AI Technical Summary
Traditional lithium-ion battery binders have a high swelling rate in the electrolyte and poor adhesion. Toxic solvents are used in the preparation process, which results in complex processes and high costs.
Using low-swelling soap-free core-shell emulsion binder, through a combination of hydrophilic monomers, hydrophobic monomers, reactive emulsifiers and cross-linking agents, the shell and core layer structures are designed to block electrolyte penetration and adjust mechanical properties. Reduce emulsifier foaming and side reactions.
It significantly reduces the swelling rate of the binder, improves the bonding strength and mechanical properties, ensures the stability and cycle performance of the lithium-ion battery pole pieces, and reduces production costs and environmental pollution.
Smart Images

Figure CN115838455B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of new energy and new materials, and in particular to a low-swelling soap-free core-shell emulsion binder and a preparation method and application thereof. Background Art
[0002] Lithium-ion batteries have the advantages of high energy density, low cost, no memory effect, and long cycle life. They are widely used in electronic equipment, electric vehicles, grid energy storage and other fields. Lithium-ion battery binder is a kind of high molecular polymer. It can stabilize the active material slurry and ensure the uniformity of the slurry during the production and processing of lithium-ion batteries. At the same time, it can bind the active material, conductive agent and current collector to improve the structural stability of the battery pole. With the continuous explosion of the domestic new energy vehicle market, the domestic demand for lithium-ion batteries has further expanded, and the demand for binders has also increased.
[0003] Traditional emulsion adhesives (such as styrene-butadiene emulsion SBR) contain small molecule emulsifiers, which easily produce more bubbles during the slurry process of battery manufacturing, affecting the coating performance of the electrode. During the drying process of the electrode, it is easy to cause the adhesive to float, affecting the adhesion of the active material to the current collector. Traditional acrylic emulsion adhesives contain a large number of ester functional groups with strong affinity for the electrolyte. In the electrolyte environment, the adhesive will absorb liquid and swell, causing the adhesive to lose its bonding activity, resulting in the de-powdering of the battery electrode, etc., seriously affecting the stability of the electrode structure.
[0004] Patent CN114685705A "Application of a low swelling vinylidene fluoride copolymer as a lithium battery binder" discloses a vinylidene fluoride copolymer formed by copolymerization of vinylidene fluoride monomer, vinyl fluoride monomer and 1,1-monofluoromonochloroethylene monomer, and its swelling rate in the electrolyte is ≤20%. Its shortcomings are: on the one hand, the binder needs to use toxic organic solvents such as N-methylpyrrolidone (NMP) during use, which pollutes the environment; on the other hand, there are multiple gases in the synthetic raw materials, which have very strict requirements on the synthetic process and synthetic equipment, and the preparation cost is high. Summary of the invention
[0005] The purpose of the present invention is to provide a low swelling soap-free core-shell emulsion binder in view of the problems of high swelling rate and poor bonding force of existing lithium ion battery negative electrode binders in electrolyte. The binder has polar groups and a cross-linked network structure in the shell layer, which can effectively block the penetration of the electrolyte and reduce the swelling of the binder. At the same time, the strong polar groups provide bonding force; the core layer structure can play a role in adjusting the mechanical properties of the binder and absorbing and buffering external stress. The binder does not contain a small molecule emulsifier, which can reduce the foaming phenomenon of the emulsifier in the battery homogenization process and avoid the potential side reaction between the small molecule emulsifier and the internal materials of the battery during the battery cycle.
[0006] The purpose of the present invention is achieved through the following technical solutions:
[0007] The invention provides a low-swelling soap-free core-shell emulsion adhesive, which comprises the following components: a hydrophilic monomer, a hydrophobic monomer, a reactive emulsifier and a crosslinking agent.
[0008] Furthermore, the hydrophilic monomer of the low swelling soap-free core-shell emulsion binder can be a combination of one or more of itaconic acid, acrylic acid, methacrylic acid, N-vinyl pyrrolidone, ammonium acrylate, and methacrylamide.
[0009] Furthermore, the hydrophobic monomer of the low swelling soap-free core-shell emulsion binder can be a combination of one or more of ethyl acrylate, butyl acrylate, butyl methacrylate, 2-ethylethyl acrylate, lauryl acrylate, methyl acrylate, methyl methacrylate, acrylonitrile, 2-methoxyethyl acrylate, ethoxyethoxyethyl acrylate, octadecyl acrylate, and octadecyl methacrylate.
[0010] Furthermore, the reactive emulsifier of the low swelling soap-free core-shell emulsion binder can be a combination of one or more of allyl ether sulfonates, acrylamide sulfonates, maleic acid derivatives, and allyl alkyl succinate sulfonates.
[0011] Furthermore, the crosslinking agent of the low swelling soap-free core-shell emulsion adhesive is a combination of one or more of an aziridine crosslinking agent, a polycarbodiimide crosslinking agent, N,N-methylenebisacrylamide, and divinylbenzene.
[0012] The present invention also provides a method for preparing the low swelling soap-free core-shell emulsion binder, comprising the following steps:
[0013] Step 1, adding water, a reactive emulsifier, 5%-50%wt of a hydrophilic monomer, 5%-50%wt of a hydrophobic monomer, and a pH regulator to a reaction vessel filled with condensation reflux, and adjusting the pH to 3-7;
[0014] Step 2: Under stirring, an inert gas is introduced by bubbling or vacuuming to exclude oxygen;
[0015] Step 3: Heat the reactor to 50-90°C, add a water-soluble initiator, and react for 0.5-2h under mechanical stirring;
[0016] Step 4, adding the remaining hydrophilic monomer and hydrophobic monomer dropwise for 1-4 hours, and keeping warm for 4-24 hours;
[0017] Step 5, adding a cross-linking agent and keeping warm for 1-2 hours;
[0018] Step 6, cooling to 30-50°C, adding a pH adjuster, and adjusting the pH to 7-9;
[0019] Step eight, filtering through a filter screen to obtain a polymer emulsion binder.
[0020] Further, the solid content of the low swelling soap-free core-shell emulsion accounts for 20-50%wt of the total weight of the low swelling soap-free core-shell emulsion;
[0021] Further, the hydrophilic monomer is used in an amount of 30-50%wt based on the solid content of the low swelling soap-free core-shell emulsion;
[0022] Further, the amount of the hydrophobic monomer is 35-65%wt based on the solid content of the low swelling soap-free core-shell emulsion;
[0023] Further, the amount of the reactive emulsifier is 5-10%wt based on the solid content of the low swelling soap-free core-shell emulsion;
[0024] Furthermore, the water-soluble initiator is a combination of one or more of sodium persulfate, potassium persulfate, ammonium persulfate, and azobisisobutylamidine hydrochloride, and the amount of the water-soluble initiator is 0.1%-2%wt based on the solid content of the low-swelling soap-free core-shell emulsion.
[0025] Furthermore, the pH adjuster is a combination of one or more of sodium hydroxide, lithium hydroxide, ammonia water, potassium hydroxide and sodium bicarbonate.
[0026] The present invention also provides a lithium ion battery negative electrode, comprising a negative electrode substrate and a negative electrode material coated on the negative electrode substrate, wherein the negative electrode material contains a negative electrode active material, a conductive agent and the low swelling soap-free core-shell emulsion binder.
[0027] The negative electrode substrate can be all known negative electrode substrates for lithium ion batteries, including but not limited to copper foil. The negative electrode active material can be all known negative electrode active materials for lithium ion batteries, such as but not limited to graphite, soft carbon, hard carbon, lithium titanate, silicon, silicon carbon, silicon oxygen carbon, silicon tin alloy, tin, tin carbon or germanium. The conductive agent can be all known negative electrode conductive agents for lithium ion batteries, including but not limited to Super P, carbon nanotubes and Ketjen black.
[0028] The negative electrode of the lithium ion battery is prepared as follows: the negative electrode active material, the conductive agent and the polymer emulsion binder are added into an appropriate amount of water to form an electrode slurry, wherein the polymer emulsion binder accounts for 1%-20%wt based on the solid content of the electrode slurry (i.e., based on the total weight of the negative electrode material), and then the electrode slurry is coated on the negative electrode substrate and dried to form the negative electrode of the lithium ion battery.
[0029] The present invention provides a lithium ion battery, comprising a positive electrode, a negative electrode, a separator and an electrolyte, wherein the negative electrode is the negative electrode of the lithium ion battery prepared according to the method of the present invention.
[0030] Compared with the prior art, the present invention has the following advantages and beneficial technical effects:
[0031] The low swelling soap-free core-shell emulsion binder of the present invention is designed with a core-shell structure. The cross-linked network structure of the shell layer can reduce the penetration of the electrolyte, ensure the low swelling characteristics of the binder, and the strong polar group can provide bonding strength; the core layer structure can adjust the mechanical properties of the binder, absorb and buffer the stress generated by the volume change of the active material in the battery during the charge and discharge process; the soap-free system can reduce the influence of the emulsifier on the floating of the binder during the battery homogenization process, and further ensure the bonding ability of the binder. Therefore, the low swelling soap-free core-shell emulsion binder of the present invention plays a key role in the stability of the lithium ion battery pole piece and the battery cycle stability. By using the low swelling soap-free core-shell emulsion binder of the present invention to prepare the negative electrode of the lithium ion battery, and then making the lithium ion battery, the obtained lithium ion battery has good cycle performance, and still has 90.37% of the capacity after 300 cycles, and can form a thinner SEI film, which is more conducive to the transmission of lithium ions. Moreover, the low swelling soap-free emulsion binder and the lithium ion battery negative electrode synthesis process of the present invention are simple, easy to operate, and have high production efficiency, which is suitable for popularization and application. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 These are the 180° peeling test results of the graphite negative electrode sheets prepared with the polymer emulsion binders of Examples 1-4 of the present invention and the graphite negative electrode sheets prepared with the binders of Comparative Examples 1-2.
[0033] Figure 2 The figure is a cycle capacity retention rate diagram of button-type half-cells prepared using the pole pieces of Example 1 of the present invention and Comparative Example 1.
[0034] Figure 3 This is an AC impedance test diagram of a button-type half-cell prepared using the pole pieces of Example 1 of the present invention and Comparative Example 1. DETAILED DESCRIPTION
[0035] The present invention is further described in detail below in conjunction with the embodiments and drawings, but the embodiments of the present invention are not limited thereto. Any other changes, modifications, substitutions, combinations, and simplifications made without departing from the spirit and principle of the present invention shall be equivalent replacement methods and are included in the protection scope of the present invention.
[0036] Example 1
[0037] In a 1L reactor equipped with condensation reflux, add 350g of deionized water, 7.5g of 2-acrylamido-2-methylpropanesulfonic acid sodium, 6g of acrylic acid, and 7.95g of butyl acrylate. Add sodium hydroxide to adjust the pH value of the system to 6. Use nitrogen bubbling for 60min, then heat to 80℃, add 0.75g of ammonium persulfate, react for 0.5h under mechanical stirring, drop 54g of acrylic acid and 71.55g of butyl acrylate, add dropwise, add after 2h, keep warm for 12h, add 3g of trimethylolpropane-tri[3-(2-methylaziridinyl)]propionate crosslinker, keep warm for 1h, cool to 30℃, add sodium hydroxide to adjust the pH value of the system to 7, and filter through a 100-mesh filter to obtain a low-swelling core-shell emulsion adhesive.
[0038] Graphite, conductive agent Super P and the prepared polymer emulsion binder were mixed in a mass ratio of 95:1:4, and adjusted into slurry with an appropriate amount of deionized water. The slurry was coated on a copper foil and dried to prepare a pole piece.
[0039] Example 2
[0040] In a 1L reactor equipped with condensation reflux, add 350g of deionized water, 6.5g of reactive emulsifier ER-10, 6g of acrylic acid and 2g of acrylamide, 8g of butyl acrylate and 2g of methyl methacrylate. Add lithium hydroxide and adjust the pH value of the system to 6. After evacuation, introduce nitrogen, then heat to 80°C, add 0.75g of potassium persulfate, react for 1h under mechanical stirring, drop 48g of acrylic acid and 4g of acrylamide, 60g of butyl acrylate and 10g of methyl methacrylate, add dropwise, add dropwise for 2h, keep warm for 4h, add 1g of trimethylolpropane-tri(3-aziridine) propionate crosslinker, keep warm for 2h, cool to 40°C, add lithium hydroxide to adjust the pH value of the system to 8, and filter through a 100-mesh filter to obtain a low-swelling core-shell emulsion adhesive.
[0041] Graphite, conductive agent Super P and the prepared polymer emulsion binder were mixed in a mass ratio of 95:1:4, and adjusted into slurry with an appropriate amount of deionized water. The slurry was coated on a copper foil and dried to prepare a pole piece.
[0042] Example 3
[0043] In a 1L reactor equipped with condensation reflux, add 450g of deionized water, 5g of sodium vinyl sulfonate, 6g of acrylic acid, and 7.95g of butyl acrylate. Add potassium hydroxide to adjust the pH value of the system to 6. Use nitrogen bubbling for 60min, then heat to 90°C, add 1g of azobisisobutyronitrile hydrochloride, react for 0.5h under mechanical stirring, drop 54g of acrylic acid and 71.55g of butyl acrylate, add dropwise, add after 2h, keep warm for 12h, add 3g of pentaerythritol-tri(3-aziridine) propionate crosslinker, keep warm for 1.5h, cool to 30°C, add potassium hydroxide to adjust the pH value of the system to 7, and filter through a 100-mesh filter to obtain a low-swelling core-shell emulsion adhesive.
[0044] Graphite, conductive agent Super P and the prepared polymer emulsion binder were mixed in a mass ratio of 95:1:4, and adjusted into slurry with an appropriate amount of deionized water. The slurry was coated on a copper foil and dried to prepare a pole piece.
[0045] Example 4
[0046] In a 1L reactor equipped with condensation reflux, add 450g of deionized water, 15g of sodium 2-acrylamido-2-methylpropanesulfonate, 20g of itaconic acid, and 48g of lauryl acrylate. Add ammonia water to adjust the pH value of the system to 6. Evacuate and introduce argon, then heat to 80°C, add 1g of ammonium persulfate, react for 0.5h under mechanical stirring, add 60g of itaconic acid and 48g of lauryl acrylate dropwise, add for 3h, keep warm for 24h, add 4g of trimethylolpropane-tri[3-(2-methylaziridinyl)]propionate crosslinker, keep warm for 1h, cool to 30°C, add ammonia water to adjust the pH value of the system to 9, and filter through a 100-mesh filter to obtain a low-swelling core-shell emulsion adhesive.
[0047] Graphite, conductive agent Super P and the prepared polymer emulsion binder were mixed in a mass ratio of 95:1:4, and adjusted into slurry with an appropriate amount of deionized water. The slurry was coated on a copper foil and dried to prepare a pole piece.
[0048] Example 5
[0049] In a 1L reactor equipped with condensation reflux, add 390g deionized water, 16.8g reactive emulsifier X-1025, 32g acrylic acid, 10g N-vinyl pyrrolidone, 32.5g butyl acrylate and 20g acrylonitrile. Add sodium hydroxide to adjust the system pH to 6. Use nitrogen bubbling for 60min, then heat to 50℃, add 0.75g ammonium persulfate, react for 2h under mechanical stirring, add 42g acrylic acid, 32.5g butyl acrylate and 20g acrylonitrile dropwise, add after 2h, keep warm for 12h, add 3g polycarbodiimide crosslinker, keep warm for 1h, cool to 50℃, add sodium hydroxide to adjust the system pH to 7, and filter through a 100-mesh filter to obtain a low-swelling core-shell emulsion adhesive.
[0050] Graphite, conductive agent Super P and the prepared polymer emulsion binder were mixed in a mass ratio of 95:1:4, and adjusted into slurry with an appropriate amount of deionized water. The slurry was coated on a copper foil and dried to prepare a pole piece.
[0051] Comparative Example 1
[0052] Comparative tests were conducted using styrene butadiene emulsion and sodium carboxymethyl cellulose binders instead of the polymer emulsion binder in Examples 1-4. Graphite, conductive agent Super P, styrene butadiene emulsion and carboxymethyl cellulose were mixed in a mass ratio of 95:1:2.4:1.6, and a suitable amount of deionized water was added to prepare a slurry. The slurry was coated on a copper foil and dried to prepare a pole piece.
[0053] Comparative Example 2
[0054] A comparative test was conducted by replacing the polymer emulsion binder in Examples 1 to 4 with a conventional negative electrode acrylic emulsion LA133 binder. Graphite, conductive agent Super P, styrene butadiene emulsion and carboxymethyl cellulose were mixed in a mass ratio of 95:1:2.4:1.6.
[0055] The battery electrodes prepared in Examples 1-4 and Comparative Example 1 were subjected to a 180° peeling force test. The test results are as follows: Figure 1 .Depend on Figure 1 It can be seen that the peeling force of the soap-free core-shell emulsion binders prepared in Examples 1-4 of the present invention is significantly higher than that of the control sample SBR, and also has a certain advantage over LA133. On the one hand, the reason is that the strong polar groups in the shell layer of the binder of the present invention provide high bonding force, and on the other hand, the binder of the present invention does not contain a small molecule emulsifier, which reduces the floating of the binder during the slurry coating process, ensuring the uniform dispersion of the binder in the electrode.
[0056] The binders of Examples 1-4 were dried, cut into polymer films with a diameter of 12 mm and a thickness of about 1 mm, and immersed in electrolyte (EC:DEC:DMC=1:1:1) respectively. The swelling rate of the binder was tested after standing in a glove box for 72 hours. Another SBR emulsion binder was taken as a control sample and treated in the same manner as above. The swelling rate test results are shown in Table 1.
[0057] Table 1
[0058] sample Swelling rate (%) Example 1 5% Example 2 11% Example 3 9% Example 4 19% Comparative Example 1 340% Comparative Example 2 31%
[0059] As can be seen from Table 1, the swelling rate of the low-swelling soap-free core-shell emulsion binder provided by the present invention in the electrolyte is less than 20%, which is significantly lower than that of Comparative Example 1 and Comparative Example 2. It can be seen that the cross-linked network structure of the shell layer can significantly reduce the penetration of the electrolyte. The binder of the present invention has lower swelling characteristics in the electrolyte environment and can better maintain the integrity of the electrode.
[0060] The pole pieces prepared in Example 1 and Comparative Example 1 were prepared into CR2025 button-type half-cells in a glove box and subjected to a long cycle test. The capacity retention rate was as follows: Figure 2 As shown. Figure 2 It can be seen that the capacity retention rate of the binder of the present invention is still 90.37% after 300 cycles, while the capacity retention rate of comparative example 1 is only 52.39%. The battery prepared by using the present invention has higher cycle performance.
[0061] The electrodes prepared in Example 1 and Comparative Example 1 were used to prepare CR2025 button-type half-cells in a glove box. After activation, AC impedance tests were performed under the condition of 0.5 SOC. The test results are shown in FIG. Figure 3 As shown. Figure 3 It can be seen that Example 1 has a lower SEI impedance of 0.54Ω, while the SEI impedance of Comparative Example 1 is as high as 14Ω. The binder of the present invention forms a thinner SEI film due to its lower swelling rate, and is therefore more conducive to the transmission of lithium ions.
[0062] The above specific examples are used to illustrate the present invention, which is only used to help understand the present invention and is not intended to limit the present invention. A person skilled in the art of the present invention may also make several simple deductions, modifications or substitutions based on the concept of the present invention. These deductions, modifications or substitutions also fall within the scope of the claims of the present invention.
Claims
1. A low swelling soap-free core-shell emulsion binder, characterized in that: The invention comprises the following components: a hydrophilic monomer, a hydrophobic monomer, a reactive emulsifier, and a crosslinking agent; the solid content of the low swelling soap-free core-shell emulsion binder accounts for 20%-50%wt of the total weight of the low swelling soap-free core-shell emulsion binder, and based on the solid content of the low swelling soap-free core-shell emulsion, the hydrophilic monomer accounts for 30%-50%wt, the hydrophobic monomer accounts for 35%-65%wt, the reactive emulsifier accounts for 5%-10%wt, and the crosslinking agent accounts for 0-5%wt; The hydrophilic monomer is a combination of one or more of itaconic acid, acrylic acid, methacrylic acid, N-vinyl pyrrolidone, and methacrylamide; The reactive emulsifier is a combination of one or more of allyl ether sulfonate, acrylamide sulfonate, and allyl alkyl succinate sulfonate; The cross-linking agent is an aziridine cross-linking agent or a polycarbodiimide cross-linking agent; The method for preparing the low swelling soap-free core-shell emulsion binder comprises the following steps: Step 1: Add water, reactive emulsifier, 5%-50%wt hydrophilic monomer, 5%-50%wt hydrophobic monomer, and pH regulator to a reaction vessel filled with condensation reflux, and adjust the pH to 3-7; Step 2: Under stirring, an inert gas is introduced by bubbling or vacuuming to exclude oxygen; Step 3: Heat the reactor to 50-90°C, add a water-soluble initiator, and react for 0.5-2h under mechanical stirring; Step 4, adding the remaining hydrophilic monomer and hydrophobic monomer dropwise for 1-4 hours, and keeping warm for 4-24 hours; Step 5, adding a cross-linking agent and keeping warm for 1-2 hours; Step 6, cooling to 30-50°C, adding a pH adjuster, and adjusting the pH to 7-9; Step eight, filtering through a filter screen to obtain a polymer emulsion binder.
2. A low swelling soap-free core-shell emulsion binder according to claim 1, characterized in that: The hydrophobic monomer is a combination of one or more of ethyl acrylate, butyl acrylate, butyl methacrylate, lauryl acrylate, octadecyl acrylate, octadecyl methacrylate, methyl acrylate, methyl methacrylate, acrylonitrile, 2-methoxyethyl acrylate, and ethoxyethoxyethyl acrylate.
3. The method for preparing the low swelling soap-free core-shell emulsion binder according to any one of claims 1 to 2, characterized in that: The following steps are involved: Step 1: Add water, reactive emulsifier, 5%-50%wt hydrophilic monomer, 5%-50%wt hydrophobic monomer, and pH regulator to a reaction vessel filled with condensation reflux, and adjust the pH to 3-7; Step 2: Under stirring, an inert gas is introduced by bubbling or vacuuming to exclude oxygen; Step 3: Heat the reactor to 50-90°C, add a water-soluble initiator, and react for 0.5-2h under mechanical stirring; Step 4, adding the remaining hydrophilic monomer and hydrophobic monomer dropwise for 1-4 hours, and keeping warm for 4-24 hours; Step 5, adding a cross-linking agent and keeping warm for 1-2 hours; Step 6, cooling to 30-50°C, adding a pH adjuster, and adjusting the pH to 7-9; Step eight, filtering through a filter screen to obtain a polymer emulsion binder.
4. The method for preparing the low swelling soap-free core-shell emulsion binder according to claim 3, characterized in that: The water-soluble initiator is a combination of one or more of sodium persulfate, potassium persulfate, ammonium persulfate, and azobisisobutylamidine hydrochloride, and the amount of the water-soluble initiator is 0.1%-2%wt based on the solid content of the low-swelling soap-free core-shell emulsion; The pH regulator is a combination of one or more of lithium hydroxide, sodium hydroxide, potassium hydroxide, ammonia water, and sodium bicarbonate.
5. A lithium ion battery negative electrode, characterized in that: The negative electrode of the lithium ion battery comprises a negative electrode substrate and a negative electrode material coated on the negative electrode substrate, wherein the negative electrode material comprises a negative electrode active material, a conductive agent and the low swelling soap-free core-shell binder according to any one of claims 1 to 2.
6. The lithium ion battery negative electrode according to claim 5, characterized in that: The negative electrode of the lithium ion battery is prepared as follows: the negative electrode active material, the conductive agent and the low swelling soap-free core-shell binder are added into water to form an electrode slurry, and the low swelling soap-free core-shell binder accounts for 1%-20%wt of the solid content of the electrode slurry; then the electrode slurry is coated on the negative electrode substrate, and dried to form the negative electrode of the lithium ion battery.
7. A lithium ion battery comprising a positive electrode, a negative electrode, a separator and an electrolyte, characterized in that: The negative electrode is a lithium ion battery negative electrode as claimed in any one of claims 5 to 6.