.
[0089] A piezoelectric thin film structure is provided, which includes a support substrate 11, a low refractive index layer 12 and a piezoelectric thin film layer 2 stacked sequentially; wherein the material of the support substrate 11 is aluminum nitride, the material of the low refractive index layer 12 is silicon dioxide, and the material of the piezoelectric thin film layer 2 is lithium niobate; the piezoelectric thin film layer 2 of the piezoelectric thin film structure is bonded to the waveguide 31 of the SOI substrate to obtain the bonded structure; the silicon layer and silicon dioxide layer in the SOI substrate that are far away from the waveguide 31 are removed to obtain the optical chip substrate structure.
[0090] Example 3
[0091] See Figure 3 An SOI substrate is provided. The surface of a silicon substrate on the insulating substrate is oxidized to obtain an SOI substrate with an oxide layer 6 on the surface. The oxide layer 6 is patterned to obtain a patterned SOI substrate. The surface of the patterned SOI substrate has multiple spaced grooves. Waveguides 31 are deposited in the multiple spaced grooves using low-pressure chemical vapor deposition. The material of the waveguides 31 includes silicon nitride. The grooves are through-hole structures penetrating the oxide layer 6. The thickness of the isolation structure 32 is greater than the thickness of the waveguide 31, but the difference is less than or equal to 300 nanometers, thereby effectively ensuring the flatness of the surface of the waveguide layer 3.
[0092] A piezoelectric thin film structure is provided, comprising a support substrate 11, a low refractive index layer 12, and a piezoelectric thin film layer 2 stacked sequentially; wherein the support substrate 11 is made of silicon, the low refractive index layer 12 is made of silicon dioxide, and the piezoelectric thin film layer 2 is made of lithium niobate; the piezoelectric thin film layer 2 of the piezoelectric thin film structure is bonded to the waveguide 31 of the SOI substrate to obtain the bonded structure; the silicon layer and silicon dioxide layer in the SOI substrate that are far from the waveguide 31 are removed to obtain the optical chip substrate structure.
[0093] The optical chip substrate structure formed by the above embodiments 1-3 uses a high-temperature low-pressure chemical vapor deposition method to grow the silicon nitride thin film layer 4, which results in the waveguide 31 having low optical loss and avoids direct etching of the lithium niobate thin film layer, further reducing loss; and after bonding, the processing interface is on the SOI substrate and the thermal oxide layer formed thereon, not on the bonding interface between the lithium niobate thin film layer and the waveguide 31, avoiding detachment caused by insufficient strength during the bonding process, and detachment of the top processed waveguide 31 layer.
[0094] The above description is only an optional embodiment of this application and is not intended to limit this application. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the protection scope of this application.
Claims
1. A method for fabricating an optical chip substrate structure, characterized in that, include: Provide a silicon-on-insulator (SOI) substrate on an insulating substrate; The surface of the silicon substrate on the insulating substrate is oxidized to obtain an SOI substrate with an oxide layer (6) on the surface; The oxide layer (6) is patterned to obtain a patterned SOI substrate; The patterned SOI substrate has multiple spaced grooves on its surface; Waveguides (31) are deposited in the plurality of spaced grooves using low-pressure chemical vapor deposition; the material of the waveguides (31) includes silicon nitride; the plurality of grooves are arranged along a first direction; the first direction is a direction perpendicular to the axis of the substrate structure (1); Provide a piezoelectric thin film structure; The piezoelectric thin film layer (2) of the piezoelectric thin film structure is bonded to the waveguide (31) of the SOI substrate to obtain the bonded structure; the material of the piezoelectric thin film layer (2) is lithium niobate; the bonding vacuum degree should be less than 10. -3 millibar; bonding temperature greater than 50℃; Remove the silicon layer and silicon dioxide layer in the SOI substrate that are far from the waveguide (31) to obtain the optical chip substrate structure; the waveguide (31) and the piezoelectric thin film layer (2) can form a composite waveguide.
2. The method according to claim 1, characterized in that, Methods for removing the silicon and silicon dioxide layers in the SOI substrate that are far from the waveguide (31) include mechanical polishing and selective chemical removal.
3. The method according to claim 1, characterized in that, The piezoelectric thin film structure includes a support substrate (11), a low refractive index layer (12), and a piezoelectric thin film layer (2) stacked sequentially. When the material of the supporting substrate (11) is silicon, before bonding the piezoelectric thin film layer (2) of the piezoelectric thin film structure to the waveguide (31) of the SOI substrate to obtain the bonded structure, the method further includes: A barrier layer (5) is deposited on the support substrate (11) of the piezoelectric thin film structure. The process of removing the silicon layer and silicon dioxide layer away from the waveguide (31) in the SOI substrate to obtain the optical chip substrate structure includes: Remove the silicon layer in the SOI substrate that is away from the waveguide (31); The silicon dioxide layer and the barrier layer (5) in the SOI substrate that are far from the waveguide (31) are removed by selective removal of chemical reagents to obtain the optical chip substrate structure.
4. An optical chip substrate structure, characterized in that, It is prepared by the method as described in claim 1; The optical chip substrate structure includes a substrate structure (1), a piezoelectric thin film layer (2), a waveguide layer (3), and a silicon thin film layer (4) stacked sequentially. The waveguide layer (3) includes waveguides (31) and isolation structures (32) arranged alternately along the first direction.
5. The optical chip substrate structure according to claim 4, characterized in that, The width of the waveguide (31) ranges from 0.5 to 5 micrometers; The width of the isolation structure (32) is greater than 10 micrometers.
6. The optical chip substrate structure according to claim 4, characterized in that, The difference between the thickness of the isolation structure (32) and the thickness of the waveguide (31) is greater than or equal to zero and less than or equal to 300 nanometers.
7. The optical chip substrate structure according to claim 4, characterized in that, An isolation layer is provided between the waveguide layer (3) and the silicon thin film layer (4); The material of the isolation layer is the same as that of the isolation structure (32).
8. The optical chip substrate structure according to claim 7, characterized in that, The thickness of the isolation layer ranges from 0 to 300 nanometers.
9. The optical chip substrate structure according to claim 4, characterized in that, The substrate structure (1) includes a stacked support substrate (11) and a low refractive index layer (12).
10. The optical chip substrate structure according to claim 9, characterized in that, The material of the supporting substrate (11) is any one of silicon, silicon oxide, sapphire, diamond, aluminum nitride, quartz, gallium nitride and silicon carbide; The material of the low refractive index layer (12) includes silicon dioxide.
11. The optical chip substrate structure according to claim 4, characterized in that, The thickness of the piezoelectric thin film layer (2) ranges from 200 to 1000 nanometers; The thickness of the silicon thin film layer (4) ranges from 100 to 500 nanometers.
12. The optical chip substrate structure according to claim 4, characterized in that, The material of the isolation structure (32) includes silicon dioxide; The material of the silicon thin film layer (4) includes monocrystalline silicon.
Citation Information
Patent Citations
Photoelectric monolithic integration system based on lithium niobate-silicon nitride wafer
CN111276562A
Photoelectric monolithic integration system based on multi-material system
CN111474745A
Loading strip-shaped optical waveguide integrated structure and preparation method thereof
CN111965755A
Preparation method of hybrid integrated photoelectric chip substrate structure and substrate structure