Functional vertical wood board and preparation method thereof

By incorporating a mixture of filler units and adhesive into the vertical timber panels, and combining microwave heating and hot pressing, the problem of delamination of the vertical timber panels under environmental changes was solved, thereby improving the bonding strength and agent utilization efficiency.

CN115949870BActive Publication Date: 2026-11-24NANJING FORESTRY UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202211557758.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-06
Publication Date
2026-11-24
Estimated Expiration
2042-12-06

AI Technical Summary

Technical Problem

Existing vertical timber boards are prone to dimensional changes and delamination when the ambient temperature and humidity change. Furthermore, the bonding strength is insufficient when using other shaped timber segments, and the impregnation treatment consumes a lot of chemicals and time.

Method used

Vertical wood panels impregnated with functional agents are formed by placing a mixture of filler material and adhesive between the wood segments and the filler units to create densely pressed filler units. Combined with microwave heating and hot pressing, the impregnation depth and loss rate of the agents are optimized.

Benefits of technology

It improves bonding strength, reduces the amount of chemicals used and soaking time, prevents degumming, and can adapt to changes in the size of wood segments when the environment changes, thus slowing down the rate of chemical loss.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115949870B_ABST
    Figure CN115949870B_ABST
Patent Text Reader

Abstract

This application discloses a functional composite board and its preparation method, including a vertical wood board. At least one surface layer of the vertical wood board is a functional impregnation layer formed by impregnation with a functional agent. The vertical wood board includes a main unit and a filling unit. The main unit includes multiple arrayed wood segments and / or partial wood segments, the longitudinal direction of which is at an angle to the surface of the composite board. The filling unit is a mixture of filler and adhesive, which, after being compacted, fills the gaps between adjacent wood segments and / or partial wood segments and bonds them together. The filling unit can, to a certain extent, mitigate the morphological change caused by the expansion of the wood segment ends after absorbing the agent, resulting in a larger diameter at both ends than in the middle, and avoids the problem of uneven morphological changes in the longitudinal direction of the wood segments due to moisture absorption during impregnation and drying after impregnation, thus preventing delamination.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of engineered wood products technology, specifically to a functional vertical wood product prepared by impregnating vertical wood products whose main unit is wood segment with a functional agent; this invention also relates to a method for preparing such a functional vertical wood product. Background Technology

[0002] Vertical wood panels are composite boards made by gluing together wood segments with cross-sectional shapes such as rectangles, squares, pentagons, hexagons, and octagons. These segments are typically rotary-cut wood cores or rod-shaped timber processed from small-diameter lumber. The cross-section of the wood is the front surface. Because the cross-section perpendicular to the fiber direction forms the usable surface of vertical wood panels, it has more impregnation channels, allowing for higher impregnation efficiency and greater impregnation depth during the impregnation process.

[0003] The Chinese patent database discloses relevant technical solutions for products and preparation methods of vertical wood panels. For example, the invention patent with publication number CN104210013B, entitled "A Method for Manufacturing Large-Section Hexagonal Prism Laminated Wood", describes a technical solution for producing large-section hexagonal prism laminated wood by applying glue to three sides of hexagonal prism and isosceles trapezoidal wood segments, assembling a hexagonal prism mold, and applying pressure in three directions to glue them together. The resulting laminated wood can be sawn into vertical wood panels for further utilization. However, the vertical wood panels prepared by the above technical solutions (1) have width and length directions that are radial to the wood segments, so the panels undergo relatively large dimensional changes due to changes in ambient temperature and humidity, which easily leads to delamination between adjacent wood segments; (2) the shape of the wood segments used is limited to rectangular prisms, square prisms, and hexagonal prisms due to process limitations. If other polyhedral prisms are used, large pores will be left between the glued surfaces of adjacent wood segments, increasing the amount of glue applied and affecting the bonding strength; (3) the dimensional change rate of rotary-cut wood cores or small-diameter timber is relatively large, and adjacent wood segments are tightly bonded. Therefore, if the surface thickness of the vertical wood panel (one end of the wood segment) is impregnated with the agent and undergoes large dimensional expansion, while the unimpregnated part retains its original size, delamination of the wood segments is more likely to occur. Conversely, if overall impregnation is chosen, a very large amount of agent and impregnation time are required. Summary of the Invention

[0004] The purpose of this invention is to overcome the above-mentioned technical problems and thus provide a functional composite board and its preparation method.

[0005] To achieve the above objectives, one embodiment of the present invention provides a functional vertical wood panel, comprising a vertical wood panel, wherein at least one surface layer of the vertical wood panel is a functional impregnation layer formed by impregnation with a functional agent; the vertical wood panel includes a main unit and a filling unit, wherein the main unit includes a plurality of arrayed wood segments and / or partial wood segments, the longitudinal direction of the wood segments being at an angle to the surface of the composite panel; the filling unit is a mixture of filler and adhesive, which, after being compacted and pressed, fills the gaps between adjacent wood segments and / or partial wood segments and bonds the wood segments and / or partial wood segments together.

[0006] Preferably, the functional impregnation layer includes a main unit impregnation layer and a filler unit impregnation layer, which are formed by the functional agent impregnating and penetrating the main unit and the filler unit respectively. The thickness of the main unit impregnation layer is 1.5 to 3.0 times that of the filler unit impregnation layer.

[0007] Preferably, the functional agent is one or a mixture of flame retardants and antifungal agents.

[0008] Preferably, the longitudinal direction of the wood segment and / or part of the wood segment forms an angle of 50° to 90° with the surface of the vertical wood board.

[0009] Preferably, the wood segment is in the form of a cylinder, prism, cube, or elliptical cylinder; or

[0010] The wood segments are partially cylindrical, partially prismatic, partially cubic, or partially elliptical.

[0011] Preferably, the filler material is one or a mixture of several particles, chips, or fibers.

[0012] To achieve the above objectives, one embodiment of the present invention provides a method for preparing the above-mentioned functional vertical wood panel, comprising the following steps:

[0013] The impregnation process involves impregnating the composite board with the functional pharmaceutical agent under normal pressure to obtain an intermediate product;

[0014] In the process of sealing the surface, the intermediate product is placed in a thermo-pressure environment to compress at least one surface layer of the intermediate product.

[0015] Preferably, the impregnation process is carried out at room temperature.

[0016] Preferably, before the impregnation process, the composite board is preheated in a microwave environment at a temperature of 50-60°C for 50-70 seconds.

[0017] Preferably, the surface sealing process involves heating at least one surface layer of the intermediate product with a hot plate at a temperature of 140–150°C for a preheating time of 10–30 seconds; subsequently, pressure of 2.5–2.7 MPa is applied to the surface layer for a pressing time of 70–90 seconds.

[0018] In summary, compared with the prior art, the beneficial effects of the present invention are:

[0019] 1. The filler material in the filler unit has a certain elasticity after being compacted and bonded by the adhesive film. Furthermore, the dimensional changes (elastic changes) between different parts of the filler unit are not correlated or interconnected. This can, to a certain extent, absorb the expansion of the wood segment ends after absorbing the agent, resulting in a larger diameter at both ends than in the middle section. This avoids the problem of uneven morphological changes in the longitudinal direction of the wood segment during impregnation and drying after impregnation, which can lead to degumming.

[0020] 2. By causing the fibers of the thick layer impregnated with functional agents to undergo morphological changes such as twisting and folding, the vertical pathways of the wood segments and parts of the wood segments are also twisted and folded, thereby partially blocking the pathways for agent leakage and achieving the technical effect of slowing down the rate of agent leakage. Attached Figure Description

[0021] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0022] Figure 1 This is a structural schematic diagram of the functional vertical wood panel of Embodiment 1 of this application.

[0023] Figure 2 This is a schematic diagram of a method for preparing the vertical wood board according to Embodiment 1 of this application.

[0024] Figure 3 This is a schematic diagram of another method for preparing the vertical wood board of Embodiment 1 of this application.

[0025] Figure 4 This is a schematic diagram of the structure of the main unit impregnation layer and the filling unit impregnation layer in Embodiment 1 of this application.

[0026] Figure 5 This is a structural schematic diagram of the functional vertical wood panel of Embodiment 2 of this application.

[0027] Figure 6 This is a structural schematic diagram of the functional vertical wood panel of Embodiment 9 of this application.

[0028] In the diagram: 100, vertical wood panel; 200, particleboard; 900, functional impregnation layer; 101, wood segment; 102, partial wood segment; 103, filling unit; 104, assembly hole; 105, first veneer; 106, second veneer; 901, main unit impregnation layer; 902, filling unit impregnation layer. Detailed Implementation

[0029] To enable those skilled in the art to better understand the technical solutions in this application, the technical solutions in the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort should fall within the scope of protection of this application.

[0030] Example 1

[0031] Reference Figure 1 The illustration shows a functional vertical wood panel, comprising a vertical wood panel 100, with two surface layers 900 formed by impregnation with a functional agent. The vertical wood panel 100 includes a main unit and a filling unit 103. The main unit comprises multiple arrayed wood segments 101 and partial wood segments 102, with the longitudinal direction L0 of the wood segments 101 and partial wood segments 102 parallel and at an angle to the surface of the vertical wood panel 100. The longitudinal direction of the wood segments 101 or partial wood segments 102 refers to the longitudinal direction of the wood, i.e., the height direction formed during the tree's growth. The filling unit 103 is a composite pressed material, a mixture of filler and adhesive, compacted and filled into the gaps between adjacent wood segments 101 and partial wood segments 102, bonding the wood segments 101, partial wood segments 102, and wood segments 101 and partial wood segments 102 together.

[0032] With the above structure, and by providing the filler unit 103, which is a mixture of filler material and adhesive, the required bonding strength can be achieved with only an acceptable amount of adhesive, regardless of the cross-sectional shape of the wood segment 101. This is because the filler unit 103 fills the gaps between wood segments 101, between some wood segments 102, and between wood segments 101 and some wood segments 102. Furthermore, the filler unit 103, formed by compacting the mixture, can be considered a single unit, effectively bonding the wood segments 101 and / or some wood segments 102. This significantly reduces the amount of adhesive used to bond the wood segments 101 and / or some wood segments 102 while ensuring bonding strength.

[0033] Furthermore, the filling material in the filling unit 103, after being compacted and bonded by the adhesive film, possesses a certain degree of elasticity. Although the filling unit 103 can be considered a single unit after pressing and gluing, the dimensional changes between different parts of the filling unit 103 are not correlated or interconnected. This allows it to absorb, to some extent, the expansion and contraction changes along any length of the wood segment 101. After the vertical wood board 100 is soaked in the functional agent, the material on both the surface layers of the vertical wood board 100 absorbs the agent. The filling unit 103 in the surface layer experiences a relatively small amount of impregnation due to the adhesive, while the wood segment 101 or part of the wood segment 102 experiences a relatively large amount of impregnation, resulting in relatively large dimensional expansion at both ends of the wood segment 101 or part of the wood segment 102. At this time, the filling unit 103 can undergo different dimensional changes due to compression at different locations along with the shape changes of the wood segment 101 or part of the wood segment 102. This effectively absorbs the dimensional changes of the wood segment 101 and part of the wood segment 102 after impregnation with the agent, avoiding the problem of delamination. During the drying process after impregnation, the filling unit 103 can undergo a certain degree of dimensional expansion to accommodate the shrinkage of the wood segment 101. Of course, the dimensional expansion of the filling unit 103 under drying conditions is a compression rebound that occurs after the pressure is removed or reduced, rather than a dimensional change caused by wet expansion and dry contraction.

[0034] Specifically, in this embodiment, the wood segment 101 is a short segment of a pentagonal prism, and the partial wood segment 102 is formed by cutting a short segment of a pentagonal prism with the same shape and specifications as the wood segment 101 parallel to the fiber direction. This is done to remove a portion of the complete wood segment so that the specifications of the vertical wood board 100 meet the design requirements. Of course, the wood segment 101 can also be other prisms, such as a cube, hexagonal prism, or octagonal prism, and the partial wood segment 102 is correspondingly a partial cube, a partial hexagonal prism, or a partial octagonal prism. At the same time, those skilled in the art should know that the cutting is to obtain the vertical wood board 100 that meets the specifications required for production; therefore, it is also possible that the obtained vertical wood board 100 consists entirely of wood segments 101 or entirely of partial wood segments 102.

[0035] The longitudinal direction of wood segments 101 and some wood segments 102 is perpendicular to the surface of the vertical wood board 100. In other words, the longitudinal direction of wood segments 101 and some wood segments 102 constitutes the thickness of the vertical wood board 100. Multiple wood segments 101 are placed vertically in a rectangular array. In this embodiment, gaps are even intentionally reserved between adjacent wood segments 101. Filling units 103 bond adjacent wood segments 101 and fill the gaps between adjacent wood segments 101 to obtain the blank of the vertical wood board 100. The vertical wood board 100 with the required specifications and dimensions is obtained by cutting. During the cutting process, some wood segments 101 become some wood segments 102. The intentionally reserved gaps provide space for the expansion and contraction and shape changes of the wood segments 101. The filling units 103 filled in the gaps form a flat surface of the vertical wood board 100 and provide elastic constraints for the changes of the wood segments 101.

[0036] The filler material in filler unit 103 is one or a mixture of granules, chips, or fibers. The selection of the filler material is mainly based on the type of wood segment 101. When the wood segment 101 is rod-shaped wood processed from small-diameter timber, a material with relatively high elasticity or compression recovery should be selected, such as wood shavings. When the wood segment 101 is rotary-cut wood core material, a material with relatively low elasticity or compression recovery can be selected, such as wood-plastic composite particles. Alternatively, two or three filler materials can be selected and mixed according to the characteristics of the tree species. In this embodiment, the selected filler material is wood chips, specifically C-type wood shavings, with a size of (0.8~1.2)cm × (5~7)cm × (0.01~0.03) (width × length × thickness).

[0037] The vertical timber board 100 of this application is prepared by the following process.

[0038] First, select a specific particleboard 200. The specific particleboard 200 refers to a particleboard that uses C-type wood shavings and whose shavings are (0.8~1.2)cm×(5~7)cm×(0.01~0.03)cm (width×length×thickness). The particleboard 200 has dimensions of 122cm×244cm×2cm (width×length×thickness).

[0039] Subsequently, referring to Figure 2 As shown, long log segments are produced. Small-diameter timber is processed into long, pentahedral log segments using a rod-shaped processing device. The cross-sectional shape of each long log segment is a regular pentagon inscribed in a circle with a radius of 5 cm. These long log segments are then sawn into log segments 101 with a length of 2 cm. Simultaneously, the substrate for the vertical wood panel is produced. Multiple arrays of assembly holes 104 are made along the width and length of the particleboard 200 using methods such as punching, wire cutting, and drilling. The assembly holes 104 are through holes, allowing the log segments 101 to be inserted into them, forming a clearance fit of 0.05–0.08 mm.

[0040] Next, adhesive is applied to the five vertical surfaces of the wood segment 101 and then inserted into the assembly hole 104. The adhesive used is a mixture of white glue and hot melt adhesive powder, with a mass ratio of white glue to hot melt adhesive powder of 1:1. The mixed adhesive fills the gap between the wood segment 101 and the assembly hole 104 while bonding them together. The hot melt adhesive powder in the mixed adhesive melts and flows during the heat curing process, achieving the purpose of uniformly filling the gap. After cooling, it forms an adhesive layer with a certain degree of toughness. Thus, the adhesive layer formed by the mixed adhesive can buffer the impact of the expansion and contraction of the wood segment 101 on the base plate of the vertical wood board during use, making the structure of the vertical wood board 100 more stable. The remaining part of the particleboard 200 after the hole is made, together with the adhesive layer of the mixed adhesive, forms the filling unit 103 of this embodiment.

[0041] Next, the particleboard with the inserted wood segments 101 is placed in a hot press and the mixed adhesive is heat-cured at a hot pressing temperature of 155-165℃ (e.g., 160±2℃) to obtain the blank material of the vertical wood board.

[0042] Finally, the rough blanks of the vertical timber are sawn into vertical timber boards 100 that meet the required dimensions and specifications.

[0043] Of course, 100mm vertical wood panels can also be prepared through other methods, see reference... Figure 3 For example, by first pressing a square piece of wood 120 and then cutting it to obtain a vertical wood board 100.

[0044] First, take a long pentahedral log segment 110 and lay it side-by-side on a continuous conveyor with baffles on both sides to form a long log segment layer. Spread a mixture to fill the gaps between the long log segments 110. Repeat the above steps to obtain a square blank. The distance from the surface of the natural mixture layer formed by spreading the mixture to each long log segment layer to the surface of that long log segment layer is 10% of the thickness of the long log segment layer. The distance from the surface of the natural mixture layer formed by spreading the mixture to the surface of the last long log segment layer to the surface of the last long log segment layer is 30% of the thickness of the long log segment layer.

[0045] Subsequently, the square blank is pre-pressed through multiple sets of pressure rollers. The pressure rollers are at room temperature and the pressure is 0.9–1.0 MPa. The multiple sets of pressure rollers can provide continuous pressure to the first intermediate product for 0.5 minutes. The pre-pressing process can promote the uniform distribution of the mixture in the gaps between adjacent long timber segments 110.

[0046] Next, under conditions of confinement on both sides, pressure is applied to both sides of the first intermediate product to obtain square material 120. This pressure is provided by multiple sets of heated rollers, the temperature of which is 125±2℃ and the pressure is 2.2~2.3MPa. The multiple sets of heated rollers can provide continuous pressure to the first intermediate product for 10 minutes. Under this pressure, the mixture is compressed to form filling unit 103.

[0047] Next, the square piece 120 is sawn in a cutting direction perpendicular to the longitudinal direction of the long timber segment 110 to obtain the vertical timber board 100.

[0048] Finally, the vertical wood boards are dried to a moisture content of 12-14%, with an internal moisture content deviation of less than 2%.

[0049] The resulting vertical wood board 100 is then impregnated with a functional agent to obtain the functional vertical wood board of this embodiment. The impregnation treatment involves completely immersing the vertical wood board 100 in a chemical bath under normal pressure for 45 minutes. The functional agent is a prior art antifungal agent. After removing the vertical wood board 100 from the chemical bath, it is dried in a kiln to a moisture content of 12-14%.

[0050] Reference Figure 4 As shown, due to the different hygroscopic properties of the main unit and the filling unit, the functional impregnation layer 900 of the functional vertical wood board obtained after impregnation includes a main unit impregnation layer 901 and a filling unit impregnation layer 902, which are formed by the functional agent impregnating and penetrating into the main unit and the filling unit respectively. In this embodiment, the thickness of the main unit impregnation layer 901 is 1.5-1.7 mm, and the thickness of the filling unit impregnation layer 902 is 0.5-0.6 mm; after drying to 12-14%, the thickness of the main unit impregnation layer 901 is 1.1-1.3 mm, and the thickness of the filling unit impregnation layer 902 is 0.6-0.7 mm.

[0051] Example 2

[0052] The difference between Example 2 and Example 1 is that, referring to... Figure 5 As shown, the long wood segment 110 is a rotary-cut core of hardwood (oak) and is cylindrical in shape. After impregnation, the thickness of the main unit impregnation layer 901 is 1.1–1.2 mm, and the thickness of the filler unit impregnation layer 902 is 0.5–0.6 mm; after drying to 12–14%, the thickness of the main unit impregnation layer 901 is 1.0–1.1 mm, and the thickness of the filler unit impregnation layer 902 is 0.5 mm.

[0053] Example 3

[0054] The difference between Example 3 and Example 1 is that the long wood segment 110 is a rotary-cut core of hardwood (oak) in cylindrical shape; the filler material is wood fiber with a fiber length of 2-3 mm. After impregnation, the thickness of the main unit impregnation layer 901 is 1.1-1.2 mm, and the thickness of the filler unit impregnation layer 902 is 0.6-0.7 mm; after drying to 12-14%, the thickness of the main unit impregnation layer 901 is 1.0-1.1 mm, and the thickness of the filler unit impregnation layer 902 is 0.6 mm.

[0055] Example 4

[0056] The difference between Example 4 and Example 3 is that, before the impregnation process, the vertical wood panel 100 is passed through a microwave heating tunnel to preheat it in a microwave environment. The temperature of the microwave environment formed by the microwave heating tunnel is 58±2℃, and the preheating time is 65s. In other words, after the vertical wood panel 100 leaves the microwave heating tunnel, the temperature of the main unit is 56~57℃, and the temperature of the filling unit is 53~54℃.

[0057] After being impregnated at room temperature in Example 1, the thickness of the main unit impregnation layer 901 is 1.2–1.3 mm, and the thickness of the filler unit impregnation layer 902 is 0.6–0.7 mm; after drying to 12–14%, the thickness of the main unit impregnation layer 901 is 1.0–1.1 mm, and the thickness of the filler unit impregnation layer 902 is 0.6–0.7 mm.

[0058] Example 5

[0059] The difference between Example 5 and Example 4 is that, in the subsequent impregnation process, the functional agent in the agent tank is a fire-retardant agent of the prior art, but the agent temperature is maintained at 60±2℃, and the impregnation time is 25 minutes. After impregnation, the thickness of the impregnation layer 901 of the main unit is 1.5-1.6 mm, and the thickness of the impregnation layer 902 of the filler unit is 0.7-0.8 mm; after drying to 12-14%, the thickness of the impregnation layer 901 of the main unit is 1.3 mm, and the thickness of the impregnation layer 902 of the filler unit is 0.6-0.7 mm.

[0060] Example 6

[0061] The difference between Example 6 and Example 5 lies in the process of sealing the intermediate product after impregnation. This sealing process involves placing the intermediate product under a thermo-pressure environment to compress the impregnated surface layer. In this example, both surfaces of the intermediate product are compressed, so the sealing process needs to be performed simultaneously or sequentially on both surfaces. Specifically, firstly, the upper and lower pressure plates of the hot press are heated to 147±2℃, and the distance between the upper and lower pressure plates is controlled within 25mm. Then, the intermediate product is placed on the lower pressure plate, and the upper pressure plate is quickly closed. After preheating without pressure for 20 seconds, the upper pressure plate is pressurized until the gauge pressure reaches 2.7MPa, with a compression of 8%. This pressure is maintained for 85 seconds after reaching the compression target. After the pressure holding time is reached, the pressure is released, and the upper and lower pressure plates are allowed to cool to room temperature before being opened. Finally, the functional vertical wood board of this example with a moisture content of 12-14% is obtained through kiln drying.

[0062] In this embodiment, the surface-sealing process achieves the advantages of (1) utilizing the longitudinal direction of wood segments 101 and some wood segments 102 on the surface of the vertical wood board 100 to achieve a relatively large impregnation depth, and (2) further opening up the longitudinal pathways of wood segments 101 and some wood segments 102 under microwave heat, while avoiding the problem of rapid drug loss caused by the longitudinal direction of wood segments 101 and some wood segments 102 on the surface of the vertical wood board 100. The means to achieve this is to compress the longitudinal portion of wood segments 101 and some wood segments 102 through hot pressing. Generally, a compression of 8-10% can achieve complete compression of the drug impregnation thickness layer. By causing the fibers in this part to undergo morphological changes such as twisting and folding, the vertical pathways of wood segments 101 and some wood segments 102 are also twisted and folded, thereby partially sealing the drug loss pathways and achieving the technical effect of slowing down the drug loss rate.

[0063] Those skilled in the art will know that wood has relatively high longitudinal strength, so it is more difficult to compress than glued and cured fiber materials, meaning it requires greater pressure to be compressed. This embodiment overcomes the inertia of existing research and takes a different approach, combining microwave preheating, functional agent impregnation, and hot pressing. As a result, (1) under the same moisture content, due to the thermal barrier effect of the adhesive in the filler unit, the temperature of the main unit is higher than that of the filler unit after passing through the microwave thermal environment; and (2) during the impregnation process, the main unit can absorb more agents and make the impregnated layer of the main unit have a higher moisture content after impregnation. Generally speaking, the moisture content of the impregnated layer of the main unit after impregnation can reach 80-85%, while the moisture content of the impregnated layer of the filler unit is about 65%; at this time, (3) after the pressure plate of the hot press acts on the impregnated surface of the vertical wood board 100, due to the thermal barrier effect of the adhesive in the filler unit, the two will reach different preheating temperatures. The main unit reaches a higher preheating temperature than the filler unit. Combined with the higher moisture content of the main unit after impregnation, the two can reach the yield point at the same time and can be softened and compressed at the same time.

[0064] In summary, this embodiment utilizes the special structure of the vertical wood board 100 and combines microwave heating with hot pressing to simultaneously improve the amount of drug impregnation and slow down the rate of drug loss by taking advantage of the longitudinal characteristics of the wood.

[0065] After impregnation, the thickness of the main unit impregnation layer 901 is 1.6–1.7 mm, and the thickness of the filler unit impregnation layer 902 is 0.7–0.8 mm. After the surface sealing process, the main unit impregnation layer 901 and its underlying layer of a certain thickness are compressed. After compression, the thickness of the main unit impregnation layer 901 is 0.7–0.8 mm, and the thickness of the filler unit impregnation layer 902 is 0.4–0.5 mm. From the difference in the thickness changes of the main unit impregnation layer 901 and the filler unit impregnation layer 902 after compression, it can be seen that the compression of the main unit and the filler unit during the surface sealing process is slightly different. The former is closer to surface densification compression, while the latter is closer to overall densification compression. Specifically, although the thickness of the main unit impregnation layer 901 and the filler unit impregnation layer 902 is compressed, the drug loading of both remains unchanged because the upper and lower surfaces of the vertical wood board 100 are covered by pressure plates until cooled to room temperature during the surface sealing process, and no drug loss occurs during this process. In the subsequent drying process, after the moisture content of the functional vertical wood board is dried to 12–14%, the thickness of the main unit impregnation layer 901 remains 0.7–0.8 mm, and the thickness of the filler unit impregnation layer 902 is 0.4–0.5 mm. The drug impregnation depth (thickness of the main unit impregnation layer 901 and the filler unit impregnation layer 902) before and after drying demonstrates, to some extent, the effect of the surface sealing process on reducing and mitigating drug loss.

[0066] Example 7

[0067] The difference between Example 7 and Example 6 is that the material used to form the wood segment 101 is small-diameter timber, and the shape of the wood segment 101 is cylindrical. The surface sealing process of this example is as follows: First, the upper and lower pressure plates of the hot press are heated to 142±2℃, and the distance between the upper and lower pressure plates is controlled within 25mm; then, the intermediate product is placed on the lower pressure plate and the upper pressure plate is quickly closed. After preheating without pressure for 12s, the upper pressure plate is pressurized until the gauge reading pressure reaches 2.5MPa, with a compression of 8%. After reaching the compression, the pressure is maintained for 80s. After the pressure holding time is reached, the pressure is released and the upper and lower pressure plates are allowed to cool to room temperature before being opened. Finally, the functional vertical wood board of this example with a moisture content of 12-14% is obtained by kiln drying.

[0068] After impregnation, the thickness of the main unit impregnation layer 901 is 2.1–2.2 mm, and the thickness of the filler unit impregnation layer 902 is 0.8–1.0 mm. After the surface sealing process, the thickness of the main unit impregnation layer 901 is 0.9–1.0 mm, and the thickness of the filler unit impregnation layer 902 is 0.6 mm. After the drying process, the thickness of the main unit impregnation layer 901 remains 0.9–1.0 mm, and the thickness of the filler unit impregnation layer 902 is 0.55 mm.

[0069] Example 8

[0070] The difference between Example 8 and Example 6 is that the functional agent is a mixture of flame retardant and antifungal agent, wherein both the flame retardant and antifungal agent are commercially available, and the ratio of the two is 1:1.

[0071] Example 9

[0072] The difference between Example 9 and Example 6 is that the longitudinal direction of the wood segments 101 and some wood segments 102 in the main unit forms an angle of 60±5° with the surface of the vertical wood board. Specifically, the angle formed between the longitudinal direction L0 and the surface of the vertical wood board 100 is directional. Specifically, the plane formed by the axial direction of multiple wood segments 101 or some wood segments 102 arranged along the length direction of the vertical wood board 100 is perpendicular to the surface of the vertical wood board 100, and the plane formed by the axial direction of multiple wood segments 101 or some wood segments 102 arranged along the width direction of the vertical wood board 100 forms an angle of 60°±5° with the surface of the vertical wood board 100. Meanwhile, since the wood segments 101 or some wood segments 102 have inter-wood differences, even if the blanks are assembled in the same way, the angle between the wood segments 101 or some wood segments 102 in the vertical wood board 100 obtained after angled sawing will differ from the surface; an error within 5° is acceptable.

[0073] After impregnation, the thickness of the main unit impregnation layer 901 is 1.2–1.3 mm, and the thickness of the filler unit impregnation layer 902 is 0.8–1.0 mm. After the surface sealing process, the thickness of the main unit impregnation layer 901 is 0.65–0.7 mm, and the thickness of the filler unit impregnation layer 902 is 0.6 mm. After the drying process, the thickness of the main unit impregnation layer 901 is 0.62 mm, and the thickness of the filler unit impregnation layer 902 is 0.55 mm.

[0074] The product performance parameters of the functional vertical wood panels in Examples 1 to 9 are shown in Table 1. Among them, (1) the hexahedral vertical wood panel made according to the technical solution disclosed in Chinese Invention Patent No. CN104210013B, and the vertical wood panel was impregnated with an anti-mildew agent for 45 minutes at room temperature and pressure to obtain the functional vertical wood panel of control group 1; (2) ordinary high-density fiberboard was impregnated with a flame retardant agent for 45 minutes at room temperature and pressure to obtain the functional artificial board of control group 2; (3) the impregnation depth was expressed by the thickness of the impregnation layer 901 of the main unit and the impregnation layer 902 of the filling unit, and was observed and measured by adding colored pigments, such as ink, to the functional agent; (4) the agent loss rate was evaluated by the agent loss that occurred during the drying process and calculated according to the following formula:

[0075]

[0076] Where x represents the drug loss rate, in percentages.

[0077] D0—Depth of drug impregnation before drying, in mm;

[0078] D1—Depth of drug impregnation after drying, mm.

[0079] Table 1. Performance Parameters of Functional Vertical Wood Panels

[0080]

[0081] The above description is for illustrative purposes and not for limitation. Many embodiments and applications beyond the provided examples will become apparent to those skilled in the art upon reading the above description. Therefore, the scope of this teaching should not be determined by reference to the above description, but rather by reference to the appended claims and the full scope of their equivalents. For purposes of completeness, all articles and references, including patent applications and publications, are incorporated herein by reference. The omission of any aspect of the subject matter disclosed herein in the preceding claims is not intended as a waiver of that subject matter, nor should it be construed as an indication that the applicant has not considered that subject matter as part of the disclosed application subject matter.

Claims

1. A functional vertical wood panel, comprising a vertical wood panel, wherein at least one surface layer of the vertical wood panel is a functional impregnation layer formed by impregnation with a functional agent, the vertical wood panel comprising a main unit and a filling unit, the main unit comprising a plurality of arrayed wood segments and / or some wood segments, the longitudinal direction of the wood segments forming an angle with the surface of the vertical wood panel; characterized in that, The filling unit is a mixture of filler material and adhesive, which is compacted and pressed to fill the gaps between adjacent wood segments and / or partial wood segments and to bond the wood segments and / or partial wood segments together; the filler material is one or a mixture of granules, chips or fibers; The functional impregnation layer includes a main unit impregnation layer and a filler unit impregnation layer, which are formed by impregnating and penetrating the functional agent into the main unit and the filler unit respectively. The thickness of the main unit impregnation layer is 1.5 to 3.0 times that of the filler unit impregnation layer. The method for preparing the vertical timber board includes the following steps: The preheating process involves placing the vertical wooden board in a microwave environment for preheating. The temperature of the microwave environment is 50~60℃, and the preheating time is 50~70s. The impregnation process involves impregnating the vertical wood panels with the functional pharmaceutical agent under normal temperature and pressure conditions to obtain an intermediate product; In the process of sealing the surface, the intermediate product is placed in a thermo-pressure environment to compress at least one surface layer of the intermediate product; The surface sealing process involves heating at least one surface layer of the intermediate product with a hot plate at a temperature of 140-150°C for a preheating time of 10-30 seconds; subsequently, pressure of 2.5-2.7 MPa is applied to the surface layer for a pressing time of 70-90 seconds.

2. The functional vertical wood panel according to claim 1, characterized in that, The functional agent is one or a mixture of flame retardants and antifungal agents.

3. The functional vertical wood panel according to claim 1, characterized in that, The longitudinal direction of the wood segment and / or part of the wood segment forms an angle of 50° to 90° with the surface of the vertical wood board.

4. The functional vertical wood panel according to claim 1, characterized in that, The timber segments are in the form of cylinders, prisms, cubes, or elliptical cylinders; or The wood segments are partially cylindrical, partially prismatic, partially cubic, or partially elliptical.

Citation Information

Patent Citations

  • A manufacturing method for large cross-section hexagonal glued laminated timber

    CN104210013B

  • Impregnation densified veneer enhanced laminated veneer lumber and a manufacturing method thereof

    CN102179842A

  • Novel modularized integrated stone-bamboo composite wall component manufacturing method

    CN105863156A