Highly stable outer packaging material for battery devices
By using nickel-plated steel plates and gradient-distributed anti-corrosion layers in the metal-plastic composite film of lithium-ion batteries, the problem of separation between the metal layer and the outer substrate resin layer under high temperature and high humidity conditions is solved, thereby improving the battery's durability and service life.
Patent Information
- Application Number
- CN202211488618.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2022-09-02
- Filing Date
- 2022-11-25
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-11-25
AI Technical Summary
In existing lithium-ion batteries, the metal-plastic composite film is prone to separation between the metal layer and the outer substrate resin layer under high temperature and high humidity conditions, leading to blistering and corrosion of the battery casing and affecting the battery's lifespan.
Nickel-plated steel sheet is used as the intermediate metal layer, and a gradient distribution of anti-corrosion layer is formed on its surface. The anti-corrosion layer is formed by treatment with anti-corrosion liquid, which includes trivalent chromium compounds, inorganic acids, organic resins and crosslinking agents, etc., to improve the bonding strength between the metal layer and the outer substrate resin layer.
It improves the durability and damp heat peel strength of the metal-plastic composite film, prevents the separation of the metal layer from the outer substrate resin layer in high temperature and high humidity environments, and extends the battery's service life.
Smart Images

Figure CN115799734B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the technical field of lithium-ion batteries, and more specifically to an outer packaging material for a highly stable battery device. Background Technology
[0002] Currently, lithium-ion batteries are mainly divided into three categories: square, cylindrical, and pouch. The square and cylindrical batteries mainly use hard shells such as aluminum alloy and stainless steel. The aluminum alloy shell can be made of aluminum material, while the pouch shell, which is made of metal and resin, uses a metal-plastic composite film, which greatly improves the problem of inflexible shape design of hard-pack batteries.
[0003] The metal-plastic composite film consists of, from the outside in, an outer substrate resin layer, a middle metal layer, an inner adhesive layer, and a heat-fused resin layer. As a battery outer casing material, the metal-plastic composite film is required to have temperature and humidity resistance to prevent problems such as delamination of the battery casing and ensure battery life.
[0004] Generally, the metals in the metal-plastic composite film used for lithium-ion battery packaging require anti-corrosion treatment. If the anti-corrosion treatment is ineffective, the adhesion between the outer substrate resin layer and the intermediate metal layer may become unstable under harsh environments during battery use, such as high temperature and high humidity, causing separation between the two. This can lead to blistering of the outer layer of the battery casing or corrosion of the intermediate metal layer, resulting in a drastically shortened battery life. Therefore, the anti-corrosion treatment of the metals has a significant impact on the metal-plastic composite film.
[0005] Currently, the main components of the anti-corrosion treatment solution for metal-plastic composite films are trivalent chromium compounds, fluorides, aminophenolic resins, and phosphoric acid. After being treated with this anti-corrosion solution, the corrosion resistance of the metal-plastic composite film can be improved in some common electrolyte environments. However, during long-term use, moisture may penetrate the battery packaging, causing the intermediate metal layer to separate from the outer substrate resin layer, resulting in blistering on the outer layer of the battery casing. In this case, the anti-corrosion treatment effect of the solution will be unsatisfactory, easily causing interlayer separation of the metal-plastic composite film used in lithium-ion batteries, thus affecting the promotion and use of metal-plastic composite films in the lithium-ion battery field. Summary of the Invention
[0006] In view of this, the present invention aims to provide a metal-plastic composite film that solves the shortcomings of existing metal-plastic composite films, such as poor durability and low peel strength between the metal layer and the outer substrate resin layer, while improving the durability and wet heat peel strength of the metal-plastic composite film.
[0007] To achieve the above objectives, the technical solution of the present invention is implemented as follows:
[0008] This invention provides a highly stable outer packaging material for battery devices, characterized in that it includes an intermediate metal layer and an anti-corrosion layer formed by treating the intermediate metal layer with corrosion resistance.
[0009] Characteristically, it further comprises an outer substrate resin layer, an inner adhesive layer, and a hot-melt resin layer; the outer substrate resin layer is disposed on the intermediate metal layer, the intermediate metal layer is disposed on the inner adhesive layer, and the inner adhesive layer is disposed on the hot-melt resin layer; wherein the anti-corrosion layer is disposed between the outer substrate resin layer and the intermediate metal layer.
[0010] Characteristically, it further includes an outer adhesive layer, an outer substrate resin layer disposed on the outer adhesive layer, and the outer adhesive layer disposed on the anti-corrosion layer.
[0011] Characteristically, the metal of the intermediate metal layer is nickel-plated steel sheet, and the thickness of the nickel plating layer of the nickel-plated steel sheet is 0.5μm to 20μm.
[0012] A key feature is that the carbon and metal components of the anti-corrosion layer are distributed in a gradient.
[0013] Characteristically, the elemental composition of the anti-corrosion layer on the resin layer side of the outer substrate is distributed in a gradient. The outermost layer of the anti-corrosion layer on the resin layer side of the outer substrate has a carbon (C) content greater than or equal to 40% and less than or equal to 100%, a nickel (Ni) content less than or equal to 10%, and a fluorine (F) content less than or equal to 10%. In the layer 40 nm below the surface of the anti-corrosion layer, the carbon (C) content is less than or equal to 10%, the nickel (Ni) content is greater than or equal to 30% and less than or equal to 100%, and the fluorine (F) content is less than or equal to 20%.
[0014] Characteristically, the anti-corrosion layer is formed by drying an anti-corrosion liquid, which mainly contains trivalent chromium compounds, inorganic acids, organic resins, crosslinking agents, and solvents composed of water or organic solvents, or mixtures thereof.
[0015] Characteristically, the crosslinking agent contains at least one of the following: amino resin, melamine resin, phenolic resin, epoxy compound, end-capped isocyanate compound, oxazoline compound, carbodiimide compound, condensate of formaldehyde and alkyl alcohol having 1 to 4 carbon atoms, condensate of carbolic acid and formaldehyde, and derivatives of the above substances.
[0016] Characteristically, the anti-corrosion liquid used to form the anti-corrosion layer contains at least one of the following: trivalent chromium compound and crosslinking agent: chromium nitrate and chromium fluoride; and the anti-corrosion liquid used to form the anti-corrosion layer contains titanium (Ti) compound or zirconium (Zr) compound, with contents of 0 to 0.6% and 0 to 2.8%, respectively.
[0017] Characteristically, the inorganic acid in the anti-corrosion solution used to form the anti-corrosion layer is at least one of phosphoric acid, nitric acid, and hydrofluoric acid; the organic resin is at least one of acrylic resin, methacrylic resin, hydroxyacrylic resin, polyvinyl alcohol resin, and phenolic resin; the titanium (Ti) compound is at least one of titanium fluoride and titanium nitrate; the zirconium (Zr) compound is at least one of zirconium fluoride and zirconium nitrate; and the organic solvent is at least one of isopropanol, ethanol, and ethylene glycol butyl ether.
[0018] The beneficial effects of this invention are as follows:
[0019] 1) This invention provides a highly stable outer packaging material for battery devices. The intermediate metal layer is treated with corrosion resistance, thereby solving the shortcomings of poor durability and low peel force between the metal layer and the outer substrate resin layer of existing metal-plastic composite films. At the same time, it improves the durability and wet heat peel strength of the metal-plastic composite film.
[0020] 2) This invention provides a method for forming an anti-corrosion layer by drying an intermediate metal layer with an anti-corrosion liquid. The configuration of the anti-corrosion layer significantly improves the durability of the outer packaging material for lithium-ion battery devices and exhibits excellent resistance to damp heat.
[0021] 3) The present invention provides a high-durability battery, which reduces the poor durability of the battery device by using an outer packaging material containing the above-mentioned high-stability battery device, improves the disadvantage of low peel force between the metal layer and the outer substrate resin layer, and exhibits excellent resistance to damp heat.
[0022] 4) This invention proposes for the first time that the intermediate metal layer is made of nickel-plated steel plate material, and the elements in the surface anti-corrosion layer are distributed in a gradient. By controlling the carbon (C) content in the outermost layer of the anti-corrosion layer and the content of intermediate metal elements and fluorine (F) elements in the inner layer (40nm), the initial peel strength between the intermediate metal layer and the outer substrate resin layer of the metal-plastic composite film and its resistance in high temperature and high humidity environments can be improved. Attached Figure Description
[0023] Figure 1 The structure of the outer packaging material for the high-stability battery device provided by the present invention.
[0024] Component labeling explanation
[0025] 1…Outer substrate resin layer
[0026] 2…Intermediate metal layer
[0027] 3…Inner adhesive layer
[0028] 4…functional layer heat-fused resin layer
[0029] 5…Outer adhesive layer
[0030] 6… Anti-corrosion layer Detailed Implementation
[0031] The specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings. It should be understood that the specific embodiments described herein are for illustration and explanation only and are not intended to limit the present invention.
[0032] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.
[0033] The present invention provides an outer packaging material for a high-stability lithium-ion battery device.
[0034] This invention provides a highly stable outer packaging material (or metal-plastic composite film) for lithium-ion battery devices. This highly stable outer packaging material mainly comprises an outer substrate resin layer 1, an intermediate metal layer 2, an inner adhesive layer 3, and a heat-fused resin layer 4. The outer substrate resin layer 1 is disposed on the intermediate metal layer 2, the intermediate metal layer 2 is disposed on the inner adhesive layer 3, and the inner adhesive layer 3 is disposed on the heat-fused resin layer 4. The intermediate metal layer 2 undergoes corrosion-resistant treatment to form an anti-corrosion layer 6, which is disposed between the outer substrate resin layer 1 and the intermediate metal layer 2.
[0035] Specifically, it further includes an outer adhesive layer 5, an outer substrate resin layer 1 disposed on the outer adhesive layer 5, and the outer adhesive layer 5 disposed on the anti-corrosion layer 6 formed by the intermediate metal layer 2 after corrosion resistance treatment.
[0036] Specifically, the metal of the intermediate metal layer 2 is nickel-plated steel plate.
[0037] Specifically, the nickel plating thickness of the nickel-plated steel sheet ranges from 0.5 μm to 20 μm.
[0038] Specifically, the intermediate metal layer 2 forms an anti-corrosion layer 6 at least on the side of the outer substrate resin layer 1. The special anti-corrosion solution used mainly comprises trivalent chromium compounds, inorganic acids, organic resins, crosslinking agents, and solvents composed of water or organic solvents, or mixtures thereof. The proportions of the trivalent chromium compounds, inorganic acids, organic resins, water or organic solvents, or mixtures thereof are 1.9 to 6%, 0.3 to 6%, 0.6 to 6%, and 78.6 to 97.2%, respectively. The crosslinking agent accounts for 0.01 to 30% by mass of the solid components of the anti-corrosion layer 6, or 0.05 to 15% by mass based on the solid components of the solution used to form the anti-corrosion layer 6.
[0039] The anti-corrosion liquid is dried to form the anti-corrosion layer 6. The elemental composition of the intermediate metal anti-corrosion layer on both sides of the outer substrate resin layer 4 is distributed in a gradient. The outermost layer of the anti-corrosion layer 6 on both sides of the outer substrate resin layer 4 has a carbon (C) content greater than or equal to 40% and less than or equal to 100%, a nickel (Ni) content less than or equal to 10%, and a fluorine (F) content less than or equal to 10%. In the layer 40 nm below the surface of the anti-corrosion layer, the carbon (C) content is less than or equal to 10%, the nickel (Ni) content is greater than or equal to 30% and less than or equal to 100%, and the fluorine (F) content is less than or equal to 20%.
[0040] Specifically, the trivalent chromium compound and crosslinking agent in the anti-corrosion liquid used to form the anti-corrosion layer 6 are composed of at least one of chromium nitrate and chromium fluoride.
[0041] Specifically, the trivalent chromium compound is preferably at least one of chromium nitrate and chromium fluoride. Its function is to form a coordination cross-linking structure centered on chromium (Cr) atoms on the surface of the intermediate metal, and the trivalent chromium compound increases the degree of cross-linking of the anti-corrosion film on the surface of the intermediate metal.
[0042] Specifically, the crosslinking agent contains at least one of the following: amino resin, melamine resin, phenolic resin, epoxy compound, end-capped isocyanate compound, oxazoline compound, carbodiimide compound, condensate of formaldehyde and alkyl alcohol having 1 to 4 carbon atoms, condensate of carbolic acid and formaldehyde, and derivatives of the above substances.
[0043] Specifically, the crosslinking agent contains at least one of the following inorganic crosslinking materials: silicon compounds such as silicon dioxide, zirconium compounds such as ammonium zirconium fluoride or ammonium zirconium carbonate, metal chelates such as titanium chelates, and metal salts such as Ca, Al, Mg, Fe, and Zn.
[0044] Specifically, the anti-corrosion liquid used to form the anti-corrosion layer 6 contains titanium (Ti) compounds or zirconium (Zr) compounds, with contents of 0 to 0.6% and 0 to 2.8%, respectively.
[0045] Specifically, the inorganic acid in the anti-corrosion liquid used to form the anti-corrosion layer 6 is composed of at least one of phosphoric acid, nitric acid, and hydrofluoric acid; the organic resin is composed of at least one of acrylic resin, methacrylic resin, hydroxyacrylic resin, polyvinyl alcohol resin, and phenolic resin; the Ti compound is composed of at least one of titanium fluoride and titanium nitrate; the Zr compound is composed of at least one of zirconium fluoride and zirconium nitrate; and the organic solvent is composed of at least one of isopropanol, ethanol, and ethylene glycol butyl ether.
[0046] Specifically, the organic resin is composed of at least one of the following: acrylic resin, methacrylic resin, hydroxyacrylic resin, polyvinyl alcohol resin, olefin resin, and phenolic resin; the organic resin plays a role in improving the film-forming properties of the intermediate metal surface anti-corrosion layer and its adhesion to the inner adhesive layer 3.
[0047] Specifically, the inorganic acid is composed of at least one of phosphoric acid, nitric acid, and hydrofluoric acid, and the inorganic acid plays the role of removing the oxide film on the surface of the intermediate metal.
[0048] Specifically, titanium (Ti) compounds or zirconium (Zr) compounds serve as secondary central crosslinking points, enhancing the corrosion resistance of the intermediate metal surface.
[0049] Specifically, the organic solvent is composed of at least one of isopropanol, ethanol, and ethylene glycol butyl ether. The organic solvent reduces the surface tension of the anti-corrosion liquid and increases the leveling properties of the anti-corrosion liquid on the intermediate metal surface.
[0050] Specifically, if the nickel (Ni) content in the surface layer of the anti-corrosion layer 6, which has a gradient distribution of elements, is more than 10%, the degree of cross-linking reaction inside the anti-corrosion layer 6 is too high, the passivation layer is in a hard and brittle state, resulting in low composite strength. Furthermore, it is prone to cracking or pinholes in the subsequent molding process of the composite film, resulting in poor temperature and humidity resistance and causing delamination between the outer substrate resin layer 1 and the anti-corrosion layer 6.
[0051] A battery with stable bonding properties, characterized in that it comprises a highly stable outer packaging material for a battery device containing all of the above.
[0052] The characteristics of the corrosion-resistant layer 6 of the outer packaging material are as follows:
[0053] In lithium-ion battery packaging materials, forming an anti-corrosion layer on the intermediate metal layer in contact with the outer substrate resin layer ensures stable uniformity of the intermediate metal layer surface, reduces changes in adhesion (wetting properties), and prevents delamination between the outer substrate resin layer and the intermediate metal layer in long-term storage under high temperature and high humidity environments. Preferably, an anti-corrosion liquid is applied to at least the intermediate metal layer in contact with the outer substrate resin side to form an anti-corrosion layer; more preferably, anti-corrosion layers are formed on both sides of the intermediate metal layer. Forming an anti-corrosion layer on the intermediate metal layer in contact with the heat-fused resin layer prevents hydrogen fluoride generated from the reaction of electrolyte and moisture from corroding the intermediate metal layer surface, preventing separation between the intermediate metal layer and the heat-fused resin layer. Simultaneously, it maintains the uniformity of the intermediate metal layer surface, minimizing changes in adhesion (wetting properties), and effectively prevents delamination between the intermediate metal layer and the heat-fused resin layer in the metal-plastic composite film.
[0054] In this patent, the anti-corrosion layer is characterized by a gradient distribution of carbon components from the anti-corrosion layer and metal components from the intermediate metal layer between the outer substrate resin layer and the intermediate metal layer. That is, because the carbon components of the anti-corrosion layer from the outer substrate resin layer side increase the carbon components of the outer substrate resin layer in contact with the anti-corrosion layer, the stability of the composite of the outer substrate resin and the intermediate metal is ensured. If the adhesion between the outer substrate resin layer and the passivation layer is unstable, long-term storage in a high-temperature and high-humidity environment will lead to a decrease in adhesion and unstable peel strength. The measured increase in intermediate metal component in the anti-corrosion layer with depth indicates an increase in the adhesion between the anti-corrosion layer and the intermediate metal layer, and a gradual increase in the ability to resist external moisture intrusion. However, if the intermediate metal content in the measured anti-corrosion layer is too high, and the content of nickel (Ni) in the intermediate metal element on the surface of the anti-corrosion layer is greater than 10%, then the cross-linking reaction between the intermediate metal element and the anti-corrosion liquid is excessive. The resulting anti-corrosion layer has high hardness and is brittle. During subsequent molding and processing, the anti-corrosion layer is prone to cracking and pinholes, which leads to the intrusion of external moisture into the anti-corrosion layer, reduces the adhesion between the outer substrate resin layer and the passivation layer, and ultimately causes the outer substrate resin layer and the passivation layer to delaminate.
[0055] The composition of the anti-corrosion layer exhibits a sloping gradient distribution. Therefore, it can be inferred that the effective components in the anti-corrosion liquid will react with the resin components of the anti-corrosion layer on the side where the heat-fusion resin layer is formed. For example, the reaction products of the resin in the anti-corrosion layer with chromium (Cr), titanium (Ti), and zirconium (Zr), the reaction products of inorganic acid with chromium (Cr), and the reaction products of fluoride or inorganic acid in the intermediate metal layer and the anti-corrosion layer.
[0056] Building upon the above, this patent further specifies that the anti-corrosion layer is formed by drying the anti-corrosion liquid. The outermost layer of the anti-corrosion layer on the outer substrate resin layer side has a carbon (C) content greater than or equal to 40% and less than or equal to 100%, a nickel (Ni) content less than or equal to 10%, and a fluorine (F) content less than or equal to 10%. In the 40nm layer below the surface of the anti-corrosion layer, the carbon (C) content is less than or equal to 10%, the nickel (Ni) content is greater than or equal to 30% and less than or equal to 100%, and the fluorine (F) content is less than or equal to 20%. If the carbon (C) content of the outermost layer of the anti-corrosion layer on the outer substrate resin layer side is less than 40% or the nickel (Ni) content is greater than 10%, as mentioned above, the adhesion strength between the anti-corrosion layer and the outer substrate resin layer will be unstable and subject to the influence of external temperature and humidity, resulting in a decrease in peel strength during storage.
[0057] In this patent, the elements or components of the intermediate metal layer refer to the constituent elements of the intermediate metal layer and the intermediate metal layer elements detected in the products formed by the reaction of the constituent materials or electrolyte of the aforementioned anti-corrosion layer with the intermediate metal layer. When the intermediate metal layer is a nickel-plated steel plate, although it is a nickel-derived component, it also includes other added alloying components.
[0058] When determining the elements using the method described later, the elements detected in this patent include not only the components from the intermediate metal layer, but also the constituent elements of the anti-corrosion layer. Examples include carbon (C), oxygen (O), nitrogen (N), chromium (Cr), phosphorus (P), silicon (Si), fluorine (F), titanium (Ti), zirconium (Zr), and cerium (Ce).
[0059] Sometimes, trace amounts of metallic elements are added to the material forming the anti-corrosion layer. During measurement, if the element cannot be distinguished from the element from the intermediate metal layer, it can be measured entirely as a metallic element from the intermediate metal layer. Alternatively, it can be assumed that the metallic element added to the anti-corrosion layer is uniformly dispersed within the anti-corrosion layer, and the amount of metallic element added to the anti-corrosion layer can be subtracted from the amount of metallic element detected.
[0060] When the anti-corrosion layer is multi-layered, it can be judged by the single layer in contact with the intermediate metal layer, or by the entire multi-layered part.
[0061] As an example of an anti-corrosion layer, the anti-corrosion layer of the present invention may mainly comprise a film obtained by a coating-type anti-corrosion treatment, wherein the coating-type anti-corrosion treatment contains at least one component selected from rare earth element oxide sols, anionic polymers, and cationic polymers. The coating agent may also contain phosphoric acid, phosphates, or crosslinking agents for crosslinking the polymer. In the rare earth element oxide sol, particles of rare earth element oxides (e.g., particles with an average particle size of less than 100 nm) are dispersed in a liquid dispersion medium. Rare earth element oxides mainly include cerium oxide, yttrium oxide, neodymium oxide, lanthanum oxide, etc., with cerium oxide being preferred from the viewpoint of further improving adhesion. The rare earth element oxides included in the anti-corrosion layer may be used alone or in combination of two or more. As the liquid dispersion medium for the rare earth element oxide sol, various solvents such as water, alcohol solvents, hydrocarbon solvents, ketone solvents, ester compound solvents, and ether solvents may be used, with water being preferred. As cationic polymers, they mainly include polyethyleneimine, complex ionic polymers formed from polymers having polyethyleneimine and carboxylic acids, primary amine Graff-Torcelain acrylic resins grafted with primary amines onto the acrylic backbone, polyacetic acid or its derivatives, and aminophenols. As anionic polymers, copolymers with poly(methyl)acrylic acid or its salts, or (methyl)acrylic acid and its salts as main components are preferred. The crosslinking agent is preferably a compound having any one of the following functional groups: isocyanate group, glycidyl group, carboxyl group, oxazoline group, or silane coupling agent.
[0062] More specifically, as an example of an anti-corrosion layer, the anti-corrosion liquid of the present invention is mainly an aqueous solution composed of a trivalent chromium compound, an inorganic acid, an organic resin, a crosslinking agent, a titanium (Ti) compound or a zirconium (Zr) compound, and an organic solvent, wherein the proportions of the trivalent chromium compound, the inorganic acid, the organic resin, the titanium (Ti) compound or the zirconium (Zr) compound, the organic solvent, and water are 1.9 to 6%, 0.3 to 6%, 0.6 to 6%, 0 to 0.6%, 0 to 2.8%, and 78.6 to 97.2%, respectively. The crosslinking agent accounts for 0.01 to 30% by mass of the solid components of the anti-corrosion layer, or 0.05 to 15% by mass of the solid components in the solution used to form the anti-corrosion layer.
[0063] The trivalent chromium compound and crosslinking agent are composed of at least one of chromium nitrate and chromium fluoride; the inorganic acid is composed of at least one of phosphoric acid, nitric acid, and hydrofluoric acid; the organic resin is composed of at least one of acrylic resin, methacrylic resin, hydroxyacrylic resin, polyvinyl alcohol resin, olefin resin, and phenolic resin; the titanium (Ti) compound is composed of at least one of titanium fluoride and titanium nitrate; the zirconium (Zr) compound is composed of at least one of zirconium fluoride and zirconium nitrate; and the organic solvent is composed of at least one of isopropanol, ethanol, and ethylene glycol butyl ether.
[0064] By adding a crosslinking agent, the crosslinking density of the anti-corrosion layer can be increased, thereby stabilizing the layer's resistance to the electrolyte and hydrogen fluoride produced by the reaction of the electrolyte with water. More optimally, the crosslinking agent can be added to the anti-corrosion solution that forms the anti-corrosion layer.
[0065] Crosslinking agents can be organic or inorganic. Inorganic crosslinking agents include at least one of the following: silicon compounds such as silicon dioxide; zirconium compounds such as ammonium zirconium fluoride and ammonium zirconium carbonate; metal chelates such as titanium chelates; and inorganic crosslinking compounds of metal salts such as Ca, Al, Mg, Fe, and Zn. Organic crosslinking agents are preferably at least one of the following: amino resins, melamine resins, phenolic resins, epoxy compounds, terminal isocyanate compounds, oxazoline compounds, carbodiimide compounds, condensates of formaldehyde and alkyl monohydric alcohols having 1 to 4 carbon atoms, condensates of carbolic acid and formaldehyde, and derivatives of the above substances.
[0066] The crosslinking agent comprises 0.01 to 30% by mass of the solid components of the anti-corrosion layer, or 0.05 to 15% by mass of the solid components in the solution used to form the anti-corrosion layer. When the crosslinking agent content is below 0.05%, the improvement in corrosion resistance by adding the crosslinking agent is minimal. When the content exceeds 15%, the crosslinking density of the anti-corrosion layer increases, making the anti-corrosion layer too hard. This makes it prone to cracking and peeling during molding and processing, resulting in reduced corrosion resistance.
[0067] In addition, as an anti-corrosion layer formed by chemical formation, there are now a variety of anti-corrosion liquids known, which mainly contain phosphates, nitric acid, chromates, fluorides and rare earth oxides.
[0068] Chemical treatments using phosphates and chromates mainly include, for example, chromium chromate treatment, chromium phosphate treatment, phosphate-chromate treatment, and chromate treatment. Examples of chromium compounds used in these treatments include chromium nitrate, chromium fluoride, chromium sulfate, chromium acetate, chromium oxalate, chromium diphosphate, chromium acetate, chromium chloride, and chromium sulfate. Chromate treatment methods mainly include etching chromate treatment, electrolytic chromate treatment, and coating chromate treatment, but coating chromate treatment is preferred. In this coating chromate treatment, a treatment solution mainly composed of metal phosphate salts such as chromium (Cr) phosphate, titanium (Ti) phosphate, zirconium (Zr) phosphate, and lead (Zn) phosphate, or a treatment solution mainly composed of non-metallic phosphate salts and mixtures thereof, is mixed with synthetic resin on the degreased surface. This mixture is then applied using known coating methods such as roller coating, gravure printing, and immersion coating, followed by drying. The treatment solution can use various solvents such as water, alcohol-based solvents, hydrocarbon-based solvents, ketone-based solvents, ester-based solvents, and ether-based solvents, but water is preferred. Additionally, the resin component used can be a water-soluble polymer such as aminophenol or polyacrylic acid resin.
[0069] As an example of an anti-corrosion layer, an anti-corrosion layer is formed by coating particulate matter containing metal oxides such as aluminum oxide, titanium oxide, cerium oxide, and tin oxide, as well as precipitated barium sulfate, dispersed in phosphoric acid onto the surface of an intermediate metal layer and then sintering it at a temperature above 150°C.
[0070] As a method for applying the anti-corrosion liquid, firstly, at least the inner thermal bonding resin layer of the intermediate metal layer is degreased using methods such as alkaline impregnation, electrolytic cleaning, acid cleaning, electrolytic acid cleaning, oxygen activation, and heat treatment (annealing) during calendering. Secondly, the anti-corrosion liquid of this invention is applied to the surface of the intermediate metal layer by means of rod coating, roller coating, gravure coating, immersion, etc., and a high-temperature chemical reaction is carried out. The wet film weight of the anti-corrosion liquid on the intermediate metal layer ranges from 1.6 to 3.2 g / m². 2 After applying the anti-corrosion liquid, heat-treat at a high temperature of 130 to 200°C for 0.5 to 5 minutes to form an anti-corrosion layer.
[0071] While there is no particular limitation on the thickness of the anti-corrosion layer, from the perspective of the adhesion between the intermediate metal layer and the hot-melt resin layer, it is preferably 1 nm to 3.0 μm, and more preferably 1 nm to 1.5 μm.
[0072] The trivalent chromium compound and crosslinking agent in the anti-corrosion solution forming the anti-corrosion treatment layer are preferably one of chromium nitrate and chromium fluoride. Chromium nitrate and chromium fluoride react with the resin, intermediate metal layer, and inorganic acid in the anti-corrosion layer. Chromium fluoride can improve the temperature and humidity resistance of the anti-corrosion layer and ensure the stability of the peel strength between the outer substrate resin layer and the intermediate metal layer during long-term storage.
[0073] Titanium (Ti) compounds or zirconium (Zr) compounds can improve the stability and uniformity of the reaction of chromium with resins, metals, and inorganic acids. Titanium (Ti) compounds are preferably titanium fluoride or titanium nitrate. Zr compounds are preferably zirconium fluoride or zirconium nitrate.
[0074] Inorganic acids can remove the surface oxide film of the intermediate metal layer, allowing the metal to react rapidly with the components in the anti-corrosion layer to form a strong chromium reaction product. This ensures the stability of the peel strength between the heat-fused resin layer and the intermediate metal layer during long-term storage of the composite film. Phosphoric acid, nitric acid, and hydrofluoric acid are preferred as the inorganic acid.
[0075] As mentioned above, organic resins can improve the adhesion stability between the intermediate metal layer and the outer substrate resin layer. Furthermore, in the anti-corrosion layer, the reaction products of chromium (Cr), titanium (Ti), and zirconium (Zr) are resistant to external moisture, thus improving the peel strength stability between the outer substrate resin layer and the intermediate metal layer. Preferably, the organic resin contains one of the following: acrylic resin, methacrylic resin, hydroxyacrylic resin, polyvinyl alcohol resin, olefin resin, or phenolic resin.
[0076] Organic solvents can be used alone or added to water. They can improve the wettability of the anti-corrosion solution and enhance the reaction stability between the anti-corrosion layer and the intermediate metal layer. Additionally, they can reduce the surface tension of the anti-corrosion solution, improving the uniformity of the coating film. Isopropanol, ethanol, and ethylene glycol butyl ether can be selected as organic solvents.
[0077] The characteristics of the outer substrate resin layer 1 of the outer packaging material are as follows:
[0078] In this invention, the outer substrate resin layer is provided to enable it to perform its function as a substrate for lithium-ion battery packaging materials. The outer substrate resin layer is located on the outer side of the lithium-ion battery packaging material.
[0079] Regarding the raw materials that form the resin layer of the outer substrate, the function of the substrate is limited to having at least insulation properties, and there are no particular restrictions.
[0080] There are various methods for preparing the outer substrate resin layer. For example, it can be a resin film formed directly from resin, or it can be a resin coating. The resin film can be an unstretched film or a stretched film. The stretched film can be a uniaxially stretched film or a biaxially stretched film, with biaxially stretched films being preferred. Methods for preparing a biaxially stretched film include, for example, step-by-step biaxial stretching, blown film forming, and simultaneous stretching. Resin coating methods include, for example, roll coating, gravure coating, and extrusion coating.
[0081] The resin forming the outer substrate resin layer can be, for example, polyester, polyamide, polyolefin, epoxy resin, acrylic resin, fluoropolymer, polyurethane, silicone resin, phenolic resin, or a modified form of these resins. Furthermore, the resin forming the outer substrate resin layer can be a copolymer of these resins, a modified form of the copolymer, or a mixture of these resins.
[0082] Single or multiple layers are preferred
[0083] Among the resins used to form the outer substrate resin layer, polyester and polyamide are preferred.
[0084] Specifically, examples of polyesters include polyethylene terephthalate (PET), polybutylene terephthalate (PET), polyethylene naphthalate (PET), polyethylene isophthalate (PET), and copolyesters. Furthermore, examples of copolyesters include copolyesters with PET as the main repeating unit. Specifically, copolymer polyesters formed by polymerizing PET as the main repeating unit with PET (hereinafter referred to as copolyesters (terephthalate / isophthalate)), copolyesters (terephthalate / adipate), copolyesters (terephthalate / sodium isophthalate), copolyesters (terephthalate / phenyl dicarboxylate), and copolyesters (terephthalate / decane dicarboxylate) are produced. These polyesters can be used alone or in combination of two or more.
[0085] In addition, examples of polyamides include aliphatic polyamides such as nylon 6, nylon 66, nylon 610, nylon 12, nylon 46, and copolymers of nylon 6 and nylon 66; and aromatic polyamides such as hexamethylenediamine-isophthalic acid-terephthalic acid copolymers containing structural units derived from terephthalic acid and / or isophthalic acid, such as nylon 6I, nylon 6T, nylon 6IT, and nylon 6I6T (where I represents isophthalic acid and t represents terephthalic acid), and polyamide MXD6 (polyamide PACM6 (polybis(4-aminocyclohexyl)methane azidoamide)). These polyamides can be used alone or in combination of two or more.
[0086] The outer substrate resin layer preferably contains at least one of polyester film, polyamide film, and polyolefin film; preferably contains at least one of stretched polyester film, stretched polyamide film, and stretched polyolefin film; more preferably contains at least one of stretched polyethylene terephthalate film, stretched polybutylene terephthalate film, stretched nylon film, and stretched polypropylene film; and more preferably contains at least one of biaxially oriented polyethylene terephthalate film, biaxially oriented polybutylene terephthalate film, biaxially oriented nylon film, and biaxially oriented polypropylene film.
[0087] The outer substrate resin layer can be a single layer or composed of two or more layers. When the outer substrate resin layer is composed of two or more layers, it can be a composite film formed by the action of an adhesive, or it can be a resin composite film with two or more layers formed by co-extrusion of resin. Alternatively, the outer substrate resin layer can be a resin composite film with two or more layers formed by co-extrusion of resin in an unstretched state, or it can be used after uniaxial or biaxial stretching.
[0088] In the outer substrate resin layer, specific examples of laminates consisting of two or more resin films include composite films of polyester and nylon films, nylon composite films with two or more layers, and polyester composite films with two or more layers. Laminates of stretched nylon and stretched polyester films, stretched nylon composite films with two or more layers, and stretched polyester composite films with two or more layers are preferred. For example, when the outer substrate resin layer is a two-layer resin composite film, composite films of polyester resin films, polyamide resin films, or polyester resin films are preferred. Composite films of polyethylene terephthalate (PET) films, polybutylene terephthalate (PET) films, nylon films, or polyethylene terephthalate (PET) films and nylon films are more preferred. In addition, polyester resin is difficult to change color when the electrolyte is attached to the surface. Therefore, when using a resin composite film with two or more outer substrate resin layers, it is preferable that the polyester resin film is located on the outermost layer of the outer substrate resin layer.
[0089] When the outer substrate resin layer is a resin composite film with two or more layers, the two or more resin films can also be laminated using an adhesive. As a preferred adhesive, a liquid adhesive with the same composition as the outer layer adhesive can be used. Furthermore, there are no particular limitations on the method for laminating two or more resin films; dry lamination, sandwich lamination, extrusion lamination, thermal lamination, etc., can be used, with dry lamination being preferred. When laminating using the dry lamination method, a reactive polyurethane adhesive is preferred as the outer layer reactive adhesive. In this case, the thickness of the adhesive layer can be approximately 2 to 5 μm. When forming the outer substrate resin layer using a resin coating method, the resin can be first dissolved in an organic solvent, and then the outer substrate resin layer can be formed by coating. Coating resins can include polyamide resins, polyimide resins, polyurethane resins, epoxy resins, acrylic resins, polyester resins, phenolic resins such as polyamide resins, polyimide resins, fluorinated copolymer resins, and polyester resins, as well as amino resins such as polyester resins, polycarbonate resins, urea resins, and melamine resins.
[0090] In addition, one or more additives such as lubricants, flame retardants, anti-blocking agents, antioxidants, light stabilizers, tackifiers, and antistatic agents can be added to the surface and interior of the outer substrate resin layer.
[0091] From the viewpoint of improving the formability of packaging materials for lithium-ion batteries, it is preferable to coat a lubricant onto the surface of the resin layer of the outer substrate. There are no particular limitations on the lubricant, but amide-based lubricants are preferred. Amide lubricants include saturated fatty acid amides, unsaturated fatty acid amides, substituted amides, hydroxymethylamides, saturated fatty acid diamides, unsaturated fatty acid diamides, fatty acid amides, and aromatic diamides. For example, saturated fatty acid amides can include lauryl amide, palmitamide, stearamide, behenamide, and hydroxystearamide. For example, unsaturated fatty acid amides can include oleamide and erucamide. Substituted amides include N-oleopalmitamide, N-stearamide, N-stearamide, N-oleostearamide, and N-stearamide. Additionally, hydroxymethylamides include hydroxymethylstearamide. Saturated fatty acid diamides include methylene distearate, ethylene bis-octanoate, ethylene bis-laurate, ethylene bis-stearate, ethylene bis-hydroxystearate, ethylene bis-benzylamide, hexamethylene distearate hexamethylene bis-benzylamide, hexamethylene hydroxystearate, n,n'-distearate adipamide, and n,n'-distearate sebacic acid amide. Unsaturated fatty acid diamides include ethylene dioleamide, ethylene dierucamide, hexamethylene dioleamide, n,n'-dioleoyl adipamide, and n,n'-dioleoyl sebacic acid amide. Fatty acid ester amides include stearamide ethyl stearate. Additionally, aromatic diamides include isophthalic acid bis-stearate, isophthalic acid bis-hydroxystearate, and n,n'-distearate isophthalic acid amide. Lubricants can be used alone or in combination of two or more types.
[0092] When a lubricant is present on the surface of the outer substrate resin layer, there are no particular limitations on the coating amount, but a coating of approximately 3 mg / m² is preferred. 2 More preferably, a coating concentration of 4 to 30 mg / m² is applied. 2 about.
[0093] The lubricant present on the surface of the outer substrate resin layer can be a lubricant that seeps out from the substrate resin layer containing lubricant, or a lubricant that is coated on the surface of the outer substrate resin layer.
[0094] Regarding the thickness of the outer substrate resin layer, there are no particular restrictions as long as it fulfills its function as a substrate. When the outer substrate resin layer is a resin composite film with two or more layers, the thickness of each resin film layer is preferably around 2 to 30 μm.
[0095] In this invention, the outer substrate resin layer can be a single-layer or multi-layer composite film formed from one or more of the following polymer materials: blown nylon, synchronous or asynchronous biaxially oriented nylon, synchronous or asynchronous biaxially oriented polyethylene terephthalate (PET), synchronous or asynchronous biaxially oriented polybutylene terephthalate (PBT), and polyimide (PI). The outer substrate resin can be bonded to the intermediate metal layer by one or a combination of co-extrusion, coating, lamination, and thermal bonding. The total thickness of the outer substrate resin layer is 5 to 35 μm. If the thickness is less than 5 μm, the formability and insulation properties are relatively poor. Furthermore, if it exceeds 35 μm, the total thickness of the metal-plastic composite film becomes too thick, and the advantage of the metal-plastic composite film, namely its flexibility, deteriorates.
[0096] The characteristics of the outer adhesive layer 5 of the outer packaging material are as follows:
[0097] In the lithium-ion battery packaging material of the present invention, when the outer substrate resin layer and the intermediate metal layer are composited, an outer adhesive layer may or may not be provided as needed. The outer adhesive layer is formed for the purpose of improving the adhesion between the outer substrate resin layer and the intermediate metal layer.
[0098] The outer adhesive layer is formed by an adhesive capable of bonding the outer substrate resin layer and the intermediate metal layer. There are no limitations on the adhesive used to form the outer adhesive layer; for example, it can be a two-component curing adhesive (two-component adhesive) or a one-component curing adhesive (one-component adhesive). Furthermore, the adhesive used to form the outer adhesive layer can be any of the following: chemically reactive, solvent-evaporative, heat-melting, or hot-pressing. Additionally, the outer adhesive layer can be a single layer or multiple layers.
[0099] The outer adhesive layer is a two-component polyurethane adhesive formed by using polyester polyols and polyurethane-modified polyols as the main diols and aromatic or aliphatic isocyanates as curing agents. The curing agent can be selected based on the functional groups of the adhesive components, such as from polyfunctional epoxy resins, polymers containing methanesulfonic acid, polioamine resins, inorganic acids, etc. In addition, the main agents used in the outer adhesive layer include polyester resins such as polyethylene terephthalate, polyethylene terephthalate, polyethylene naphthalate, polyethylene isophthalate, and copolyester; polyether resins; polyurethane resins; epoxy resins; phenolic resins; polyamide resins such as nylon 6, nylon 66, and nylon 12; polyolefin resins such as polyolefins, cyclic polyolefins, acid-modified polyolefins, and acid-modified cyclic polyolefins; polyvinyl acetate; cellulose; (meth)acrylic resins; polyimide resins; polycarbonate; amino resins such as urea resin and melamine resin; rubbers such as chloroprene rubber, nitrile rubber, and styrene-butadiene rubber; and silicone resins. These adhesive components can be used individually or in combination of two or more.
[0100] More preferably, the outer adhesive layer of this invention comprises one or two of binary or multi-component polyesters, polyurethane-modified polyesters, and isocyanates. Isocyanates are not specifically defined as compounds having two or more isocyanate groups in their molecules. Examples include one or more mixtures of polymers such as isophorone diisocyanate (IPDI), toluene diisocyanate (TDI), diphenylmethane-4,4'-diisocyanate (MDI), and 1,6-hexamethylene diisocyanate (HDI).
[0101] Furthermore, other components can be added to the outer adhesive layer as long as it does not impair adhesion; these can include colorants, thermoplastic elastomers, tackifiers, fillers, etc. By including colorants in the outer adhesive layer, the packaging materials for lithium-ion batteries can be colored. Pigments, dyes, and other colorants can be used. Additionally, one type of colorant can be used, or a mixture of two or more can be used.
[0102] There are no particular limitations on the type of pigment, as long as it does not impair the adhesion of the outer adhesive layer. Organic pigments, for example, can be azo, phthalocyanine, quinacridone, anthraquinone, dioxazine, indigo, perylene, and isoindoline pigments; inorganic pigments, such as carbon black, titanium dioxide, cadmium, lead, and isoindoline pigments, can be used.
[0103] In colorants, carbon black is preferred, for example, to make the packaging material for lithium-ion batteries appear black.
[0104] There are no particular restrictions on the average particle size of the pigment; it can be selected from approximately 0.05 to 5 μm, preferably from approximately 0.08 to 2 μm. Furthermore, the average particle size of the pigment is the median particle size measured by a laser diffraction / scattering particle size distribution measuring device.
[0105] There are no particular restrictions on the pigment content in the outer adhesive layer, as long as the packaging material for lithium-ion batteries is colored; preferably, it is about 5 to 60%, more preferably 10 to 40%.
[0106] The thickness of the outer adhesive layer is only required to bond the outer substrate resin layer 1 and the intermediate metal layer 3. There are no particular limitations. As a preferred range, it can be listed as about 1 to 10 μm, and more preferably about 2 to 5 μm.
[0107] The coloring layer is a layer that is disposed between the outer substrate resin layer and the intermediate metal layer as needed. The colored metal-plastic composite film can be formed directly by adding pigment to the outer adhesive layer, or the coloring layer can be formed between the outer substrate resin layer and the outer adhesive layer. Alternatively, the coloring layer can be disposed on the outside of the outer substrate resin layer.
[0108] A coloring layer can be formed, for example, by applying an ink containing a colorant to the surface of the outer substrate resin layer 1, the surface of the outer adhesive layer A, or the surface of the intermediate metal layer. Pigments, dyes, or other colorants can be used. Furthermore, only one type of colorant can be used, or two or more can be mixed.
[0109] As a specific example of a colorant contained in a coloring layer, one can refer to the example described in the outer adhesive layer.
[0110] The characteristics of the middle metal layer 2 of the outer packaging material are as follows:
[0111] In the outer packaging materials for lithium-ion batteries, the intermediate metal layer is a barrier layer that can at least prevent moisture from penetrating.
[0112] In this patent, the metal material used as the intermediate metal layer is a nickel-plated steel plate.
[0113] When the intermediate metal layer is nickel-plated steel sheet, the nickel plating layer provides rust and corrosion protection, while also improving surface cleanliness. By forming the corrosion-resistant layer (described later) on the nickel-plated surface, durability is significantly improved through the corrosion resistance of the nickel plating layer and its synergistic effect with the corrosion-resistant layer. The thickness of the nickel plating layer should be less than 20 μm. Preferably, it is between 1 μm and 5 μm. While corrosion resistance is improved when the thickness exceeds 20 μm, cracking is more likely to occur due to external pressure loads such as during molding.
[0114] Furthermore, the surface cleanliness of the intermediate metal layer significantly impacts its anti-corrosion effect, making its management crucial. Surface cleanliness can be managed using either a wettability test with a wetting reagent or a contact angle as an indicator. For wettability, a grade D or higher is preferred, ideally grade B. For contact angle, when tested with pure water, the angle should be 25° or less, preferably 20° or less, and more preferably 15° or less. Wetness below grade D or a contact angle exceeding 25° can lead to deterioration in reactivity or initial adhesion with the anti-corrosion layer (described later). If reactivity deteriorates, the reaction between the anti-corrosion layer and the intermediate metal layer becomes insufficient, resulting in decreased resistance to electrolyte penetration (the battery's contents) and resistance to hydrogen fluoride generated during the reaction between the electrolyte and water. Over time, the adhesion of the anti-corrosion layer to the intermediate metal layer decreases, the anti-corrosion layer dissolves, and the intermediate metal layer and anti-corrosion layer may peel off, shortening battery life. The same situation occurs when the initial adhesion between the anti-corrosion layer and the intermediate metal layer deteriorates.
[0115] The method for testing the surface wettability of the intermediate metal layer can be adopted according to "National Standard of the People's Republic of China GB / T225638.5-2016, Metals, Test Methods, Part 5: Determination of wettability". The method for testing the contact angle of the intermediate metal layer can be adopted according to "National Standard of the People's Republic of China GB / T22638.9-2008, Metals, Test Methods, Part 9: Determination of hydrophilicity".
[0116] The characteristics of the inner adhesive layer 3 of the outer packaging material are as follows:
[0117] In the lithium-ion battery packaging material of the present invention, the inner adhesive layer is an intermediate layer provided to firmly bond the intermediate metal layer to the hot-melt resin layer.
[0118] The inner adhesive layer is formed of a resin capable of bonding the intermediate metal layer and the hot-melt resin layer. The hot-melt resin layer can be made of polyolefins, cyclic polyolefins, or modified polyolefin resins such as carboxylic acid-modified polyolefins, carboxylic acid-modified cyclic polyolefins, methacrylic acid-modified polyolefins, acrylic acid-modified polyolefins, crotonic acid-modified polyolefins, and imide-modified polyolefins. From the viewpoint of improving the adhesion between the intermediate metal layer and the hot-melt resin layer, modified polyolefin resins such as acrylic acid, methacrylic acid, maleic acid, anhydrous maleic anhydride, and polyamide are preferred as the modified polyolefin. The resin constituting the inner adhesive layer may or may not contain a polyolefin backbone, but it is preferred to contain a polyolefin backbone. Whether the resin constituting the inner adhesive layer contains a polyolefin backbone can be analyzed using methods such as infrared spectroscopy or gas chromatography-mass spectrometry; the analytical method is not particularly limited. The polyolefin and its modified resin used in the inner adhesive layer are the same as those used in the hot-melt resin layer, which are polypropylene resins or copolymers of propylene and ethylene.
[0119] From the perspective of ensuring the long-term stability of packaging materials for lithium-ion batteries, the inner adhesive layer can also be a resin combination containing an acid-modified polyolefin and a curing agent. As an acid-modified polyolefin, maleic anhydride or acrylic acid-modified polyolefins are particularly preferred.
[0120] As a curing agent, any curing agent that can cure acid-modified polyolefins is acceptable; there are no particular limitations. Epoxy-based curing agents, polyfunctional isocyanate-based curing agents, carbodiimide-based curing agents, oxazoline-based curing agents, and other curing agents can be used.
[0121] As an epoxy curing agent, any compound having at least one epoxy group is acceptable; there are no particular limitations. Examples include bisphenol A diglycidyl ether, modified bisphenol A diglycidyl ether, phenolic varnish glycidyl ether, glycerol polyglycidyl ether, and polyglycerol polyglycidyl ether epoxy resins.
[0122] As a multifunctional isocyanate-based curing agent, there are no particular limitations as long as the compound has two or more isocyanate groups in its molecule. For example, it can be a component resulting from the polymerization or addition of isophorone diisocyanate (PDI), hexamethylene diisocyanate (HDI), toluene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), or a reaction product of such mixtures with other polymers.
[0123] As a carbodiimide-based curing agent, there are no particular limitations as long as the compound has at least one carbodiimide group (-N=C=N-) in its molecule. Polycarbodiimide compounds having at least two or more carbodiimide groups are preferred.
[0124] As an oxazoline-based curing agent, there are no particular limitations as long as it is a compound with an oxazoline skeleton.
[0125] From the perspective of improving the adhesion between the inner adhesive layer and the hot-melt resin layer, the curing agent can also be composed of two or more compounds.
[0126] The thickness of the inner adhesive layer is not particularly limited as long as it functions as an adhesive layer. It is preferably about 1 to 80 μm, and more preferably about 1 to 50 μm.
[0127] The main components of the inner adhesive layer in this invention are one or more of the following: modified polyolefin resin, polyolefin resin, block copolymer polypropylene resin (B-PP) with a polypropylene (PP) content of more than 50%, random copolymer polypropylene resin (R-PP), and homopolymer polypropylene resin (H-PP), forming a single layer or two or more film layers.
[0128] When laminating the intermediate metal layer and the hot-melt adhesive layer, the inner adhesive layer can be applied using either a solution-based inner adhesive layer or a hot-melt inner adhesive resin layer.
[0129] The solution-type inner adhesive layer is based on an acid-modified polyolefin resin and uses one or more of the following as hardeners: isocyanate, epoxy resin, or oxazoline-based resins, or amine compounds such as triethylamine or N,N-dimethylethanolamine. After being dissolved in at least one or more solvents such as water, ethanol, isopropanol, ethyl acetate, methyl ethyl ketone, toluene, or methylcyclohexane, it is uniformly coated onto the corrosion-resistant metal surface. Heating causes the solvent to evaporate, achieving the desired thickness of the inner adhesive layer, preferably around 1 to 10 μm, more preferably 1 to 5 μm. A thickness less than 1 μm reduces the adhesion between the intermediate metal layer and the heat-fused resin layer, causing adhesion problems. A thickness exceeding 10 μm does not present adhesion problems, but the hardened resin layer forms after the curing agent reaction, resulting in poor bending resistance and reduced flexibility of the metal-plastic composite film, posing a risk of cracking during bending and potential delamination between the intermediate metal layer and the heat-fused resin layer. The acid-modified polyolefin resin in the solution-type inner layer adhesive has a melting point of 60 to 155°C, a weight-average molecular weight of 10,000 to 150,000, and an acid value of 0.5 to 200 mg KOH / g. Under curing agent-free conditions, the solution-type inner layer adhesive mainly consists of acid-modified polyolefin and amine compounds as hardeners, with a ratio of acid-modified polyolefin to amine compound of 10:1 to 125:1, preferably 15:1 to 50:1. The acid used for modification of the polyolefin is maleic acid, fumaric acid, methacrylic acid, etc., and the amine compound is at least one of triethylamine or N,N-2-methylethanolamine. The acid-modified polyolefin is polypropylene with a melting point above 110°C, and the polypropylene content is above 50%.
[0130] If the melting point is below 60℃, the heat resistance is low, and the intermediate metal layer and the thermosetting resin layer may peel off at high temperatures. Conversely, if the melting point exceeds 155℃, the heat resistance is better, but the reaction with the curing agent forms a hard resin layer with poor flexibility. This reduces the flexibility of the metal-plastic composite film, or causes cracks when bent, leading to peeling between the intermediate metal layer and the thermosetting resin layer. If the weight-average molecular weight is below 10,000, the resin has high fluidity when heated, causing significant thinning during heat sealing. This lowers the adhesion strength between the intermediate metal layer and the thermosetting resin layer (when reacting with the curing agent), resulting in sealing problems. If the weight-average molecular weight exceeds 150,000, the intermediate metal layer and the thermosetting resin layer (when reacting with the curing agent) will form a hard resin layer, resulting in poor flexibility. This reduces the flexibility of the metal-plastic composite film, or causes cracks when bent, leading to peeling between the intermediate metal layer and the thermosetting resin layer. If the acid value of the acid-modified polyolefin resin is less than 0.5 mg KOH / g, there are few curing reaction points with the curing agent, resulting in unstable adhesion between the intermediate metal layer and the hot-melt resin layer. If the acid value exceeds 200 mg KOH / g, the curing reaction between the curing agent and the acid-modified polyolefin resin is too vigorous, forming a hard resin layer, which deteriorates the bending resistance, reduces the flexibility of the metal-plastic composite film, or causes cracks when bent, leading to delamination between the intermediate metal layer and the hot-melt resin layer.
[0131] The inner adhesive layer used for the intermediate metal layer and the hot-melt resin layer is a hot-melt type inner adhesive. The resin used in the hot-melt type inner adhesive layer is an acid-modified polyolefin resin with a melting point of 135 to 165°C and an MFR (230°C) of 3 to 15 g / 10 min. The thickness of the formed inner adhesive layer is 2 to 80 μm, preferably 5 to 50 μm. The degree of modification of the acid-modified polyolefin resin used in the hot-melt type inner adhesive is 1% to 15%, preferably 3% to 12%. When the melting point of the acid-modified polyolefin resin is below 135°C, heating will cause the resin to become more fluid. During pressure heat sealing, the thickness will become significantly thinner, and the adhesion strength between the intermediate metal layer and the hot-melt resin layer will decrease, resulting in sealing problems. When the melting point is above 165℃, the fluidity is relatively low during pressure heat sealing, and the heat resistance is improved. However, when combined with the intermediate metal layer, the amount of thermal shrinkage increases, leading to increased internal stress and a decrease in the adhesion between the hot-melt inner layer adhesive and the intermediate metal layer. Therefore, during long-term storage, peeling from the intermediate metal layer may occur. Furthermore, the heating during heat sealing further causes thermal shrinkage, reducing the adhesion between the adhesive and the intermediate metal layer, lowering the sealing strength, and making sealing a major problem. If the MFR (230℃) of the acid-modified polyolefin resin is below 3g / 10min, the extrusion film formation is prone to instability when it is extruded onto the intermediate metal layer after hot melting. If the MFR (230℃) of the acid-modified polyolefin resin is above 15g / 10min, heating will increase the resin fluidity, resulting in significant thinning during pressure heat sealing. This reduces the adhesion strength between the intermediate metal layer and the hot-melt resin layer, leading to sealing problems. When the thickness of the hot-melt inner adhesive layer is less than 2μm, it cannot absorb excessive heat shrinkage during lamination with the intermediate metal layer. Therefore, the adhesion to the intermediate metal layer decreases due to increased internal stress. During long-term storage, peeling from the intermediate metal layer may occur. While a hot-melt inner adhesive layer thickness exceeding 80μm does not cause physical property problems, it increases production costs, so its use is best avoided. When the modification degree of the hot-melt inner adhesive layer is less than 1%, the adhesion to the intermediate metal layer becomes unstable. If the modification degree exceeds 15%, although physical property problems do not occur, production costs increase, so this phenomenon is best avoided.
[0132] The characteristics of the heat-melt resin layer 4 of the outer packaging material are as follows:
[0133] In the outer packaging material for lithium-ion batteries of the present invention, the heat-sealing resin layer is equivalent to the innermost layer, and is a layer (heat-sealing layer) that performs the function of heat-sealing resin layers to heat-seal the battery components by heat-sealing each other during battery assembly.
[0134] For the resin that constitutes the heat-fusion resin layer, heat-fusion-compatible resins are preferred, with no particular restrictions. Resins containing polyolefin backbones, such as polyolefins and acid-modified polyolefins, are preferred.
[0135] Specifically, examples of polyolefins include low-density polyethylene, medium-density polyethylene, high-density polyethylene, linear low-density polyethylene, and other polyethylene-ethylene-α-olefin copolymers; homopolymer polypropylene, polypropylene block copolymers (e.g., propylene-ethylene block copolymers), and random copolymers of polypropylene (e.g., propylene-ethylene random copolymers); propylene-α-olefin copolymers; and ethylene-butene-propylene terpolymers. Polypropylene is preferred. The polyolefin resin used as a copolymer can be a block copolymer or a random copolymer. One or more of these polyolefin resins can be used alone.
[0136] Acid-modified polyolefins are polymers modified by block polymerization or graft polymerization of polyolefins with an acid component. As acid-modified polyolefins, copolymers formed by copolymerizing the aforementioned polyacrylic acid or methacrylic acid with polar molecules can also be used. Furthermore, as the acid component used in acid modification, carboxylic acids or sulfonic acids such as maleic acid, acrylic acid, itaconic acid, crotonic acid, maleic anhydride, and itaconic anhydride, as well as their anhydrides, can be used; acrylic acid or maleic acid and their anhydrides are preferred.
[0137] The heat-fusion resin layer can be composed of a single type of resin or a combination of two or more types of resin. Furthermore, the heat-fusion resin layer can consist of a single layer or two or more layers of the same or different resins.
[0138] The hot-melt resin layer may also contain slip agents, as needed. The presence of slip agents in the hot-melt resin layer improves the moldability of the outer packaging material for lithium-ion batteries. There are no particular restrictions on the type of slip agent; it can be selected from known sources. One type of slip agent can be used alone, or two or more can be used in combination.
[0139] There are no particular limitations on the type of slip agent used, but amide-based slip agents are preferred. A single slip agent can be used, or two or more can be used in combination. As an amide-based slip agent, it is preferred to apply it to the surface of the aforementioned outer substrate resin layer.
[0140] When a slip agent is present on the surface of the hot-melt resin layer, its content is not particularly limited, but from the viewpoint of improving the formability of materials for electronic packaging, a content of 10 to 50 mg / m³ is preferred. 2 Further preferred values are 15 to 40 mg / m². 2 .
[0141] The slip agent present on the surface of the heat-fused resin layer can be a slip agent that oozes from the resin constituting the heat-fused resin layer, or a slip agent that is coated on the surface of the heat-fused resin layer.
[0142] There are no particular restrictions on the thickness of the heat-fusion resin layer, as long as it can perform the function of sealing the battery element after the heat-fusion resin layers are heat-fused together. It can be selected to be less than about 100μm, and more preferably about 25 to 80μm.
[0143] The hot-melt resin layer may also contain antioxidants as needed. A hot-melt resin layer containing antioxidants can inhibit thermal degradation during the manufacturing process. There are no special restrictions on the type of antioxidant; it can be selected from known sources. One antioxidant can be used alone, or two or more can be used in combination.
[0144] The hot-melt bonding resin in this invention is a single layer or composite layer composed of one or more of the following: acid-modified polyolefin resin, homopolymer polypropylene resin, block copolymer polypropylene resin, random copolymer polypropylene resin, and polyethylene resin.
[0145] The resin used in the heat-fusion bonding resin layer is a single layer or composite layer composed of one or more of the following resins: a melting point of 120 to 162°C, more preferably 130 to 162°C, an MFR (at 230°C) of 2 to 15 g / 10 min, more preferably 3 to 12 g / 10 min, and a thickness of 20 to 120 μm, more preferably 25 to 80 μm. Furthermore, when the inner heat-fusion bonding resin layer is a composite layer, the resin on the reverse side in contact with the intermediate metal layer has a thickness of 2 μm or more and a melting point of 130 to 152°C. When the melting point is below 120°C, the resin has high fluidity during heating, and the thickness decreases during pressure heat sealing, resulting in reduced adhesion to the intermediate metal layer. Furthermore, pressurization causes the squeezed resin inside the battery to flow to the unsqueezed edges. Expansion, contraction, and bending forces during battery processing can cause cracks, allowing electrolyte to seep into the intermediate metal layer. This reduces the insulation resistance of the heat-fused resin layer, leading to leakage and shortening battery life. When the melting point exceeds 162°C, the increased crystallinity of the resin results in relatively lower fluidity during pressurized heat sealing and improved heat resistance. However, highly crystalline resins form a hard and brittle resin layer during heat sealing. Therefore, under conditions of battery expansion, contraction, and bending forces, the resin layer is prone to cracking, resulting in unstable long-term sealing. When the resin's MFR (230°C) is below 2 g / 10 min, the resin's fluidity is low during pressurized heat sealing, making it difficult to achieve stable sealing. When the resin's MFR (230°C) exceeds 15 g / 10 min, the resin's fluidity is too high during pressurized heat sealing, resulting in significant resin thinning and difficulty in achieving stable sealing. Furthermore, applying pressure causes the squeezed resin inside the battery to flow to the unsqueezed edges. Expansion, contraction, and bending forces during battery processing can cause cracks. Electrolyte can then seep through these cracks into the intermediate metal layer, reducing the insulation resistance of the heat-fused resin layer and leading to leakage, thus shortening battery life. When the thickness of the heat-fused resin layer is less than 20μm, it is difficult to achieve a uniform heat-fused section and stable sealing because the thickness cannot adequately cover deviations in the mechanical dimensions and conditions of the heat-sealing device. Additionally, applying pressure causes the squeezed resin inside the battery to flow to the unsqueezed edges, thinning the heat-fused resin layer. Expansion, contraction, and bending forces during battery processing can easily cause cracks. Electrolyte can then seep through these cracks into the intermediate metal layer, reducing the insulation resistance of the heat-fused resin layer, causing leakage, and shortening battery life. When the thickness of the heat-fused resin layer exceeds 120μm, the water vapor permeation will increase, the moisture inside the battery will increase, and the reaction with the electrolyte will produce gas, which will easily lead to the danger of expansion, cracking and leakage, and reduce battery life. Excessive hydrogen fluoride will corrode the anti-corrosion metal layer, resulting in a decrease in the adhesion strength between the intermediate metal layer and the heat-fused resin layer, which will easily lead to problems such as electrolyte leakage.
[0146] Metal-plastic composite film lamination process
[0147] 1. Degreasing treatment of the intermediate metal layer: The surface wettability of the intermediate metal layer is 65 dyn / cm, preferably 70 dyn / cm or higher, or the titration contact angle of distilled water is less than 15 degrees, preferably less than 10 degrees. If the wettability or surface water contact angle of the intermediate metal layer exceeds the given range, it indicates that there is a possibility that the rolling oil from the manufacturing stage may still remain on the metal. Therefore, the adhesion between the anti-corrosion layer, the intermediate metal layer, and the outer substrate resin layer becomes poor. During long-term storage of the battery, there is a risk of detachment between the intermediate metal layer and the outer substrate resin layer, which can easily lead to a short battery life. As a preventive measure, annealing treatment at 150°C or higher can be performed, or degreasing can be performed by plasma, corona treatment, or alkaline solution. The alkaline degreasing method involves immersing the metal in an alkaline solution at 50 to 65°C for a certain period of time, then washing it twice with deionized water, and then drying it to obtain the degreased metal.
[0148] 2. Formation of the anti-corrosion layer on the intermediate metal layer: After applying an anti-corrosion liquid to the surface of the intermediate metal layer on the side in contact with the outer substrate resin layer, it is heat-treated at high temperature for a period of time.
[0149] 3. Formation and lamination of the outer adhesive layer: A polyurethane adhesive dissolved in an organic solvent is coated between the intermediate metal layer and the outer substrate resin layer. Heating at a certain temperature for a certain time allows the organic solvent to evaporate, forming the outer adhesive layer. Further lamination of the outer substrate resin layer, outer adhesive layer, and intermediate metal layer is carried out under certain temperature and pressure. After storage at a certain temperature for a certain time, the outer adhesive layer undergoes a curing reaction, resulting in a composite resin layer consisting of the outer substrate resin layer, outer adhesive layer, and intermediate metal layer. When the lamination of the outer substrate resin layer and intermediate metal layer does not use an outer adhesive layer, the intermediate metal layer and outer substrate resin layer are laminated by heating and pressurizing. The outer substrate resin layer is then film-formed through heat treatment, ultraviolet treatment, and electron beam treatment to obtain the composite resin layer consisting of the outer substrate resin layer and intermediate metal layer.
[0150] 4. Lamination of the hot-melt resin layer: The composite film consisting of the outer substrate resin layer and the intermediate metal layer can be laminated with the hot-melt resin layer using different lamination methods, as illustrated below: a. Dry lamination method: A solution-type inner layer adhesive composed of a main agent, curing agent, and organic solvent is applied to the corrosion-resistant surface of the intermediate metal layer of the composite film consisting of the outer substrate resin layer and the intermediate metal layer. The solution-type inner layer adhesive is dried to form an inner layer adhesive layer, which is then thermally laminated with the bonding surface of the hot-melt resin layer under certain temperature and pressure. After curing, a composite product of outer substrate resin layer / outer layer adhesive layer / intermediate metal layer / inner layer adhesive layer / hot-melt resin layer is formed. Preferably, the bonding surface of the hot-melt resin layer in contact with the inner layer adhesive layer is pre-treated with corona discharge. Additionally, a curing treatment not exceeding 60°C of the inner adhesive layer's melting point temperature can be performed; b. Melt extrusion method: A hot-melt inner adhesive layer of a certain thickness is formed on the corrosion-resistant surface of the intermediate metal layer by melt extrusion of the hot-melt inner adhesive resin. Furthermore, thermal bonding is performed on the surface of the inner adhesive layer and the bonding surface of the hot-melt resin layer to form a composite product of outer substrate resin layer / outer adhesive layer / intermediate metal layer / inner adhesive layer / hot-melt resin layer. To improve the peel strength between the intermediate metal layer and the hot-melt resin layer, a heat treatment not exceeding 60°C of the inner adhesive layer's melting point temperature can be performed; c. Melt extrusion method: The hot-melt inner adhesive layer and the hot-melt resin layer are co-extruded to form a composite product of outer substrate resin layer / outer adhesive layer / intermediate metal layer / inner adhesive layer / hot-melt resin layer. After the surface of the intermediate metal layer in contact with the inner adhesive layer is treated with anti-corrosion, a heat treatment not exceeding 60°C of the melting point of the inner adhesive layer can be performed to improve the peel strength between the intermediate metal layer and the hot-melt resin layer; d. Hot bonding method: The resin main agent with a melting point above 100°C and the curing agent are dissolved in an aqueous or organic solvent to form an aqueous solution-type inner adhesive. This is applied to the anti-corrosion treated surface of the metal layer of the composite layer consisting of the outer substrate resin layer and the intermediate metal layer, and the solution-type inner adhesive is dried to form the inner adhesive layer. Under certain temperature and pressure, the bonding surface with the hot-melt resin layer is thermally bonded to form a composite product of outer substrate resin layer / outer adhesive layer / intermediate metal layer / inner adhesive layer / hot-melt resin layer. To improve the peel strength between the intermediate metal layer and the hot-melt resin layer, a heat treatment not exceeding 60°C of the melting point of the inner adhesive layer can be performed. The hot melt resin layer can also be formed by extrusion or by using a film. When using a film, it is preferable that the bonding surface of the hot melt resin layer in contact with the inner adhesive layer is pre-treated with corona.
[0151] The peel strength test between the intermediate metal layer and the outer substrate resin layer of the finished metal-plastic composite film is as follows.
[0152] Initial peel strength test
[0153] The finished metal-plastic composite film was prepared into straight strips, each 100*15mm in size. A tensile testing device was used to conduct a peel test between the intermediate metal layer and the outer substrate resin layer. The peeled outer substrate resin layer was placed in the upper clamp of the tensile testing device, and the intermediate metal layer in the lower clamp. A T-shaped peel with a 180° angle was then performed at a stretching speed of 50mm / min. The peel strength between the intermediate metal layer and the outer substrate resin layer was then measured. The peel strength was measured by taking the average value of the peel strength over a distance of 10mm to 40mm when the outer substrate resin layer and the intermediate metal layer moved a distance of 50mm. Five films were tested in parallel.
[0154] High temperature and high humidity resistance test of metal-plastic composite film products
[0155] The metal-plastic composite film was prepared into a sheet shape of 92(TD)*76(MD)mm. A deep-drawing test device was used to form the metal-plastic composite film, with a drawing depth of 7mm, a surface pressure of 1MPa, and a drawing time of 5s. The formed size was 62(TD)*46(MD)mm. After forming, the sample was observed in a dark room using a light source to check its integrity (paying special attention to whether the four corners were damaged). If the sample was cracked, it was discarded and re-cut until a complete sample was selected. The intact deep-drawn sample was placed with the groove facing down on a module (the module was placed inside the groove). The module dimensions were 61*45mm, and the height was 5.5mm. Then, downward pressure was applied directly above the groove of the sample to deform it (deformation depth 1.5mm). The temperature and humidity of the constant temperature and humidity chamber were adjusted to 65℃·90%RH. After stabilization, the sample that had undergone the deep-drawing and deformation treatment and remained intact was placed in the constant temperature and humidity chamber (the sample was laid flat). Observe whether the outer substrate resin layer lifts off the molded area after 5, 10, and 30 days. Perform parallel tests with 10 samples per group.
[0156] Compared with the prior art, the positive effects of the present invention are:
[0157] For the first time, it is proposed that the intermediate metal layer is made of nickel-plated steel plate material, and the elements in the anti-corrosion layer on the surface of the intermediate metal layer are distributed in a gradient. By controlling the carbon (C) content in the outermost layer of the anti-corrosion layer and the content of intermediate metal elements and fluorine (F) elements in the inner layer (40nm), the initial peel strength between the intermediate metal layer and the outer substrate resin layer of the metal-plastic composite film and its resistance in high temperature and high humidity environments can be improved.
[0158] There are no particular limitations on the preparation method of outer packaging materials, as long as the anti-corrosion layer specified in the aforementioned case can be obtained, and known methods for preparing outer packaging materials can be used.
[0159] The following description of the preparation method of outer packaging materials for devices with stable bonding properties and batteries is not intended to limit this case.
[0160] 1. Composite
[0161] The metal-plastic composite film is composed of an outer substrate resin layer, an outer adhesive layer A (3μm), an intermediate metal layer, an inner adhesive layer B, and a heat-fused resin layer. The thicknesses of the outer substrate resin layer and the intermediate metal layer may be varied depending on the specific embodiment.
[0162] The lamination method is as follows: The outer substrate resin layer film in contact with the outer adhesive layer A is subjected to corona treatment. Specifically, a non-crystalline polyester polyol with a weight-average molecular weight of 5000, a Tg of 50℃, and a hydroxyl value of 25 mg KOH / g is mixed with a non-crystalline polyester polyol with a weight-average molecular weight of 20000, a Tg of -17℃, and a hydroxyl value of 8 mg KOH / g at a weight ratio of 3:2. Toluene diisocyanate (TDI) is added to form an outer adhesive liquid with an NCO / OH ratio of 6.2, which is then coated onto the intermediate metal, forming adhesive layer A (3 μm) on the intermediate metal. After thermal lamination of the outer adhesive layer A and the outer substrate resin layer film on the intermediate metal, a curing treatment is performed at 80℃ for 3 days to form an outer substrate resin layer / outer adhesive layer A (3 μm) / intermediate metal layer. Both sides of the intermediate metal layer are pre-treated with anti-corrosion coating.
[0163] Both sides of the metal layer have been pre-treated for corrosion protection.
[0164] The anti-corrosion liquid used in Examples 1-8 and Comparative Example 1 was evenly coated onto both sides of the intermediate metal using a coating roller, and then baked at 190°C for 2 minutes. The wet film weight of the anti-corrosion layer treatment liquid was 5 g / m². 2 .
[0165] Comparative Examples 2 and 3 were heated to 100°C for 2 minutes. The wet film weight of the anti-corrosion coating solution was 5 g / m². 2 .
[0166] Finally, the inner adhesive layer B and the hot-melt resin layer are laminated onto the metal surface of the semi-finished product: outer substrate resin layer / outer adhesive layer A (3μm) / middle metal layer.
[0167] Melt-type inner adhesive layer B composite method: The molten resin used for the inner adhesive layer is anhydrous maleic anhydride-modified polypropylene. A 15μm thick adhesive layer is formed on the corrosion-resistant surface of the intermediate metal layer in contact with the hot-melt resin layer. Further, it is composited with a 30μm thick hot-melt resin. The inner adhesive layer and the hot-melt resin layer are composited onto the corrosion-resistant surface of the intermediate metal layer in contact with the hot-melt resin layer via melt co-extrusion. The inner adhesive layer used is 60% (by weight) of anhydrous maleic anhydride-modified random copolymer polypropylene with a melting point of 140℃, an MFR (230℃) of 5 g / 10 min, and an anhydrous maleic anhydride modification degree of 10% on the random copolymer polypropylene. It also has a melting point of 160℃, an MFR (230℃) of 2.6 g / 10 min, and a density of 0.87 g / cm³. 3 A copolymer elastomer of propylene and butene comprising 24% (by weight), with a melting point of 130°C, an MFR (at 230°C) of 9.5 g / 10 min, and a density of 0.91 g / cm³. 3 It is a mixture consisting of 8% (by weight) of ethylene and propylene crystalline copolymer elastomer and 8% (by weight) of low-density polyethylene with a melting point of 105°C and an MFR (230°C) of 12 g / 10 min.
[0168] The hot-melt resin layer consists of two layers, and its structure is as follows:
[0169] The resin layer in contact with the inner adhesive layer is a mixture of random copolymer polypropylene with a melting point of 155°C and an MFR (230°C) of 4 g / 10 min, 33% of amorphous propylene elastomer, and 5% of low-density polyethylene with a melting point of 110°C and an MFR (230°C) of 7.5 g / 10 min, by weight ratio.
[0170] Innermost resin layer: a layer composed of random copolymer polypropylene with a melting point of 155℃ and an MFR (230℃) of 15g / 10min;
[0171] The thickness ratio of the resin layer in contact with the inner adhesive layer to the innermost resin layer is 8:2.
[0172] After the intermediate metal layer is laminated with the inner adhesive layer and the hot-melt resin layer, it is heat-treated at 180°C for 2 seconds. This forms a composite product consisting of an outer substrate resin layer / outer adhesive layer A (3μm) / intermediate metal layer / inner adhesive layer B-1 (15μm) / hot-melt resin layer (30μm).
[0173] The peel strength test between the intermediate metal layer and the outer substrate resin layer of the finished metal-plastic composite film is as follows.
[0174] (1) Initial peel strength test (the results are shown in Table 1)
[0175] The finished metal-plastic composite film was prepared into straight strips, each 100*15mm in size. A tensile testing device was used to conduct a peel test between the intermediate metal layer and the outer substrate resin layer. The peeled outer substrate resin layer was placed in the upper clamp of the tensile testing device, and the intermediate metal layer in the lower clamp. A T-shaped peel with a 180° angle was then performed at a stretching speed of 50mm / min. The peel strength between the intermediate metal layer and the outer substrate resin layer was then measured. The peel strength was measured by taking the average value of the peel strength over a distance of 10mm to 40mm when the outer substrate resin layer and the intermediate metal layer moved a distance of 50mm. Five films were tested in parallel.
[0176] (2) High temperature and high humidity resistance test of metal-plastic composite film finished product (the results are shown in Table 1)
[0177] The metal-plastic composite film was prepared into a sheet shape of 92(TD)*76(MD)mm. A deep-drawing test device was used to form the metal-plastic composite film, with a drawing depth of 7mm, a surface pressure of 1MPa, and a drawing time of 5s. The formed size was 62(TD)*46(MD)mm. After forming, the sample was observed in a dark room using a light source to check its integrity (paying special attention to whether the four corners were damaged). If the sample was cracked, it was discarded and re-cut until a complete sample was selected. The intact deep-drawn sample was placed with the groove facing down on a module (the module was placed inside the groove). The module dimensions were 61*45mm, and the height was 5.5mm. Then, downward pressure was applied directly above the groove of the sample to deform it (deformation depth 1.5mm). The temperature and humidity of the constant temperature and humidity chamber were adjusted to 65℃·90%RH. After stabilization, the sample that had undergone the deep-drawing and deformation treatment and remained intact was placed in the constant temperature and humidity chamber (the sample was laid flat). Observe whether the outer substrate resin layer lifts off the molded area after 5, 10, and 30 days. Perform parallel tests with 10 samples per group.
[0178] 3. Measurement Method
[0179] (1) Measurement of water contact angle
[0180] The water contact angle of the metal surface was measured using a German KRUSS DSA25 contact angle meter. The metal was placed flat on the instrument's worktable, and the amount of water dispensed from the syringe was controlled to be 2 μml each time. The dispensing rate was 2.67 μmL / s, and the contact angle value at which the water droplet just fell onto the metal surface was recorded.
[0181] (2) Dyne value determination
[0182] Using the German Arcotest dyne pen, draw two straight lines 10cm long on the metal surface. If the lines shrink by more than 10% within 3 seconds, it indicates that the dyne value of the metal surface does not reach the dyne value of the dyne pen at this time. Select a dyne pen with a lower dyne value for retesting.
[0183] (3) Elemental analysis of anti-corrosion layer
[0184] The elemental distribution at the surface, 20 nm, and 40 nm depths of the anti-corrosion layer on a metal surface was determined using an XPS (Shimadzu, UK, AXIS supra) via the ESCA method. Ar ions were sputtered onto the metal sample surface at a beam diameter of 800 μm, a voltage of 15 kV, a sputtering depth of 5 nm, a sputtering rate of 3 nm / min, and 7 sputtering cycles. The signal source detection depth was 5 nm, the detection limit was 1‰, and the number of detection cycles was 8.
[0185] Example 1
[0186] The intermediate metal layer is made of nickel-plated steel plate. The metal thickness is 50 μm, and the nickel plating layer thickness is 2 μm. The water contact angle is 20°. Both sides of the metal are treated with anti-corrosion coating. The elemental composition of each layer in the anti-corrosion coating on both sides is as shown in Table 1. The content ratio of chromium fluoride, hydrofluoric acid, and polyvinyl alcohol resin on the metal surface is 15:1:3, and the chromium (Cr) content of the metal surface coating is 10 mg / m³. 2 .
[0187] Example 2
[0188] The intermediate metal layer is made of nickel-plated steel sheet. The metal thickness is 50 μm, and the nickel plating layer thickness is 2 μm. The dyn value is 75 dyn / cm. Both sides of the metal are treated with anti-corrosion coating. The elemental composition of each layer in the anti-corrosion coating on both sides is as shown in Table 1. The content ratio of chromium fluoride, hydrofluoric acid, polyvinyl alcohol resin, and titanium fluoride on the intermediate metal surface is 15:1:3:2, and the chromium (Cr) content of the metal surface coating is 15 mg / m³. 2 .
[0189] Example 3
[0190] The intermediate metal layer is made of nickel-plated steel sheet. The metal thickness is 50 μm, and the nickel plating layer thickness is 2 μm. The water contact angle is 10°. Both sides of the metal are treated with anti-corrosion coating. The elemental composition of each layer in the anti-corrosion coating on both sides of the metal is shown in Table 1. The content ratio of chromium phosphate and chromium fluoride, phosphoric acid, and phenolic resin on the intermediate metal surface is 5:2:1, and the chromium (Cr) content of the coating on the metal surface is 12 mg / m³. 2 .
[0191] Example 4
[0192] The intermediate metal layer is made of nickel-plated steel sheet. The metal thickness is 50 μm, and the nickel plating layer thickness is 12 μm. The water contact angle is 15°. The metal is cleaned with an alkaline cleaning agent, and both sides of the metal undergo anti-corrosion treatment. The elemental composition of each layer in the anti-corrosion layer on both sides of the metal is as shown in Table 1. The content ratio of chromium nitrate, phosphoric acid, and acrylic resin on the intermediate metal surface is 2:2:1, and the chromium (Cr) content of the metal surface coating is 30 mg / m³. 2 .
[0193] Example 5
[0194] The intermediate metal layer is made of nickel-plated steel sheet. The metal thickness is 50 μm, and the nickel plating layer thickness is 17 μm. The water contact angle is 15°, and the metal is cleaned with an alkaline cleaning agent. Both sides of the metal are treated with anti-corrosion coating. The elemental composition of each layer in the anti-corrosion coating on both sides of the metal is as shown in Table 1. The content ratio of chromium nitrate, phosphoric acid, and acrylic resin on the intermediate metal surface is 2:2:1, and the chromium (Cr) content of the coating on the metal surface is 25 mg / m³. 2 .
[0195] Example 6
[0196] The intermediate metal layer is made of nickel-plated steel sheet. The metal thickness is 50 μm, and the nickel plating layer thickness is 2 μm. The water contact angle is 15°. Both sides of the metal are treated with anti-corrosion. The crosslinking agent content in the anti-corrosion solution is 0.06%. The elemental composition of each layer in the anti-corrosion layer on both sides of the metal is shown in Table 1. The content ratio of chromium nitrate, phosphoric acid, and acrylic resin on the intermediate metal surface is 2:2:1, and the chromium (Cr) content of the metal surface coating is 15 mg / m³. 2 .
[0197] Example 7
[0198] The intermediate metal layer is made of nickel-plated steel sheet. The metal thickness is 50 μm, and the nickel plating layer thickness is 2 μm. The water contact angle is 15°. Both sides of the metal are treated with anti-corrosion. The crosslinking agent content in the anti-corrosion solution is 8.3%. The elemental composition of each layer in the anti-corrosion layer on both sides of the metal is shown in Table 1. The content ratio of chromium nitrate, phosphoric acid, and acrylic resin on the intermediate metal surface is 2:2:1, and the chromium (Cr) content of the metal surface coating is 15 mg / m³. 2 .
[0199] Example 8
[0200] The intermediate metal layer is made of nickel-plated steel sheet. The metal thickness is 50 μm, and the nickel plating layer thickness is 5 μm. The water contact angle is 15°. Both sides of the metal are treated with anti-corrosion. The crosslinking agent content in the anti-corrosion solution is 14.93%. The elemental composition of each layer in the anti-corrosion layer on both sides of the metal is shown in Table 1. The content ratio of chromium nitrate, phosphoric acid, and acrylic resin on the intermediate metal surface is 2:2:1, and the chromium (Cr) content of the metal surface coating is 15 mg / m³. 2 .
[0201] Comparative Example 1
[0202] The intermediate metal layer is made of nickel-plated steel plate with a thickness of 50 μm, and the nickel plating layer is 2 μm thick. The water contact angle is 15°. Both sides of the metal are treated with anti-corrosion coating. The elemental composition of each layer in the anti-corrosion coating on both sides is as shown in Table 1. The content ratio of chromium fluoride, hydrofluoric acid, and polyvinyl alcohol resin on the metal surface is 2:1:5, and the chromium (Cr) content of the coating on the metal surface is 5 mg / m³. 2 .
[0203] In Examples 1-8, the initial peel strength of the metal-plastic composite film was above 6.5 N / 15 mm. After molding, no floating or delamination occurred after 5 days of storage in a high temperature and high humidity environment (90% at 60°C). However, the content of trivalent chromium compounds in the anti-corrosion liquid used in this comparative example was relatively low.
[0204] The surface has a carbon (C) content of 76%, and the element content from the intermediate metal layer is 10%. 40 nm from the surface of the anti-corrosion layer inwards, the carbon (C) content is 14%, which is relatively high, while the element content from the intermediate metal layer is 29%, which is relatively low.
[0205] At this point, although the initial strength is 7.3 N / 15 mm, after molding, it floats and delaminates after being stored in a high temperature and high humidity environment (90% at 60℃) for 5 days, indicating poor durability.
[0206] Comparative Example 2
[0207] The intermediate metal layer is made of nickel-plated steel sheet with a thickness of 50 μm and a nickel plating layer thickness of 2 μm. The dyn value is 75 dyn / cm. Both sides of the metal are treated with anti-corrosion coatings. The elemental composition of each layer in the anti-corrosion coatings on both sides is shown in Table 1. The content ratio of chromium nitrate, phosphoric acid, and acrylic resin on the intermediate metal surface is 1:2:1, and the chromium (Cr) content on the metal surface coating is 15 mg / m³. 2 .
[0208] Comparative Examples 1-8: The heating conditions for forming the anti-corrosion layer in this comparative example are 100°C for 2 minutes.
[0209] The surface carbon (C) content is 38%, which is low, while the element content from the intermediate metal layer is 52%, which is high. 40 nm inward from the surface of the anti-corrosion layer, the carbon (C) content is 59%, which is also high.
[0210] At this point, the initial strength was 4.2 N / 15 mm, which is lower than that of the example.
[0211] It can be inferred that when the content of intermediate metal elements in the anti-corrosion layer is too high, the degree of bridging reaction is too high, resulting in an anti-corrosion layer that is hard and brittle, which is not conducive to forming and is prone to cracking or pinholes. This leads to moisture intrusion into the damaged parts when stored in harsh environments, causing delamination and floating.
[0212] Comparative Example 3
[0213] The intermediate metal layer is made of nickel-plated steel sheet with a thickness of 50 μm and a nickel plating layer thickness of 0.2 μm. The dyn value is 75 dyn / cm. Both sides of the metal are treated with anti-corrosion coating. The crosslinking agent content in the anti-corrosion solution is 25%. The elemental composition of each layer in the anti-corrosion coating on both sides of the metal is shown in Table 1. The content ratio of chromium nitrate, phosphoric acid, and acrylic resin on the intermediate metal surface is 1:2:1, and the chromium (Cr) content on the metal surface coating is 15 mg / m³. 2 .
[0214] Comparative Examples 1-8: The heating conditions for forming the anti-corrosion layer in this comparative example are 100°C for 2 minutes.
[0215] The surface contains 74% carbon (C), while the elemental content from the intermediate metal layer is 7%. 40 nm inwards from the surface of the anti-corrosion layer, the carbon (C) content is 6%, and the elemental content from the intermediate metal layer is 78%.
[0216] At this point, the initial strength was 12.7 N / 15 mm. Although it showed better peel strength in the initial stage compared with the example, the excessively high content of crosslinking agent in the anti-corrosion liquid led to an excessively high degree of crosslinking reaction in the anti-corrosion layer. This resulted in a hard and brittle anti-corrosion layer, which was not conducive to molding and was prone to cracking or pinholes. As a result, when stored in harsh environments, moisture could penetrate into the damaged areas, causing delamination and floating.
[0217]
[0218] Therefore, this invention has excellent durability and high stability, and has extremely high industrial application value.
[0219] The above content involving common knowledge will not be described in detail, as those skilled in the art will understand.
[0220] The above descriptions are merely some specific embodiments of the present invention and are not intended to limit the invention. Any modifications, equivalent substitutions, or improvements made within the spirit and principles of the present invention should be included within the scope of protection of the present invention. The technical scope of this invention is not limited to the contents of the specification, but must be determined according to the scope of the claims.
Claims
1. A high-stability outer packaging material for battery devices, characterized in that: include: Outer substrate resin layer; and An intermediate metal layer and an anti-corrosion layer formed by corrosion-resistant treatment of the intermediate metal layer, wherein the anti-corrosion layer is disposed between the outer substrate resin layer and the intermediate metal layer, wherein: From the outermost layer of the anti-corrosion layer on the resin layer side of the outer substrate, along the thickness direction of the anti-corrosion layer, the carbon content of the anti-corrosion layer decreases in a gradient, while the nickel (Ni) content increases in a gradient. The anti-corrosion layer is formed by drying an anti-corrosion liquid, which mainly contains trivalent chromium compounds, inorganic acids, organic resins, crosslinking agents, and solvents composed of water or organic solvents, or mixtures thereof. The elemental composition of the anti-corrosion layer on the resin layer side of the outer substrate is distributed in a gradient. The outermost layer of the anti-corrosion layer on the resin layer side of the outer substrate has a carbon (C) content greater than or equal to 40% and less than or equal to 100%, a nickel (Ni) content less than or equal to 10%, and a fluorine (F) content less than or equal to 10%. In the layer 40nm below the surface of the anti-corrosion layer, the carbon (C) content is less than or equal to 10%, the nickel (Ni) content is greater than or equal to 30% and less than or equal to 100%, and the fluorine (F) content is less than or equal to 20%.
2. The outer packaging material according to claim 1, characterized in that: The intermediate metal layer is a nickel-plated steel plate, and the thickness of the nickel plating layer on the nickel-plated steel plate is from 0.5 μm to 20 μm.
3. The outer packaging material according to claim 1, characterized in that: The crosslinking agent contains at least one of the following: amino resin, melamine resin, phenolic resin, epoxy compound, end-capped isocyanate compound, oxazoline compound, carbodiimide compound, condensate of formaldehyde and alkyl monool having 1 to 4 carbon atoms, condensate of carbolic acid and formaldehyde, and derivatives of the above substances.
4. The outer packaging material according to claim 1, characterized in that: The anti-corrosion liquid used to form the anti-corrosion layer contains at least one of the following trivalent chromium compounds: chromium nitrate and chromium fluoride. The anti-corrosion liquid used to form the anti-corrosion layer contains titanium (Ti) compounds or zirconium (Zr) compounds, with contents of 0 to 0.6% and 0 to 2.8%, respectively.
5. The outer packaging material according to claim 4, characterized in that: The corrosion-resistant liquid used to form the corrosion-resistant layer contains at least one inorganic acid, namely phosphoric acid, nitric acid, or hydrofluoric acid; at least one organic resin, namely acrylic resin, methacrylic resin, hydroxyacrylic resin, polyvinyl alcohol resin, olefin resin, or phenolic resin; at least one titanium (Ti) compound, namely titanium fluoride or titanium nitrate; at least one zirconium (Zr) compound, namely zirconium fluoride or zirconium nitrate; and at least one organic solvent, namely isopropanol, ethanol, or ethylene glycol butyl ether.
6. The outer packaging material according to any one of claims 1-5, characterized in that: It further includes an inner adhesive layer and a hot-melt resin layer; the intermediate metal layer is disposed on the inner adhesive layer, and the inner adhesive layer is disposed on the hot-melt resin layer.
7. The outer packaging material according to claim 6, characterized in that: It further includes an outer adhesive layer, wherein the outer substrate resin layer is disposed on the outer adhesive layer, and the outer adhesive layer is disposed on the anti-corrosion layer.
Citation Information
Patent Citations
Ferronickel-mild steel composite material and preparation method thereof
CN106498451A
Metal composite film and electrochemical device
CN112563632A