Glass-ceramic dielectric material, sintered body, method for manufacturing sintered body, and high-frequency circuit component
By using a layered glass-ceramic dielectric material, with an inner layer containing crystalline glass powder of specific composition and an outer layer of alumina, combined with low-temperature sintering and diopside-based crystal precipitation, the problems of dielectric loss and strength in the high-frequency region are solved, and a high-frequency circuit board material with low loss and high strength is realized.
Patent Information
- Application Number
- CN202211195023.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-09-29
- Filing Date
- 2022-09-28
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-09-28
AI Technical Summary
Existing glass-ceramic dielectric materials have insufficient dielectric loss tangent in the high-frequency region above 20GHz, resulting in large transmission losses and insufficient bending strength, making it difficult to meet the requirements of high-frequency circuit boards.
A glass-ceramic dielectric material with a layered structure is used. The inner layer contains crystalline glass powder of 50-60% SiO₂, 20-30% CaO, and 15-21% MgO, while the outer layer is formed of alumina. The diopside system is crystallized and precipitated by heat treatment at 800-1000℃. Silver or silver alloy is preferred as the inner conductor, and the sintering temperature is controlled below 1000℃.
It achieves low dielectric loss tangent and high bending strength in the high-frequency region above 20GHz, making it suitable as a high-frequency circuit substrate. It can be fired simultaneously with low-melting-point metal materials and is suitable for high-frequency circuit components with resin motherboards.
Smart Images

Figure BDA0003869276040000071
Abstract
Description
Technical Field
[0001] This invention relates to glass-ceramic dielectric materials, sintered bodies, and high-frequency circuit components that are precursors of sintered bodies having low dielectric loss tangent and high mechanical strength, which are advantageous for signal processing, in the high-frequency region above 20 GHz. Background Technology
[0002] Alumina ceramics are widely used as wiring substrates and circuit components. However, alumina ceramics have a relatively high relative permittivity of 10, which results in slower signal processing speeds. Furthermore, the use of high-melting-point tungsten in the conductor material leads to higher conductor losses.
[0003] To overcome this drawback, glass-ceramic dielectric materials composed of glass powder and ceramic powder have been developed, and the sintered body is used as the dielectric layer. For example, the sintered body of a glass-ceramic dielectric material using diopside as the main crystallized glass powder has a relative permittivity of 7.3 to 7.8 at 0.1 GHz, which is lower than that of alumina ceramic materials. Furthermore, it can be sintered at temperatures below 1000 °C, thus offering the advantage of being able to be simultaneously sintered with low-melting-point metals such as Ag and Cu, which have low conductor loss, and thus be used as inner conductors (see Patent Document 1).
[0004] Existing technical documents
[0005] Patent documents
[0006] Patent Document 1: Japanese Patent Application Publication No. 10-120436 Summary of the Invention
[0007] The problem the invention aims to solve
[0008] However, in recent years, mobile communication devices represented by 5G and local area network communication fields such as WiFi have used frequency bands of up to 20GHz and above. In such high-frequency regions, there is a strong demand for further reduction of dielectric loss tangent in ceramic dielectric materials.
[0009] The transmission loss of electromagnetic waves in a circuit is proportional to the product of the square root of the dielectric constant of the circuit substrate, the dielectric loss tangent, and the frequency of the electromagnetic wave. The glass-ceramic dielectric material disclosed in the aforementioned patent document exhibits high dielectric properties at 10.1 GHz, but its dielectric loss tangent is not sufficiently low in the high-frequency region above 20 GHz, thus resulting in increased transmission loss.
[0010] In addition, the bending strength is relatively low at about 200 MPa, which is insufficient for use as a high-frequency circuit board.
[0011] The purpose of this invention is to provide a precursor of a sintered body having low dielectric loss tangent and high bending strength in a high-frequency region above 20 GHz, namely a glass-ceramic dielectric material, a sintered body, and a high-frequency circuit component.
[0012] means for solving problems
[0013] The laminated glass-ceramic dielectric material of the present invention is characterized in that it has at least a laminated structure formed by stacking an outer layer, an inner layer, and another outer layer in that order, wherein the outer layers are formed of alumina with a thickness of 0.1 to 5 μm, and the inner layers contain crystalline glass powder of 50 to 60% SiO2, 20 to 30% CaO, and 15 to 21% MgO by mass as a glass composition.
[0014] It should be noted that, in this invention, "crystalline glass powder" refers to amorphous glass powder that has the property of precipitating crystals from a glass matrix upon heat treatment. "Heat treatment" refers to heat treatment at 800–1000°C for 10 minutes or more.
[0015] The inner layer of the laminated glass-ceramic dielectric material of the present invention is preferably a green sheet laminate or a printed laminate.
[0016] The laminated glass-ceramic dielectric material of the present invention preferably has an inner layer that is substantially free of ceramic powder. "Substantially free of ceramic powder" means that the content of ceramic powder in the inner layer is less than 0.1% by mass.
[0017] The laminated glass-ceramic dielectric material of the present invention preferably contains a metal conductor in the inner layer.
[0018] The preferred metal conductor in the laminated glass-ceramic dielectric material of the present invention is silver or a silver alloy.
[0019] The sintered body of the present invention is a sintered body formed by sintering the above-mentioned layered glass-ceramic dielectric material, preferably with diopside-based crystals as the main crystals precipitated from the inner glass matrix. It should be noted that "diopside-based crystals" refers to diopside crystals (CaMg(Si2O6)) and diopside solid solution crystals.
[0020] The sintered body of the present invention is characterized in that it has at least a stacked structure formed in the order of outer layer, inner layer, and outer layer, wherein the outer layer is formed of alumina with a thickness of 0.1 to 5 μm, and the inner layer contains 50 to 60% SiO2, 20 to 30% CaO, and 15 to 21% MgO by mass, and diopside crystals are precipitated.
[0021] The sintered body of the present invention preferably has a three-point bending strength of 250 MPa or higher. It should be noted that "three-point bending strength" refers to the value evaluated based on JIS R1601.
[0022] The sintered body of the present invention preferably has a dielectric loss tangent of 0.0009 or less at a measured temperature of 25°C and 28 GHz.
[0023] The sintered body of the present invention preferably has a relative permittivity of 8.0 or less at a measurement temperature of 25°C and 28 GHz.
[0024] It should be noted that "dielectric loss tangent" and "relative permittivity" refer to the values measured at a temperature of 25°C and a frequency of 28GHz, according to the method for measuring the microwave dielectric properties of fine ceramic substrates (JIS R1641).
[0025] The sintered body of the present invention preferably has a coefficient of thermal expansion of 8 to 10 ppm / ℃. It should be noted that the "coefficient of thermal expansion" refers to the value measured using a thermomechanical analysis device within a temperature range of 30 to 380℃.
[0026] The preferred method for manufacturing the sintered body of the present invention is to sinter the above-mentioned laminated glass-ceramic dielectric material.
[0027] The method for manufacturing the sintered body of the present invention preferably involves firing at a temperature below 1000°C.
[0028] The high-frequency circuit component of the present invention is a high-frequency circuit component having a dielectric layer, wherein the dielectric layer is preferably the sintered body described above.
[0029] Invention Effects
[0030] The laminated glass-ceramic dielectric material of the present invention can be sintered at low temperatures below 1000°C, allowing the use of low-melting-point metals such as silver, silver alloys, or copper as the inner conductor. Furthermore, it exhibits a low dielectric loss tangent in the high-frequency region above 20 GHz and a relatively high flexural strength of 250 MPa or more. Therefore, the glass-ceramic dielectric material of the present invention is suitable as a high-frequency circuit component mounted on a resin-based motherboard. Detailed Implementation
[0031] The laminated glass-ceramic dielectric material of the present invention is a laminate formed by stacking an outer layer, an inner layer, and another outer layer in that order. The inner layer contains crystalline glass powder and the outer layer is formed of alumina.
[0032] First, let's explain the inner layer.
[0033] The glass powder constituting the inner layer preferably contains, by mass%, 50-60% SiO2, 20-30% CaO, and 15-21% MgO. The reasons for limiting the content range of each component as described above are explained below. It should be noted that in the description of the content range of each component, the percentage refers to mass%.
[0034] SiO2 is a constituent component of diopside-based crystals and is a network formation component that contributes to glass formation. The SiO2 content is 50-60%, preferably 53-57%, and particularly 54-56%. If the SiO2 content is too low, vitrification becomes difficult. On the other hand, if the SiO2 content is too high, the melting temperature tends to be higher, and diopside-based crystals are difficult to precipitate.
[0035] CaO is a constituent component of diopside-based crystals and lowers the softening point of crystalline glass powder. The CaO content is 20-30%, preferably 23-29%, and particularly 25-27%. If the CaO content is too low, the softening point becomes too high. Furthermore, crystallinity decreases, and the dielectric loss tangent tends to increase. On the other hand, if the CaO content is too high, vitrification becomes difficult. Additionally, the dielectric loss tangent tends to increase.
[0036] MgO is a constituent component of diopside-based crystals and lowers the softening point of crystalline glass powder. The MgO content is 15–21%, particularly preferably 17–20%. If the MgO content is too low, the softening point becomes too high. Furthermore, the dielectric loss tangent tends to increase. On the other hand, if the MgO content is too high, vitrification becomes difficult. Additionally, crystallinity decreases, and the dielectric loss tangent tends to increase.
[0037] In addition to the above-mentioned components, Al2O3, B2O3, ZnO, etc. can be added up to 3% each, within a range that does not impair dielectric properties.
[0038] It should be noted that alkali metal oxides (Li₂O, Na₂O, K₂O) are components that lower the sintering temperature and increase the dielectric loss tangent. Therefore, the content of Li₂O + Na₂O + K₂O is less than 2%, preferably less than 1%, less than 0.5%, and particularly less than 0.1%. Specifically, the content of Li₂O is preferably less than 0.5%, and particularly less than 0.1%. The content of Na₂O is preferably less than 0.5%, and particularly less than 0.1%. The content of K₂O is preferably less than 0.5%, and particularly less than 0.1%. Here, "Li₂O + Na₂O + K₂O" refers to the combined amount of Li₂O, Na₂O, and K₂O.
[0039] The inner layer is preferably a raw sheet laminate or a printed laminate.
[0040] If the inner layer contains ceramic powder, it can improve the dielectric properties and / or strength, potentially hindering the densification of the sintered body. Therefore, the inner layer of the present invention preferably does not contain ceramic powder.
[0041] The laminated glass-ceramic dielectric material of the present invention can be fired at temperatures below 1000°C, thus enabling the introduction of a low-melting-point metal conductor into the inner layer. Silver or a silver alloy, which exhibits low conductor loss, is preferably used as the aforementioned metal conductor.
[0042] Furthermore, it is preferable that, if firing is performed, diopside-based crystals precipitate out as the main crystals from the crystalline glass powder contained in the inner layer. By precipitating diopside-based crystals in the inner layer, it is easier to reduce the relative permittivity and dielectric loss tangent.
[0043] The thickness of the inner layer is preferably 0.1 to 3.0 mm.
[0044] Next, the outer layer will be explained.
[0045] The outer layer is formed of alumina. Alumina has high strength and a coefficient of thermal expansion of 7 to 7.7 ppm / °C, which is close to that of the highly expandable inner layer. Therefore, it is suitable for improving the mechanical strength of the glass-ceramic dielectric material of the present invention.
[0046] Furthermore, the outer layer is preferably formed on the surface of the inner layer with a thickness of 0.1–5 μm, particularly 0.3–4 μm. If the outer layer is too thin, the mechanical strength is easily reduced. On the other hand, if the outer layer is too thick, the outer layer may peel off.
[0047] Next, the characteristics of the sintered body of the present invention will be described.
[0048] In the sintered body of the present invention, the three-point bending strength is preferably 250 MPa or higher, particularly 260 MPa or higher. If the three-point bending strength is too low, cracking and other defects are likely to occur in the sintered body. It should be noted that the lower limit of the three-point bending strength is not particularly limited, but in practice it is 100 MPa or higher.
[0049] In the sintered body of the present invention, the dielectric loss tangent is preferably below 0.0009, and particularly below 0.0008, at 25°C and 28GHz. If the dielectric loss tangent is too high, the loss of transmitted signal is likely to increase. It should be noted that the lower limit of the dielectric loss tangent is not particularly limited, but in practice it is above 0.0001.
[0050] In the sintered body of the present invention, the relative permittivity at 25°C and 28GHz is preferably 8.0 or less, particularly 7.5 or less. If the relative permittivity is too high, the signal processing speed is likely to slow down. It should be noted that the lower limit of the relative permittivity is not particularly limited, and in practice it is 5.0 or more.
[0051] In the sintered body of the present invention, the coefficient of thermal expansion is preferably 8 to 10 ppm / ℃, particularly 8.5 to 9 ppm / ℃. If the coefficient of thermal expansion of the sintered body is too low, strain is easily generated due to the difference in thermal expansion when thermal cycling is applied after brazing to the resin motherboard. On the other hand, if the coefficient of thermal expansion is too high, the thermal shock resistance is reduced. It should be noted that the "coefficient of thermal expansion" is a value measured using a thermomechanical analysis device within a temperature range of 30 to 380℃.
[0052] Furthermore, the method for manufacturing the sintered body of the present invention is described below.
[0053] First, a slurry is prepared by adding a specified amount of binder, plasticizer, and solvent to the aforementioned crystalline glass powder. Suitable binders include, for example, polyvinyl butyral resin and methacrylic acid resin; suitable plasticizers include, for example, dibutyl phthalate; and suitable solvents include, for example, toluene and methyl ethyl ketone.
[0054] Next, the slurry of the aforementioned crystalline glass powder is formed into a green sheet using a doctor blade method, dried, cut to a specified size, and then machined to form through holes. For example, a silver conductor or a low-resistance metal material serving as an electrode is printed onto the through holes and the surface of the green sheet. Then, multiple such green sheets are stacked to obtain a laminated green sheet.
[0055] The above-mentioned laminated green sheets can be further coated with alumina paste to form a uniform alumina layer, followed by firing to obtain a sintered body. It should be noted that the alumina layer can be formed by firing the laminated green sheets, printing alumina paste onto the surface, and firing again. Furthermore, the thickness of the alumina layer can be varied by adjusting the viscosity of the paste.
[0056] The sintered body produced in this way can also have conductors and electrodes inside and on the surface. It should be noted that, from the point of view of using low-melting-point metal materials such as silver and copper with low conductor loss, it is desirable to have a firing temperature below 1000℃, especially 800 to 950℃.
[0057] The high-frequency circuit component of the present invention can be fabricated by forming a coil with wiring, or by attaching a chip of Si-based or GaAs-based semiconductor elements to the surface of a sintered body fabricated in the manner described above.
[0058] Example
[0059] The present invention will now be described based on embodiments, but the present invention is not limited to these embodiments.
[0060] Table 1 shows the embodiments (samples No. 1 to 4) and comparative examples (samples No. 5 and 6) of the present invention.
[0061] Table 1
[0062]
[0063] Each sample was prepared as follows. First, glass raw materials containing various oxides were prepared according to the glass composition shown in the table. After uniform mixing, the mixture was placed in a platinum crucible and melted at 1500–1580°C for 3 hours. The molten glass was then formed into a thin sheet using a water-cooled roller. Next, the obtained glass film was coarsely pulverized, then alcohol was added, and the mixture was wet-milled using a ball mill. The powder was obtained by classifying the powder according to an average particle size of 1.5–3 μm.
[0064] Next, a slurry was prepared by adding 15% by mass of polyvinyl butyral as a binder, 4% by mass of butyl benzyl phthalate as a plasticizer, and 30% by mass of toluene as a solvent to the glass powder. The slurry was then formed into 150 μm green sheets using a doctor blade method, dried, cut to a specified size, and four green sheets were stacked and integrally bonded by hot pressing. Further, the stacked green sheets, coated with an alumina slurry to form a uniform alumina layer on the surface, were fired at 900°C for 1 hour to obtain a glass-ceramic product.
[0065] For each sample thus obtained, the firing temperature, whether silver can be fired simultaneously, precipitation crystallization, three-point bending strength, dielectric loss tangent, relative permittivity, and coefficient of thermal expansion were evaluated. The results are shown in Table 1.
[0066] The firing temperature describes the lowest temperature at which ink is applied to sintered bodies fired at various temperatures and then wiped off without leaving any ink residue (i.e., dense sintering has been achieved).
[0067] Regarding whether silver can be fired simultaneously, silver conductors are printed onto the raw film before firing and fired simultaneously. The silver wiring is then visually inspected to see if it has changed color or broken.
[0068] The precipitated crystals were identified using a powder X-ray diffraction apparatus (RIGABYTE RINT2100).
[0069] Three-point bending strength is evaluated according to JIS R1601.
[0070] The dielectric loss tangent and relative permittivity were determined by sintering the green sheet material at the firing temperature shown in the table, processing it into a size of 25 mm × 50 mm × 0.1 mm, and using it as a test sample. The determination was based on the microwave dielectric properties of fine ceramic substrates (JIS R1641) at a test temperature of 25 °C and a frequency of 28 GHz.
[0071] The coefficient of thermal expansion is determined using a thermomechanical analysis device within a temperature range of 30–380℃.
[0072] As can be clearly seen from Table 1, samples No. 1 to 4, used as examples, exhibit high three-point bending strengths of 260 to 270 MPa due to the alumina layer thickness of 0.5 to 3 μm. Furthermore, they have small dielectric loss tangents of 0.0003 to 0.0007. On the other hand, sample No. 5, with a low SiO2 content of 49% and a high MgO content of 26%, was not vitrified. Sample No. 6, lacking an alumina layer on the glass surface, exhibits a bending strength as low as 190 MPa.
Claims
1. A laminated glass-ceramic dielectric material, characterized in that, It has at least a stacked structure formed in the order of outer layer, inner layer, and outer layer, wherein the outer layer is formed of alumina with a thickness of 0.1 μm to 5 μm, and the inner layer contains crystalline glass powder containing, by mass, 50% to 60% SiO2, 20% to 30% CaO, and 15% to 21% MgO as glass.
2. The laminated glass-ceramic dielectric material of claim 1, wherein, The inner layer is a raw sheet laminate or a printed laminate.
3. The laminated glass-ceramic dielectric material of claim 1, wherein, The inner layer does not actually contain ceramic powder.
4. The laminated glass-ceramic dielectric material according to any one of claims 1 to 3, characterized in that, The inner layer contains a metallic conductor.
5. The laminated glass-ceramic dielectric material of claim 4, wherein, The metallic conductor is silver or a silver alloy.
6. A sintered body, characterized by, It is a sintered body formed by sintering the laminated glass-ceramic dielectric material according to any one of claims 1 to 5, wherein diopside crystals precipitate from the inner glass matrix as the main crystals.
7. A laminated glass-ceramic sintered body, characterized by, It has at least a stacked structure formed by stacking an outer layer, an inner layer, and another outer layer in that order, wherein the outer layer is formed of alumina with a thickness of 0.1 μm to 5 μm, and the inner layer contains, by mass % 50% to 60% SiO2, 20% to 30% CaO, and 15% to 21% MgO, and contains diopside crystals.
8. The sintered body according to claim 6 or 7, characterized in that, The three-point bending strength is above 250 MPa.
9. The sintered body according to claim 6 or 7, characterized in that, The dielectric loss tangent at a temperature of 25℃ and a frequency of 28GHz was measured to be below 0.0009.
10. The sintered body according to claim 6 or 7, characterized in that, The relative permittivity was measured to be below 8.0 at a temperature of 25℃ and a frequency of 28GHz.
11. The sintered body according to claim 6 or 7, characterized in that, The coefficient of thermal expansion of the inner layer is 8ppm / ℃ to 10ppm / ℃.
12. A method for manufacturing a sintered body, characterized in that, The laminated glass-ceramic dielectric material according to any one of claims 1 to 5 is sintered.
13. The method for manufacturing a sintered body according to claim 12, characterized in that, Firing is carried out at a temperature below 1000℃.
14. A high-frequency circuit component, characterized in that, It is a high-frequency circuit component having a dielectric layer, wherein the dielectric layer is a sintered body as described in any one of claims 6 to 11.
Citation Information
Patent Citations
Glass ceramic dielectric material
JP1998120436A
Crystalline glass powder
CN103221355A
Glass ceramic dielectric body
CN111801308A