Semiconductor memory device and method of manufacturing the same

By using a nitrogen-containing silicon oxide film as an intermediate film in a three-dimensional memory cell array, the problem of upper array non-flatness transfer caused by lower array non-flatness is solved, memory cell failure and semiconductor layer thinning are prevented, and the reliability of memory cells is improved.

CN115776822BActive Publication Date: 2026-11-20KIOXIA CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202210100215.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-09-06
Filing Date
2022-01-27
Publication Date
2026-11-20
Estimated Expiration
2042-01-27

AI Technical Summary

Technical Problem

In a three-dimensional memory cell array, the unevenness of the upper array due to the unevenness of the lower array surface can lead to memory cell failures and thinning of the channel semiconductor layer, potentially causing electrical disconnection problems.

Method used

An intermediate film is provided between the first stack and the second stack. The intermediate film is composed of a nitrogen-containing silicon oxide film to prevent the semiconductor body from being cut and to improve the flatness and thickness uniformity of the memory cells.

Benefits of technology

By setting an intermediate film, memory cell failures are prevented, the thickness of the semiconductor body is maintained, electrical connection problems caused by cutting are avoided, and the reliability of the memory cell is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115776822B_ABST
    Figure CN115776822B_ABST
Patent Text Reader

Abstract

Embodiments of the present invention relate to a semiconductor memory device and a manufacturing method thereof. A semiconductor memory device according to an embodiment of the present invention includes a first stack including a plurality of first electrode films stacked in a first direction and electrically isolated from each other, and a second stack disposed above the first stack and including a plurality of second electrode films stacked in the first direction and electrically isolated from each other. An intermediate film is disposed between the first stack and the second stack. A pillar portion includes a semiconductor layer disposed to extend in the first direction in the first stack and the second stack and in the intermediate film, and forms a memory cell at an intersection of the semiconductor layer and at least one of the first electrode films and at an intersection of the semiconductor layer and at least one of the second electrode films. The intermediate film includes a silicon oxide film containing nitrogen.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Cross-reference of related applications

[0002] This application is based on and claims the priority of Japanese Patent Application No. 2021-144550, filed on September 6, 2021, the entire contents of which are incorporated herein by reference. Technical Field

[0003] Embodiments of the present invention relate to a semiconductor memory device and a method for manufacturing the same. Background Technology

[0004] For example, semiconductor devices such as NAND flash memory can include a three-dimensional memory cell array with multiple memory cells arranged in three dimensions. The number of stacked layers in a three-dimensional memory cell array is increasing every year, and the memory cell array can be formed as a separate array including a lower array and a upper array.

[0005] In the case where a memory cell array is formed as a lower array and an upper array, if the surface flatness of the lower array is poor, the unevenness of the lower array surface is transferred to the multilayer film in the upper array. This transfer of unevenness can lead to failure of the memory cells in the upper array.

[0006] Furthermore, due to the uneven shape of the middle portion (junction portion) between the lower and upper arrays, the channel semiconductor layer in the memory hole may become thinner, thus causing electrical disconnection. Summary of the Invention

[0007] A semiconductor memory device according to an embodiment of the present invention includes: a first stack including a plurality of first electrode films stacked and electrically isolated from each other in a first direction; and a second stack disposed above the first stack and including a plurality of second electrode films stacked and electrically isolated from each other in the first direction. An intermediate film is disposed between the first stack and the second stack. A pillar portion includes a semiconductor layer configured to extend in the first stack and the second stack and in the intermediate film in the first direction, and memory cells are formed at intersections of the semiconductor layer with at least one of the first electrode films and at intersections of the semiconductor layer with at least one of the second electrode films. The intermediate film includes a nitrogen-containing silicon oxide film.

[0008] According to the embodiments described, it is possible to prevent memory cell failures caused by dicing of the semiconductor body. Attached Figure Description

[0009] Figure 1A This is a schematic perspective view of an example of a semiconductor memory device according to the first embodiment;

[0010] Figure 1B yes Figure 1A A schematic plan view of the stacking in the middle;

[0011] Figure 2A This is a schematic cross-sectional view of an example of a memory cell with a three-dimensional configuration;

[0012] Figure 2B This is a schematic cross-sectional view of an example of a memory cell with a three-dimensional configuration;

[0013] Figure 3 This is a schematic plan view of an example of a semiconductor memory device according to the first embodiment;

[0014] Figure 4 It is a cross-sectional view illustrating an example of a more detailed configuration of the stack;

[0015] Figure 5 It is a cross-sectional view illustrating an example of the configuration of the joint between the upper and lower arrays;

[0016] Figure 6 This is a cross-sectional view illustrating an example of a method for manufacturing a semiconductor memory device according to the first embodiment;

[0017] Figure 7 This is a diagram illustrating the compliance of semiconductor memory devices. Figure 6 A cross-sectional view of an example of a manufacturing method illustrated in the figure;

[0018] Figure 8 This is a diagram illustrating the compliance of semiconductor memory devices. Figure 7 A cross-sectional view of an example of a manufacturing method illustrated in the figure;

[0019] Figure 9 This is a diagram illustrating the compliance of semiconductor memory devices. Figure 8 A cross-sectional view of an example of a manufacturing method illustrated in the figure;

[0020] Figure 10 This is a diagram illustrating the compliance of semiconductor memory devices. Figure 9 A cross-sectional view of an example of a manufacturing method illustrated in the figure;

[0021] Figure 11 This is a diagram illustrating the compliance of semiconductor memory devices. Figure 10 A cross-sectional view of an example of a manufacturing method illustrated in the figure;

[0022] Figure 12 This is a diagram illustrating the compliance of semiconductor memory devices. Figure 11 A cross-sectional view of an example of a manufacturing method illustrated in the figure;

[0023] Figure 13 This is a diagram illustrating the compliance of semiconductor memory devices. Figure 12 A cross-sectional view of an example of a manufacturing method illustrated in the figure;

[0024] Figure 14 This is a diagram illustrating the compliance of semiconductor memory devices. Figure 13 A cross-sectional view of an example of a manufacturing method illustrated in the figure;

[0025] Figure 15 This is a diagram illustrating the compliance of semiconductor memory devices. Figure 14 A cross-sectional view of an example of a manufacturing method illustrated in the figure;

[0026] Figure 16 It was by Figure 13 A cross-sectional view of the area enclosed by the dashed box in the image;

[0027] Figure 17 This is a cross-sectional view illustrating an example of the configuration of the joint portion according to the second embodiment; and

[0028] Figure 18 This is a cross-sectional view illustrating an example of a method for manufacturing a semiconductor memory device according to the second embodiment. Detailed Implementation

[0029] Various embodiments will now be explained with reference to the accompanying drawings. The invention is not limited to the described embodiments. In this specification and the drawings, elements identical to those described in the foregoing drawings are denoted by similar reference numerals, and detailed explanations of these reference numerals are omitted where appropriate.

[0030] (First Embodiment)

[0031] Figure 1A This is a schematic perspective view of an example of a semiconductor memory device 100a according to the first embodiment. Figure 1B yes Figure 1A A schematic plan view of stack 2. In this specification, the stacking direction of stack 2 is assumed to be the Z direction. For example, a direction that intersects the Z direction at a right angle is assumed to be the Y direction. For example, a direction that intersects both the Z and Y directions at a right angle is assumed to be the X direction. Figure 2A and 2B This is a schematic cross-sectional view of an example of a memory cell with a three-dimensional configuration. Figure 3 This is a schematic plan view of an example of a semiconductor memory device according to the first embodiment.

[0032] like Figure 1AAs illustrated in the figure, the semiconductor memory device 100a according to the first embodiment is a non-volatile memory containing memory cells with a three-dimensional arrangement.

[0033] Semiconductor memory device 100a includes a substrate portion 1, a stack 2, and a deep trench ST. Figure 1B 3) Plate-like portion in the middle, shallow narrow groove SHE ( Figure 1B The plate-like portion 4) and multiple columnar portions CL.

[0034] The substrate portion 1 includes a substrate 10, an interlayer dielectric film 11, a conductive layer 12, and a semiconductor portion 13. The interlayer dielectric film 11 is disposed on the substrate 10. The conductive layer 12 is disposed on the interlayer dielectric film 11. The semiconductor portion 13 is disposed on the conductive layer 12.

[0035] Substrate 10 is a semiconductor substrate, for example, a silicon substrate. The conductivity type of silicon (Si) is, for example, p-type. For example, a device isolation region 10i is disposed in the surface region of substrate 10. For example, the device isolation region 10i is an insulating region containing silicon oxide (SiO2) and defines an active region AA in the surface region of substrate 10. The source and drain regions of transistor Tr are disposed in the active region AA. Transistor Tr configures peripheral circuitry (CMOS (Complementary Metal-Oxide-Semiconductor) circuitry) for non-volatile memory. The CMOS circuitry is disposed below the built-in source layer BSL and on substrate 10. For example, an interlayer dielectric film 11 contains silicon oxide and covers transistor Tr. A wire 11a is disposed in the interlayer dielectric film 11. A portion of wire 11a is electrically connected to transistor Tr. Conductive layer 12 contains doped polysilicon or a conductive metal such as tungsten (W). For example, a semiconductor portion 13 contains silicon. For example, the conductivity type of silicon is n-type. Semiconductor portion 13 may be formed of multiple layers, and a portion thereof may contain undoped silicon. In addition, the conductive layer 12 or the semiconductor portion 13 may be omitted.

[0036] The conductive layer 12 and the semiconductor portion 13 serve as a memory cell array. Figure 1B The common source line is 2m. The conductive layer 12 and the semiconductor portion 13 are electrically connected to each other as a single layer and are also collectively referred to as the "built-in source layer BSL".

[0037] Stack 2 is disposed above substrate 10 and positioned in the Z direction relative to conductive layer 12 and semiconductor portion 13 (built-in source layer BSL). Stack 2 is configured with a plurality of electrode films 21 and a plurality of insulating films 22 alternately stacked in the Z direction. For example, electrode films 21 contain conductive metals such as tungsten. For example, insulating films 22 contain silicon oxide. Insulating films 22 insulate electrode films 21 from each other. The number of stacks of each of electrode films 21 and insulating films 22 can be any number. For example, insulating films 22 can be air gaps. For example, insulating film 2g is disposed between stack 2 and semiconductor portion 13. For example, insulating film 2g contains silicon oxide. Insulating film 2g may contain a high-dielectric material having a higher relative permittivity than silicon oxide. For example, the high-dielectric material can be a metal oxide.

[0038] The electrode film 21 includes at least one source-side selected gate (SGS), a plurality of word lines (WL), and at least one drain-side selected gate (SGD). The source-side selected gate (SGS) is the gate electrode of a source-side selected transistor (STS). The word lines (WL) serve as the gate electrodes of memory cells (MC). The drain-side selected gate (SGD) is the gate electrode of a drain-side selected transistor (STD). The source-side selected gate (SGS) is disposed in the lower region of the stack 2. The drain-side selected gate (SGD) is disposed in the upper region of the stack 2. The lower region is the region of the stack 2 closer to the substrate portion 1, and the upper region is the region of the stack 2 farther from the substrate portion 1. The word lines (WL) are disposed between the source-side selected gate (SGS) and the drain-side selected gate (SGD).

[0039] For example, the thickness in the Z-direction of one of the insulating films 22 that insulates the source-side select gate SGS from the word line WL may be greater than the thickness in the Z-direction of the insulating film 22 that insulates the word lines WL from each other. Furthermore, a cover insulating film (not illustrated) may be disposed on the uppermost insulating film 22 furthest from the substrate portion 1. For example, the cover insulating film contains silicon oxide.

[0040] Semiconductor memory device 100a includes a plurality of memory cells MC connected in series between a source-side select transistor STS and a drain-side select transistor STD. The configuration in which the source-side select transistor STS, memory cells MC, and drain-side select transistor STD are connected in series is referred to as a "memory string" or "NAND string". For example, a memory string is configured to correspond to each pillar portion CL and is connected to a bit line BL via a contact Cb. The bit line BL is positioned above the stack 2 and extends in the Y direction.

[0041] A deep slot ST and a shallow slot SHE are disposed in stack 2. The deep slot ST extends in the X direction and is disposed in stack 2 to penetrate stack 2 from the top end of stack 2 to the base portion 1. A plate-shaped portion 3 is a conductor disposed in the deep slot ST. The plate-shaped portion 3 is formed of a conductive film electrically insulating from stack 2 through an insulating film (not illustrated) disposed on the inner wall of the deep slot ST, embedded in the deep slot ST, and electrically connected to the built-in source layer BSL. The plate-shaped portion 3 may be filled with an insulating material such as silicon oxide. Meanwhile, the shallow slot SHE extends in the X direction and is disposed from the top end of stack 2 to the middle of stack 2. The shallow slot SHE penetrates the upper region of the drain-side select gate SGD disposed in stack 2. For example, a plate-shaped portion 4 is disposed in the shallow slot SHE ( Figure 1B In, for example, plate-shaped portion 4 is made of silicon dioxide.

[0042] like Figure 1B As illustrated in the diagram, stack 2 includes stepped regions 2s and memory cell array 2m. The stepped regions 2s are located at the edges of stack 2. The memory cell array 2m is sandwiched between or surrounded by the stepped regions 2s. Deep slots ST are configured to extend through the memory cell array 2m from one end of the stepped regions 2s to the other end of the stack 2 through the stepped regions 2s. Shallow slots SHE are located at least within the memory cell array 2m.

[0043] like Figure 3 The diagram illustrates that the memory cell array 2m includes cell regions (cells) and tapered regions (taperes) arranged in the X direction. A stepped region 2s includes a stepped region (step) at one end in the X direction. For example, the tapered region is positioned between the cell regions and the stepped region. The tapered region can be positioned between the cell regions, although... Figure 3 The diagram is not provided. The stepped region is the area in which multiple conductors 37a are disposed. The tapered region is the area in which conductors 37b and 37c are disposed. For example, conductors 37a to 37c extend in the Z direction. For example, each of conductors 37a is electrically connected to electrode film 21. For example, conductor 37b is electrically connected to the built-in source layer BSL. For example, conductor 37c is electrically connected to conductor 11a.

[0044] Stack 2 sandwiched in Figure 1BThe portion between the two plate-shaped portions 3 illustrated in the diagram is called a "block". For example, a block is the smallest unit used for erasing data. Plate-shaped portions 4 are disposed within the block. The stack 2 between plate-shaped portions 3 and 4 is called a "finger". The drain-side select gate (SGD) is divided for each finger. Therefore, during data writing and reading, it is possible to place a finger within a block in a selected state using the drain-side select gate (SGD).

[0045] like Figure 2A As illustrated in the diagram, each of the pillar portions CL is disposed in a memory via MH formed in the stack 2. Each pillar portion CL penetrates the stack 2 from the top end of the stack 2 in the Z direction and is disposed in the stack 2 and the built-in source layer BSL. Each pillar portion CL includes a semiconductor body 210, a memory film 220, and a core layer 230. The pillar portion CL includes a core layer 230 disposed at its center, a semiconductor body 210 disposed around the core layer 230, and a memory film 220 disposed around the semiconductor body 210. The semiconductor body 210 is electrically connected to the built-in source layer BSL. The memory film 220, as a charge storage component, has a charge trapping portion between the semiconductor body 210 and the electrode film 21. The pillar portions C1, selected one by one from the corresponding fingers, are collectively connected to a bit line BL via a contact Cb. For example ( Figure 3 Each of the pillar portions CL is disposed in a cell region (cell). In each of the pillar portions CL, a memory cell MC is formed at each of the intersection points of the word line WL (excluding the drain-side selected gate SGD and the source-side selected gate SGS) in the semiconductor body 210 extending in the Z direction and the electrode film 21 in the stack 2. A drain-side selected transistor STD and a source-side selected transistor STS are formed at the intersection points of the semiconductor body 210 and the drain-side selected gate SGD and the source-side selected gate SGS, respectively.

[0046] For example, the shape of the memory hole MH in the XY plane is circular or elliptical, such as... Figure 2B The diagram illustrates this. A block insulating film 221a, configured to cover a portion of the memory film 220, may be disposed between the electrode film 21 and the insulating film 22. For example, the block insulating film 221a is a silicon oxide film or a metal oxide film. An example of a metal oxide is aluminum oxide. A barrier film 221b may be disposed between the electrode film 21 and the insulating film 22, and between the electrode film 21 and the memory film 220. For example, in the case where the electrode film 21 is made of tungsten, titanium nitride, for example, is chosen as the barrier film 221b. The block insulating film 221a prevents charge from tunneling backward from the electrode film 21 towards the memory film 220. The barrier film 221b improves the adhesion between the electrode film 21 and the block insulating film 221a.

[0047] For example, the semiconductor body 210 is tubular in shape with a bottom. For example, the semiconductor body 210 contains silicon. For example, the silicon contained here is polycrystalline silicon obtained by crystallizing amorphous silicon. For example, the semiconductor body 210 is made of undoped silicon. The semiconductor body 210 may be made of p-type silicon. The semiconductor body 210 serves as the channel for each of the drain-side select transistor (STD), the memory cell (MC), and the source-side select transistor (STS).

[0048] In addition to the block insulating film 221a, a portion of the memory film 220 is disposed between the inner wall of the memory via MH and the semiconductor body 210. For example, the memory film 220 is tubular in shape. The memory film 220 is removed from the region surrounding the semiconductor body 210 in a portion of the semiconductor portion 13 connected to the built-in source layer BSL. Each memory cell MC contains a storage region between the semiconductor body 210 and the electrode film 21, which acts as a word line WL, and is stacked in the Z direction. For example, the memory film 220 includes a covering insulating film 221, a charge storage film 222, and a tunnel insulating film 223. The semiconductor body 210, the charge storage film 222, and the tunnel insulating film 223 extend in the Z direction.

[0049] An insulating film 221 is disposed between the insulating film 22 and the charge storage film 222. For example, the insulating film 221 contains silicon oxide. When the sacrificial film (not illustrated) is replaced with the electrode film 21 (during the replacement process), the insulating film 221 protects the charge storage film 222 from etching. During the replacement process, the insulating film 221 can be removed from between the electrode film 21 and the memory film 220. In this case, for example, a block insulating film 221a is disposed between the electrode film 21 and the charge storage film 222, such as... Figure 2A and 2B The diagram illustrates this. In cases where the replacement process is not used to form the electrode film 21, the covering insulating film 221 may be omitted.

[0050] A charge storage film 222 is disposed between the block insulating film 221a and the overlay insulating film 221 and tunnel insulating film 223. For example, the charge storage film 222 contains silicon nitride and includes trap sites therein for trapping charges. A portion of the charge storage film 222 sandwiched between the electrode film 21, which acts as the word line WL, and the semiconductor body 210 configures the storage region of the memory cell MC as a charge trapping portion. The threshold voltage of the memory cell MC depends on the presence of charge in the charge trapping portion or changes according to the amount of charge trapped in the charge trapping portion. Accordingly, the memory cell MC retains information.

[0051] A tunnel insulating film 223 is disposed between the semiconductor body 210 and the charge storage film 222. For example, the tunnel insulating film 223 contains silicon oxide or silicon oxide and silicon nitride. The tunnel insulating film 223 is a potential barrier located between the semiconductor body 210 and the charge storage film 222. For example, when electrons are injected from the semiconductor body 210 into the charge trapping portion (in a write operation) and when vias are injected from the semiconductor body 210 into the charge trapping portion (in an erase operation), the electrons and vias respectively tunnel through (tunnel through) the potential barrier formed by the tunnel insulating film 223.

[0052] The core layer 230 is embedded within the space of the tubular semiconductor body 210. For example, the core layer 230 is columnar in shape. For example, the core layer 230 contains silicon oxide and is insulating.

[0053] Figure 3 Each of the pillar portions CLHR is disposed in a hole formed in the stack 2. The hole penetrates the stack 2 from the top end in the Z direction and is disposed in the stack 2 and the built-in source layer BSL. Each of the pillar portions CLHR contains at least an insulator. For example, the insulator is silicon oxide. Each of the pillar portions CLHR may have the same configuration as the pillar portion CL. For example, each of the pillar portions CLHR is disposed in a stepped region (stepped) and a tapered region (conical). The pillar portion CLHR acts as a support component to maintain the gap formed in the stepped region and the tapered region when the sacrificial film (not illustrated) is replaced with the electrode film 21 (during the replacement process). A plurality of pillar portions CLC4 are disposed in the tapered region (conical) of the stack 2. Each pillar portion CLC4 includes a conductor 37b or 37c. The conductor 37b is electrically insulated from the stack 2 by an insulator 36b. The conductor 37b is electrically connected to the built-in source layer BSL. The conductor 37c is electrically insulated from the stack 2 by an insulator 36c. The conductor 37c is electrically connected to any of the conductors 11a. The stepped region (step) further includes the conductor 37a, which acts as a contact with the electrode film 21 in the stack 2, and the insulator 36a disposed around the conductor 37a.

[0054] The pillar portion CL (i.e., memory hole MH) is arranged in a hexagonal, tightly packed configuration between two deep slots ST that are adjacent to each other in the Y direction in the planar layout. The shallow slot SHE is positioned to overlap with some pillar portions in the pillar portion CL, such as... Figure 3 The diagram in frame B4 illustrates this. No memory cells are formed in the pillar portion CL below the shallow slot SHE.

[0055] As the number of stacked layers increases, this three-dimensional memory cell array 2m can be formed in multiple separate steps. This is because as the stacking in the memory cell array 2m becomes thicker, it becomes more difficult to form the memory aperture MH in the desired shape. For example, the memory cell array 2m can be formed as two separate stacks comprising a lower array L2m and an upper array U2m, as... Figure 4 The diagram in the image is explained.

[0056] Figure 4 This is a cross-sectional view illustrating an example of a more detailed configuration of stack 2. Figure 4 The configuration of the memory cell array 2m and the stepped region 2s is illustrated in the parallel diagram.

[0057] The memory cell array 2m comprises a lower array L2m and an upper array U2m. The stepped region comprises a lower array L2s and an upper array U2s.

[0058] The lower arrays L2m and L2s are disposed on the built-in source layer BSL. The upper arrays U2m and U2s are disposed above the lower arrays L2m and L2s. The lower arrays L2m and L2s and the upper arrays U2m and U2s each contain alternatingly stacked electrode films 21 and insulating films 22 in the Z-direction. Electrode films 21 adjacent to each other in the Z-direction are electrically isolated from each other by the insulating films 22. The insulating films 22 are disposed between adjacent electrode films 21 in the Z-direction to electrically isolate these electrode films 21 from each other. A bonding portion JT is disposed between the lower arrays L2m and L2s and the upper arrays U2m and U2s. The configuration of the bonding portion JT will be described later.

[0059] Pillar portions CL are disposed within the upper array U2m and lower array L2m of the memory cell array 2m, extending in the Z direction. Each pillar portion CL penetrates both the upper array U2m and the lower array L2m and reaches the built-in source layer BSL. The pillar portion CL has a reference... Figure 2A and 2B The configuration described.

[0060] The column-shaped CLHRs are positioned within the upper array U2s and lower array L2s of the stepped region 2s, extending in the Z direction. Each column-shaped CLHR penetrates both the upper array U2s and the lower array L2s and reaches the built-in source layer BSL. The column-shaped CLHRs are derived from the reference... Figure 3 The silicon oxide film is formed as described. Additionally, a step TRC is formed in the stepped region 2s to connect the wire (contact) 37a to the electrode film 21 from the Z direction.

[0061] An intermediate film 50 is disposed between the upper arrays U2m and U2s and the lower arrays L2m and L2s. For example, a nitrogen-containing silicon oxide film is used as the intermediate film 50. The nitrogen concentration of the intermediate film 50 is higher than that of the insulating film 22. By disposing this intermediate film 50 above the lower arrays L2m and L2s, it is possible to maintain the surface flatness of the lower arrays L2m and L2s during manufacturing. Therefore, it is possible to improve the flatness of the upper arrays U2m and U2s formed above the lower arrays L2m and L2s. This improvement will be described later.

[0062] Figure 5 This is a cross-sectional view illustrating an example configuration of the junction JT between the upper array U2m and the lower array L2m. The junction JT between the upper array U2s and the lower array L2s also has a similar configuration.

[0063] An insulating film 60 and an intermediate film 50 are disposed in the junction JT between the upper array U2m and the lower array L2m. The insulating film 60 is disposed between the intermediate film 50 and the lower array L2m. For example, the insulating film 60 comprises a silicon oxide film. The insulating film 60 is thicker than the insulating film 22. The intermediate film 50 is disposed between the insulating film 60 and the upper array U2m. For example, the intermediate film 50 comprises a nitrogen-containing silicon oxide film. The nitrogen concentration of the intermediate film 50 is higher than that of the insulating film 60. Therefore, the intermediate film 50 has a higher nitrogen concentration than both the insulating films 22 and 60.

[0064] The upper portion of the insulating film 60 (the portion closer to the upper array U2m in the Z direction) is farther from the axis of the pillar portion CL than the upper array U2m and the lower array L2m in a direction parallel to the XY plane. Therefore, the upper portion of the insulating film 60 is recessed relative to the upper array U2m and the lower array L2m in the XY plane direction to form a recess RCS in the bonding portion JT. The memory film 220 and the semiconductor body 210 are embedded in the recess RCS. That is, the width W60 of the pillar portion CL in the upper portion of the insulating film 60 is greater than the width Wup of the pillar portion CL in the upper array U2m and the width Wlow of the pillar portion CL in the lower array L2m.

[0065] Furthermore, the intermediate film 50 protrudes further toward the pillar portion CL in the XY plane direction than the upper portion of the insulating film 60, and the depth of the recess RCS in the XY plane direction is reduced at the location of the intermediate film 50. Therefore, the insulating film 60 is recessed relative to the intermediate film 50 in the XY plane direction. That is, the width W60 of the pillar portion CL in the upper portion of the insulating film 60 is greater than the width W50 of the pillar portion CL in the intermediate film 50.

[0066] It is sufficient that the side surface of the intermediate film 50 on the pillar portion CL side is substantially flush with the side surface of each of the electrode film 21 and the insulating film 22 on the pillar portion CL side. However, the lower end of the intermediate film 50 on the pillar portion CL side is rounded by etching for residue removal, as described later. Therefore, it is possible to form the semiconductor body 210 on the inner wall of the memory hole MH in the bonding portion JT with satisfactory coverage, making it possible to prevent the semiconductor body 210 from being thinned or cut in the bonding portion JT.

[0067] In the absence of the intermediate film 50, the lower end of the sacrificial film, which serves as the lowest film of the upper array U2m, does not become rounded but instead has a sharp corner during the manufacturing process prior to the replacement process described later. This is because the sacrificial film (silicon nitride film) is hardly etched during the etching process used to remove residues (e.g., oxides) from the memory vias MH. In this case, the width of the pillar portion CL changes abruptly from the width Wup in the upper array U2m to the width W60 in the insulating film 60 in the bonding portion JT. Consequently, the memory film 220 and the semiconductor body 210 bend significantly from the Z direction to the XY plane at the boundary between the upper array U2m and the insulating film 60. As a result, the semiconductor body 210 may become thinner and be cut around the boundary between the upper array U2m and the insulating film 60. This cutting is more likely to occur as semiconductor devices become more integrated and the semiconductor body 210 becomes thinner.

[0068] Meanwhile, according to an embodiment of the present invention, an intermediate film 50 is disposed in the bonding portion JT, and the lower end of the intermediate portion 50 on the pillar portion CL side is rounded. This configuration facilitates changing the width of the pillar portion CL from the width Wup in the upper array U2m or the width W50 in the intermediate film 50 to the width W60 in the insulating film 60. Accordingly, the memory film 220 and the semiconductor body 210 are slightly curved from the Z direction to the XY plane direction at the boundary between the upper array U2m and the insulating film 60.

[0069] As described above, by providing the intermediate film 50, the coverage of the semiconductor body 210 is improved, and the thickness of the semiconductor body 210 can also be made nearly uniform in the bonding portion JT, thus preventing the semiconductor body 210 from being cut. As a result, it is possible to prevent memory cell failures caused by cutting the semiconductor body 210.

[0070] Next, a method for manufacturing a semiconductor memory device 100a according to an embodiment of the present invention will be described.

[0071] Figures 6 to 15 This is a cross-sectional view illustrating an example of a method for manufacturing a semiconductor memory device 100a according to the first embodiment.

[0072] First, a substrate portion 1 is formed. In this step, the substrate portion 1 comprises a stacked structure of a conductive layer 12, an insulating film 131, a sacrificial film 132, an insulating film 133, and a semiconductor portion 13a. A conductive material, such as doped polysilicon or a metal, is used for the conductive layer 12. An insulating material, such as silicon oxide, is used for the insulating films 131 and 133. For example, a silicon nitride film is used as the sacrificial film 132. A conductive material, such as doped polysilicon, is used for the semiconductor portion 13a. Later in the process, the insulating films 131, 132, and 133 will be replaced with a conductor. This conductor, together with the conductive layer 12 and the semiconductor portion 13a, forms a built-in source layer (BSL).

[0073] Next, above the substrate portion 1, multiple sacrificial films 21a and multiple insulating films 22 are alternately stacked in the Z direction. Thus, a stack of sacrificial films 21a and insulating films 22 is formed in the regions of the lower arrays L2m and L2s. An insulating material, such as silicon nitride, is used for the sacrificial films 21a. An insulating material, such as silicon oxide, is used for the insulating films 22. The sacrificial films 21a are stacked in the Z direction and isolated from each other by the insulating films 22. The sacrificial films 21a will be replaced with electrode films 21 in a later process.

[0074] Next, the lower array L2s in the stepped region 2s is processed to form the stepped TRC. Then, for example, an insulating film 60 is formed on the stepped TRC and the stack by CVD (chemical vapor deposition). An insulating material such as silicon oxide, formed using TEOS (tetraethoxysilane), is used for the insulating film 60. Next, the surface of the insulating film 60 is planarized by, for example, CMP (chemical mechanical polishing).

[0075] Then, for example, lower holes LMH and LHR are formed to penetrate the stack in the Z direction by RIE (reactive ion etching).

[0076] Next, a resist film (not illustrated) is filled into the lower holes LMH and LHR, and its upper portion is removed. This exposes the side surface of the upper portion of the insulating film 60. Subsequently, the side surface of the upper portion of the insulating film 60 is etched using the resist film as a mask. Accordingly, the diameter of the opening in the upper portion of the insulating film 60 is made larger than the diameter of the lower holes LMH or LHR in the lower portion of the insulating film 60 and the lower array L2m or L2s. That is, since the diameter of the lower holes LMH and LHR is increased in the upper portion of the insulating film 60, even if the positions of the upper holes UMH and UHR are slightly shifted from the lower holes LMH and LHR during the formation of the upper holes UMH and UHR, as described later, the upper holes UMH and UHR can still communicate with the lower holes LMH and LHR, respectively. Therefore, the positions of the upper holes UMH and UHR can be easily aligned with the lower holes LMH and LHR.

[0077] Next, the resist film in the lower holes LMH and LHR is removed, and then the sacrificial film 70 is temporarily filled in the lower holes LMH and LHR. A material that can be selectively etched relative to the silicon nitride film and silicon oxide film (e.g., carbon or amorphous silicon) is used for the sacrificial film 70. The sacrificial film 70 will be replaced with pillar portions CL and CLHR in a later process. Therefore, it is sufficient for the sacrificial film 70 to seal the openings of the lower holes LMH and LHR. A void can be created below the sacrificial film 70. Next, for example, the surfaces of the insulating film 60 and the sacrificial film 70 are planarized by CMP. Accordingly, a Figure 6 The structure is illustrated in the diagram.

[0078] Next, an intermediate film 50 is formed above the stack of the lower arrays L2m and L2s, as follows: Figure 7 The diagram below illustrates this. For example, a silicon nitride film is initially formed as an intermediate film 50.

[0079] In the case where a silicon oxide film is initially formed as an intermediate film 50, the sacrificial film 70 (for example, made of carbon) can be oxidized and scraped during the deposition of the intermediate film 50. In this case, the surface of the sacrificial film 70 is recessed in the Z direction relative to the surface of the insulating film 60, and the surface of the intermediate film 50 deposited on the films 70 and 60 also becomes uneven, resulting in poor flatness of the intermediate film 50.

[0080] On the other hand, according to an embodiment of the present invention, a silicon nitride film is initially formed as an intermediate film 50. Accordingly, oxidation of the sacrificial film 70 (for example, made of carbon) can be prevented during the formation of the intermediate film 50. Therefore, the sacrificial film 70 hardly sinks relative to the surface of the insulating film 60, and the surface flatness of the intermediate film 50 is maintained.

[0081] Next, the intermediate film 50 is oxidized. In this step, the intermediate film 50 is oxidized, for example, by ISSG (In-situ Steam Generation). ISSG oxidation is a technique that forms an oxide film by directly introducing hydrogen and oxygen into a chamber and generating water vapor (H2O) inside. Accordingly, the intermediate film 50 is changed to a nitrogen-containing silicon oxide film. Since the intermediate film 50 is a silicon oxide film obtained by oxidizing a silicon nitride film, its nitrogen concentration is higher than that of the insulating films 22 and 60.

[0082] Next, on the intermediate membrane 50, the sacrificial membrane 21a and the insulating membrane 22 are alternately stacked in the Z direction, as follows: Figure 8The diagram illustrates this. Accordingly, a stack of sacrificial film 21a and insulating film 22 is formed in the regions of the upper arrays U2m and U2s. An insulating material such as silicon nitride is used for the sacrificial film 21a. An insulating material such as silicon oxide is used for the insulating film 22. The sacrificial films 21a are stacked in the Z direction and isolated from each other by the insulating film 22. The sacrificial film 21a will be replaced with an electrode film 21 in a later process. At this step, in the case where the lower holes LMH and LHR are filled with carbon as a sacrificial film 70, it is possible to reduce the possibility of warping of the stack in the regions of the lower arrays L2m and L2s due to the thermal history during the formation of the stack of, for example, the upper arrays U2m and U2s.

[0083] Next, the upper array U2s in the stepped region 2s is processed to form the stepped TRC, as shown below. Figure 9 The diagram illustrates this. In this case, the intermediate film 50 acts as a stopper, preventing the step TRC in the upper array U2s from reaching the insulating film 60, and keeping the sacrificial film 70 in the lower aperture LHR covered by the intermediate film 50. Correspondingly, the sacrificial film 70 in the lower aperture LHR is protected from scratching, for example, during the removal of the mask material used to process the upper array U2s. Additionally, a stopper film 80 is formed on the upper array U2m. For example, a silicon nitride film is used as the stopper film 80.

[0084] Next, insulating films 81 and 82 are formed on the stack of the upper arrays U2s and U2m. For example, a silicon oxide film is used as the insulating film 81. For example, a silicon nitride film is used as the insulating film 82. Accordingly, an insulating film is obtained. Figure 9 The structure is illustrated in the diagram.

[0085] Next, the insulating films 82 and 81 in the region excluding the step region 2s of the memory cell array 2m are etched back using photolithography and etching, such as... Figure 10 The diagram illustrates this.

[0086] Next, insulating film 90 is deposited on the upper arrays U2m and U2s, and the position to the stopper film 80 is planarized by CMP, such as... Figure 11 The diagram illustrates this. Therefore, the insulating film 90 is embedded in the stepped region 2s. For example, a silicon oxide film is used as the insulating film 90. Subsequently, the stopper film 80 on the upper array U2m is removed.

[0087] Next, a mask material HM is formed above the upper arrays U2m and U2s, such as... Figure 12The diagram illustrates the process. The mask material HM is patterned into upper apertures UMH and UHR using photolithography and etching. Next, using RIE, the mask material HM is used as a mask to process the stack of upper arrays U2m and U2s with the intermediate film 50. Accordingly, upper apertures UMH and UHR are formed to penetrate the stack of upper arrays U2m and U2s with the intermediate film 50 in the Z direction. Upper apertures UMH and UHR are formed to correspond to positions directly above lower apertures LMH and LHR, respectively. In this step, the opening in the upper portion of the insulating film 60 is widened to have a diameter wider than that of the lower portion of the insulating film 60 and the lower apertures LMH and LHR in the lower arrays L2m and L2s. Therefore, the upper apertures UMH and UHR can be easily aligned with their corresponding lower apertures LMH and LHR, respectively. Consequently, the upper apertures UMH and UHR can be easily connected to their corresponding lower apertures LMH and LHR, respectively.

[0088] Next, the sacrificial membrane 70 in the lower holes LMH and LHR is removed via the upper holes UMH and UHR, as follows: Figure 13 The illustration is as follows. In the case where the sacrificial film 70 is made of carbon, for example, the sacrificial film 70 is oxidized and removed by using an ashing device. Accordingly, the sacrificial film 70 can be easily removed.

[0089] Next, the inner walls of the upper holes UMH and UHR, and the lower holes LMH and LHR, are etched using, for example, a hydrofluoric acid solution (BHF (buffered hydrogen fluoride)). Accordingly, residues in the upper holes UMH and UHR, and the lower holes LMH and LHR, are removed.

[0090] At this step, the intermediate film 50 and the insulating film 60 on the inner wall of the bonding portion JT are lightly etched. According to an embodiment of the invention, the intermediate film 50 is a silicon oxide film obtained by oxidizing a silicon nitride film via ISSG oxidation, and therefore has a higher nitrogen concentration than the insulating films 22 and 60. Therefore, the etching rate of the intermediate film 50 is higher than that of the sacrificial film 21a but lower than that of the insulating films 22 and 60. Accordingly, the intermediate film 50 is lightly etched and rounded at its lower end of the side surface exposed in the upper aperture UMH. However, the intermediate film 50 does not move away from the upper aperture UMH in the XY plane direction to a large extent. Furthermore, the angled lower end of the sacrificial film 21a, which is the lowermost film in the upper array U2m, is not exposed by the etching progress in the Z direction from the bottom surface of the intermediate film 50 exposed in the widened portion of the lower aperture LMH.

[0091] Figure 16 It was by Figure 13 A cross-sectional view of the area enclosed by the dashed box in the image. (See also...) Figure 16As illustrated in the diagram, the width W60 of the lower hole LMH in the upper portion of the insulating film 60 where the recess RCS is formed is greater than the width Wlow of the lower hole LMH and the width Wup of the upper hole UMH in the lower portion of the insulating film 60, and increases in the direction away from the center of the upper hole UMH. Meanwhile, the intermediate film 50 protrudes further towards the center of the upper hole UMH than the upper portion of the insulating film 60. Therefore, the width W50 of the upper hole UMH in the intermediate film 50 is smaller than the width W60 of the lower hole LMH in the upper portion of the insulating film 60, as shown in the diagram. Figure 16 The diagram illustrates this. Furthermore, since the lower end of the intermediate film 50 is rounded, it becomes easier to change the depth of the recessed RCS in the XY plane direction. Therefore, it is possible to form the semiconductor body 210 with satisfactory coverage on the inner wall of the memory hole MH in the bonding portion JT, making it possible to prevent the semiconductor body 210 from becoming thinner or being cut in the bonding portion JT. The inner walls of the holes formed by the lower hole LHR and the upper hole UHR in the stepped region 2s also have the same shape.

[0092] In this embodiment of the invention, for the insulating film 22, insulating film 60, and intermediate film 50 formed from silicon oxide films, the insulating film 22 may, for example, be formed from a silicon oxide film having a higher density than the insulating film 60 and the intermediate film 50. This configuration allows the etching rate of the insulating film 22 to be lower than the etching rates of the insulating film 60 and the intermediate film 50. Furthermore, the intermediate film 50 is formed from a silicon oxide film having a higher nitrogen concentration than the insulating film 60. Therefore, the etching rate of the intermediate film 50 can be lower than the etching rate of the insulating film 60.

[0093] Next, an insulating film, such as a silicon oxide film, is embedded in the upper hole UHR and the lower hole LHR in the stepped region 2s to form the pillar portion CLHR, as shown. Figure 14 The diagram illustrates this. When the sacrificial membrane 21a is later replaced with the electrode membrane 21, the pillar portion CLHR acts as a support for the insulating membrane 22.

[0094] Furthermore, a memory film 220 is formed on the inner walls of the lower aperture LMH and the upper aperture UMH in the region of the memory cell array 2m. For example, a covering insulating film 221, a charge storage film 222, and a tunnel insulating film 223 are formed on the inner walls of the lower aperture LMH and the upper aperture UMH in the aforementioned order.

[0095] Next, a semiconductor body 210 is formed inside the memory film 220 in the upper hole UMH and lower hole LMH in the region of the memory cell array 2m, such as Figure 15 The diagram in the image is explained.

[0096] At this step, the upper portion of the insulating film 60 is recessed in the XY plane relative to the upper arrays U2m and U2s and the lower arrays L2m and L2s, and the lower end of the intermediate film 50 becomes rounded. Therefore, at the boundary between the intermediate film 50 and the insulating film 60 (the boundary between the upper aperture UMH and the lower aperture LMH), the bending of the semiconductor body 210 is mitigated. Accordingly, a satisfactory coverage of the semiconductor body 210 is obtained in the bonding portion JT, making it possible to prevent the semiconductor body 210 from being cut.

[0097] Furthermore, in the region of the memory cell array 2m, a core layer 230 is embedded inside the memory film 220 and the semiconductor body 210 in the upper hole UMH and the lower hole LMH.

[0098] Subsequently, a slot ST is formed (see Figure 1A and 1B By means of a slot ST, insulating films 131 and 133 and sacrificial film 132 in the region of the memory cell array 2m are replaced with conductive material (e.g., polysilicon) to form an internal source layer BSL. Furthermore, sacrificial film 21a is removed via the slot ST. Thus, spaces are formed between insulating films 22 adjacent to each other in the Z direction. Conductive material (e.g., tungsten) is embedded in these spaces via the slot ST, thereby forming an electrode film 21 between the insulating films 22. Accordingly, an electrode film 21 is formed. Figure 4 The diagram illustrates stack 2.

[0099] Subsequently, contacts and bit lines (neither illustrated) are formed. Accordingly, the semiconductor memory device 100a according to an embodiment of the present invention is completed. The semiconductor memory device 100a can be formed by forming a CMOS circuit of a substrate portion 1 on another substrate and bonding the substrate having a stack 2 and the substrate having the CMOS circuit to each other.

[0100] According to an embodiment of the present invention, an intermediate film 50 is formed on the insulating film 60 and the sacrificial film 70 in the lower holes LMH and LHR. Since the intermediate film 50 is a silicon nitride film in the initial formation stage, oxidation of the sacrificial film 70 (for example, made of carbon) can be prevented. Therefore, it is possible to maintain the surface flatness of the intermediate film 50. By maintaining a satisfactory surface flatness of the intermediate film 50, the surface flatness of the upper arrays U2m and U2s formed thereon also becomes satisfactory.

[0101] Furthermore, according to an embodiment of the present invention, an intermediate film 50 is disposed between the insulating film 60 and the upper arrays U2m and U2s. A silicon oxide film having a higher nitrogen concentration than the insulating film 60 is used as the intermediate film 50. Therefore, the intermediate film 50 has a lower etching rate than the insulating film 60, and the lower end of the intermediate film 50 is rounded, although the intermediate film 50 protrudes more in the XY plane direction in the bonding portion JT than the upper portion of the insulating film 60. This configuration softens the step at the boundary between the upper array U2m and the insulating film 60 and also softens the bending of the semiconductor body 210 in the bonding portion JT. As a result, a satisfactory coverage of the semiconductor body 210 is obtained in the bonding portion JT, making it possible to prevent the semiconductor body 210 from being cut.

[0102] In the first embodiment described above, the intermediate film 50 is initially formed as a silicon nitride film and then oxidized to become a nitrogen-containing silicon oxide film. However, the intermediate film 50 can be a silicon oxide film formed using ULT (ultra-low temperature) technology. In ULT technology, a silicon oxide film is formed in a low-temperature atmosphere, for example, at room temperature, using an aminosilane such as a dialkylaminosilane as a material. In this case, since formation can be performed in a low-temperature atmosphere, the sacrificial film 70 (for example, made of carbon) is less likely to be oxidized during the deposition of the silicon oxide film, thereby maintaining the surface smoothness of the intermediate film 50. In addition, the silicon oxide film formed by this ULT technology has a higher nitrogen and carbon concentration than, for example, a silicon oxide film formed using TEOS, because the former uses an aminosilane as a material. Therefore, the silicon oxide film formed by ULT technology has a lower etching rate than a silicon oxide film formed using TEOS. Accordingly, in the case where a silicon oxide film formed by ULT technology is used as the intermediate film 50, the same effects as in the embodiments described above can be obtained.

[0103] (Second Embodiment)

[0104] Figure 17 This is a cross-sectional view illustrating an example configuration of the bonding portion JT according to a second embodiment. In the second embodiment, the intermediate film 50 includes a portion film 50a and a portion film 50b. Similar to the intermediate film 50 according to the first embodiment, the portion film 50a includes a nitrogen-containing silicon oxide film.

[0105] For example, partial membrane 50a is a silicon oxide membrane formed using ULT technology with an aminosilane, such as a dialkylaminosilane. In this case, partial membrane 50a is a silicon oxide membrane containing nitrogen and carbon. The nitrogen and carbon concentrations of partial membrane 50a are higher than those of partial membrane 50b.

[0106] Partial film 50b is disposed on partial film 50a and is a silicon oxide film with a lower nitrogen concentration and / or carbon concentration than partial film 50a. Similar to insulating film 60, partial film 50b may be, for example, a silicon oxide film formed using TEOS. According to this technology, it is possible to form silicon oxide films at a higher productivity than partial film 50a.

[0107] In this case, like the insulating film 60, the partial film 50b has a higher etching rate than the partial film 50a. However, when forming the lower array L2m, the partial film 50b is not provided, and when forming the memory hole MH after stacking the upper array U2m, the partial film 50b is only slightly etched at the lower end of the side surface exposed in the memory hole MH by hydrofluoric acid solution (BHF). Therefore, unlike the upper portion of the insulating film 60, the partial film 50b is not recessed in the direction away from the pillar portion CL (XY plane direction). The partial film 50b, together with the partial film 50a, rounds at the lower end on the side of the pillar portion CL. Therefore, the upper portion of the insulating film 60 is recessed in the XY plane direction relative to the upper array U2m and the lower array L2m to form a recess RCS in the bonding portion JT. At the same time, portions of membranes 50a and 50b protrude more in the XY plane direction between the insulating membrane 60 and the upper array U2m than the insulating membrane 60 towards the pillar portion CL.

[0108] In part of membrane 50a, the width W50a of the memory hole MH (pillar portion CL) is slightly larger than the widths Wup and Wlow of the memory hole MH (pillar portion CL) in the upper array U2m and the lower array L2m. Additionally, in part of membrane 50b, the width W50b of the memory hole MH is approximately equal to or slightly smaller than the width W50a.

[0109] According to the second embodiment, since a portion 50a of the intermediate film 50 is disposed in the bonding portion JT, the lower ends of both portions 50a and 50b are rounded, causing the curvature of the inner wall of the memory hole MH from the Z direction to the XY plane to be gentler at the boundary between the upper array U2m and the insulating film 60. Therefore, the coverage of the semiconductor body 210 is improved, and the semiconductor body 210 can be prevented from being cut in the bonding portion JT. Furthermore, compared to using only portion 50a, when processing the upper array U2s, the intermediate film 50, including both portions 50a and 50b, enhances the protection of the sacrificial film 70 in the lower hole LHR.

[0110] As described above, by providing an intermediate film 50 comprising partial films 50a and 50b, the coverage of the semiconductor body 210 is improved, and the thickness of the semiconductor body 210 in the bonding portion JT can also be nearly uniform. As a result, the semiconductor body 210 is prevented from being cut, thus preventing memory cell failures caused by cutting of the semiconductor body 210.

[0111] The other configurations of the second embodiment are the same as the corresponding configurations of the first embodiment. Therefore, the second embodiment can achieve the same effects as those of the first embodiment.

[0112] Next, a method for manufacturing the semiconductor memory device 100a according to the second embodiment will be described.

[0113] Figure 18 This is a cross-sectional view illustrating an example of a method for manufacturing a semiconductor memory device 100a according to the second embodiment.

[0114] Reference Figure 6 Following the described process, an intermediate film 50 is formed above the stack of the lower arrays L2m and L2s, as shown below. Figure 18 The diagram below illustrates this. Intermediate membrane 50 includes portions of membranes 50a and 50b.

[0115] Partial film 50a is a silicon oxide film formed using the ULT technology described above. The silicon oxide film formed using this ULT technology has a higher nitrogen and carbon concentration than, for example, a silicon oxide film formed using TEOS. Furthermore, according to the ULT technology, it is possible to form a silicon oxide film in a low-temperature atmosphere at approximately room temperature, and compared to a silicon oxide film formed using TEOS, partial film 50a is less likely to oxidize the sacrificial film 70 (for example, made of carbon). Therefore, the sacrificial film 70 is less recessed relative to the surface of the insulating film 60, and the surface flatness of the lower arrays L2m and L2s is easily maintained. In addition, recesses RCS are formed in the side surfaces of the upper portion of the insulating film 60 in the lower holes LMH and LHR. With this configuration, even when the positions of the upper holes UMH and UHR are slightly shifted from the lower holes LMH and LHR, the upper holes UMH and UHR can still communicate with the lower holes LMH and LHR, respectively.

[0116] Next, a partial film 50b is formed on partial film 50a. For example, a silicon oxide film formed using TEOS is used as partial film 50b. However, since partial film 50b is formed on partial film 50a, partial film 50b hardly oxidizes the sacrificial film 70. Partial film 50b has a lower nitrogen and carbon concentration than partial film 50a and a higher etching rate than partial film 50a.

[0117] After that, execute the reference. Figures 8 to 15The process described. In Figure 13 During the process illustrated in the diagram, etching is performed using a hydrofluoric acid solution (BHF), thereby creating an inner wall of the memory hole MH in the bonding portion JT. Figure 17 The shape is illustrated in the figure. Thereafter, the same processes as those in the first embodiment are performed, so that the semiconductor memory device 100a according to the second embodiment is completed.

[0118] According to the second embodiment, an intermediate film 50 is formed on the insulating film 60 and the sacrificial film 70 in the lower holes LMH and LHR. The intermediate film 50 includes a silicon oxide film formed by ULT technology as a partial film 50a. The partial film 50a covers the insulating film 60 and the sacrificial film 70. With this configuration, the surface flatness of the lower arrays L2m and L2s (insulating film 60 and sacrificial film 70) can be maintained, and the surface flatness of the upper arrays U2m and U2s also becomes satisfactory.

[0119] Furthermore, the upper portion of the insulating film 60 is recessed in the bonding portion JT in the XY plane direction relative to the upper arrays U2m and U2s and the lower arrays L2m and L2s. Simultaneously, a silicon oxide film with a higher nitrogen and carbon concentration than the insulating film 60 and the partial film 50b is used as the partial film 50a. Therefore, the partial film 50a has a lower etching rate than the insulating film 60 and the partial film 50b, and protrudes more in the XY plane direction in the bonding portion JT than the upper portion of the insulating film 60. Although the same silicon oxide film as the insulating film 60 is used as the partial film 50b, the partial film 50b is disposed between the partial film 50a and the upper array U2m, and is only slightly etched with hydrofluoric acid solution (BHF) when forming memory holes MH in the upper array U2m. Therefore, unlike the upper portion of the insulating film 60, the partial film 50b is recessed in a direction away from the pillar portion CL (XY plane direction). Meanwhile, the portion of film 50b, together with the portion of film 50a etched by hydrofluoric acid solution (BHF), becomes rounded at its lower end on the pillar portion CL side. Correspondingly, the curvature of the inner wall of the memory hole MH from the Z direction to the XY plane is reduced at the boundary between the upper array U2m and the insulating film 60. Therefore, embedding the memory film 220 and the semiconductor body 210 in the memory hole MH becomes easier, and the curvature of the semiconductor body 210 in the bonding portion JT is reduced. Accordingly, a satisfactory coverage of the semiconductor body 210 is obtained in the bonding portion JT, and cutting of the semiconductor body 210 is prevented.

[0120] While specific embodiments have been described, these embodiments are presented by way of example only and are not intended to limit the scope of the invention. In fact, the novel methods and configurations described herein can be embodied in many other forms; furthermore, various omissions, substitutions, and changes can be made to the form of the methods and systems described herein without departing from the spirit of the invention. It is intended that the appended claims and their equivalents cover such forms or modifications that fall within the scope and spirit of the invention.

Claims

1. A semiconductor memory device, comprising: A first stack comprising a plurality of first electrode films stacked in a first direction and electrically isolated from each other; The second stack is disposed above the first stack and contains a plurality of second electrode films stacked in the first direction and electrically isolated from each other; An intermediate membrane is disposed between the first stack and the second stack; The pillar portion includes a semiconductor layer configured to extend in the first stack and the second stack and in the intermediate film in the first direction, and a memory cell is formed at the intersection of the semiconductor layer with at least one of the first electrode films and at the intersection of the semiconductor layer with at least one of the second electrode films. A first insulating film is disposed between the first electrode films; and A second insulating film is disposed between the second electrode films; wherein The intermediate membrane comprises a nitrogen-containing silicon oxide membrane. The nitrogen concentration of the intermediate membrane is higher than that of the first insulating membrane and the second insulating membrane.

2. The semiconductor memory device of claim 1, further comprising a third insulating film, the third insulating film comprising a silicon oxide film disposed between the intermediate film and the first stack, wherein... The nitrogen concentration of the intermediate membrane is higher than that of the third insulating membrane.

3. The semiconductor memory device according to claim 2, wherein the third insulating film is thicker than the first insulating film and the second insulating film.

4. The semiconductor memory device according to claim 2, wherein The third insulating film includes a recessed portion in a direction away from the post portion, the portion extending within the third insulating film, and The intermediate film protrudes further toward the pillar portion than the portion of the third insulating film.

5. The semiconductor memory device of claim 4, wherein a portion of the third insulating film on the side closer to the second stack in the first direction is recessed relative to the first stack and the second stack.

6. The semiconductor memory device according to claim 2, wherein the carbon concentration of the intermediate film is higher than the carbon concentration of the third insulating film.

7. The semiconductor memory device of claim 1, wherein the intermediate film comprises: a first portion film comprising a nitrogen-containing silicon oxide film; and a second portion film disposed on the first portion film and comprising a silicon oxide film having a lower nitrogen concentration than the first portion film.

8. The semiconductor memory device according to claim 7, wherein the carbon concentration of the first portion of the film is higher than the carbon concentration of the second portion of the film.

9. The semiconductor memory device according to claim 2, wherein The intermediate membrane comprises: a first portion membrane comprising a nitrogen-containing silicon oxide film; and a second portion membrane disposed on the first portion membrane and comprising a silicon oxide film having a lower nitrogen concentration than the first portion membrane. The third insulating film includes a recessed portion in a direction away from the post portion, the portion extending within the third insulating film, and The first and second portions of the membrane protrude more toward the pillar portion than the portion of the third insulating membrane.

10. The semiconductor memory device of claim 9, wherein the carbon concentration of the first portion of the film is higher than the carbon concentration of the second portion of the film.

11. A method for manufacturing a semiconductor memory device, the method comprising: A first stack is formed, the first stack comprising a plurality of first sacrificial layers stacked in a first direction and isolated from each other; A first hole is formed in the first direction, penetrating the first stack; A carbon-containing sacrificial membrane is filled into the first pore; An intermediate film is formed above the first stack in which the first hole is formed, the intermediate film comprising a nitrogen-containing silicon oxide film; A second stack is formed on the intermediate film, the second stack comprising a plurality of second sacrificial layers stacked and isolated from each other in the first direction; A second hole is formed that penetrates the second stack and the intermediate film in the first direction and corresponds to the first hole; and A semiconductor layer is formed on the inner wall of the first and second holes via a charge storage film to form pillar portions in the first and second holes; wherein The formation of the intermediate membrane comprises: A silicon nitride film is formed over the first stack, and The silicon nitride film is oxidized to form the silicon oxide film containing nitrogen.

12. The method of manufacturing a semiconductor memory device according to claim 11, wherein... The first stack is a stack of the first sacrificial layer and the first insulating film. The second stack is a stack of the second sacrificial layer and the second insulating film, and The nitrogen concentration of the intermediate membrane is higher than that of the first insulating membrane and the second insulating membrane.

13. The method for manufacturing a semiconductor memory device according to claim 11, further comprising: Prior to the formation of the first aperture, a third insulating film comprising a silicon oxide film is formed on the first stack, wherein In the formation of the first hole, the first hole penetrates the third insulating film on the first stack, and In the formation of the intermediate film, a silicon oxide film is formed on the third insulating film, the silicon oxide film having a higher nitrogen concentration than the third insulating film.

14. The method for manufacturing a semiconductor memory device according to claim 13, wherein, In the formation of the first hole, the upper portion of the third insulating film is recessed relative to the inner wall of the first stack in a direction intersecting the first direction.

15. The method of manufacturing a semiconductor memory device according to claim 13, wherein the carbon concentration of the intermediate film is higher than the carbon concentration of the third insulating film.

16. The method of manufacturing a semiconductor memory device according to claim 11, wherein the formation of the intermediate film comprises: A first partial film is formed over the first stack, the first partial film comprising a nitrogen-containing silicon oxide film, and A second partial film is formed on the first partial film, the second partial film comprising a silicon oxide film having a lower nitrogen concentration than the first partial film.

17. The method of manufacturing a semiconductor memory device according to claim 16, wherein the carbon concentration of the first portion of the film is higher than the carbon concentration of the second portion of the film.

Citation Information

Patent Citations

  • Monitoring and control module

    JP2021144550A

  • 3D memory device having semiconductor plug formed using a back substrate thinning

    CN109496355A

  • Memory stack having silicon oxynitride gate-to-gate dielectric layer and method of forming same