strain relaxation layer
By forming a first epitaxial crystal layer with high initial conductivity on a crystal template layer and etching pores, combined with conductive material channels, the strain management problem in epitaxial growth is solved, improving the internal quantum efficiency and light generation efficiency of InGaN-based LEDs, making them suitable for high-resolution light-emitting device arrays.
Patent Information
- Application Number
- CN202180048539.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-07-16
- Filing Date
- 2021-07-14
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2041-07-14
AI Technical Summary
Existing technologies struggle to effectively manage strain during epitaxial growth, leading to reduced internal quantum efficiency in InGaN-based LED structures, especially in high-indium-content quantum wells where light emission wavelengths are longer. Furthermore, it is difficult to form high-quality relaxor InGaN layers to improve performance.
A first epitaxial crystalline layer with initial high electrical conductivity is formed on a crystalline template layer, and pores are formed in this layer by electrochemical etching. Combined with conductive material channels, the electrical connection of the strain relaxation layer is realized, and strain is managed by the plastic deformation of pores and interfaces.
The formation of a high-quality strain relaxation layer was achieved, which improved the internal quantum efficiency and light generation efficiency of the LED structure, making it suitable for high-resolution light-emitting device arrays.
Smart Images

Figure CN115777152B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a template and a method for forming a template. In particular, but not only therein, this invention relates to a template and a method for forming a template, which enables the growth of strain-relaxed crystalline materials to form a practical device. Background Technology
[0002] Epitaxially grown crystal devices, such as light-emitting diodes (LEDs), are typically formed using techniques like metal-organic chemical vapor deposition (MOCVD) and molecular beam epitaxy (MBE) to provide crystal structures with layers of different compositions. The different compositions that may be needed, for example, to achieve specific emission recombination, can lead to mismatches between the lattice parameters of the layers. This mismatch typically results in high strain, which in turn leads to a decrease in internal quantum efficiency (IQE). This is a known problem in forming indium gallium nitride (InGaN)-based LED structures, especially when using high indium content in InGaN quantum wells (QWs) to provide longer wavelength light emission, such as red light emission.
[0003] In such cases, attempts to reduce the strain of the underlying layer to improve device performance often present other challenges. For example, in InGaN-based devices, growing quantum wells on a relaxed InGaN layer with an in-plane lattice constant greater than that of gallium nitride (GaN) reduces strain, thereby improving IQE. However, achieving a high-quality relaxed InGaN layer while simultaneously enabling carrier injection into the quantum well to form a functional device is problematic because high-quality n-type layers with preferred doping levels are typically and advantageously formed from n-type doped GaN, and are not easily achieved for materials with this composition that require strain reduction to improve the IQE of InGaN-based red LEDs.
[0004] Because porous GaN is compliant and rich in fractured bonds, it allows for the transmission of misfit dislocations at the porous GaN / InGaN interface, thus porous GaN layers have been proposed as a mechanism to reduce strain in subsequent growth layers. However, such porous GaN exhibits high electrical resistance, making it generally unsuitable for forming functional devices. Summary of the Invention
[0005] To mitigate at least some of the aforementioned problems, a method is provided for forming a strain-relaxed layer in an epitaxial crystalline structure. The method includes: providing a crystalline template layer comprising a material having a first naturally relaxed in-plane lattice parameter; forming a first epitaxial crystalline layer on the crystalline template layer, wherein the initial electrical conductivity of the first epitaxial crystalline layer is higher than the electrical conductivity of the crystalline template layer; forming a second epitaxial crystalline layer on the first epitaxial crystalline layer, wherein the electrical conductivity of the second epitaxial crystalline layer is lower than the initial electrical conductivity of the first epitaxial crystalline layer, the second epitaxial crystalline layer comprising a material having a second naturally relaxed in-plane lattice parameter. The in-plane lattice parameters of the naturally relaxed crystal layer are different from the in-plane lattice parameters of the first naturally relaxed crystal template layer; pores are formed in the first epitaxial crystal layer by electrochemical etching of the first epitaxial crystal layer, so as to achieve strain relaxation in the second epitaxial crystal layer by plastic deformation of the bonds in the first epitaxial crystal layer and / or at the interface between the first epitaxial crystal layer and the second epitaxial crystal layer; and one or more channels containing conductive material are formed, the one or more channels passing through at least the first epitaxial crystal layer and the second epitaxial crystal layer, thereby realizing electrical connection to the crystal template layer through the first epitaxial crystal layer and the second epitaxial crystal layer.
[0006] An epitaxial crystal structure is also provided, comprising: a crystal template layer comprising a material having a first naturally relaxed in-plane lattice parameter; a first epitaxial crystal layer formed on the crystal template layer; a second epitaxial crystal layer formed on the first epitaxial crystal layer, wherein the second epitaxial crystal layer comprises a material having a second naturally relaxed in-plane lattice parameter different from the first naturally relaxed in-plane lattice parameter of the crystal template layer; one or more pores formed in the first epitaxial crystal layer such that any strain in the second epitaxial crystal layer is relaxed by plastic deformation of bonds in the first epitaxial crystal layer and / or at the interface between the first and second epitaxial crystal layers; and one or more channels comprising a conductive material formed to pass through at least the first and second epitaxial crystal layers, thereby enabling electrical connections through the first and second epitaxial crystal layers to the crystal template layer.
[0007] Advantageously, the porosification of the initial high-conductivity layer is combined with the formation of one or more channels, enabling the relaxation of a crystalline layer having intrinsic, relaxed, in-plane lattice parameters different from those of the underlying template layer. This relaxation can be achieved in devices that would otherwise be difficult to realize, while simultaneously enabling electrical connections to the underlying template layer in a manner that improves device formation.
[0008] Preferably, the volume density of the pores formed in the first epitaxial layer between the crystallization template layer and the second epitaxial layer is greater than 50%, more preferably greater than 60%, and more preferably greater than 70%. Advantageously, the porosity in the first epitaxial layer is controlled to promote plastic deformation of the bonds at the interfaces in and / or between the first epitaxial layers.
[0009] Preferably, the second epitaxial layer includes at least one V-shaped pit, and more preferably, the depth of the at least one V-shaped pit is substantially the combined thickness of the first and second epitaxial layers. Advantageously, this depth of V-shaped pit enables electrical connection with the underlying crystal template layer.
[0010] Preferably, the method includes enlarging the at least one V-shaped pit, wherein enlarging the at least one V-shaped pit includes etching material from the sidewalls of the at least one V-shaped pit to expose at least a portion of the crystalline template layer. Advantageously, the V-shaped pit facilitates electrical connection between the crystalline template layer and the layer subsequently formed on the second epitaxial crystalline layer through a porous, high-resistivity first epitaxial crystalline layer.
[0011] Preferably, the method includes etching through at least the second epitaxial layer to form one or more islands in the second epitaxial layer. Advantageously, the formation of the islands controls the relaxation of the second epitaxial layer.
[0012] Preferably, the method includes patterning the second epitaxial layer, wherein the patterning includes at least one of photolithography and a self-assembled Ni hard mask. Advantageously, using a self-assembled Ni hard mask to pattern the second epitaxial layer enables the formation of narrow channels for strain relaxation and electrical connection to the underlying crystalline template layer.
[0013] Preferably, the method includes forming the crystal template layer on a patterned template layer. Advantageously, by controlling the underlying morphology of the crystal template layer, the formation of improved devices is facilitated. Advantageously, it can provide the formation of LED devices and LED device arrays, such as high-resolution micro-LED arrays with improved light strain management, more efficient light generation, and more efficient light extraction.
[0014] Preferably, the patterned template layer is patterned to provide trenches, and preferably, forming the crystallization template layer includes forming an epicrystalline growth material in these trenches to provide V-grooves, thereby enabling the formation of two-dimensional domains at least partially defined by valleys in the second epitaxial crystallization layer. Advantageously, the formation of the trenches allows for adjustment of the valley size through epicrystalline growth of the material in the trenches.
[0015] Preferably, the patterned template layer is patterned to provide one or more epicrystalline growth structures. Preferably, forming the patterned crystalline template layer includes at least partially covering the crystalline template layer to provide one or more apertures, and forming epicrystalline growth material within the one or more apertures, thereby providing the one or more epicrystalline growth structures. Advantageously, epicrystalline growth on a patterned substrate can be used to provide structures protruding from an initially substantially flat planar substrate. Such morphology can be used to improve the light-emitting characteristics of LED devices, combined with improved strain management of the underlying crystalline material forming the LED device.
[0016] Preferably, when the crystal template layer is patterned to provide one or more epicrystalline growth structures, forming one or more channels including the conductive material passing through at least the first epitaxial crystal layer and the second epitaxial crystal layer includes removing material from one or more sidewalls of the one or more epitaxial growth structures. Advantageously, material removal to form channels passing through at least the first epitaxial crystal layer and the second epitaxial crystal layer enables electrical connection to the crystal template layer through the first epitaxial crystal layer and the second epitaxial crystal layer.
[0017] Preferably, the method includes planarizing at least a portion of the second epitaxial layer to form a third epitaxial layer, the third epitaxial layer being pseudocrystalline along with the second epitaxial layer. Advantageously, the third epitaxial layer provides a surface for forming a functional device.
[0018] Preferably, the method includes forming a material in the one or more channels, preferably wherein the material forms a portion of the third epitaxial layer. Preferably, the third epitaxial layer is a conductive layer, preferably the third epitaxial layer is in electronic communication with the crystal template layer, and / or wherein the third epitaxial layer forms part of an active region configured to emit light in response to carrier recombination. Advantageously, the device formed on the third epitaxial layer can then contact and be electrically connected to the underlying crystal template. Advantageously, when the active region of the third epitaxial layer is formed and configured to emit light in response to carrier recombination, light generation efficiency is improved. Advantageously, when the active region of the third epitaxial layer is formed on the sidewalls of a patterned crystal template layer, improved electrical connection and carrier injection into the third epitaxial layer, coupled with the strain-relaxed second epitaxial layer, provide improved light generation from a device at least partially formed on the second epitaxial layer.
[0019] Preferably, at least one of the crystal template layer, the first epitaxial crystal layer, the second epitaxial crystal layer, and the third epitaxial crystal layer comprises a semiconductor material, preferably a group III-V based material, more preferably a group III-V based material. Advantageously, the technique used to provide such a material can provide a high-quality crystalline material with a low defect density.
[0020] Preferably, the epitaxial crystal structure forms part of the light-emitting device. Advantageously, strain relaxation is managed in conjunction with conductivity to form a high-quality, practical device.
[0021] Preferably, the light-emitting device forms part of a light-emitting pixel array. Advantageously, the light-emitting pixel array can be formed on a strain-relaxed layer, such that the in-plane lattice parameters are suitable for the material requirements, thus providing a higher quality device that can be electrically connected on both sides, thereby increasing the pixel density in the array.
[0022] Other aspects of the invention will be apparent from the description and the appended claims. Attached Figure Description
[0023] The detailed description of the embodiments of the present invention is given only by way of examples and reference drawings, wherein: Figure 1A A cross-sectional view showing the epitaxial crystal structure; Figure 1B show Figure 1A A cross-sectional view of the epitaxial crystal structure after further processing; Figure 2A A cross-sectional view showing an epitaxial crystal structure containing V-shaped pits; Figure 2B show Figure 2A A cross-sectional view of the epitaxial crystal structure after further processing; Figure 2C show Figure 2B A cross-sectional view of the structure after further processing; Figure 3A A cross-sectional view showing an epitaxial crystal structure containing V-shaped pits and V-shaped grooves; Figure 3B show Figure 3A A cross-sectional view of the structure after further processing; Figure 3C show Figure 3B A plan view of the structure; Figure 3D show Figure 3B A cross-sectional view of the structure after further processing; Figure 4A show Figure 1B A cross-sectional view of the structure after further processing; Figure 4B show Figure 4A A cross-sectional view of the structure after further processing; Figure 5A A cross-sectional view showing the epitaxial structure formed on a template; and Figure 5B show Figure 5A The cross-sectional view of the structure after further processing. Detailed Implementation
[0024] The following describes the formation of a strain-relaxed epitaxial layer on which a functional solid-state device can be formed. This structure and the method for forming this structure solve some of the problems mentioned above. Figures 1A to 5B The formation of strain-relaxed layers in epitaxial crystal structures is described, wherein the strain-relaxed layers have inherent, natural lattice parameters that differ from those of the substrate on which the strain-relaxed layers are formed. Forming such strain-relaxed layers means that subsequent layers with inherent lattice parameters more closely aligned with the strain-relaxed layers can be formed, and thus can be formed with higher crystal quality and fewer defects.
[0025] The methods and structures described herein are based on group III-V crystalline materials, particularly nitride-based semiconductor materials. However, those skilled in the art will understand that the techniques described herein can be applied to different crystal structures and semiconductor materials, such as other group III-V or group II-VI crystalline materials, in other embodiments. Advantageously, this structure not only provides a template layer for forming a material with natural lattice parameters more closely aligned with the template compared to the underlying bulk substrate layer, but also allows for the formation of a material with natural lattice parameters more closely aligned with the template on a conductive template, thus enabling the formation of practical functional devices with high crystal quality, such as high-resolution arrays of light-emitting diode (LED) devices.
[0026] Figure 1A A cross-sectional view of the epitaxial structure 100A is shown. The epitaxial structure 100A provides an initial template for forming a device and is formed by metal-organic chemical vapor deposition (MOCVD). In other embodiments, alternative and / or additional growth and / or deposition techniques may be used to provide the epitaxial layers described herein. In this embodiment, molecular beam epitaxy (MBE) is used. Light-emitting diode (LED) devices are typically formed by providing a growth substrate on which multiple epitaxial layers of semiconductor crystalline material are grown and / or deposited to form a functional device. For gallium nitride (GaN)-based LED devices, n-type doped n-GaN is typically provided as a base layer for forming pn junctions. The structure provided by the epitaxial structure 100A is fabricated to enable the formation of a device, such as an LED device with high-quality crystalline material, while simultaneously enabling the device to be formed on a conductive layer.
[0027] exist Figure 1A The diagram shows a growth substrate 102. The growth substrate 102 is formed of silicon. In other embodiments, alternative and / or additional materials may be used to form the substrate, such as sapphire, silicon carbide, or any other suitable substrate material. On the growth substrate 102, n-type doped n-GaN is provided, which effectively serves as a crystallization template layer 104. Although the crystallization template layer 104 is shown as an n-type GaN layer, in other embodiments, alternative and / or additional layers, such as buffer layers, are included to control the characteristics of the n-GaN layer (e.g., crystal quality, doping level, thickness, etc.). The thickness of the crystallization template layer 104 is approximately 1000 nm, and it is laid with a density of 5 × 10⁻⁶ nm. 18 at / cm 3 The concentration of doping is varied. In other embodiments, the crystal template layer 104 is formed with different thicknesses and different doping concentrations, while still achieving the functionality described herein. In other embodiments, the crystal template layer 104 is a p-type doped layer to provide the functionality described herein, and the composition of subsequently formed layers is adjusted accordingly.
[0028] A first epitaxial layer 106 is formed on top of an n-type template layer 104, and the first epitaxial layer 106 is formed of gallium nitride (GaN). Therefore, the first epitaxial layer 106 has the same natural, relaxed, in-plane lattice constant as the template layer 104. In other embodiments, the first epitaxial layer 106 is formed of a different material than the template layer 104 and is pseudocrystalline. The first epitaxial layer 106 is formed as a highly doped layer, wherein the doping results in an initial doping contrast between the highly doped first epitaxial layer 106 and the n-type template layer 104. This contrast allows the first epitaxial layer 106 to become porosilicated in subsequent steps, as described below. Figure 1B The first epitaxial layer is approximately 30 nm thick and initially has a thickness of 1 × 10⁻⁶ nm. 20 at / cm 3The doping concentration is on the order of magnitude. This doping concentration is achieved using Si. In other embodiments, co-doping of Si and Al is used to achieve such a doping concentration while preventing excessive surface roughening. In other embodiments, the first epitaxial layer 106 is formed alternatively and / or additionally using different techniques, concentrations, and thicknesses. Advantageously, after porosification, a highly defective layer is provided using a thin first epitaxial layer 106 on the order of 30 nm, where broken bonds allow for the movement of dislocations. In other embodiments, the thickness of the first epitaxial layer 106 is between 1 nm and 300 nm, preferably between 20 nm and 50 nm. In other embodiments, the first epitaxial layer 106 is initially doped with a concentration of 8 × 10⁻⁶. 18 at / cm 3 and 5 × 10 20 at / cm 3 Between and preferably in 3 × 10 19 at / cm 3 and 1 × 10 20 at / cm 3 The first epitaxial layer 106 is co-doped with Al and Si in molar fractions between 0.5% and 10%, and preferably between 1% and 3%.
[0029] A second epitaxial layer, namely an undoped layer 108, is provided above the first epitaxial layer 106. The undoped second epitaxial layer 108 is a layer whose lattice constant is inherently different from that of the crystal template layer 104 and the first epitaxial layer 106. Figure 1AIn one embodiment, the second epitaxial layer 108 is an undoped indium gallium nitride (InGaN) layer. The thickness of the undoped second epitaxial layer 108 is approximately 100 nm to 150 nm. Advantageously, the second epitaxial layer 108 has a thickness capable of achieving elastic relaxation. Therefore, the growth of the second epitaxial layer 108 causes the second epitaxial layer 108 to be initially strained by the underlying material of the crystal template layer 104 and the first epitaxial layer 106, such that the different inherent, natural, in-plane lattice parameters of the second epitaxial layer 108 are pseudomorphically aligned with the inherent, natural, in-plane lattice parameters of the first epitaxial layer 106. In other embodiments, the second epitaxial layer 108 may be formed to different thicknesses while achieving the functions described herein. In one embodiment, the thickness of the second epitaxial layer 108 is between 100 nm and 500 nm. In other embodiments, the thickness of the second epitaxial layer 108 is preferably between 150 nm and 200 nm. The second epitaxial layer 108 is a bulk InGaN layer with an In content between 0% and 25%, preferably between 6% and 15%. While the second epitaxial layer 108 is a bulk InGaN layer, in other embodiments, it is a multilayered superlattice structure with alternative chemical compositions, providing an average indium content between 0% and 25% in the InGaN, preferably between 6% and 15%. In embodiments where the second InGaN epitaxial layer is a superlattice structure, the lattice constant, inherently different from that of the crystal template layer 104, relates to the average composition of the entire superlattice layer forming the second epitaxial layer.
[0030] Providing an epitaxial structure 100A with a high doping contrast between the first epitaxial layer 106, the template layer 104, and the second epitaxial layer 108 enables the initially highly doped first epitaxial layer 106 to become porosilicated. Porosilicated first epitaxial layer 106 occurs through an electrochemical process. An electrochemical etching process can be selectively used to etch the epitaxial layers, such that the most conductive layer is etched first. Epitaxial structures (e.g.) Figure 1A Porosification of the buried layer in the epitaxial structure 100A can occur via threading dislocation nuclei in the second epitaxial layer 108. Advantageously, it is not necessary to erode the topmost second epitaxial layer 108 and not to pattern the second epitaxial layer 108 to porosilicate the lower surface layer. Although the second epitaxial layer 108 is described as an undoped layer 108, in other embodiments, the undoped second epitaxial layer 108 has a doping level that provides sufficient conductivity contrast to enable porosification of the lower surface layer according to the methods described herein.
[0031] Electrochemical etching of the epitaxial structure 100A causes porosity in the first epitaxial layer 106 through line packing or other openings in the undoped InGaN of the second epitaxial layer 108, enabling this electrochemical process to occur in the subsurface first epitaxial layer 106. This is facilitated by the high doping contrast between the n-type crystalline template layer 104 and the first epitaxial layer 106, meaning that only the first epitaxial layer 106 becomes porosity during electrochemical etching of this layer. Advantageously, the doping contrast allows for control of the porosity process because when the first epitaxial layer 106 has pores formed therein, the porosity of the first epitaxial layer 106' becomes high-resistivity, thus halting the formation of pores through the electrochemical process used to porosilicate the first epitaxial layer 106.
[0032] Therefore, once the epitaxial structure 100A has been electrochemically etched to provide a porous first epitaxial crystal layer 106', the first epitaxial crystal layer 106 becomes a porous and compliant epitaxial crystal layer 106'.
[0033] Figure 1B A fabricated version of epitaxial structure 100A is shown. Epitaxial structure 100B is a fabricated version of epitaxial structure 100A, wherein the first epitaxial layer 106 has been porosized to provide pores filling the first epitaxial layer 106'. This porosization enables strain relaxation of the undoped InGaN second epitaxial layer 108. This strain relaxation requires expansion of the second epitaxial layer 108. As described below, the lateral expansion of the second epitaxial layer 108 is controlled to provide a beneficial structure. The degree of porosization of the first epitaxial layer 106' depends on the volume, porosity, and GaN material density, and depends on the electrochemical etching process. While the electrochemical etching process beneficially provides compliant material in the underlying surface layer, the conductivity of the porosized first epitaxial layer 106' is reduced compared to the high-doped conductivity of the initially formed first epitaxial layer 106.
[0034] As described above, the initial strain to the second epitaxial layer 108 of the first epitaxial layer 106 should cause it to expand for relaxation. (See reference...) Figures 2A to 5B The expansion of the second epitaxial layer 108 is controlled by forming appropriate gaps and / or channels.
[0035] exist Figure 2A The image shows a cross-sectional view of epitaxial structure 200A, which is a processed epitaxial structure. Figure 1B The described epitaxial structure 100B has a crystal template layer 104, a porous first epitaxial crystal layer 106', and a second epitaxial crystal layer 108. The epitaxial structure 200A further shows V-shaped pits 202 in the surface of the second epitaxial crystal layer 108. These V-shaped pits 202 are formed during the formation of the n-type crystal template layer 104. Figure 2A The top layer 105 of the crystallization template layer 104 is shown. The top layer 105 is also formed of GaN; however, by altering the growth conditions during the formation of the crystallization template layer 104, V-shaped pits can be formed in the top layer 105. For example, lowering the growth temperature can induce V-shaped pits in the top layer 105 of the crystallization template layer 104. The thickness of this top layer 105 is on the order of 50 nm. Advantageously, this thickness will produce V-shaped pits in subsequent layers of appropriate thickness, thereby enabling the formation of channels through the epitaxial structure 200A. In other embodiments, the top layer 105 is designed to provide the configuration of the functions described herein. A cross-sectional view of the epitaxial structure 200A shows a V-shaped pit; however, in other embodiments, additional V-shaped pits are formed across the flat surface of the top layer 105 of the crystallization template layer. In this embodiment, such V-shaped pits are randomly formed on the top layer 105 of the crystallization template layer.
[0036] The formation of V-shaped pits in the top layer 105 of the crystallization template layer 104 causes the V-shaped pits to propagate through subsequently grown layers. Therefore, based on the V-shaped pits formed in the top layer 105 of the crystallization template layer 104, V-shaped pits 202 are formed in the surface of the second epitaxial crystallization layer 108. In other embodiments, additional and / or alternative techniques are used to form the V-shaped pits 202 in the second epitaxial crystallization layer 108.
[0037] Once one or more V-shaped pits 202 are formed in the second epitaxial crystallization layer 108, the epitaxial structure 200A is processed to enlarge the V-shaped pits 202, thereby opening one or more channels and exposing at least a portion of the crystallization template layer 104 and / or the top layer 105 of the crystallization template layer 104. This is in Figure 2B The image shows that the sidewalls of the V-shaped pit 202 have been etched.
[0038] Figure 2B The image shows a cross-sectional view of the epitaxial structure 200B, which has undergone further processing. Figure 2A The epitaxial structure 200A. In Figure 2B The image shows the enlargement of the V-shaped pit 202 by etching the sidewalls of the V-shaped pit 202. This is achieved through wet etching. Figure 2A The epitaxial structure 200A enables anisotropic etching. Wet etching is performed at high temperature using potassium hydroxide (KOH). In other embodiments, additional and / or alternative techniques are used to etch and enlarge the V-shaped pits 202. For example, tetramethylammonium hydroxide (TMAh) is used.
[0039] like Figure 2BAs shown, the sidewalls 208 of the undoped InGaN second epitaxial layer 108 are etched to provide an open path to the conductive GaN. Subsequently, the sidewalls 206 of the porous first epitaxial layer 106 and the sidewalls 205 of the top layer 105 of the V-shaped pits are enlarged. The etched V-shaped pits 202 are essentially the sum of the thickness of the porous first epitaxial layer 106' and the thickness of the undoped InGaN second epitaxial layer 108. Advantageously, this enlargement provides a pathway for electrical connection through the epitaxial structure 200B to the n-type crystalline template layer 104. Once the etching of the sidewalls 205, 206, 208 of the V-shaped pits 202 is complete to provide one or more channels at least through the porous first epitaxial layer 106' and the second epitaxial layer 108, the epitaxial structure 200B is further processed, as follows: Figure 2C As shown.
[0040] Figure 2C A cross-sectional view of the epitaxial structure 200C is shown, which has undergone further processing. Figure 2B The epitaxial structure 200B. In Figure 2C The image shows a conductive material, specifically an n-type material 210 formed within a channel, which is constructed from... Figure 2A The enlarged V-shaped pit 202 described in 2D provides this. The n-type material 210 also forms a third epitaxial layer, which is a thin pseudocrystalline layer of the n-type material 210 on top of the undoped InGaN second epitaxial layer 108. The n-type material 210 is in electrical contact with the n-type material of the crystal template layer 104, advantageously enabling current diffusion and facilitating contact via the n-doped side of the epitaxial structure 200C in the subsequently formed device. The n-type material 210 planarizes the structure. When formed from GaN, the planarized layer of the n-type material 210 is under tensile stress when the undoped InGaN second epitaxial layer 108 relaxes. Although the conductive n-type material 210 is formed from GaN, in other embodiments, the conductive material 210 is formed from a different material. In this embodiment, the conductive n-type material 210 is formed from InGaN, with an In content between 0% and 6%. The conductive material 210 is formed as a layer with a thickness between 5 nm and 300 nm, and preferably between 20 nm and 100 nm.
[0041] Although the conductive material formed in one or more channels provided by the V-shaped pit 202 is an n-type material 210, which is shown to planarize the structure, in other embodiments, alternatively or additionally, the conductive n-type material 210 partially planarizes or does not planarize the second epitaxial layer 108, while still at least partially filling one or more channels provided by the V-shaped pit 202 with conductive material, thereby providing conductivity to the relative strain relaxation region formed after the relaxation of the second epitaxial layer 108.
[0042] Another layer 212 is formed on top of the n-type material 210. In an embodiment, the other layer 212 is a multilayer epitaxial structure having an active region associated with providing red light from the InGaN-based quantum well (QW). Advantageously, the other layer 212 benefits from being formed on a conductive layer that is pseudocrystalline, similar to the second epitaxial layer 108. Although the other layer 212 is shown as being disposed on the n-type material 210, in other embodiments, the other layer 212 is disposed on both the n-type material 210 and the second epitaxial layer 108. In other embodiments, the other layer 212 includes one or more LED devices, and in other embodiments, it forms an array of devices, such as a high-resolution array of microLED devices. In other embodiments, another layer 212 alternatively and / or additionally forms a portion of the n-type material 210 and / or replaces the n-type material, thereby advantageously enabling carriers to be directly injected through another layer 212, which is at least partially formed on the sidewalls of the n-type crystal template layer 104, into portions of the strain-relaxed material formed on the second epitaxial crystal layer 108, such as the V-shaped pit top layer 105 of the crystal template layer 104.
[0043] Although according to Figures 2A to 2C The enlarged V-shaped pits 202 of structure 200 are described to provide a pathway for the formation of conductive material on the second epitaxial layer 108 and to promote strain relaxation in the second epitaxial layer 108. The position and density of the V-shaped pits 202 in the top layer 105 of the crystal template layer 104 are, to some extent, random. Appropriate growth techniques are used to control the density of the V-shaped pits 202 in the top layer 105 to achieve electrical connections in a controlled manner.
[0044] Figures 3A to 3D It showed a combination Figures 2A to 2C Further structures in epitaxial structures 200A to C are used to provide further control over the resulting template structure.
[0045] Figure 3A A cross-sectional view of the epitaxial structure 300A is shown. Epitaxial structure 300A was fabricated using additional steps. Figure 2A The structure in the middle is 200A.
[0046] Figure 3A A trench 304 formed in a crystallization template layer 104 is shown. The trench 304 is formed using a photolithography technique that uses patterning and etching steps to form the trench 304. In other embodiments, the crystallization template layer 104 uses different techniques to set the trench 304. The trench 304 is formed according to any beneficial structure of the crystallization template layer 104 to be subsequently processed.
[0047] Once the trench 304 is formed in the crystallization template layer 104, subsequent epitaxial layers 105, 106, and 108 are formed. This formation results in V-grooves 302 in the epitaxial structure 300A corresponding to the trench 304. V-shaped pits are also formed in the top layer 105 of the crystallization template layer 104 and are provided by layer propagation to provide both V-shaped pits 202 and V-grooves 302. In other embodiments, V-grooves 302 are provided without V-shaped pits 202.
[0048] Although trench 304 is shown as being formed in the crystallization template layer 104 prior to the formation of subsequent epitaxial layers, thereby enabling the formation of channels at least through the porous first epitaxial crystallization layer 106' and the second epitaxial crystallization layer 108, in other embodiments, trench 304 is formed by patterning the crystallization template layer 104 with a mask and forming a grain-attached growth material on the mask-patterned crystallization template layer 104. This technique is used to provide column arrays, each column having a regular trapezoidal cross-section perpendicular to the substrate, as described, for example, in WO 2020 / 008200 A1. As per [reference to...] Figure 5A and 5B In further detail, in other embodiments, this mask-patterned crystallization growth on the crystalline template layer 104 is used to provide an underlayer for forming an array of light-emitting devices. In other embodiments, the morphology of the crystalline template layer 104 is controlled by patterning and / or other techniques to provide a suitable underlayer substrate for improving device formation.
[0049] Once the V-groove 302 is formed, the process continues similarly to that shown in Figure 2. Figure 3B The image shows a cross-sectional view of the epitaxial structure 300B, which has undergone further processing. Figure 3A The epitaxial structure of 300A.
[0050] exist Figure 3B The image shows V-shaped pits 202 and V-shaped grooves 302 enlarged by etching the sidewalls. This is achieved through wet etching. Figure 3A The epitaxial structure 300A can achieve anisotropic etching of the epitaxial structure 300A. For example... Figure 3BAs shown, the sidewalls 308 of the second epitaxial layer 108 are etched. Subsequently, the sidewalls 306 of the porous first epitaxial layer 106' and the sidewalls 305 of the V-groove top layer 105 are enlarged. Advantageously, this enlargement provides space for the expansion and thus strain relaxation of the undoped InGaN second layer 108, and provides a pathway for the epitaxial crystals to be electrically connected to the n-type crystal template layer 104 via the epitaxial structure 300B. Advantageously, forming the V-groove 302 in this way provides a method for adjusting the width of the gaps in the subsequently formed material. This is beneficial in cases where forming V-grooves at a sufficiently small scale is impractical, for example, using photolithography to form V-grooves in the already formed epitaxial structure to provide a conduction path for the n-type material.
[0051] Through the Figure 3B The structure 300B is annealed to promote strain relaxation. In other embodiments, additional and / or alternative techniques are used to promote strain relaxation. Once the sidewalls 305, 306, and 308 of the V-groove 302 have been etched, the epitaxial structure 300B is further processed, such as... Figure 3D As shown. Figure 3C It showed Figure 3B A plan view 300C of the structure is shown. It shows V-shaped pits 202 randomly distributed in the surface of the second epitaxial layer 108. It also shows V-shaped grooves 302 forming a hexagonal pattern. Thus, the V-shaped grooves 302 isolate portions of the second epitaxial layer 108 of InGaN to form islands or domains by at least partially forming valleys around one or more islands in the second epitaxial layer 108, such that the valleys at least partially surround one or more islands in the second epitaxial layer 108. Although the V-shaped grooves 302 are shown in a hexagonal configuration, in other embodiments, the V-shaped grooves 302 are alternatively and / or additionally formed in any suitable configuration. Advantageously, this photolithographic patterning and etching based on the crystal template layer 104 forms two-dimensional islands in the second epitaxial layer 108, which provides strain-relaxed islands with lateral dimensions on the order of 1 μm to 10 μm. The formation of such islands is highly controllable and provides relaxation islands comparable in size to devices that can be formed on the relaxation islands, such as micro-LED devices with pixel sizes on the order of 1 μm to 10 μm. In other embodiments, the lateral dimensions of the islands are controlled such that the dimensions of the provided strain-relaxed islands are suitable for forming devices based on subsequently formed crystalline layers.
[0052] Once provided Figure 3B The epitaxial structure 300B is then planarized. This is shown in... Figure 3D middle. Figure 3D Structure 300D is shown, which has already undergone further processing. Figure 3BAn epitaxial structure 300B is shown. It illustrates an n-type material 210 formed in channels provided by V-grooves 302 and V-pits 202. These random V-pits 202, filled with the n-type material 210, provide uniform electron injection into subsequent layers. Figure 2C Similar to the epitaxial structure 200C, a subsequent pseudocrystalline layer 212 is formed on the planarization layer of the n-type material 210. When formed from n-GaN, the planarization layer of the n-type material 210 is under tensile stress because the underlying second epitaxial crystal layer 108 is relaxed. Although the conductive material formed in one or more channels provided by the V-groove 302 and / or etched V-groove 302 is shown as the conductive n-type material 210 for planarizing the structure, in other embodiments, alternatively or additionally, the conductive n-type material 210 partially planarizes or does not planarize the second epitaxial crystal layer 108, while still at least partially filling the conductive material into one or more channels provided by the V-groove 202 and / or V-groove 302, thereby providing conductivity to the relatively strain-relaxed region formed after the relaxation of the second epitaxial crystal layer 108.
[0053] Although the additional layer 212 is shown to be disposed on the n-type material 210, in other embodiments, the additional layer 212 is disposed on both the n-type material 210 and the second epitaxial crystal layer 108. In other embodiments, the additional layer 212 includes one or more LED devices, which in this embodiment form an array of devices, such as a high-resolution array of micro-LED devices. In other embodiments, the additional layer 212 alternatively and / or additionally forms a portion of the n-type material 210 and / or replaces the n-type material, thereby advantageously allowing carriers to be directly injected into portions of the strain-relaxed material formed on the second epitaxial crystal layer 108, such as the sidewalls of the enlarged V-groove 302, through the additional layer 212, which is at least partially formed on the sidewalls of the n-type crystal template layer 104.
[0054] Although the trenches 304 are formed in the crystal template layer 104 using photolithography and etching techniques, different patterning techniques are used in other embodiments. Furthermore, although the relative cross-sectional dimensions of the V-shaped pits 202 and V-shaped grooves 302 are... Figures 3A to 3D The V-groove 302 is shown to be significantly deeper than the V-pit 202, but in other embodiments, the V-groove 302 and the V-pit 202 have different relative dimensions. Advantageously, the V-pit 202 and the V-groove 302 effectively provide channels for electrical connections between the crystallization template layer 104 and the layers formed on the insulating second epitaxial crystallization layer 108. Advantageously, the V-pit 202 facilitates the uniform injection of electrons into the subsequently grown layers.
[0055] Advantageously, the V-groove 302 facilitates the relaxation of the second epitaxial crystal layer 108, and the V-pit 202 provides a channel for electrical connection with the crystal template layer 104. If the subsequently formed device (e.g., an LED device providing pixels with defined light-emitting surfaces) has a light-emitting surface area greater than the density of the V-groove 302, the structure may not require the V-pit 202, as current diffusion is sufficient through the V-groove 302. The V-pit 202 is particularly advantageous in providing sufficient current diffusion in the LED device associated with the pixel when, for example, the light-emitting surface area of the pixel is less than the density of the V-groove 302.
[0056] Figure 4A A cross-sectional view of epitaxial structure 400A is shown. Epitaxial structure 400A is Figure 1B A fabricated version of the epitaxial structure 100B. In order to provide a porous first epitaxial crystal layer 106' and then laterally relax the second epitaxial crystal layer 108, a channel is formed through the epitaxial structure 400A.
[0057] An epitaxial structure 400A is patterned on the surface of the second epitaxial layer 108 using a self-assembled hard mask. A nickel (Ni) film is evaporated onto the surface of the second epitaxial layer 108. The nickel film is then annealed to form random droplets. Dry etching is then used to form channels 402 through the epitaxial structure 400A to provide channels for the conductive n-type crystal template layer 104. The nickel mask is then removed using a wet cleaning technique. While the porosification of the first epitaxial layer 106 occurs before the formation of the channels 402, in other embodiments, alternatively or additionally, the channels 402 are formed before the porosification of the first epitaxial layer 106. Advantageously, these channels 402 formed to pass through the first epitaxial layer 106 (or the porosified first epitaxial layer 106') and the second epitaxial layer 108 at least partially define the periphery of two-dimensional domains or islands in the second epitaxial layer 108.
[0058] Once channel 402 is established, the process moves to... Figure 4B .exist Figure 4B The image shows a cross-sectional view of the epitaxial structure 400B, which is further processed to form a planarization layer 404 of the material in the channel 402. Figure 4AThe epitaxial structure 400A. Although the conductive material 404 formed in one or more channels is an n-type material 404, such as n-type GaN, which is shown to planarize the structure, in other embodiments, alternatively or additionally, the conductive n-type material 404 partially planarizes or does not planarize the second epitaxial crystal layer 108, while still at least partially filling one or more channels provided by channel 402 with conductive material 404, thereby providing conductivity to the relative strain relaxation region formed after relaxation of the second epitaxial crystal layer 108.
[0059] Another layer 412, using the InGaN red light emitting active region as an example, is then connected to the reference. Figure 2C and Figure 3D Another layer 212, as described, is formed on material 404 in a similar manner. In other embodiments, this other layer 412 forms one or more LED structures. In other embodiments, such LED structures form part of an array of LED devices, such as a high-resolution array of micro-LED devices. Although the other layer 412 is shown as being disposed on n-type material 404, in other embodiments, the other layer 412 is disposed on both n-type material 404 and the second epitaxial crystal layer 108. In other embodiments, the other layer 412 includes one or more LED devices, and in another embodiment, it forms an array of devices, such as a high-resolution array of micro-LED devices. In other embodiments, the other layer 412 alternatively and / or additionally forms a portion of n-type material 404 and / or replaces that n-type material, thereby advantageously enabling carriers to be directly injected through the other layer 412, which is at least partially formed on the sidewalls of the n-type crystal template layer 104, into portions of the strain-relaxed material formed on the second epitaxial crystal layer 108, for example, through the sidewalls of the channels 402 formed to the crystal template layer 104.
[0060] Advantageously, the small and dense self-assembled nickel droplets can produce very narrow gaps, thus facilitating strain relaxation and planarization. For narrow gaps, planarization can be achieved over short distances. Further filling these densely distributed gaps with n-type material 210 provides good current flow through the epitaxial structure 400B.
[0061] Advantageously, hard masks (e.g.) are used. Figure 4A and 4BThe self-assembled nickel hard mask can form densely packed two-dimensional islands in the second epitaxial layer 108, with lateral dimensions on the order of 250 nm to 1000 nm. Advantageously, islands formed at this scale not only facilitate planarization but also provide a uniform strain relaxation layer when the lateral dimensions of the islands are smaller than the lateral dimensions of the devices formed in the layer on the relaxation islands (e.g., the pixel size of a micro-LED device is typically greater than 1000 nm). This means that a strain relaxation layer with unknown dimensions can be effectively provided when the scale of the islands is smaller than the scale of the functional devices formed on the relaxation islands.
[0062] exist Figure 5A and 5B The image shows a porous first epitaxial crystal layer 106' and a second epitaxial crystal layer 108 formed on a crystal template layer 104, the morphology of which is provided by patterning the crystal template layer 104.
[0063] Figure 5A A cross-sectional view of the epitaxial structure 500A formed on a patterned substrate is shown. A reference is also shown. Figures 1A to 4B The crystallization template layer 104 is described. The crystallization template layer 104 is patterned using a mask 502 deposited using known techniques. Although the mask 502 is shown in cross-section, those skilled in the art will understand that the mask 502 may be formed in two dimensions to provide an array of apertures on the crystallization template layer. The mask 502 is formed using silicon dioxide. In other embodiments, the mask 502 is alternatively and / or additionally formed using other materials. The attached growth 504 of n-type GaN on the masked crystallization template layer results in the formation of GaN structures electrically connected to the n-type GaN crystallization template layer 104. The attached growth 504 is shown as forming... Figure 5A The structure has a trapezoidal cross-section; however, those skilled in the art will understand that this morphology of the epicrystalline growth 504 extends to three dimensions and is related to the underlying crystalline structure of the material used for the epicrystalline growth 504 structure. Once grown, the epicrystalline growth 504 structure becomes part of the crystalline template layer 104.
[0064] Figure 5A and 5BThe dimensions of the trapezoidal attached crystal growth 504 structure vary as a function of the height of the trapezoidal pyramid. The lateral dimension of the trapezoidal feature is on the order of 4 μm at the bottom and 3 μm at the top, with a height of approximately 1 μm. In other embodiments, the lateral dimension of the trapezoidal feature is controlled to provide alternative or additional features of different sizes. In other embodiments, the dimensions of the attached crystal growth 504 feature are controlled to provide laterally sized islands in the second epitaxial layer 108 suitable for forming microLED devices with pixel sizes on the order of 1 μm to 10 μm. Alternatively or additionally, island regions with lateral dimensions less than 1 μm are provided in the second epitaxial layer 108. Advantageously, forming two-dimensional islands in the second epitaxial layer 108 based on this photolithographic patterning and attached crystal growth provides strain relaxation islands with lateral dimensions on the order of 1 μm to 10 μm or smaller. The formation of such islands is highly controllable and provides relaxation islands comparable in size to devices that can be formed on the relaxation islands, such as micro-LED devices with pixel sizes on the order of 1 μm to 10 μm.
[0065] Once the 504 epitaxial growth structure is formed, the first highly doped epitaxial layer 106 is formed, such as... Figures 1A to 4B The first epitaxial crystal layer 106 is formed on the top and sidewalls of the attached crystal growth 504, which is formed in the aperture of the mask 502. The thickness of the first epitaxial crystal layer 106 on the top of the attached crystal growth 504 feature is approximately 30 nm. The growth rate of the crystalline material on different crystal planes, for example, the growth rate provided by the top and sidewalls of the attached crystal growth 504 structure, can be different and can be controlled, for example, by changing the growth rate of the crystalline material and the composition of the crystalline material. Therefore, the thickness of the crystalline layer deposited on different planes of the attached crystal growth 504 structure can be different. The thicknesses of the first epitaxial crystal layer 106 and the second epitaxial crystal layer 108 have been described above with respect to the layer thickness that is generally perpendicular (and therefore parallel to) the main growth direction to the underlying planar substrate. In the case that the thickness of the first epitaxial crystal layer 106 on the top of the attached crystal growth 504 feature is approximately 30 nm, the thickness of the first epitaxial crystal layer 106 on the sidewalls of the attached crystal growth 504 feature is on the order of 1 to 3 nm. In other embodiments, the thickness of the first epitaxial layer 106 on the sidewalls is varied. Advantageously, a relatively thin first epitaxial layer 106 on the sidewalls of the attached growth 504 feature means that the first epitaxial layer 106 on the sidewalls of the attached growth 504 feature can be directly etched away, as described below, to provide a channel to the underlying n-GaN.
[0066] Subsequently, a second epitaxial layer 108 is formed on the first epitaxial layer 106, for example, referring to... Figures 1A to 4B As described above. Figures 1A to 4BThe second epitaxial crystal layer 108 is initially strained by the crystal template layer 104 and the underlying material of the first epitaxial crystal layer 106, causing the different inherent, natural, and in-plane lattice parameters of the second epitaxial crystal layer 108 to pseudomorphically align with the inherent, natural, and in-plane lattice parameters of the first epitaxial crystal layer 106. The thickness of the second epitaxial crystal layer 108 at the top of the attached crystal growth 504 feature is between 100 nm and 150 nm. (As mentioned above...) Figure 5A As described in the first epitaxial crystalline layer 106, the growth rates of the crystalline material on different crystal planes can be different, for example, those provided by the top and sidewalls of the attached crystal growth 504 structure may differ. In the case where the thickness of the second epitaxial crystalline layer 108 on the top of the attached crystal growth 504 feature is approximately 100 to 150 nm, the thickness of the second epitaxial crystalline layer 108 on the sidewalls of the attached crystal growth 504 feature is on the order of 5 to 20 nm. In other embodiments, the thickness of the second epitaxial crystalline layer 108 on the sidewalls is varying.
[0067] Electrochemical etching of the epitaxial structure 500A causes porosity in the first epitaxial layer 106 through line packing or other openings in the undoped InGaN of the second epitaxial layer 108, enabling this electrochemical process to occur in the subsurface first epitaxial layer 106. The high doping contrast between the n-type crystalline template layer 104 and the first epitaxial layer 106 facilitates this, meaning that only the first epitaxial layer 106 becomes porosity during electrochemical etching of this layer. Advantageously, the doping contrast allows for control of the porosity process because when the first epitaxial layer 106 has pores formed therein, the porosity of the first epitaxial layer 106' becomes high-resistivity, thus stopping the electrochemical process used to porosilicate the first epitaxial layer 106. The porosity of the first epitaxial layer 106' is shown in... Figure 5B .
[0068] Figure 5B The epitaxial structure 500B is shown, which has undergone further processing. Figure 5AStructure 500A is provided to offer an array of light-emitting structures. It illustrates a porous first epitaxial layer 106' formed on top of the attached growth 504 structure and a second epitaxial layer 108 formed on the porous first epitaxial layer 106'. The porous first epitaxial layer 106 results in the removal of material from the channels between the attached growth 504 structures, which are located on the sidewalls of the attached growth 504 structure. In other embodiments, material from the sidewalls of the attached growth 504 structure is removed in different ways to form channels through the porous first epitaxial layer 106' and the second epitaxial layer 108, forming a path through layers 106', 108 to the n-type GaN of the attached growth 504 structure formed on the crystal template layer 104. Advantageously, in GaN-based structures, for example... Figure 5A and 5B The described epitaxial structures 500A and 500B typically have a growth direction perpendicular to the c-plane, and the etching rate of the inclined surface (e.g., the sidewalls of the attached growth 504 structure) is faster than that of the c-plane material (e.g., the material formed on top of the attached growth 504 structure). This means that the porous first epitaxial layer 106' and the second first epitaxial layer 108 can be etched from the sidewalls of the attached growth 504 structure at a faster rate than the material formed on top of the attached growth 504 structure. Therefore, it is beneficial to remove material to form channels through the porous first epitaxial layer 106' and the second epitaxial layer 108 to n-GaN.
[0069] Removing the porosity of the first epitaxial layer 106' and the second epitaxial layer 108 effectively creates two-dimensional domains or islands within the second epitaxial layer 108. Porositizing the first epitaxial layer 106 causes strain relaxation in the undoped InGaN second epitaxial layer 108. This strain relaxation requires expansion of the second epitaxial layer 108. As described herein, the lateral expansion of the second epitaxial layer 108 is controlled to provide a beneficial structure. The degree of porositization of the first epitaxial layer 106' depends on the volume, porosity, and GaN material density, and is dependent on the electrochemical etching process. While the electrochemical etching process beneficially provides compliant material in the underlying surface layer, the conductivity of the porositized first epitaxial layer 106' is reduced compared to the high-doped conductivity of the initially formed first epitaxial layer 106. Advantageously, the porosity of the first epitaxial crystal layer 106' and the second epitaxial crystal layer 108 is removed to effectively generate two-dimensional domains or islands in the second epitaxial crystal layer 108, and also to establish channels for the electrical connection between the subsequently grown layers grown on the second epitaxial crystal layer 108 and the crystal template layer 104.
[0070] Another floor, 506 (similar to the above) Figures 2A to 4BAnother layer (212, 412) is conformally deposited and formed on the relaxed second epitaxial crystal layer 108. This other layer 506 is the active region. The other layer 506 includes one or more quantum wells, such as InGaN-based quantum wells, which are designed to emit light with a dominant wavelength corresponding to red light during carrier injection and recombination. In other embodiments, the other layer 506 includes additional and / or alternative layers that benefit from the formation on the relatively relaxed second epitaxial crystal layer 108. The other layer 506 is a third epitaxial crystal layer that provides a conductive path from the n-GaN epitaxial growth 504 forming a portion of the crystal template layer 104 to the portion of the active region formed on the relaxed second epitaxial crystal layer 108.
[0071] A p-type region 508 is formed on another layer 506. The p-type region 508 is conformally deposited and formed on the top of the attached growth structure 504 and on the sidewalls of the attached growth structure 504. The p-type region 508 is formed of p-type doped GaN. In other embodiments, the p-type region 508 is formed with additional and / or replacement layers.
[0072] Advantageously, Figure 5B Structure 500B provides an array of light-emitting diode structures with active regions formed on a relatively strain-relaxed layer (with a lattice constant closer to that of the material forming the active region), thereby providing a high-quality light-emitting region with higher efficiency. Forming this active region on the attached crystal growth 504 structure improves light extraction from the device based on this high-quality light-emitting region and improves collimation.
[0073] Advantageously, when a third epitaxial layer, electrically connected by a porous first epitaxial layer 106' and a second epitaxial layer 108, forms a partial active region on one or more sidewalls of one or more epitaxial growth 504 structures, it provides a DC electron path between the active regions of another layer 506 on the islands of the crystal template layer 104 and the second epitaxial layer 108. Advantageously, this implantation can be controlled and the implanted sidewalls can reduce the forward voltage of the multi-quantum well (MQW) structure that forms a portion of this other layer 506 with a high operating current.
[0074] Although Figure 5B Mask 502 is shown, but in other embodiments, mask 502 is removed after the attached growth 504 step. Furthermore, although another layer 506 and p-type region 508 are conformally formed on the attached growth 504 structure, individual structures can be selectively separated, thereby enabling the formation of multiple individually addressable light-emitting diode structures with a common n-type electrode formed by the crystal template layer 104.
[0075] Advantageously, the techniques and structures described herein provide a method for forming a relatively strain-relaxed layer on a conductive template layer, while simultaneously achieving electrical connections between the conductive template layer and layers subsequently grown on the relatively strain-relaxed layer. Advantageously, an epitaxial crystalline layer having an inherent in-plane lattice parameter different from that of the crystalline template layer is formed on an intermediate layer, such that, in the case where the epitaxial crystalline layer is formed relative to the intermediate layer pseudomorphic, the porous intermediate layer, together with the channels formed through the porous intermediate layer and the epitaxial crystalline layer, achieves strain relaxation in the epitaxial crystalline layer and provides a pathway for injecting current into the device formed on the relaxed epitaxial crystalline layer.
[0076] Advantageously, the formation and filling of channels with material to achieve electrical connections overcomes the difficulties associated with using high-resistivity layers for strain relaxation, thereby providing a functional device. Advantageously, the use of channels having faces angled relative to a direction perpendicular to the planar growth direction of the epitaxial layer provides an inclined surface on which connections to the underlying crystalline template layer can be generated, while simultaneously providing strain-relaxed light-emitting structures on separate islands of a relative strain-relaxing material having an intrinsic in-plane lattice parameter different from that of the crystalline template layer on which the relative strain-relaxing material is formed.
[0077] Advantageously, light-emitting diode (LED) devices can be formed in Figures 1A to 5B Structurally, it is advantageous to form an LED array with pixel-associated characteristics on the strain relaxation layer, while simultaneously achieving n-type contacts through n-type regions, even when the strain relaxation uses a high-resistivity porous layer. This eliminates the need to form conductive layers of material from the same side of the device or to form contacts for p-type and n-type layers within the LED device. This is particularly advantageous for longer-wavelength InGaN-based light-emitting devices, such as LEDs configured to emit light with a main peak wavelength corresponding to red light, formed from nitride materials, where undoped InGaN strain relaxation islands can be used instead of typically poor-quality, thicker InGaN conductive layers. Furthermore, enabling conduction to form n-type contacts on the side of the device opposite to the p-type contacts means that pixels associated with the LED devices in the array can be arranged more closely, thereby improving the resolution of display devices based on such arrays.
[0078] Although the processes described herein are given in a particular order, those skilled in the art will understand that alternative and / or additional sequences of steps and processes may be implemented in other embodiments, while achieving the provided functionality.
Claims
1. A method for forming a strain-relaxed layer in an epitaxial crystalline structure, the method comprising: A crystallization template layer is provided, the crystallization template layer comprising a material having a first natural relaxation in-plane lattice parameter; A first epitaxial crystal layer is formed on the crystal template layer, wherein the initial conductivity of the first epitaxial crystal layer is higher than the conductivity of the crystal template layer; A second epitaxial crystal layer is formed on the first epitaxial crystal layer, wherein the electrical conductivity of the second epitaxial crystal layer is lower than the initial electrical conductivity of the first epitaxial crystal layer, and the second epitaxial crystal layer includes a material having a second naturally relaxed in-plane lattice parameter, which is different from the first naturally relaxed in-plane lattice parameter of the crystal template layer. By electrochemically etching the first epitaxial layer to form pores, strain relaxation in the second epitaxial layer is achieved through plastic deformation of the bonds in the first epitaxial layer and / or at the interface between the first and second epitaxial layers; and One or more channels containing conductive material are formed, the one or more channels passing through at least the first epitaxial crystal layer and the second epitaxial crystal layer, thereby realizing an electrical connection to the crystal template layer through the first epitaxial crystal layer and the second epitaxial crystal layer.
2. The method as described in claim 1, wherein, Between the crystallization template layer and the second epitaxial crystallization layer, the volume density of the pores formed in the first epitaxial crystallization layer is greater than 50%.
3. The method as described in claim 1, wherein, The second epitaxial layer contains at least one V-shaped pit.
4. The method of claim 3, further comprising enlarging the at least one V-shaped pit.
5. The method of claim 1, comprising etching through at least the second epitaxial layer to form one or more islands in the second epitaxial layer.
6. The method of claim 1, comprising forming the crystallization template layer on the patterned template layer.
7. The method of claim 6, wherein the patterned template layer is patterned to provide grooves.
8. The method of claim 6, wherein the crystallization template layer is patterned to provide one or more epicrystalline growth structures.
9. The method of claim 1, further comprising planarizing at least a portion of the second epitaxial layer to form a third epitaxial layer, wherein the third epitaxial layer and the second epitaxial layer are pseudocrystalline, wherein... The conductive material forms part of the third epitaxial crystalline layer.
10. The method of claim 9, wherein, The third epitaxial layer is a conductive layer.
11. The method of claim 1, comprising a third epitaxial crystal layer, wherein at least one of the crystal template layer, the first epitaxial crystal layer, the second epitaxial crystal layer and the third epitaxial crystal layer comprises a semiconductor material.
12. An epitaxial crystal structure, comprising: A crystal template layer comprising a material having a first natural relaxation in-plane lattice parameter; A first epitaxial crystallization layer is formed on the crystallization template layer; A second epitaxial crystal layer is formed on the first epitaxial crystal layer, wherein the second epitaxial crystal layer includes a material having a second naturally relaxed in-plane lattice parameter, which is different from the first naturally relaxed in-plane lattice parameter of the crystal template layer. One or more pores formed in the first epitaxial layer, such that any strain in the second epitaxial layer is relaxed by plastic deformation of the bonds in the first epitaxial layer and / or at the interface between the first and second epitaxial layers; and One or more channels containing conductive material are formed to pass through at least the first epitaxial crystal layer and the second epitaxial crystal layer, thereby achieving an electrical connection through the first epitaxial crystal layer and the second epitaxial crystal layer to the crystal template layer.
13. The epitaxial crystal structure as described in claim 12, comprising a third epitaxial crystal layer, wherein the third epitaxial crystal layer and the second epitaxial crystal layer are pseudocrystalline.
14. The epitaxial crystal structure as described in claim 12, wherein, Between the crystallization template layer and the second epitaxial crystallization layer, the volume density of the one or more pores formed in the first epitaxial crystallization layer is greater than 50%.
15. The epitaxial crystal structure as described in claim 12, wherein, The second epitaxial layer contains at least one V-shaped pit.
16. The epitaxial crystal structure as described in claim 15, wherein, The at least one V-shaped pit exposes at least a portion of the crystallization template layer.
17. The epitaxial crystal structure of claim 12, comprising one or more islands formed in the second epitaxial crystal layer.
18. The epitaxial crystal structure of claim 17, comprising one or more valleys that at least partially surround the one or more islands in the second epitaxial crystal layer, thereby enabling the formation of one or more two-dimensional domains.
19. The epitaxial crystal structure of claim 13, wherein the conductive material forms a portion of the third epitaxial crystal layer.
20. The epitaxial crystal structure as described in claim 13, wherein, The third epitaxial layer is a conductive layer.
21. The epitaxial crystal structure of claim 12, comprising a third epitaxial crystal layer, wherein at least one of the crystal template layer, the first epitaxial crystal layer, the second epitaxial crystal layer and the third epitaxial crystal layer comprises a semiconductor material.
22. A light-emitting device comprising an epitaxial crystal structure as described in any one of claims 12 to 21.
23. A light-emitting pixel array, comprising at least one light-emitting device as described in claim 22.
24. A method for forming a light-emitting device, comprising the method as described in any one of claims 1 to 11.
25. A method of forming an array of light-emitting pixels, comprising the method of claim 24.
Citation Information
Patent Citations
Monolithic LED array and a precursor thereto
WO2020008200A1
Transfer of a thin layer from a wafer comprising a buffer layer
CN1666330A