Polypropylene resin foamed particles and method for producing the same
By introducing silica particles and advanced fatty acid amides into the polypropylene resin foam particles to form a weld layer, the problem of weld layer deposits during in-mold molding is solved, achieving good weldability and surface smoothness.
Patent Information
- Application Number
- CN202210792280.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-08-06
- Filing Date
- 2022-07-05
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-07-05
AI Technical Summary
When producing polypropylene resin foamed granules in an in-mold mold for extended periods, the deposits on the weld layer tend to accumulate in the mold, affecting the smoothness of the molded surface.
A fusion layer containing silica particles and advanced fatty acid amides is used, with the weight ratio of silica particles to advanced fatty acid amides being 1:0.2 to 1:8, and the total content being more than 0.05% by weight and less than 3% by weight. This ensures that the resin melting point of the fusion layer is lower than that of the core layer, improves weldability, and inhibits the accumulation of deposits.
While maintaining good weldability of foamed particles during in-mold forming, it effectively inhibits the accumulation of deposits in the forming mold, thereby improving the surface smoothness and production efficiency of the molded body.
Smart Images

Figure CN115703899B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to polypropylene resin foamed granules and their manufacturing method. Background Technology
[0002] Polypropylene resin foamed granules, formed by in-mold molding, are used in various applications such as packaging materials, automotive components, and building materials. The foamed granules constituting such foamed granule molded bodies are manufactured, for example, in the following manner.
[0003] First, polypropylene resin particles are dispersed in an aqueous medium containing an inorganic dispersant within a container. Next, a foaming agent is impregnated into the polypropylene resin particles within the container, and the resin particles containing the foaming agent (i.e., foamable resin particles) are released from the container along with the aqueous medium to cause foaming. This process produces foamed polypropylene resin particles.
[0004] Sometimes a weld layer is formed on the surface of the foamed particles to improve the weldability between the foamed particles during in-mold molding (e.g., Patent Document 1). Foamed particles with a weld layer are obtained, for example, by preparing polypropylene resin particles having a core layer and a weld layer disposed on the surface of the core layer and foaming the resin particles. In this case, as the weld layer, a crystalline polyolefin resin having a melting point lower than that of the polypropylene resin constituting the core layer, or an amorphous polyolefin resin having a low softening point, is used.
[0005] Existing technical documents
[0006] Patent documents
[0007] Patent Document 1: Japanese Patent No. 6757871 Summary of the Invention
[0008] The problem that the invention aims to solve
[0009] As described above, foamed granules with a weld layer exhibit good weldability during in-mold molding. However, when using foamed granules with a weld layer to produce foamed granule molded articles through in-mold molding for extended periods, there is a risk of deposits from the foamed granules (specifically, deposits from the weld layer) accumulating in easily heated areas of the molding die. This accumulation of deposits may adversely affect the smoothness of the surface of the foamed granule molded article, for example.
[0010] The present invention was made in view of the above background, and provides a polypropylene resin foamed granule and a method for manufacturing the same, wherein the polypropylene resin foamed granule can maintain good weldability between the foamed granules during in-mold forming while inhibiting the accumulation of deposits in the forming mold.
[0011] means for solving problems
[0012] The main points of this invention are as follows.
[0013] [1] A polypropylene resin foamed particle, comprising a foamed core layer of polypropylene resin as the base resin and a welded layer covering the core layer, wherein,
[0014] The aforementioned weld layer comprises silica particles and higher fatty acid amides.
[0015] The total content of the aforementioned silica particles and the aforementioned higher fatty acid amide in the aforementioned weld layer is 0.05% by weight or more and 3% by weight or less.
[0016] The weight ratio of the silica particles to the higher fatty acid amide in the above-mentioned welded layer is 1:0.2 to 1:8.
[0017] [2] According to the polypropylene resin foamed particles of [1], the content of the silica particles in the above-mentioned welded layer is more than 0.01% by weight and less than 0.5% by weight.
[0018] [3] The polypropylene resin foamed particles according to [1] or [2], wherein the content of the above-mentioned advanced fatty acid amide in the above-mentioned welded layer is more than 0.05% by weight and less than 1% by weight.
[0019] [4] Polypropylene resin foamed particles according to any one of [1] to [3], wherein the weight ratio of silica particles in the above-mentioned welded layer to the above-mentioned advanced fatty acid amide is 1:0.8 to 1:6.
[0020] [5] Polypropylene resin foamed particles according to any one of [1] to [4], wherein the above-mentioned advanced fatty acid amide includes erucamide.
[0021] [6] Polypropylene resin foamed particles according to any one of [1] to [5], wherein the core layer contains higher fatty acid amides, and the content of higher fatty acid amides in the welded layer is greater than the content of higher fatty acid amides in the core layer.
[0022] [7] Polypropylene resin foamed particles according to any one of [1] to [6], wherein the substrate resin constituting the above-mentioned weld layer is at least one selected from propylene-ethylene copolymer, propylene-butene copolymer and propylene-ethylene-butene copolymer.
[0023] [8] Polypropylene resin foamed particles according to any one of [1] to [7], wherein the proportion of the welded layer in the polypropylene resin foamed particles is 0.5% by weight or more and 10% by weight or less.
[0024] [9] Polypropylene resin foamed particles according to any one of [1] to [8], wherein the bulk density of the polypropylene resin foamed particles is 10 kg / m³. 3 Above and 500kg / m 3 the following.
[0025]
[10] A method for manufacturing polypropylene resin foamed granules, comprising:
[0026] The dispersion process involves dispersing polypropylene resin particles in an aqueous medium within a container.
[0027] In the foaming agent impregnation process, a foaming agent is impregnated in the polypropylene resin particles within the aforementioned container; and
[0028] In the foaming process, the polypropylene resin particles containing the foaming agent are released from a container together with an aqueous medium to cause them to foam.
[0029] The aforementioned polypropylene resin particles have a core layer made of polypropylene resin as the base material and a welded layer that covers the core layer.
[0030] The weld layer of the aforementioned polypropylene resin particles includes silica particles and higher fatty acid amides.
[0031] The total content of silica particles and higher fatty acid amides in the aforementioned weld layer is 0.05% by weight or more and 3% by weight or less.
[0032] The weight ratio of silica particles to higher fatty acid amides in the above-mentioned welded layer is 1:0.2 to 1:8.
[0033] Invention Effects
[0034] Based on the aforementioned polypropylene resin foamed particles, it is possible to maintain good weldability between the foamed particles during in-mold molding while suppressing the accumulation of deposits in the molding mold. Attached Figure Description
[0035] Figure 1 This is a schematic diagram of the cross-section of the foamed granules.
[0036] Figure 2 This is a schematic diagram of the cross-section of multilayer resin particles.
[0037] Figure 3 This is an explanatory diagram illustrating the calculation method for the area of a high-temperature peak.
[0038] Explanation of reference numerals in the attached figures
[0039] 1: Foamed granules;
[0040] 2: Core layer;
[0041] 3: Welded layer. Detailed Implementation
[0042] In this specification, when the symbol "~" is used to describe numerical or physical property values, it is used to indicate that the value before and after it is included. Furthermore, when a numerical or physical property value is described as a lower limit, it means above or below that value; when a numerical or physical property value is described as an upper limit, it means below that value. Additionally, "weight%" and "mass%", and "parts by weight" and "parts by mass" are substantially synonymous. Furthermore, in this specification, polypropylene resin foamed particles are appropriately referred to as "foamed particles," and foamed particle molded bodies are appropriately referred to as "molded bodies." Moreover, foamed particles having a foamed core layer composed of polypropylene resin are generally referred to as polypropylene resin foamed particles.
[0043] Foamed granules can be used to manufacture molded articles. Specifically, a molded article can be manufactured by a molding process in which multiple foamed granules are filled into a molding mold and a heating medium such as steam is supplied to fuse the foamed granules together. That is, a molded article can be obtained by in-mold molding of foamed granules.
[0044] exist Figure 1 Foamed particles are illustrated in the figures, but the invention is not limited to these figures. Figure 1 As shown, the foamed particle 1 has a foamed core layer 2 and a welded layer 3, with the welded layer 3 covering the core layer 2. The foamed core layer of the foamed particle is appropriately referred to as the "foamed core layer". The shape of the foamed particle 1 is, for example, cylindrical or spherical. The concept of a sphere includes not only spheres with a perfect circular cross-section, but also ellipsoidal spheres, spheres with shapes close to circles or ellipsoids.
[0045] The welded layer 3 is a layer that covers all or part of the foamed core layer 2 (see reference). Figure 1The foamed particles 1, for example, have a so-called core-sheath structure. The weld layer 3 refers to a layer that, when in-mold molding foamed particles (i.e., single-layer foamed particles) having a single-layer foamed core layer without a weld layer, can be molded at a vapor pressure lower than the minimum vapor pressure required to obtain a foamed particle molded body (i.e., a good single-layer foamed particle molded body) in which the single-layer foamed particles are well welded together. Furthermore, a foamed particle molded body in which the foamed particles are well welded together refers to a molded body with a weld ratio of 80% or more. The method for measuring the weld ratio of the molded body is described below. Additionally, the weld layer 3 can also be composed of a resin that easily welds together at a lower temperature (specifically, a lower vapor pressure) than the resin constituting the foamed core layer 2. Examples of resins constituting the weld layer include resins with a lower melting point and a lower softening point compared to the resin constituting the core layer.
[0046] The weld layer may be based on a polyolefin resin, for example. Examples of polyolefin resins include linear low-density polyethylene, low-density polyethylene, high-density polyethylene, and other polyethylene resins; propylene-ethylene copolymers, propylene-butene copolymers, propylene-ethylene-butene copolymers, and other polypropylene resins; and mixtures thereof. From the viewpoint of adhesion to the foamed core layer, the polyolefin resin of the weld layer is preferably a polypropylene resin and / or a polyethylene resin, more preferably a polypropylene resin. The base resin constituting the weld layer is further preferably at least one propylene resin selected from propylene-ethylene copolymers, propylene-butene copolymers, and propylene-ethylene-butene copolymers. In this case, the adhesion between the foamed core layer and the weld layer is further improved, and a molded article with good mechanical properties can be stably obtained. Furthermore, the base resin composed of at least one propylene resin selected from propylene-ethylene copolymers, propylene-butene copolymers, and propylene-ethylene-butene copolymers can be composed of a single copolymer or a mixture of multiple copolymers.
[0047] When the base resin constituting the weld layer is a polyolefin resin, the melting point Tms of the polyolefin resin is preferably lower than the melting point Tmc of the polypropylene resin constituting the foamed core layer. That is, for example, Tms < Tmc is preferred. In this case, the weldability of the foamed particles during molding is improved, and it is possible to produce a molded body with excellent weldability at low temperature (specifically, lower vapor pressure) during in-mold molding. From the viewpoint of further improving this effect, Tmc-Tms ≥ 1 is preferred, more preferably Tmc-Tms ≥ 3, and even more preferably Tmc-Tms ≥ 5. From the viewpoint of further suppressing the peeling of the foamed core layer from the weld layer and the adhesion of resin to the mold during in-mold molding, Tmc-Tms ≤ 30 is preferred, more preferably Tmc-Tms ≤ 25, and even more preferably Tmc-Tms ≤ 20.
[0048] From the viewpoint of easily suppressing resin adhesion to the molding die, the melting point Tms of the polyolefin resin constituting the weld layer is preferably 100°C or higher, more preferably 110°C or higher, and even more preferably 120°C or higher. On the other hand, from the viewpoint of easily improving the weldability of the foamed particles during molding, the melting point Tms of the polyolefin resin constituting the weld layer is preferably 150°C or lower, more preferably 145°C or lower, and even more preferably 140°C or lower. The melting point of the polyolefin resin constituting the weld layer is determined based on JIS K7121:1987. Specifically, it is determined using the same conditions and methods as the polypropylene resin constituting the foamed core layer described later.
[0049] The weld layer contains silica particles and higher fatty acid amides. The total content of silica particles and higher fatty acid amides in the weld layer is 0.05% by weight or more and 3% by weight or less. Furthermore, the weight ratio of silica particles to higher fatty acid amides in the weld layer (wherein the weight of silica particles : the weight of higher fatty acid amides) is 1:0.2 to 1:8. In other words, the content of higher fatty acid amides (parts by weight) is 0.2 to 8 parts by weight relative to the content (parts by weight) of silica particles in the weld layer. Because the weld layer contains silica particles and higher fatty acid amides in the above-mentioned predetermined ratio, the foamed particles exhibit good weldability during in-mold forming while suppressing the accumulation of deposits in the molding die.
[0050] Furthermore, the content of silica particles and higher fatty acid amides in the weld layer is roughly the same as the amount of silica particles and higher fatty acid amides in the weld layer during the manufacture of foamed particles.
[0051] The weld layer, for example, is made of a resin with a lower melting point than the foam core layer. Therefore, when conventional foam particles with a weld layer are molded in-mold, the components constituting the weld layer (specifically, the resin composition) soften or melt and easily adhere to the mold. Moreover, during long-term in-mold molding, deposits accumulate in the mold, causing defects such as depressions on the surface of the molded body, thus impairing the smoothness of the molded body surface. In particular, when using a mold with complex shapes such as areas with high vent density or thin-walled sections, deposits tend to accumulate in the complex shapes of the mold. This is believed to be because during molding, heating is usually performed in a way that allows parts that are difficult to heat to be fully molded, thus the complex shapes are easily overheated. As described above, in the foam particles of this disclosure, silica particles and higher fatty acid amides are incorporated into the weld layer in the predetermined ratio, thus maintaining the weldability between the foam particles while suppressing the accumulation of deposits. Furthermore, for example, by properly cleaning the mold, the formation of such deposits can be suppressed. However, if the cleaning frequency of the forming mold increases, productivity decreases, so it is preferable to clean the forming mold at a lower frequency.
[0052] In cases where the weld layer does not contain silica particles or one or both of higher fatty acid amides, for example, the components constituting the weld layer tend to adhere to complex shapes, making it difficult to suppress the accumulation of deposits within the molding die.
[0053] If the combined content of silica particles and higher fatty acid amides in the weld layer is too low, components constituting the weld layer may easily adhere to complex shapes, making it difficult to suppress the accumulation of deposits within the molding die. On the other hand, if the combined content of silica particles and higher fatty acid amides in the weld layer is too high, there is a risk that the foamed particles may not fuse together during in-mold molding, resulting in insufficient weldability of the molded body. From the viewpoint of further suppressing the accumulation of deposits and further improving weldability, the combined content of silica particles and higher fatty acid amides in the weld layer is preferably 0.1% by weight or more and 2% by weight or less, more preferably 0.2% by weight or more and 1% by weight or less.
[0054] Furthermore, if the content of the higher fatty acid amide is too low relative to the content of silica particles, there is a risk that the content of silica particles in the weld layer becomes excessive, resulting in insufficient weldability. Conversely, if the content of the higher fatty acid amide is too high relative to the content of silica particles, there is a risk that the content of the higher fatty acid amide becomes excessive, resulting in insufficient weldability. From the viewpoint of further improving weldability, the content of the higher fatty acid amide is preferably 0.8 to 6 parts by weight, more preferably 1 to 5 parts by weight, relative to the content of silica particles in the weld layer. In other words, the weight ratio of silica particles to higher fatty acid amides in the weld layer (wherein the weight of silica particles : the weight of higher fatty acid amides) is preferably 1:0.8 to 1:6, more preferably 1:1 to 1:5.
[0055] Furthermore, the content of silica particles in the weld layer is preferably 0.01% by weight or more and 1% by weight or less. In this case, the weldability of the molded article can be sufficiently improved while further suppressing the accumulation of deposits in the molding die. From the viewpoint of further improving this effect, the content of silica particles in the weld layer is more preferably 0.01% by weight or more and less than 0.5% by weight, more preferably 0.05% by weight or more and 0.4% by weight or less, and even more preferably 0.08% by weight or more and 0.3% by weight or less.
[0056] Furthermore, the content of higher fatty acid amides in the weld layer is preferably 0.05% by weight or more and 1% by weight or less. In this case, the weldability of the molded article can be sufficiently improved while further suppressing the accumulation of deposits in the molding die. From the viewpoint of further improving this effect, the content of higher fatty acid amides in the weld layer is more preferably 0.08% by weight or more and 0.8% by weight or less, and even more preferably 0.1% by weight or more and 0.5% by weight or less.
[0057] As silica particles, silica can be synthesized using dry silica, wet silica, or other methods, and / or natural silica can be used. Wet silica is silica produced by a wet process, such as neutralizing sodium silicate solution with inorganic acids like sulfuric acid or hydrochloric acid, or by hydrolysis based on alkoxysilanes.
[0058] Common methods for manufacturing wet silica include sedimentation and gelation. Examples of silica particles manufactured by the sedimentation method include "Nipsil E-200A" manufactured by Tosoh Silica Co., Ltd. Examples of silica particles manufactured by the gelation method include "NIPGEL BY-601" and "NIPGEL BY-001" manufactured by Tosoh Silica Co., Ltd. Additionally, silica particles that have undergone surface treatment using silane coupling agents, etc., can be used as needed.
[0059] The arithmetic mean particle size based on the number of silica particles is preferably 0.1 μm or more and 30 μm or less, more preferably 0.5 μm or more and 20 μm or less, and even more preferably 1 μm or more and 10 μm or less. In this case, foamed particles that maintain weldability while suppressing the accumulation of deposits in the molding die can be stably obtained.
[0060] The arithmetic mean particle size based on the number of silica particles can be obtained as follows: Based on the volume-based particle size distribution determined by laser diffraction scattering, the particle shape is assumed to be spheres and converted into a number-based particle size distribution, thus obtaining the number-based particle size distribution. The particle size based on this number-based particle size distribution is then arithmetically averaged. Furthermore, the aforementioned particle size refers to the diameter of an imaginary sphere having the same volume as the particle.
[0061] In this specification, "higher fatty acid amide" refers to a fatty acid amide in which the hydrocarbon group has 12 or more carbon atoms. The number of carbon atoms in the hydrocarbon group of the higher fatty acid amide is preferably 12 or more and 30 or less. In this case, it is easier to maintain the weldability of the foamed particles while suppressing the accumulation of deposits in the molding die. From the viewpoint of improving this effect, the number of carbon atoms in the hydrocarbon group of the higher fatty acid amide is more preferably 16 or more and 26 or less, and even more preferably 18 or more and 24 or less. Furthermore, the number of carbon atoms in the hydrocarbon group of the higher fatty acid amide is the number of carbon atoms in the hydrocarbon group other than the carbon atoms constituting the amide group. For example, when the higher fatty acid amide is a primary amide, it is a compound represented by the general formula: RCONH2 and having a hydrocarbon group (specifically, a long-chain fatty acid group) and an amide group. In the general formula: RCONH2, R is a hydrocarbon group.
[0062] The higher fatty acid amide can be either saturated or unsaturated fatty acid amide. From the viewpoint of easily and stably obtaining molded articles with good mechanical properties while suppressing the accumulation of deposits in the molding die, unsaturated fatty acid amides are preferred. Furthermore, the higher fatty acid amide can be a primary amide, a secondary amide, or a tertiary amide. From the viewpoint of easily dispersible in the resin constituting the foamed particles and weld layer, primary amides are preferred.
[0063] Specifically, higher fatty acid amides include saturated fatty acid amides such as lauryl amide, palmitamide, stearamide, and behenamide; and unsaturated fatty acid amides such as oleamide, erucamide, and ceramide. The weld layer may contain one or more higher fatty acid amides. From the viewpoint of being able to stably obtain foamed particles that maintain weldability while inhibiting the accumulation of deposits in the molding die, the higher fatty acid amides preferably include at least erucamide.
[0064] Furthermore, when the higher fatty acid amide includes erucamide, the proportion of erucamide in the higher fatty acid amide is preferably 50% by weight or more, more preferably 60% by weight or more, even more preferably 80% by weight or more, and particularly preferably 90% by weight or more.
[0065] The proportion of the weld layer in the foamed granules is preferably 0.5% by weight or more and 10% by weight or less. In this case, it is possible to stably obtain foamed granule molded articles with excellent mechanical properties while improving the in-mold formability of the foamed granules. From the viewpoint of improving this effect, the proportion of the weld layer in the foamed granules is more preferably 1% by weight or more and 8% by weight or less, and even more preferably 2% by weight or more and 6% by weight or less.
[0066] The core layer of the foamed granules uses polypropylene resin as the base resin. Examples of polypropylene resins include propylene homopolymers or propylene copolymers containing more than 50% by weight of structural units derived from propylene.
[0067] Examples of polypropylene-based copolymers include, for instance, propylene-ethylene copolymers, propylene-butene copolymers, and propylene-ethylene-butene copolymers, which are copolymers of propylene with ethylene or α-olefins having 4 or more carbon atoms; propylene-acrylic acid copolymers; and propylene-maleic anhydride copolymers. Furthermore, these copolymers can be any of block copolymers, random copolymers, or graft copolymers. Additionally, the aforementioned polymers can be crosslinked polymers, but are preferably non-crosslinked polymers.
[0068] In addition to polypropylene-based resins, other resins, elastomers, and other polymers may be included in the base resin constituting the foamed core layer without departing from the spirit of the present invention. Examples of other polymers include thermoplastic resins and / or elastomers other than polypropylene-based resins. As a thermoplastic resin other than polypropylene-based resins, at least one resin selected from polyethylene-based resins, polystyrene-based resins, polyamide-based resins, polyester-based resins, etc., may be used. As an elastomer, olefin-based thermoplastic elastomers and / or styrene-based thermoplastic elastomers may be used.
[0069] The proportion of other polymers in the foamed core layer is approximately 40 parts by weight or less, preferably 30 parts by weight or less, more preferably 20 parts by weight or less, even more preferably 10 parts by weight or less, and particularly preferably 5 parts by weight or less, relative to 100 parts by weight of polypropylene resin.
[0070] The melting point (Tmc) of the polypropylene resin constituting the core layer of the foamed granules is preferably 135–160°C. In this case, a foamed granule molded article with an excellent balance between the in-mold formability of the foamed granules and the mechanical properties of the resulting molded article can be stably obtained. From the viewpoint of improving the mechanical properties of the resulting molded article, the melting point (Tmc) of the polypropylene resin constituting the core layer is preferably 138°C or higher, more preferably 140°C or higher. Furthermore, from the viewpoint of improving in-mold formability under lower molding pressure conditions, the melting point (Tmc) of the polypropylene resin constituting the core layer is preferably 155°C or lower, more preferably 150°C or lower, and even more preferably 146°C or lower.
[0071] The melting point of polypropylene resins was determined based on JIS K7121:1987. Specifically, as a condition conditioning process, the melting temperature was measured after a certain heat treatment (2). The condition-conditioned test piece was heated from 30°C to 200°C at a heating rate of 10°C / min, and a DSC curve was obtained. The peak temperature of the melting peak in the DSC curve was taken as the melting point. Furthermore, in the case of multiple melting peaks in the DSC curve, the peak temperature of the melting peak with the largest area was taken as the melting point.
[0072] The foamed core layer may contain higher fatty acid amides. Examples of higher fatty acid amides include those used in the welded layer described above. The higher fatty acid amide preferably contains erucamide. In this case, the proportion of erucamide in the higher fatty acid amide is preferably 50% by weight or more, more preferably 60% by weight or more, further preferably 80% by weight or more, and particularly preferably 90% by weight or more.
[0073] Furthermore, it is preferable that the foamed core layer contains higher fatty acid amides, and the content of higher fatty acid amides in the weld layer is higher than that in the foamed core layer. In this case, the secondary foaming property of the foamed particles during in-mold forming can be maintained, resulting in a molded body with excellent weldability, and the accumulation of deposits in the molding die can be stably suppressed.
[0074] From this perspective, when the foamed core layer contains higher fatty acid amides, the content of higher fatty acid amides in the foamed core layer is preferably 0.01% by weight or more and 0.5% by weight or less, more preferably 0.02% by weight or more and 0.2% by weight or less, and even more preferably 0.03% by weight or more and 0.1% by weight or less. Furthermore, the content of higher fatty acid amides in the welded layer, C... BA The content of higher fatty acid amides in the foamed core layer C CA The difference C BA -C CA Preferably, it is 0.02% by weight or more, more preferably 0.03% by weight or more, and even more preferably 0.05% by weight or more. On the other hand, the difference C... BA -C CA Preferably, it is 0.3% by weight or less, more preferably 0.2% by weight or less.
[0075] In addition, the content of higher fatty acid amides in the foamed core layer is roughly the same as the amount of higher fatty acid amides in the foamed core layer during the manufacture of foamed granules.
[0076] Foamed granules are multi-layered granules with a foamed core layer and a welded layer. The foamed core layer is composed of foamed polypropylene resin, and the welded layer is composed of foamed or non-foamed polyolefin resin. The welded layer is preferably substantially non-foamed. "Substantially non-foamed" means that it has almost no air bubble structure.
[0077] Foamed granules may contain additives. Specifically, the foamed core layer and welded layer of foamed granules may contain flame retardants, flame retardant additives, bubble regulators, antioxidants, weathering agents, crystal nucleating agents, colorants, conductive materials, antistatic agents, etc. as additives.
[0078] Preferably, the foamed core layer contains carbon black. In this case, the foamed particles are colored black. From the viewpoint of being able to impart a good black color to the molded body while maintaining the formability of the foamed particles, the carbon black content in the foamed core layer is preferably 0.5% by weight or more and 5% by weight or less, more preferably 1% by weight or more and 4% by weight or less, and even more preferably 2% by weight or more and 3% by weight or less.
[0079] Furthermore, the weld layer of the foamed particles may contain carbon black. In this case, the carbon black content in the weld layer is preferably 0.5% by weight or more and 5% by weight or less, more preferably 1% by weight or more and 4% by weight or less, and even more preferably 2% by weight or more and 3% by weight or less. In this case, while ensuring the weldability of the foamed particles, the accumulation of deposits in the molding die can be further suppressed. In addition, when the foamed core layer and the weld layer contain carbon black, it is easier to make the color of the molded article more uniform.
[0080] In addition, the carbon black content in the foamed particles and the welded layer is roughly the same as the amount of carbon black mixed in the foamed particles and the welded layer during the manufacturing of the foamed particles.
[0081] As carbon black, various types can be used, such as channel black, roll black, furnace black, thermal cracking black, and acetylene black. Among these, furnace black offers an excellent balance between dispersibility in polypropylene resins and material cost, making it the preferred carbon black for use in foamed granules.
[0082] The bulk density of the foamed granules is preferably 10 kg / m³. 3 Above and 500kg / m 3 The following applies. In this case, it is possible to achieve both increased rigidity and lightweighting of the molded body. From the viewpoint of improving this effect, the bulk density of the foamed particles is more preferably 15 kg / m³. 3 Above and 100kg / m 3 The following is a further preferred value: 18 kg / m 3 Above and 50kg / m 3 the following.
[0083] The bulk density of the foamed granules was determined using the following method. First, the foamed granules to be tested were allowed to stand for at least 24 hours in an environment with an air temperature of 23°C, a relative humidity of 50%, and a temperature of 1 atm. Then, a batch of foamed granules weighing W (in grams) was filled into a graduated cylinder, and the bottom of the cylinder was gently tapped on the ground several times to stabilize the filling height. The bulk volume V (in liters) of the foamed granules was read from the graduated cylinder's scale. The weight W of the foamed granules was then divided by the bulk volume V (i.e., W / V). The resulting value was then converted to kg / m³. 3 The bulk density of the foamed particles can be obtained (unit: kg / m³). 3 ).
[0084] The foamed granules preferably have a crystalline structure in which the inherent melting peak of the polypropylene resin (i.e., the resin-inherent peak) and more than one melting peak (i.e., the high-temperature peak) appear in the DSC curve obtained when heated from 23°C to 200°C at a heating rate of 10°C / min are observed. DSC curves were obtained using 1–3 mg of foamed granules as test samples by differential scanning calorimetry (DSC) according to JIS K7122:1987.
[0085] The inherent resin peak refers to the endothermic peak generated by the melting of the inherent crystals of the polypropylene resin constituting the foamed particles. It can be considered as the endothermic peak generated by the melting of crystals typically present in polypropylene resins. On the other hand, the endothermic peak on the high-temperature side of the inherent resin peak (i.e., the high-temperature peak) refers to the endothermic peak that appears in the DSC curve at a temperature higher than the inherent resin peak. When this high-temperature peak appears, it is presumed that there are high-melting-point secondary crystal components in the resin. Furthermore, in the DSC curve obtained by heating from 23°C to 200°C at a heating rate of 10°C / min (i.e., the first heating), cooling from 200°C to 23°C at a cooling rate of 10°C / min, and then heating again from 23°C to 200°C at a heating rate of 10°C / min (i.e., the second heating), only the endothermic peak generated by the melting of the inherent crystals of the polypropylene resin constituting the foamed particles is observed. Therefore, the inherent resin peak and the high-temperature peak can be distinguished. The temperature of the resin’s inherent peak sometimes differs slightly between the first and second heating, but the difference is usually within 5°C.
[0086] From the viewpoint of further improving the formability of foamed particles and obtaining molded bodies with better rigidity, the melting heat of the high-temperature peak of the foamed particles is preferably 5 J / g or more and 40 J / g or less, more preferably 7 J / g or more and 30 J / g or less, and even more preferably 10 J / g or more and 20 J / g or less.
[0087] In addition, the total melting heat of the foamed particles is preferably 25 J / g or more and 150 J / g or less, more preferably 35 J / g or more and 100 J / g or less, and even more preferably 50 J / g or more and 90 J / g or less.
[0088] The heat of fusion for each peak in the DSC curve of the foamed particles was determined as follows: First, approximately 2–4 mg of foamed particles were collected from the state-conditioned particle group. Using these foamed particles as test pieces, DSC curves were obtained using a differential scanning calorimeter (DSC) when the test pieces were heated from 23°C to 200°C at a rate of 10°C / min. Alternatively, multiple foamed particles can be used as test pieces. Figure 3 An example of a DSC curve is shown below. Figure 3 As exemplified, the DSC curve shows a resin-specific peak ΔH1 and a high-temperature peak ΔH2 with its apex located on the high-temperature side of the apex of the resin-specific peak ΔH1.
[0089] Next, point α at 80°C on the DSC curve is connected to point β at the melting point T of the foamed particles to obtain a straight line L1. Then, a straight line L2 parallel to the vertical axis of the graph is drawn from point γ on the DSC curve, which corresponds to the valley between the resin's intrinsic peak ΔH1 and the high-temperature peak ΔH2. The point where lines L1 and L2 intersect is designated as δ. Furthermore, point γ can also be referred to as the maximum point existing between the resin's intrinsic peak ΔH1 and the high-temperature peak ΔH2.
[0090] The area of the resin intrinsic peak ΔH1 is the area enclosed by the curve, line segment α-δ, and line segment γ-δ of the resin intrinsic peak ΔH1 portion of the DSC curve, and is used as the melting heat of the resin intrinsic peak.
[0091] The area of the high-temperature peak ΔH2 is the area enclosed by the curve, line segment δ-β, and line segment γ-δ of the high-temperature peak ΔH2 portion of the DSC curve, and is taken as the melting heat of the high-temperature peak (i.e., the heat of the high-temperature peak).
[0092] The area of the total melting peak is the area enclosed by the resin-inherent peak ΔH1 portion of the DSC curve, the high-temperature peak ΔH2 portion, and the line segment α-β (i.e., the straight line L1). This area is taken as the heat of fusion of the total melting peak (total heat of fusion).
[0093] Next, an example of a method for manufacturing foamed granules will be described. Foamed granules are manufactured, for example, by releasing polypropylene resin granules containing a foaming agent, which are dispersed in an aqueous medium within a container, together with the aqueous medium, from the container into a pressure atmosphere lower than the pressure inside the container, thereby causing the resin granules to foam.
[0094] The foamed granules are preferably manufactured by performing a dispersion process, a foaming agent impregnation process, and a foaming process. In the dispersion process, polypropylene resin granules are dispersed in an aqueous medium within a container. In the foaming agent impregnation process, a foaming agent is impregnated into the polypropylene resin granules within the container. In the foaming process, the polypropylene resin granules containing the foaming agent (i.e., foamable resin granules) are released from the container together with the aqueous medium, causing them to foam. Hereinafter, specific embodiments of the manufacturing method will be described.
[0095] The dispersion process is the process of dispersing polypropylene resin particles in an aqueous medium. Polypropylene resin particles are used that have a core layer and a weld layer covering the core layer. Hereinafter, polypropylene resin particles having a core layer and a weld layer will be appropriately referred to as "multilayer resin particles".
[0096] like Figure 2 As exemplified, the multilayer resin particle 10 has a core layer 20 made of polypropylene resin and a weld layer 30 covering the core layer 20. The core layer 20 is a substantially non-foamed layer, and the weld layer 30 is as described above.
[0097] Multilayer resin particles are manufactured, for example, as follows. First, an extrusion apparatus is prepared, comprising two extruders: a core-forming extruder and a weld-layer-forming extruder, and a co-extrusion die connected to each extruder on its downstream side. In the core-forming extruder, a polypropylene resin for core-forming and additives supplied as needed are melt-blended to produce a melt of a resin composition for core-forming. Meanwhile, in the weld-layer-forming extruder, a polyolefin resin for weld-layer-forming, silica particles, a higher fatty acid amide, and additives supplied as needed are melt-blended to produce a melt of a resin composition for weld-layer-forming. Next, the melts are combined within dies located on the downstream side of each extruder to form a sheath-core type composite consisting of a non-foamed core layer and a non-foamed weld layer covering the outer surface of the core layer. In the composite, the core layer is composed of the core-forming resin composition, and the weld layer is composed of the weld-layer-forming resin composition. Furthermore, the composite can be, for example, formed into a filament. The composite is then extruded from an extruder and granulated using various cutting methods, such as a granulator. Cutting methods can be selected from wire cutting, thermal cutting, underwater cutting, etc. This yields multilayer resin particles 10 (see reference) consisting of a core layer 20 and a welded layer 30 covering the core layer 20. Figure 2 ).
[0098] Alternatively, multilayer resin particles can be manufactured, for example, as follows: First, a polypropylene resin for core layer formation and additives as needed are supplied to an extruder for melt mixing to produce a melt of a resin composition for core layer formation. Next, the melt is extruded into, for example, a filament to form a non-foamed core layer (specifically, a non-foamed filament). Then, for example, while extruding the non-foamed core layer from the extruder, it is granulated using various cutting methods such as a granulator to obtain a granular core layer (specifically, resin particles composed of the resin composition for core layer formation). Next, for example, the granular core layer is supplied to a mixing device having a mixing function and a heating function and heated to heat the surface portion of the core layer. Next, a resin composition for weld layer formation, comprising a polyolefin resin for weld layer formation, silica particles, a higher fatty acid amide, and additives as needed, is supplied to the aforementioned mixing device. Then, the heated granular core layer is mixed with the resin composition for forming the weld layer, so that the resin composition for forming the weld layer coats the surface of the core layer. This yields multilayer resin particles. This mixing method is preferred in that it facilitates the integral formation of the weld layer 30 on the surface of the core layer 20 (see reference). Figure 2 ).
[0099] When the multilayer resin particles are cylindrical, the length of the multilayer resin particles in the column direction (length in the extrusion direction) is preferably 0.1 to 3.0 mm, more preferably 0.3 to 1.5 mm. Furthermore, the ratio of [length L in the column direction of the multilayer resin particles / diameter Φ of the multilayer resin particles (maximum length in the direction orthogonal to the extrusion direction)], i.e., the ratio of length L to diameter Φ, L / Φ, is preferably 0.5 to 5.0, more preferably 1.0 to 3.0.
[0100] Furthermore, the average mass of each multilayer resin particle (calculated from the mass of 200 randomly selected particles) is preferably adjusted to 0.1–20 mg, more preferably 0.2–10 mg, even more preferably 0.3–5 mg, and particularly preferably 0.4–2 mg. The mass ratio of the core layer to the welded layer in the multilayer resin particle (specifically, the mass of the core layer : the mass of the welded layer) is preferably 99.5 : 0.5–90 : 10, more preferably 99 : 1–92 : 8, and even more preferably 98 : 2–94 : 6.
[0101] The particle size and average mass of multilayer resin particles can be adjusted, for example, by appropriately changing the extrusion speed, traction speed, and cutting speed when the resin melt is extruded from the extruder to cut the resin melt.
[0102] As a dispersion medium (specifically, a liquid) for dispersing the multilayer resin particles obtained as described above in a closed container, an aqueous medium can be used. The aqueous medium is a dispersion medium (specifically, a liquid) with water as its main component. The proportion of water in the aqueous medium is preferably 60% by mass or more, more preferably 70% by mass or more, and even more preferably 80% by mass or more. Examples of dispersion media other than water in the aqueous medium include ethylene glycol, glycerol, methanol, and ethanol. Water is particularly preferred as the aqueous medium.
[0103] In the dispersion process, inorganic dispersants can be added to the aqueous medium. Alternatively, additives other than inorganic dispersants can be appropriately added to the aqueous medium. Examples of inorganic dispersants include alumina, tricalcium phosphate, magnesium pyrophosphate, zinc oxide, kaolin, and mica microparticles. These inorganic microparticles can be used alone or in combination of two or more. Other additives besides inorganic dispersants include dispersing aids and surfactants. Examples of dispersing aids include aluminum sulfate. Examples of surfactants include anionic surfactants such as sodium alkylbenzene sulfonate, sodium dodecylbenzene sulfonate, and sodium alkane sulfonate. Surfactants can be used alone or in combination of two or more.
[0104] The foaming agent impregnation process is the process of impregnating a multilayer resin particle with a foaming agent. The foaming agent impregnation process can be carried out after the dispersion process described above, or it can be carried out in part or in whole overlapping with the dispersion process.
[0105] In the foaming agent impregnation process, for example, a container containing multilayer resin particles is sealed, and a foaming agent is added to the sealed container, thereby impregnating the multilayer resin particles with the foaming agent. This yields foamable resin particles containing a foaming agent within the multilayer resin particles. For example, a physical foaming agent can be used as the foaming agent. The physical foaming agent can be added to the sealed container at any time before the multilayer resin particles are foamed. Alternatively, during the dispersion process, a solid foaming agent can be added together with the resin particles to an aqueous medium, and then the foaming agent, which has become gaseous through heating or the like, can impregnate the multilayer resin particles. Alternatively, the foaming agent can be injected into a sealed container in parallel with the dispersion process, or after the dispersion process, to impregnate the multilayer resin particles. For example, when using carbon dioxide as a physical foaming agent, during the dispersion process, the solid foaming agent (specifically, in the form of dry ice) can be added to the aqueous medium along with the multilayer resin particles. Alternatively, during or after the dispersion process, gaseous carbon dioxide can be pressurized into a sealed container.
[0106] When impregnating multilayer resin particles with a foaming agent, heating and / or pressurizing the sealed container can promote the impregnation of the foaming agent into the multilayer resin particles.
[0107] Furthermore, in order to adjust the crystal state of the foamed particles, the heating rate of the sealed container can be adjusted in the aforementioned dispersion process and / or foaming agent impregnation process, and the holding temperature and holding time for maintaining the sealed container at a predetermined temperature can also be adjusted. For example, it can be adjusted so that in the DSC curve obtained by differential scanning calorimetry, an endothermic peak (i.e., a high-temperature peak) appears at a position higher than the endothermic peak (i.e., the inherent peak of the resin) of the base resin constituting the core layer of the foamed particles. From the viewpoint of widening the range of molding conditions (specifically, molding temperature and molding pressure) from which a good molded article can be obtained, foamed particles exhibiting a high-temperature peak are preferred. The adjustment for obtaining the aforementioned high-temperature peak is performed, for example, by referring to the method described in Japanese Patent No. 4077745.
[0108] The foaming agent is appropriately selected from common foaming agents used to obtain foamed particles.
[0109] As a blowing agent, a physical blowing agent is preferred. Inorganic and / or organic physical blowing agents can be used. Examples of inorganic physical blowing agents include carbon dioxide, air, nitrogen, helium, argon, and water. Examples of organic physical blowing agents include aliphatic hydrocarbons such as propane, butane, and hexane; alicyclic hydrocarbons such as cyclopentane and cyclohexane; and halogenated hydrocarbons such as chloromethane, chloroethane, dichloromethane, 2,3,3,3-tetrafluoropropene, trans-1,3,3,3-tetrafluoropropene, and trans-1-chloro-3,3,3-trifluoropropene.
[0110] These physical foaming agents can be used alone or in combination of two or more. Among these foaming agents, those primarily composed of inorganic physical foaming agents such as carbon dioxide, nitrogen, or air are preferred, with carbon dioxide being even more preferred. In this specification, "primarily composed of inorganic physical foaming agents" means that the physical foaming agent contains 50 mol% or more of inorganic physical foaming agents. Preferably, the physical foaming agent contains 70 mol% or more of inorganic physical foaming agents, more preferably 90 mol% or more, and even more preferably, the physical foaming agent consists solely of inorganic physical foaming agents.
[0111] The amount of physical foaming agent added is appropriately determined based on the type of base resin constituting the multilayer resin particles, the type of foaming agent, and the bulk density of the desired foamed particles. In particular, the amount of physical foaming agent added can be determined according to the desired bulk density. For example, when carbon dioxide is used as the physical foaming agent, the amount of carbon dioxide added relative to 100 parts by weight is preferably 0.1 parts by weight or more and 30 parts by weight or less, more preferably 0.5 parts by weight or more and 15 parts by weight or less, and even more preferably 1 part by weight or more and 10 parts by weight or less.
[0112] The foaming process involves releasing multilayered resin particles containing a foaming agent (i.e., foamable resin particles) from a container along with an aqueous medium and causing them to foam, thereby obtaining foamed particles. More specifically, the foamable resin particles are foamed by releasing them together with an aqueous medium under a pressure lower than the internal pressure of the container (specifically, a sealed container). According to this foaming method, foamed particles with a low bulk density can be easily obtained.
[0113] The bulk density of foamed particles can be adjusted, for example, by appropriately changing the foaming conditions such as temperature and pressure inside the sealed container when the contents of the sealed container are released during the foaming process.
[0114] Furthermore, when manufacturing foamed particles with lower bulk density, a multi-stage foaming process can be implemented, as shown in the following two-stage foaming process. The two-stage foaming process begins by storing the foamed particles obtained as described above in a pressurized sealed container. Air or other gases are then forced into the sealed container to increase the pressure (i.e., internal pressure) within the bubbles of the foamed particles. Afterward, the foamed particles with increased internal pressure are removed from the sealed container and heated using steam or hot air, thereby causing the particles to foam. This completes the two-stage foaming process. By implementing the two-stage foaming process, foamed particles with lower bulk density (two-stage foamed particles) can be obtained. Furthermore, compared to obtaining foamed particles with lower bulk density through a single foaming process, the method of obtaining foamed particles with lower bulk density through a two-stage foaming process makes it easier to increase the bubble diameter of the final foamed particles. Foamed particle molded bodies manufactured using foamed particles obtained through the two-stage foaming process can further suppress the generation of uneven color tones. Therefore, when manufacturing foamed granules containing colorants, a two-stage foaming process is preferred.
[0115] Foamed particles are used, for example, in the manufacture of molded articles. Molded articles are manufactured, for example, by in-mold forming of foamed particles.
[0116] Specifically, first, foamed particles are filled into a mold having a cavity corresponding to the shape of the desired molded body. Next, the foamed particles filled into the mold are heated using a heating medium such as steam. The foamed particles in the cavity expand due to heating (secondary foaming) and fuse together. Thus, the foamed particles become integrated, resulting in a molded body corresponding to the shape of the cavity.
[0117] Molded bodies made from foamed granules exhibit excellent weldability. Therefore, the mechanical properties inherent in foamed granule molded bodies can be fully realized, making them suitable for various applications such as packaging materials, automotive components, and building materials.
[0118] The density of the molded body is preferably 10 kg / m³. 3 Above and 500kg / m 3 The following applies. In this case, it is possible to achieve both increased rigidity and lightweighting of the molded part. From the viewpoint of improving this effect, a density of 15 kg / m³ is more preferable for the molded part. 3 Above and 100kg / m 3 The following is a further preferred value: 18 kg / m 3 Above and 50kg / m 3 The density of the molded body is calculated by dividing the weight of the molded body by the volume calculated based on the dimensions of the molded body.
[0119] Furthermore, the foamed particles of the present invention can also be manufactured using a different manufacturing method than the manufacturing method of the present invention described above (hereinafter also referred to as the second manufacturing method). The second manufacturing method is as follows: First, resin particles for forming a foamed core layer are prepared, and after foaming to obtain a foamed core layer, a fusion layer is coated on the surface of the foamed core layer, thereby obtaining foamed particles. For example, the foamed particles can be manufactured using the second manufacturing method shown below.
[0120] First, a polypropylene resin for core layer formation and additives as needed are supplied to an extruder and melt-blended to produce a melt of a resin composition for core layer formation. Next, the melt is extruded into, for example, a filament to form a non-foamed core layer (specifically, a non-foamed filament). Then, for example, while extruding the non-foamed core layer from the extruder, it is granulated using various cutting methods such as a granulator to obtain a granular core layer (specifically, resin particles composed of the resin composition for core layer formation). Then, the granular core layer is foamed using a known foaming method to form a foamed particle body (specifically, a foamed core layer). Next, for example, the foamed core layer is supplied to a mixing device having mixing and heating functions and heated to heat the surface portion of the core layer. Next, a resin composition for weld layer formation, comprising a polyolefin resin for weld layer formation, silica particles, a higher fatty acid amide, and additives as needed, is supplied to the aforementioned mixing device. Then, the heated, foamed core layer is mixed with the resin composition for forming the weld layer, so that the resin composition for forming the weld layer coats the surface of the core layer. This yields the foamed particles of the present invention.
[0121]
Example
[0122] <Example 1>
[0123] (Manufacturing of multilayer resin particles)
[0124] A manufacturing apparatus is prepared comprising a core-forming extruder with an inner diameter of 50 mm, a multilayer filament-forming die (co-extrusion die) attached to the downstream side of the core-forming extruder, and a coating layer-forming extruder with an inner diameter of 30 mm. Furthermore, the manufacturing apparatus is configured such that the downstream side of the coating layer-forming extruder is connected to the multilayer filament-forming die, enabling the stacking of molten material for forming each layer within the die and enabling co-extrusion. As the base resin constituting the core layer, a propylene-ethylene random copolymer is used. As the propylene-ethylene random copolymer, a polypropylene-based resin is used with a melting point (i.e., melting peak temperature) of 142°C as determined by JIS K7121:1987 and a melt flow rate of 7 g / 10 min as determined by JIS K7210-1:2014 at 230°C and a load of 2.16 kg.
[0125] A core-forming material (specifically, a base resin, a bubble modifier, carbon black, and a higher fatty acid amide) for forming the core layer in an extruder for core layer formation is supplied to the extruder and melt-blended. This produces a melt containing 0.1% by weight of a bubble modifier (specifically, zinc borate) and 2.7% by weight of carbon black (specifically, furnace black), and a higher fatty acid amide (specifically, erucamide: Kao Corporation "Fatty Acid Amide E") in the amounts shown in Table 1.
[0126] As the base resin constituting the weld layer, a propylene-ethylene-butene random copolymer is used. The propylene-ethylene-butene random copolymer is a polypropylene-based resin with a melting point (i.e., melting peak temperature) of 135°C as determined by JIS K7121:1987 and a melt flow rate of 7 g / 10 min obtained at 230°C and a load of 2.16 kg as determined by JIS K7210-1:2014. The ratio of propylene content, ethylene content, and butene content as copolymer components in this polypropylene-based resin is 94:3.5:2.5 by weight (where represents propylene content: ethylene content: butene content).
[0127] A weld layer forming material (specifically, a base resin, carbon black, silica particles, and a higher fatty acid amide) for forming a weld layer in an extruder for weld layer formation is supplied to the extruder and melt-blended. This produces a melt containing 2.7% by weight of carbon black (specifically, furnace black) and silica particles and a higher fatty acid amide (specifically, erucamide: Kao Corporation's "Fatty Acid Amide E") in the amounts shown in Table 1.
[0128] The molten material for forming each layer is introduced into a multilayer wire forming die, where it flows together and is extruded from the fine orifice of a die mounted on the downstream side of the die to form a composite material (specifically, a multilayer wire) with a two-layer structure (a sheath-core structure consisting of a welded layer and a core layer). The extruded wire is water-cooled and cut using a granulator to obtain multilayer resin granules with an average weight of 1.0 mg each.
[0129] (Manufacturing of foamed granules)
[0130] 1 kg of multilayer resin particles and 3 L of water as an aqueous medium were supplied together into a sealed container with a capacity of 5 L. In addition, 0.3 parts by weight of kaolin as an inorganic dispersant and 0.004 parts by weight of surfactant (trade name: NEOGEN, manufactured by Daiichi Kogyo Pharmaceutical Co., Ltd., sodium dodecylbenzenesulfonate) (the amount of which is the active ingredient) were added to the sealed container, relative to 100 parts by weight of multilayer resin particles.
[0131] Next, carbon dioxide, used as a foaming agent, is pressurized into a sealed container to a gauge pressure of 2.0 MPa (G). Furthermore, the pressure (G) indicated in this specification refers to gauge pressure, i.e., pressure based on atmospheric pressure. Then, while stirring within the sealed container, the temperature is increased to the foaming temperature (specifically, 149.5 °C) at a rate of 2 °C / min, and maintained at this temperature for 15 minutes. This adjusts the foamed particles to exhibit a high-temperature peak in the endothermic curve determined by DSC.
[0132] Then, the contents of the sealed container (specifically, resin particles and water) were released to atmospheric pressure, resulting in a bulk density of 60 kg / m³. 3 The foamed granules (specifically, primary foamed granules). Furthermore, the same process as described above is repeated several times to ensure the quality of the foamed granules for evaluation described later.
[0133] The primary foamed granules obtained as described above were cured for 24 hours at an air temperature of 23°C, a relative humidity of 50%, and a pressure of 1 atm. Then, the cured primary foamed granules were filled into a pressurized, sealed container, and the pressure inside the container was increased from atmospheric pressure to pressurize the granules. This pressurized state was maintained for a predetermined time to increase the pressure within the bubbles. Afterward, the primary foamed granules were removed from the sealed container, resulting in primary foamed granules with an internal bubble pressure of 0.5 MPa(G). These primary foamed granules were then fed into a secondary foaming device. Steam was supplied to this device to foam the primary foamed granules, resulting in a bulk density of 27 kg / m³. 3 Foamed granules. The foamed granules obtained through two-stage foaming were used for the following measurements, manufacturing of foamed granule molded articles, etc. The results are shown in Table 1.
[0134] • Bulk density of foamed particles
[0135] First, the foamed granules to be measured were placed in an environment with an air temperature of 23°C, a relative humidity of 50%, and a temperature of 1 atm for at least 24 hours. Then, a batch of foamed granules weighing W (in grams) was filled into a graduated cylinder, and the bottom of the cylinder was gently tapped on the ground several times to stabilize the filling height. The bulk volume V (in liters) of the foamed granules was read from the graduated cylinder's scale. The weight W of the foamed granules was divided by the bulk volume V (i.e., W / V). By converting the units of the calculated value, the bulk density of the foamed granules (in kg / m³) was obtained. 3 ).
[0136] Total molten heat and high-temperature peak heat
[0137] Approximately 2 mg of foamed particles were collected from the conditioned foamed particle group. Using these foamed particles as test pieces, DSC curves were obtained using a differential scanning calorimeter (specifically, a DSC.Q1000 manufactured by TA Instruments) to heat the test piece from 23°C to 200°C at a heating rate of 10°C / min. The area of all melting peaks in the DSC curves was calculated and taken as the total heat of fusion. Additionally, the area of the high-temperature peaks in the DSC curves was calculated and taken as the high-temperature peak heat. The above measurements were performed on five foamed particles, and the arithmetic mean was used as the results for the total heat of fusion and the high-temperature peak heat.
[0138] (Manufacturing of shaped parts)
[0139] Foamed particles (specifically, secondary foamed particles) are filled into a pressurized sealed container, and the pressure inside the sealed container is increased from atmospheric pressure to pressurize the foamed particles. The pressurized state of the foamed particles is maintained for a predetermined time to increase the pressure within the bubbles of the foamed particles. Then, the foamed particles are removed from the sealed container, resulting in foamed particles with an internal bubble pressure of 0.1 MPa (G). These foamed particles are then filled into a forming mold (specifically, a die) having a forming cavity capable of forming a box-shaped molded body with a length of 200 mm × width of 150 mm × height of 50 mm and a bottom and side wall thickness of 10 mm. Heating is performed using the following method: Preheating (venting process) is performed by supplying steam to the mold with the vent valves on both sides of the mold open. Then, steam is supplied from one side of the mold for heating, and further from the other side for heating. Finally, steam is supplied from both sides of the mold for heating at a forming heating steam pressure of 0.26 MPa (G). After heating, the pressure is released, and the molded body is water-cooled until the surface pressure generated by the foaming force reaches 0.04 MPa(G). The mold is then opened, and the molded body is removed. After curing the molded body in an oven at 80°C for 12 hours, it is slowly cooled to room temperature to obtain a box-shaped molded body with an open top. This molded body has external dimensions of 200 mm in length × 150 mm in width × 50 mm in height, with a bottom and side wall thickness of 10 mm and an open top. When the 200 mm × 150 mm surface is designated as the bottom surface, the shape results in an open top surface.
[0140] Productivity evaluation
[0141] Productivity is evaluated based on the presence or absence of resin residue on the mold during repeated in-mold molding using foamed granules. Specifically, 30 consecutive cycles of in-mold molding are performed using the same mold and under the same molding conditions. The presence or absence of resin residue on the mold after molding is visually observed and evaluated according to the following criteria.
[0142] ○: No attachments were found.
[0143] ×: The condition of the attachment has been confirmed at least partially.
[0144] ·density
[0145] The density is calculated by dividing the weight of the molded body by the volume calculated based on the dimensions of the molded body.
[0146] • Weldability
[0147] The weldability of the molded body is determined based on the proportion of foam particles that undergo material failure among the foam particles exposed at the fracture surface when the molded body breaks. Specifically, firstly, test pieces (length 100mm × width 100mm × thickness: thickness of the molded body) are cut from the bottom wall of the molded body. After making a cut of about 5mm in the thickness direction of each test piece with a cutting tool, the test piece breaks at the cut. Next, the number of foam particles (n) present at the fracture surface of the molded body and the number of foam particles that undergo material failure (b) are measured. The ratio of (b) to (n) (b / n) is expressed as a percentage as the weldability (%), and is evaluated as follows.
[0148] 〇: When the welding rate is above 80%.
[0149] △: The welding rate is less than 80% but more than 40%.
[0150] ×: When the welding rate is less than 40%.
[0151] <Examples 2-4>
[0152] Examples 2-4 are examples in which the content of silica particles and higher fatty acid amides was changed compared to Example 1. Specifically, the content of silica particles and higher fatty acid amides in the weld layer of the resin particles was changed to the content shown in Table 1 to prepare the melt of the resin composition for weld layer formation. Except for this, the foamed particles and molded articles were manufactured in the same manner as in Example 1. The foamed particles and molded articles of Examples 2-4 were evaluated and measured in the same way as in Example 1. The results are shown in Table 1.
[0153] <Example 5>
[0154] This example illustrates a modification of the weight ratio of the welded layer in the foamed granules compared to Example 1. Specifically, the ratio of the core layer to the welded layer was changed by reducing the proportion of the welded layer during the extrusion of multilayer filaments, as shown in Table 1. All other than this, the foamed granules and molded articles were manufactured in the same manner as in Example 1. The foamed granules and molded articles of this example were evaluated and measured in the same way as in Example 1. The results are shown in Table 1.
[0155] <Example 6>
[0156] This example illustrates a modification to the bulk density of the foamed particles compared to Example 1. Specifically, the conditions for secondary foaming in Example 1 were changed to obtain a bulk density of 18 kg / m³. 3 The foamed particles were used to manufacture a molded article in the same manner as in Example 1. The foamed particles and molded articles of this example were evaluated and measured in the same way as in Example 1. The results are shown in Table 1.
[0157] <Comparative Example 1>
[0158] This example demonstrates a weld layer without the inclusion of silica particles and advanced fatty acid amides. Specifically, the weld layer forming material does not contain silica particles or advanced fatty acid amides, except that the foamed particles and molded articles are manufactured in the same manner as in Example 1. The foamed particles and molded articles of this example were evaluated and measured in the same way as in Example 1. The results are shown in Table 2.
[0159] <Comparative Example 2>
[0160] This example demonstrates a modification of the weld layer without the addition of a higher fatty acid amide, and a change in the silica particle content compared to Example 1. Specifically, the weld layer forming material was modified by omitting the higher fatty acid amide and altering the silica particle content in the weld layer to the levels shown in Table 2 to prepare the melt of the resin composition for weld layer formation. Except for this, the foamed particles and molded articles were manufactured in the same manner as in Example 1. The foamed particles and molded articles of this example were evaluated and measured in the same way as in Example 1. The results are shown in Table 2.
[0161] <Comparative Example 3>
[0162] This example demonstrates a modification of the weld layer without the inclusion of silica particles, and a change in the content of higher fatty acid amides compared to Example 1. Specifically, silica particles were omitted from the weld layer forming material, and the content of higher fatty acid amides in the weld layer of the resin particles was changed to the content shown in Table 2 to prepare the melt of the resin composition for weld layer formation. Except for this, the foamed particles and molded articles were manufactured in the same manner as in Example 1. The foamed particles and molded articles of this example were evaluated and measured in the same way as in Example 1. The results are shown in Table 2.
[0163] <Comparative Example 4>
[0164] This example illustrates a modification of the silica particle content compared to Example 1. Specifically, the content of silica particles in the weld layer of the resin particles was changed to the content shown in Table 2 to prepare the melt of the resin composition for weld layer formation. Except for this, the foamed particles and molded articles were manufactured in the same manner as in Example 1. The foamed particles and molded articles of this example were evaluated and measured in the same way as in Example 1. The results are shown in Table 2.
[0165] <Comparative Example 5>
[0166] This example illustrates a modification of the content of higher fatty acid amides compared to Example 1. Specifically, the content of higher fatty acid amides in the molten layer of the resin particles was changed to the content shown in Table 2 to prepare the melt of the resin composition for molten layer formation. Except for this, the foamed particles and molded articles were manufactured in the same manner as in Example 1. The foamed particles and molded articles of this example were evaluated and measured in the same way as in Example 1. The results are shown in Table 2.
[0167] <Comparative Example 6>
[0168] This example is an example in which the content of silica particles and higher fatty acid amides was changed compared to Example 1. Specifically, the content of silica particles and higher fatty acid amides in the weld layer of the resin particles was changed to the content shown in Table 2 to prepare the melt of the resin composition for weld layer formation. Except for this, the foamed particles and molded articles were manufactured in the same manner as in Example 1. The foamed particles and molded articles of this example were evaluated and measured in the same way as in Example 1. The results are shown in Table 2.
[0169]
[0170]
[0171] As can be understood from Table 1, the foamed particles according to Examples 1 to 6 can maintain good weldability between the foamed particles during in-mold molding while suppressing the accumulation of deposits in the molding mold.
[0172] As can be understood from Table 3, in Comparative Example 1, since the foamed particles did not contain silica particles or advanced fatty acid amides in the weld layer, resin deposits were observed in the molding die. Furthermore, in Comparative Example 2, where advanced fatty acid amides were not incorporated into the weld layer of the foamed particles, and in Comparative Example 3, where silica particles were not incorporated into the weld layer of the foamed particles, resin deposits were also observed in the molding die.
[0173] In Comparative Examples 4 and 5, the weight ratio of silica particles to higher fatty acid amides was poorly balanced, resulting in insufficient fusion of the foamed particles in the molded article. In Comparative Example 6, the total amount of silica particles and higher fatty acid amides was excessive, resulting in insufficient fusion of the foamed particles in the molded article.
Claims
1. A polypropylene resin foamed granule, comprising a core layer in a foamed state made of polypropylene resin as the base resin and a welded layer covering the core layer, wherein, The weld layer comprises silica particles and higher fatty acid amides. The higher fatty acid amides include erucamide. The total content of the silica particles and the higher fatty acid amide in the welded layer is 0.05% by weight or more and 1% by weight or less. The weight ratio of the silica particles to the higher fatty acid amide in the fusion layer is 1:0.2 to 1:
5.
2. The polypropylene resin foamed granules according to claim 1, wherein, The content of the silica particles in the fusion layer is more than 0.01% by weight and less than 0.5% by weight.
3. The polypropylene resin foamed granules according to claim 1 or 2, wherein, The weight ratio of silica particles to the higher fatty acid amide in the welded layer is 1:0.8 to 1:
3.
4. The polypropylene resin foamed granules according to claim 1 or 2, wherein, The core layer contains higher fatty acid amides. The content of higher fatty acid amides in the welded layer is greater than that in the core layer.
5. The polypropylene resin foamed granules according to claim 1 or 2, wherein, The substrate resin constituting the fusion layer is at least one selected from propylene-ethylene copolymer, propylene-butene copolymer, and propylene-ethylene-butene copolymer.
6. The polypropylene resin foamed granules according to claim 1 or 2, wherein, The proportion of the welded layer in the polypropylene resin foamed particles is more than 0.5% by weight and less than 10% by weight.
7. The polypropylene resin foamed granules according to claim 1 or 2, wherein, The bulk density of the polypropylene resin foamed particles is 10 kg / m³. 3 Above and 500kg / m 3 the following.
8. A method for manufacturing polypropylene resin foamed granules, comprising: The dispersion process involves dispersing polypropylene resin particles in an aqueous medium within a container. A foaming agent impregnation process, wherein a foaming agent is impregnated in the polypropylene resin particles within the container; and In the foaming process, the polypropylene resin particles containing the foaming agent are released from a container together with an aqueous medium to cause them to foam. The polypropylene resin particles have a core layer made of polypropylene resin as the base resin and a welded layer covering the core layer. The weld layer of the polypropylene resin particles comprises silica particles and higher fatty acid amides. The higher fatty acid amides include erucamide. The total content of silica particles and higher fatty acid amides in the welded layer is more than 0.05% by weight and less than 1% by weight. The weight ratio of silica particles to higher fatty acid amides in the fusion layer is 1:0.2 to 1:5.
Citation Information
Patent Citations
Microporous films from compatibilized polymeric blends
CN101688031A
Polyolefin-based resin expanded beads
CN104710645A