Dry development process of photoresist
By developing metal-side oxygen-based photoresists using plasma etching, the problems of pattern collapse and defects in high aspect ratio feature structures by wet chemical development are solved, achieving efficient and clear pattern transfer and etching selectivity, thus improving the efficiency of EUV lithography.
Patent Information
- Application Number
- CN202180046279.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-06-16
- Filing Date
- 2021-06-23
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2041-06-23
AI Technical Summary
Existing wet chemical development methods are prone to pattern collapse when processing high aspect ratio features and are difficult to completely remove photoresist, resulting in defects and impurities. They are particularly inefficient in EUV lithography.
The metal-side oxygen-based photoresist is developed using a plasma etching process. By bombarding reactive gases in a plasma chamber and reacting them with unexposed areas, volatile byproducts are formed. The unexposed areas are then developed using highly selective etching, avoiding the generation of wet byproducts and removal by mechanical force.
It achieves clear pattern transfer of high aspect ratio feature structures, reduces defect and impurity residue, improves etching uniformity and selectivity, reduces roughness caused by spin coating and drying processes, and provides an all-in-one development and pattern transfer process.
Smart Images

Figure CN115720646B_ABST
Abstract
Description
[0001] Cross-references to related applications
[0002] This application claims priority to U.S. Non-Provisional Application No. 17 / 349,534, filed June 16, 2021, which claims the benefit of U.S. Provisional Application No. 63 / 047,160, filed July 1, 2020, the entire contents of which are incorporated herein by reference. Technical Field
[0003] Several embodiments of this disclosure relate to the field of semiconductor processing, and more particularly to a method of patterning metal oxo photoresist using a non-wet process. Background Technology
[0004] For decades, lithography has been used in the semiconductor industry to create two-dimensional and three-dimensional patterns in microelectronic devices. The lithography process involves spin-coating a film (photoresist), irradiating the film with the selected pattern (exposed) by an energy source, and removing (etching) the exposed (positive-tone) or unexposed (negative-tone) areas of the film by dissolving it in a solvent. Baking is then performed to remove any remaining solvent.
[0005] Photoresist is a radiation-sensitive material that undergoes a chemical transformation in the exposed portions of the film upon irradiation, resulting in a change in solubility between exposed and unexposed areas. This change in solubility allows the exposed or unexposed areas of the photoresist to be removed (developed). As used herein, "development" refers to the process of forming a pattern in the photoresist. Once the photoresist is developed, the pattern can be transferred to the underlying thin film or substrate by etching. After pattern transfer, residual photoresist is removed, and this process is repeated multiple times to obtain two-dimensional and three-dimensional structures for use in microelectronic devices.
[0006] Several important characteristics exist in offset printing. These include sensitivity, resolution, low line-edge roughness (LER), etch resistance, and the ability to form thinner layers. Higher sensitivity requires less energy to alter the solubility of the deposited film, resulting in higher efficiency in offset printing. Resolution and LER determine the narrower the feature structures that can be achieved through offset printing. Pattern transfer requires materials with higher etch resistance to form deep structures. Higher etch resistance also enables thinner films. Thinner films further improve the efficiency of offset printing. Summary of the Invention
[0007] Several embodiments disclosed herein include methods for developing metal-side oxide photoresist using a non-wet process. In one embodiment, the method includes providing a substrate having the metal-side oxide photoresist into a chamber. In one embodiment, the metal-side oxide photoresist includes exposed regions and unexposed regions, wherein the unexposed regions have a higher carbon concentration than the exposed regions. In one embodiment, the method further includes introducing a gas into the chamber, wherein the gas reacts with the unexposed regions to generate volatile byproducts.
[0008] Several embodiments may also include a method for developing a metal-side oxide photoresist, the method comprising providing a substrate having a metal-side oxide photoresist on a substrate surface and exposing the metal-side oxide photoresist to form exposed and unexposed regions. In one embodiment, the unexposed regions contain a higher carbon concentration than the exposed regions. In one embodiment, the method may further include placing the substrate in a plasma chamber, allowing gas to flow into the plasma chamber, and bombarding the plasma chamber with plasma. In one embodiment, the plasma reacts with the unexposed regions to produce volatile byproducts. In one embodiment, the method may further include purging the plasma chamber.
[0009] Several embodiments may also include a method for developing a metal-side oxide photoresist, the method comprising providing a substrate having the metal-side oxide photoresist to a plasma chamber, wherein the metal-side oxide photoresist comprises SnOC. In one embodiment, the metal-side oxide photoresist comprises exposed regions and unexposed regions, and the unexposed regions comprise a higher carbon concentration than the exposed regions. In one embodiment, the method further comprises flowing a gas into the plasma chamber, wherein the gas comprises Cl2 and Ar, and bombarding the plasma chamber with plasma. In one embodiment, the plasma reacts with the unexposed regions to generate volatile byproducts. The method may further comprise purging the plasma chamber. Attached Figure Description
[0010] Figure 1 This is a flowchart describing a process for developing metal-side oxide photoresist using a plasma process, according to one embodiment of the present disclosure.
[0011] Figures 2A to 2D According to one embodiment of this disclosure, a description is provided. Figure 1 The flowchart shows the cross-sectional view of the substrate and photoresist.
[0012] Figure 3 This is one implementation method based on the present disclosure, which can be used for implementation. Figure 1 Cross-sectional view of the processing tools for multiple parts of the process.
[0013] Figure 4The figure shows a block diagram of an exemplary computer system according to one embodiment of the present disclosure. Detailed Implementation
[0014] This document describes a method for patterning metal-side oxide photoresist using a non-wet process. In the following description, numerous specific details, such as the reactive plasma process and material methods used for developing the photoresist, are set forth in order to provide a thorough understanding of various embodiments of this disclosure. It will be apparent to those skilled in the art that various embodiments of this disclosure can be practiced without these specific details. In other instances, well-known aspects, such as integrated circuit fabrication, have not been described in detail to avoid unnecessarily obscuring the various embodiments of this disclosure. Furthermore, it should be understood that the various embodiments illustrated in the accompanying drawings are illustrative and not necessarily drawn to scale.
[0015] To provide context, photoresist systems used in extreme ultraviolet (EUV) lithography are inefficient. In other words, existing photoresist material systems for EUV lithography require high doses to provide the solubility conversion necessary to allow the photoresist material to develop. Due to increased sensitivity to EUV radiation, organic-inorganic hybrid materials (e.g., metal-side-oxygen material systems) have been proposed as material systems for EUV lithography. Such material systems typically contain metals (e.g., tin, hafnium, zirconium, etc.), oxygen, and carbon. In some cases, metal-side-oxygen material systems may further include nitrogen and hydrogen. Metal-side-oxygen organic-inorganic hybrid materials also exhibit lower LER and higher resolution, properties necessary for forming narrow feature structures.
[0016] In metal-side oxide photoresist systems, exposure to EUV radiation leads to carbon removal and crosslinking of the metal oxide network. The difference in carbon percentage and bond strength between exposed and unexposed regions is used as a solubility conversion during development. Specifically, unexposed regions with higher carbon content and weaker bond strength are preferentially etched by the developer solution.
[0017] Metal-side oxide photoresist systems currently use wet chemical development. In other words, after exposure, the unexposed areas of the photoresist are developed using an organic solvent / alkaline solution used in conjunction with a spin-drying process. Post-baking annealing may also be included. However, wet methods can be problematic when handling high aspect ratio features (especially linear or columnar structures) due to the risk of pattern collapse. Furthermore, wet processes may fail to remove all material that should be removed, and film material / byproducts / solvents and similar substances may be trapped in smaller features because mechanical forces are used to remove solvent and dissolved byproducts. Additionally, for smaller and more complex features, solvents (typically larger molecules) have less chance of penetrating all areas of the unexposed resist. This results in partial development of the photoresist and defects. Spin-drying processes can also cause line wobble or even detachment. This limits the thickness and aspect ratio of the photoresist.
[0018] Therefore, various embodiments of this disclosure provide a plasma etching process for developing metal-side oxide photoresists. Specifically, the plasma etching process has the following advantages: 1) eliminates the generation of wet byproducts; 2) reduces waste flow due to the treatment of dry chemicals via a reduction system; 3) provides fewer defects and impurities; 4) improves LER, LWR, and any low-frequency roughness originating from surface tension, capillary forces, and spin-drying processes; 5) provides an all-in-one process for developing photoresists and transferring patterns to the underlying layer; and 6) provides high etch selectivity of unexposed areas of the metal-side oxide photoresist for exposed areas.
[0019] The various embodiments disclosed herein provide a plasma etching process performed after multiple portions of a metal-side oxide photoresist have been exposed using a suitable electromagnetic radiation source (e.g., an EUV source). In one embodiment, a substrate including the exposed metal-side oxide photoresist is placed in a plasma chamber. A gas containing reactive and inert gases flows into the plasma chamber and bombards the plasma. The reactive gas is a gas whose components react with the metal of the metal-side oxide photoresist to form volatile species. For example, reactive gases include Cl2, H2, Br2, HBr, HCl, BCl3, CH4, etc. x Cl y CH4, BBr3 and CH x Br yOne or more of the following. In one particular embodiment, the reactive gas includes HBr, and the inert gas includes Ar. In some embodiments, the gas flows into the chamber without bombarding the plasma (i.e., heat treatment). In many other embodiments, the plasma may be bombarded. In one embodiment, the etch selectivity of the unexposed metal-side oxy-oxide photoresist relative to the exposed metal-side oxy-oxide photoresist may be 10:1 or greater. In one particular embodiment, the etch selectivity is about 12:1. In one embodiment, the pattern of the developed metal-side oxy-oxide photoresist can be transferred to the underlying layer without removing the substrate from the plasma chamber.
[0020] Now for reference Figure 1 The figure, according to one embodiment of the present disclosure, provides a process 120 for developing a metal-side oxygen-based photoresist on a substrate surface. Figures 2A-2D This is a cross-sectional view of the substrate 261 and the metal-side oxygen-based photoresist 262 after each operation in process 120.
[0021] In one embodiment, process 120 may begin with operation 121, which includes providing a substrate with a metal-side oxygen-based photoresist. Figure 2A This is a cross-sectional view of substrate 261, with metal-side oxide photoresist 262 disposed on the surface of substrate 261. In one embodiment, substrate 261 may comprise any substrate material typical of a semiconductor manufacturing environment. For example, substrate 261 may comprise a semiconductor material. Substrate 261 may comprise a semiconductor device or a portion thereof. Examples of such semiconductor devices include, but are not limited to, memory devices or complementary metal-oxide-semiconductor (CMOS) transistors fabricated in a silicon substrate and packaged in a dielectric layer. Substrate 261 may also comprise a plurality of metal interconnects formed in and around the dielectric layer above the device or transistor and may be used to electrically couple components or transistors to form an integrated circuit. In one embodiment, substrate 261 may be a wafer.
[0022] In one embodiment, the metal-side oxide photoresist 262 (also simply referred to as "photoresist 262") can be any metal-side oxide material system. Such a material system typically comprises a metal (e.g., Sn, Hf, Zr, etc.), oxygen, and carbon. In a particular embodiment, photoresist 262 comprises SnOC. In addition to SnOC, several embodiments may include metal-side oxide material systems that further comprise nitrogen and hydrogen.
[0023] The photoresist 262 can be deposited on the surface of the substrate 261 using any suitable deposition process. In one embodiment, a spin-coating process is used to deposit the photoresist on the surface of the substrate 261 using a wet chemical method. In an alternative embodiment, a vapor phase process (i.e., a dry process) is used to deposit the photoresist on the surface of the substrate 261. In a vapor phase process, a metal precursor and an oxidant can be evaporated into a vacuum chamber, wherein the metal precursor and the oxidant react to deposit a metal-side oxygen-based photoresist 262 on the surface of the substrate 261. Such a dry process may be characterized by chemical vapor deposition (CVD), atomic layer deposition (ALD), plasma-enhanced chemical vapor deposition (PE-CVD), or plasma-enhanced atomic layered position (PE-ALD).
[0024] In one embodiment, process 120 may proceed to operation 122, which includes exposing portions of the metal-side oxygen-based photoresist to create exposed and unexposed areas. Figure 2B This is a cross-sectional view describing the exposure process. As shown, electromagnetic radiation 264 passes through mask 263 to expose the exposure area 262. E Unexposed area 262 U The electromagnetic radiation is blocked by mask 263 and thus unaffected by the mask. In one embodiment, the electromagnetic radiation is EUV radiation. When EUV radiation is used, the EUV radiation 264 is reflected away from the mask rather than passing through it. Although EUV radiation is specifically disclosed herein, it should be understood that any suitable wavelength of electromagnetic radiation capable of inducing a solubility conversion in the metal-side oxygen-based photoresist 262 can be used. For example, DUV radiation can be used in some embodiments.
[0025] In one implementation, the solubility conversion is provided by carbon loss in the exposed region and crosslinking of the metal-side oxygen network. Specifically, exposure to electromagnetic radiation causes carbon to escape from exposed region 262. E Removed. Unexposed area 262 U The higher carbon content and more weaker bonds in the material make it easier for unexposed areas to form patterns in subsequent non-wet development processes.
[0026] In one embodiment, process 120 may proceed to operation 123, which includes placing the substrate into a plasma chamber. In one embodiment, the plasma chamber can be any suitable chamber for bombarding plasma under sub-atmospheric pressure conditions. The plasma chamber may also include heating / cooling features to provide thermal control of the plasma process. For example, the chuck on which the substrate 261 is placed may be an actively heated and / or cooled chuck. Additionally, in some embodiments, the walls of the plasma chamber may be actively heated and / or cooled. See below for further details. Figure 3 A more detailed description of a suitable plasma chamber is provided.
[0027] In one embodiment, process 120 may proceed to operations 124 and 125, which include introducing a gas into a plasma chamber and bombarding the plasma within the plasma chamber. In one embodiment, the gas includes a reactive gas and an inert gas. Reactive gases may include Cl2, Br2, HBr, HCl, H2, BCl3, CH4, etc. x Cl y CH4, BBr3, and CH x Br y One or more of the following. In one embodiment, the inert gas may include Ar, N2, or He. In a particular embodiment, the reactive gas includes HBr, and the inert gas includes Ar. In one embodiment, the plasma formed by the reactive gas interacts with the unexposed region 262 of the metal-side oxygen-based photoresist. U The reaction can produce volatile byproducts. For example, metal M (e.g., tin) and Cl will react to form volatile MCl4. Figure 2C The image shows area 262 in the unexposed region. U Examples of photoresist developed after conversion into volatile byproducts. It should be understood that plasma bombardment is optional. In other words, in some embodiments, a non-wet process may include the influx of reactive gas into the chamber without plasma bombardment. This process can be considered a thermal process, as opposed to a plasma process. In this case, the reactive gas can directly react with the unexposed areas 262 of the metal-side oxygen-based photoresist. U The reaction does not require the ionization of reactive gases.
[0028] In one embodiment, the ratio of the inert gas flow rate to the reactive gas flow rate is between 0:1 and 50:1. For example, the inert gas flow rate could be 300 sccm, while the reactive gas flow rate could be 50 sccm. The diluted chemicals slow down the etching rate and improve etching uniformity. Uniformity is improved because the inert gas helps to distribute the reactive gas evenly throughout the plasma chamber. Furthermore, it has generally been shown that, relative to the exposed area 262E The increased flow rate of reactive gases provided unexposed areas 262 U The etching increases. In one embodiment, the pressure can be between about 1 millitor and about 100 millitors. In a particular embodiment, the pressure can be between about 5 millitors and about 20 millitors. In yet another embodiment, the pressure can be between about 1 millitor and about 10 tors.
[0029] In one embodiment, substrate 261 may have a controlled temperature during operations 124 and 125. For example, the temperature may vary between about 0°C and about 500°C. In a particular embodiment, the temperature may vary between about 50°C and about 150°C. Generally, lower temperatures (e.g., less than 500°C) are advantageous because the metal-side oxygen-based photoresist does not thermally decompose at lower temperatures. In yet another embodiment, the temperature may be less than about 200°C. For example, the temperature may be between about 40°C and about 100°C.
[0030] In one embodiment, the radio frequency (RF) power of the plasma etching process can be controlled. Generally, lower RF power improves etching selectivity. In one embodiment, the source power can be between about 200 W and about 1200 W. In a particular embodiment, the source power can be about 400 W. In one embodiment, the bias power can be between about 0 W and about 200 W. In a particular embodiment, the bias power can be about 50 W. It has been shown that increasing the bias power to about 100 watts provides unexposed regions 262 U Relative to exposed area 262 E Enhanced etch selectivity
[0031] In one embodiment, operation 125 can be implemented using a pulsed bias. The duty cycle of the pulse can be between 0% and 100%. In a particular embodiment, the duty cycle is approximately 50%. This duty cycle allows time to remove byproducts and provides less ion bombardment. Therefore, the unexposed region 262 U Relative to exposed area 262 E The etching selectivity is improved.
[0032] In one implementation, operation 125 can be performed for any desired duration. A longer time period allows for more unexposed areas 262. U Removed. In one embodiment, operation 125 may have a duration between about 5 seconds and about 120 seconds. In a particular embodiment, operation 125 may have a duration of about 15 seconds.
[0033] By altering various parameters of the plasma development process, such as those mentioned above, unexposed regions 262 of the metal-side oxygen-based photoresist are provided. UExposed area 262 relative to the metal-side oxygen-based photoresist E The photoresist exhibits high etch selectivity. For example, the etch selectivity can be about 10:1 or greater. In one particular embodiment, the etch selectivity can be about 12:1. High etch selectivity provides several benefits. One benefit is that the thickness of the photoresist can be reduced. This allows for complete development of the photoresist using a smaller dose of electromagnetic radiation.
[0034] In one embodiment, process 120 may proceed to operation 126, which includes purging the plasma chamber. Purging the plasma chamber removes byproducts from the reaction in operation 125. In one embodiment, a single cleaning may be performed after etching is completed in operation 125. In several alternative embodiments, operations 124 / 125 and 126 may define a cycle including an etching pulse and a subsequent cleaning. In several such embodiments, in order to remove the unexposed areas 262 of the photoresist... U This can be repeated multiple times.
[0035] The various embodiments disclosed herein provide additional benefits implemented within a plasma chamber. This is particularly advantageous when subsequent patterning of the substrate 261 is performed using plasma etching. Specifically, the substrate 261 does not need to be removed from the plasma chamber after the photoresist development process. That is, an all-in-one (i.e., all-in-one chamber) solution for pattern development and pattern transfer to the underlying layer is provided.
[0036] In one embodiment, process 120 may continue with optional operation 127, which includes etching substrate 261. Figure 2D It is the exposed area 262 of the metal-side oxygen-based photoresist. E The figure shows a cross-sectional view of substrate 261 after the pattern has been transferred into it. As shown, the pattern transfer can result in the formation of trenches 265 in substrate 261. In one embodiment, the etching of substrate 261 can be achieved using a plasma etching process. The plasma etching process can be performed in the same chamber used for developing metal-side oxide photoresist.
[0037] Figure 3 This is a schematic diagram of a plasma chamber according to several embodiments of the present disclosure, configured to perform plasma-based development of metal-side oxide photoresist. The plasma chamber 300 includes a grounded chamber 305. A substrate 310 is loaded through an opening 315 and clamped to a temperature-controlled chuck 320.
[0038] Processing gases are supplied from gas source 344 and flow into chamber 305 via respective mass flow controllers 349. In some embodiments, gas distribution plate 335 provides distribution of processing gases 344, such as Cl2, Br2, H2, HCl, HBr, and / or inert gases. Chamber 305 is emptied by exhaust pump 355.
[0039] When radio frequency power is applied during processing on substrate 310, plasma is formed in a chamber processing region above substrate 310. A bias power radio frequency generator 325 is coupled to a temperature-controlled chuck 320. If needed, the bias power radio frequency generator 325 provides bias power to excite the plasma. The bias power radio frequency generator 325 may have a low frequency, for example, between about 2 MHz and 60 MHz, and in one particular embodiment, is in the 13.56 MHz band. In some embodiments, the plasma chamber 300 includes a third bias power radio frequency generator 326 with a frequency in the about 2 MHz band, connected to the same radio frequency matching unit 327 as the bias power radio frequency generator 325. A source power radio frequency generator 330 is coupled via a matching unit (not shown) to a plasma generating element (e.g., a gas distribution plate 335) to provide source power to excite the plasma. The source RF generator 330 may have a frequency, for example, between 100 and 180 MHz, and in one particular embodiment, it is in the 162 MHz band. Because the substrate diameter varies over time, from 150 mm, 200 mm, 300 mm, etc., it is common in the art to normalize the power supply and bias power of the plasma etching system to the substrate area.
[0040] The plasma chamber 300 is controlled by a controller 370. The controller 370 may include a central processing unit 372, a memory 373, and an input / output interface 374. The central processing unit 372 may perform processing operations within the plasma chamber 300 according to instructions stored in the memory 373. For example, the controller 370 may execute one or more processes in the plasma chamber, such as a portion of process 120 described above.
[0041] Figure 4The illustration shows a graphical representation of a machine in an exemplary form of a computer system 400, which is executable with a set of instructions to cause the machine to perform any or more methods described herein. In several alternative embodiments, the machine may be connected (e.g., networked) to other machines in a local area network (LAN), an internal network, an external network, or the Internet. The machine may operate as a server or client machine in a client-server network environment, or as a peer machine in a peer (or distributed) network environment. The machine may be a personal computer (PC), tablet computer, set-top box (STB), personal digital assistant (PDA), cellular phone, network device, server, network router, switch, or bridge, or any machine capable of executing a set of instructions (sequentially or otherwise) specifying the actions to be taken by the machine. Furthermore, although only a single machine is shown, the term "machine" should also be understood to include any collection of machines (e.g., computers) that individually or jointly execute a set (or more) of instructions to perform any or more methods described herein.
[0042] An exemplary computer system 400 includes a processor 402, a main memory 404 (e.g., read-only memory (ROM), flash memory, dynamic random access memory (DRAM), such as synchronous dynamic random access memory (SDRAM) or Rambus dynamic random access memory (RDRAM), etc.), a static memory 406 (e.g., flash memory, static random access memory (SRAM), magnetoresistive random access memory (MRAM), etc.), and a secondary memory 418 (e.g., a data storage device), all of which communicate with each other via a bus 430.
[0043] Processor 402 represents one or more general-purpose processing devices, such as microprocessors, central processing units, or similar devices. More specifically, processor 402 may be a complex instruction set computing (CISC) microprocessor, a reduced instruction set computing (RISC) microprocessor, a very long instruction word (VLIW) microprocessor, a processor implementing other instruction sets, or a processor implementing combinations of instruction sets. Processor 402 may also be one or more special-purpose processing devices, such as application-specific integrated circuits (ASICs), field-programmable gate arrays (FPGAs), digital signal processors (DSPs), network processors, or similar devices. Processor 402 is configured to execute processing logic 426 for performing the operations described herein.
[0044] The computer system 400 may further include a network interface device 408. The computer system 400 may also include a video display unit 410 (e.g., a liquid crystal display (LCD), a light-emitting diode display (LED), or a cathode ray tube (CRT)), an alphanumeric input device 412 (e.g., a keyboard), a cursor control device 414 (e.g., a mouse), and a signal generation device 416 (e.g., a speaker).
[0045] Secondary memory 418 may include a machine-accessible storage medium (or more specifically, a computer-readable storage medium) 432, on which one or more sets of instructions (e.g., software 422) are stored to implement any one or more methods or functions described herein. Software 422 may also reside wholly or at least partially within main memory 404 and / or processor 402 during execution of computer system 400, which also constitute machine-readable storage media. Software 422 may further be transmitted or received on network 420 via network interface device 408.
[0046] Although machine-accessible storage medium 432 is shown as a single medium in the exemplary embodiment, the term "machine-readable storage medium" should be understood to include a single medium or multiple media (e.g., a centralized or distributed database, and / or associated caches and servers) that store one or more sets of instructions. The term "machine-readable storage medium" should also be understood to include any medium capable of storing or encoding a set of machine-executable instructions and enabling the machine to perform any one or more of the contents of this disclosure. Therefore, the term "machine-readable storage medium" should be understood to include, but is not limited to, solid-state storage and optical and magnetic media.
[0047] According to embodiments of this disclosure, a machine-accessible storage medium has instructions stored thereon that cause a data processing system to perform a method of developing a metal-side oxide photoresist on a substrate using a plasma process. The method includes exposing the metal-side oxide photoresist to provide exposed and unexposed regions, and placing the substrate with the exposed photoresist into a plasma chamber. In one embodiment, a gas flows into the plasma chamber and bombards the plasma. The gas may include reactive gases and inert gases. In one embodiment, the plasma reacts with the unexposed regions of the photoresist to convert the unexposed regions of the photoresist into volatile byproducts that can be removed from the plasma chamber. For example, the reactive gas may include one or more of Cl2, Br2, HBr, HCl, and H2.
[0048] Therefore, a method for forming developing metal-side oxide photoresist using plasma technology has been disclosed.
Claims
1. A method for developing metal-side oxide photoresist, comprising the following steps: A substrate having the metal-side oxide photoresist is provided into a chamber, wherein the metal-side oxide photoresist includes exposed regions and unexposed regions, and wherein the unexposed regions have a higher carbon concentration than the exposed regions; and A gas is introduced into the chamber for a duration between 5 and 120 seconds, wherein the gas reacts with the unexposed area with a selectivity of 10:1 or higher relative to the exposed area to produce volatile byproducts, and wherein the gas contains a reactive gas, which includes one or more of Br2 or HCl, the gas having a pressure between 5 and 20 mTorr in the chamber, the substrate having a temperature between 40°C and 100°C, wherein the chamber is powered by a source power between 200 W and 1200 W, and the power bias is between 0 W and 200 W.
2. The method of claim 1, further comprising the following steps: The plasma is bombarded within the chamber.
3. The method of claim 1, wherein the gas further comprises an inert gas.
4. The method of claim 3, wherein the ratio of the flow rate of the inert gas to the flow rate of the reactive gas is between 0:1 and 50:
1.
5. The method of claim 1, wherein the reaction of the gas with the unexposed area is achieved by plasma-free heat treatment.
6. The method of claim 1, wherein the power bias is pulsed, wherein the pulsed voltage has a duty cycle between 0% and 100%.
7. The method of claim 1, wherein the metal-side oxygen-based photoresist comprises SnOC.
8. The method of claim 1, wherein the exposed region comprises a cross-linked metal oxide network, and wherein the unexposed region comprises a metal oxide cluster.
9. The method of claim 1, wherein the reactive gas is Br2.
10. The method of claim 1, wherein the reactive gas is HCl.
11. A method for developing metal-side oxide photoresist, comprising the following steps: A substrate is provided, the substrate having the metal-side oxygen-based photoresist on the surface of the substrate; The metal-side oxygen-based photoresist is exposed to form exposed and unexposed regions, wherein the unexposed regions contain a higher carbon concentration than the exposed regions; The substrate is placed in the plasma chamber; A gas is introduced into the plasma chamber for a duration between 5 and 120 seconds, wherein the gas reacts with the unexposed area with a selectivity of 10:1 or higher relative to the exposed area to produce volatile byproducts, and wherein the gas contains a reactive gas, the reactive gas containing one or more of Br2 or HCl, the gas having a pressure between 5 mTorr and 20 mTorr in the plasma chamber, the substrate having a temperature between 40°C and 100°C, wherein the plasma chamber is powered by a source power between 200 W and 1200 W, and the power bias is between 0 W and 200 W; Plasma is bombarded in the plasma chamber, wherein the plasma reacts with the unexposed area to produce volatile byproducts; and Purify the plasma chamber.
12. The method of claim 11, wherein the gas further comprises an inert gas.
13. The method of claim 12, wherein the ratio of the flow rate of the inert gas to the flow rate of the reactive gas is between 0:1 and 50:
1.
14. The method of claim 11, wherein the metal-side oxygen-based photoresist comprises SnOC.
15. The method of claim 11, wherein the step of exposing the metal-side oxygen-based photoresist comprises the following steps: The metal-side oxygen-based photoresist is exposed to far-ultraviolet (EUV) radiation.
16. The method of claim 11, wherein the reactive gas is Br2.
17. The method of claim 11, wherein the reactive gas is HCl.
Citation Information
Patent Citations
Photoresist development with halide chemistries
CN114026501A
Dry development of resists
WO2020132281A1