Preparation method of titanium dioxide-tin dioxide composite nanomaterial for ammonia detection, product and application thereof
By controlling the preparation method of TiO₂-SnO₂ composite nanomaterials and utilizing the regulation of heterojunction structure and oxygen vacancies, the selectivity and stability issues of materials in ammonia detection were solved, and high-sensitivity ammonia detection was achieved.
Patent Information
- Application Number
- CN202211673854.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-26
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-12-26
AI Technical Summary
Existing simple semiconductor materials lack sufficient selectivity and long-term stability in ammonia detection, making it difficult to achieve highly sensitive detection.
TiO₂-SnO₂ composite nanomaterials were prepared by controlling the hydrolysis rates of Ti and Sn salts, and then subjected to heat treatment in a hydrogen-argon mixture to generate oxygen vacancies and form a heterojunction structure to enhance the defect control capability of the material.
This improved the sensitivity of ammonia detection and the stability of the materials, while reducing the temperature requirements for gas-sensitive reactions.
Abstract
Description
Technical Field
[0001] This invention relates to the field of gas detection, specifically to a method for preparing titanium dioxide-tin dioxide composite nanomaterials for ammonia detection, as well as its products and applications, and is a method for preparing semiconductor gas sensors. Background Technology
[0002] Metal oxide semiconductor materials have become gas-sensitive materials for detecting various toxic, harmful, flammable, and explosive gases due to their excellent stability and ease of synthesis and surface property control. However, pure semiconductor materials are not satisfactory in terms of selectivity and long-term stability. By constructing heterojunction structures during the preparation of nanomaterials, on the one hand, the difference in lattice parameters between the two materials can form a large number of defects. On the other hand, the heterojunction structure is more conducive to the catalytic reaction of the target gas on the material surface. Then, heat treatment in a reducing gas atmosphere can form a large number of oxygen defects, which is conducive to the adsorption of oxygen in the air to form active oxygen, which is beneficial to the gas-sensitive reaction. Summary of the Invention
[0003] The purpose of this invention is to provide a method for preparing titanium dioxide-tin dioxide composite nanomaterials for ammonia detection, which can achieve highly sensitive detection of ammonia.
[0004] Another object of the present invention is to provide a titanium dioxide-tin dioxide composite nanomaterial product for ammonia detection prepared by the above method.
[0005] Another object of the present invention is to provide an application of the above-mentioned product.
[0006] The objective of this invention is achieved through the following scheme: a method for preparing titanium dioxide-tin dioxide composite nanomaterials for ammonia detection, which involves controlling the hydrolysis rates of Ti salt and Sn salt, utilizing the different hydrolysis rates of anhydrous titanium tetrachloride and anhydrous tin tetrachloride to prepare TiO2-SnO2 composite nanomaterials, followed by heat treatment in a hydrogen-argon mixture of a certain concentration to generate more oxygen vacancies, thereby achieving defect control of the composite nanomaterials, including the following steps: Take 0.5~0.8 mmol of TiCl4 and 2.0~3.2 mmol of SnCl4, place them in 70 mL of glacial acetic acid, add 80~120 μL of nitric acid, stir for 30 min, and then add 1~3 mL of deionized water to obtain solution A; Take 0.05~0.08 g of PVP and place it in 30 mL of deionized water. After the PVP is completely dissolved, you will get solution B. Under stirring, solution B was slowly added dropwise to solution A. After the addition was complete, the mixture was stirred for 5 minutes. Then, it was placed in a 200 mL polytetrafluoroethylene hydrothermal reactor and hydrothermally reacted at 180-200 °C for 20-25 h. After cooling to room temperature, the sample was centrifuged, dried at 80 °C, ground, and then heat-treated in a hydrogen-argon mixture at a temperature of 650-700 °C for 1-3 h with a heating rate of 2-5 °C. After cooling to room temperature, TiO2-SnO2 composite nanomaterials were obtained. The hydrogen-argon mixture, wherein the concentration of hydrogen is 1-3%; A MEMS device with Pt interdigitated electrodes was ultrasonically cleaned with deionized water and ethanol, dried with a nitrogen gun, and the sample obtained in step four was made into a slurry and uniformly coated on the surface of the MEMS device. After drying, it was placed in a muffle furnace for heat treatment at a temperature of 400 ℃, a holding time of 1 h, and a heating rate of 2 ℃ / min. After the chamber cooled to room temperature, it was taken out to obtain a MEMS gas sensor based on TiO2-SnO2 nanomaterials.
[0007] This invention provides a titanium dioxide-tin dioxide composite nanomaterial for ammonia detection, which is prepared according to any of the methods described above.
[0008] This invention provides an application of titanium dioxide-tin dioxide composite nanomaterials for highly sensitive detection of ammonia.
[0009] The TiO2-SnO2 composite nanomaterials in this system have a large specific surface area and defects, and a heterogeneous structure, which can reduce the reaction temperature of gas-sensitive reactions and improve their sensitivity. Detailed Implementation
[0010] Example 1: A titanium dioxide-tin dioxide composite nanomaterial for ammonia detection is prepared by controlling the hydrolysis rates of Ti and Sn salts, utilizing the different hydrolysis rates of anhydrous titanium tetrachloride and anhydrous tin tetrachloride. The composite nanomaterial is then heat-treated in a hydrogen-argon mixture of a certain concentration to generate more oxygen vacancies, thus achieving defect control of the composite nanomaterial. The preparation steps are as follows: (1) Take 0.5 mmol of TiCl4 and 2.0 mmol of SnCl4, place them in 70 mL of glacial acetic acid, add 80 μL of nitric acid, stir for 30 min, and then add 1 mL of deionized water to obtain solution A; (2) Take 0.05g of PVP and place it in 30 mL of deionized water. After the PVP is completely dissolved, you will get solution B. (3) Under stirring, slowly add solution B to solution A. After the addition is complete, stir for 5 min and then place it in a 200 mL polytetrafluoroethylene hydrothermal reactor. The hydrothermal reaction is carried out at 180℃ for 20 h. After cooling to room temperature; (4) Centrifuge the sample, dry it at 80 °C and grind it. Then heat it in a hydrogen-argon mixture, where the hydrogen concentration is 1-3%. Heat it at 650 °C for 3 hours with a heating rate of 2-5 °C. After cooling to room temperature, TiO2-SnO2 composite nanomaterials are obtained.
[0011] Take a MEMS device with Pt interdigitated electrodes, clean it ultrasonically with deionized water and ethanol, dry it with a nitrogen gun, and then make the sample obtained in step (4) into a slurry. Coat it evenly on the surface of the MEMS device, dry it, and then place it in a muffle furnace for heat treatment. The heat treatment temperature is 400 ℃, the holding time is 1 h, and the heating rate is 2 ℃ / min. After the cavity cools down to room temperature, take it out to obtain a MEMS gas sensor based on TiO2-SnO2 nanomaterials.
[0012] The gas sensor of the device obtained in this embodiment has a sensitivity of 16.9 for ammonia gas at a concentration of 1 ppm when the operating temperature is 180 ℃.
[0013] Example 2: A titanium dioxide-tin dioxide composite nanomaterial for ammonia detection is prepared according to steps similar to those in Example 1, as follows: (1) Take 0.7 mmol of TiCl4 and 2.0 mmol of SnCl4, place them in 70 mL of glacial acetic acid, add 120 μL of nitric acid, stir for 30 min, and then add 2 mL of deionized water to obtain solution A; (2) Take 0.05 g of PVP and place it in 30 mL of deionized water. After the PVP is completely dissolved, you will get solution B. (3) Under stirring, slowly add solution B to solution A. After the addition is complete, stir for 5 min and then place it in a 200 mL polytetrafluoroethylene hydrothermal reactor. The hydrothermal reaction is carried out at 190 °C for 20 h. After cooling to room temperature; (4) Centrifuge the sample, dry it at 80 °C and grind it. Then place it in a hydrogen-argon mixture for heat treatment. The hydrogen concentration is 2%, the heat treatment temperature is 650 °C, the time is 2 h, the heating rate is 2 °C, and the TiO2-SnO2 composite nanomaterial is obtained after the heat is cooled to room temperature.
[0014] Take a MEMS device with Pt interdigitated electrodes, clean it ultrasonically with deionized water and ethanol, dry it with a nitrogen gun, and then make the sample obtained in step (4) into a slurry. Coat it evenly on the surface of the MEMS device, dry it, and then place it in a muffle furnace for heat treatment. The heat treatment temperature is 400 ℃, the holding time is 1 h, and the heating rate is 2 ℃ / min. After the cavity cools down to room temperature, take it out to obtain a MEMS gas sensor based on TiO2-SnO2 nanomaterials.
[0015] The gas sensor of the device obtained in this embodiment has a sensitivity of 18.8 to ammonia gas at a concentration of 1 ppm when the operating temperature is 180 ℃.
[0016] Example 3: A titanium dioxide-tin dioxide composite nanomaterial for ammonia detection is prepared according to steps similar to those in Example 1, as follows: (1) Take 0.8 mmol of TiCl4 and 3.2 mmol of SnCl4, place them in 70 mL of glacial acetic acid, add 100 μL of nitric acid, stir for 30 min, and then add 3 mL of deionized water to obtain solution A; (2) Take 0.07g of PVP and place it in 30 mL of deionized water. After the PVP is completely dissolved, solution B is obtained. (3) Under stirring, solution B is slowly added dropwise to solution A. After the addition is complete, stir for 5 min, then place it in a 200 mL polytetrafluoroethylene hydrothermal reactor and hydrothermally react at 200 °C for 20 h. After cooling to room temperature, the sample is obtained. (4) Centrifuge the sample, dry it at 80 °C and grind it. Then heat it in a hydrogen-argon mixture, where the hydrogen concentration is 3%, the heat treatment temperature is 700 °C, the time is 1 h, the heating rate is 2 °C, and after cooling to room temperature, TiO2-SnO2 composite nanomaterials are obtained.
[0017] A MEMS device with Pt interdigitated electrodes was ultrasonically cleaned with deionized water and ethanol, dried with a nitrogen gun, and the sample obtained in step four was made into a slurry and uniformly coated on the surface of the MEMS device. After drying, it was placed in a muffle furnace for heat treatment at a temperature of 400 ℃, a holding time of 1 h, and a heating rate of 2 ℃ / min. After the chamber cooled to room temperature, it was taken out to obtain a MEMS gas sensor based on TiO2-SnO2 nanomaterials.
[0018] The gas sensor of the device obtained in this embodiment has a sensitivity of 19.7 to ammonia gas at a concentration of 1 ppm when the operating temperature is 180 ℃.
Claims
1. A method for preparing a titanium dioxide-tin dioxide composite nanomaterial for ammonia detection, characterized in that, By controlling the hydrolysis rates of Ti and Sn salts, and taking advantage of the different hydrolysis rates of anhydrous titanium tetrachloride and anhydrous tin tetrachloride, TiO2-SnO2 composite nanomaterials were prepared. These nanomaterials were then heat-treated in a hydrogen-argon mixture of a certain concentration to generate more oxygen vacancies, thus achieving defect control of the composite nanomaterials. The process includes the following steps: Take 0.5~0.8 mmol of TiCl4 and 2.0~3.2 mmol of SnCl4, place them in 70 mL of glacial acetic acid, add 80~120 μL of nitric acid, stir for 30 min, and then add 1~3 mL of deionized water to obtain solution A; Take 0.05~0.08 g of PVP and place it in 30 mL of deionized water. After the PVP is completely dissolved, you will get solution B. Under stirring, solution B was slowly added dropwise to solution A. After the addition was complete, the mixture was stirred for 5 minutes. Then, it was placed in a 200 mL polytetrafluoroethylene hydrothermal reactor and hydrothermally reacted at 180-200 °C for 20-25 h. After cooling to room temperature, the sample was centrifuged, dried at 80 °C, ground, and then heat-treated in a hydrogen-argon mixture at a temperature of 650-700 °C for 1-3 h with a heating rate of 2-5 °C. After cooling to room temperature, TiO2-SnO2 composite nanomaterials were obtained. The obtained titanium dioxide-tin dioxide composite nanomaterials are used for highly sensitive detection of ammonia; among them, The hydrogen-argon mixture has a hydrogen concentration of 1-3%. 2.The method for preparing titanium dioxide-tin dioxide composite nanomaterials for ammonia detection according to claim 1, characterized in that, Prepare according to the following steps: (1) Take 0.5 mmol of TiCl4 and 2.0 mmol of SnCl4, place them in 70 mL of glacial acetic acid, add 80 μL of nitric acid, stir for 30 min, and then add 1 mL of deionized water to obtain solution A; (2) Take 0.05g of PVP and place it in 30 mL of deionized water. After the PVP is completely dissolved, you will get solution B. (3) Under stirring, slowly add solution B to solution A. After the addition is complete, stir for 5 min and then place it in a 200 mL polytetrafluoroethylene hydrothermal reactor. The hydrothermal reaction is carried out at 180 °C for 20 h. After cooling to room temperature; (4) Centrifuge the sample, dry it at 80 °C and grind it. Then heat it in a hydrogen-argon mixture, where the hydrogen concentration is 1-3%. Heat it at 650 °C for 3 hours with a heating rate of 2-5 °C. After cooling to room temperature, TiO2-SnO2 composite nanomaterials are obtained. 3.The method for preparing titanium dioxide-tin dioxide composite nanomaterials for ammonia detection according to claim 1, characterized in that, Prepare according to the following steps: (1) Take 0.7 mmol of TiCl4 and 2.0 mmol of SnCl4, place them in 70 mL of glacial acetic acid, add 120 μL of nitric acid, stir for 30 min, and then add 2 mL of deionized water to obtain solution A; (2) Take 0.05 g of PVP and place it in 30 mL of deionized water. After the PVP is completely dissolved, solution B is obtained. (3) Under stirring, slowly add solution B to solution A. After the addition is complete, stir for 5 min and then place it in a 200 mL polytetrafluoroethylene hydrothermal reactor. The hydrothermal reaction is carried out at 190 °C for 20 h. After cooling to room temperature; (4) Centrifuge the sample, dry it at 80 °C and grind it. Then place it in a hydrogen-argon mixture for heat treatment. The hydrogen concentration is 2%, the heat treatment temperature is 650 °C, the time is 2 h, the heating rate is 2 °C, and the TiO2-SnO2 composite nanomaterial is obtained after the heat is cooled to room temperature.
4. The method for preparing a titanium dioxide-tin dioxide composite nanomaterial for ammonia detection according to claim 1, characterized in that, Prepare according to the following steps: (1) Take 0.8 mmol of TiCl4 and 3.2 mmol of SnCl4, place them in 70 mL of glacial acetic acid, add 100 μL of nitric acid, stir for 30 min, and then add 3 mL of deionized water to obtain solution A; (2) Take 0.07g of PVP and place it in 30 mL of deionized water. After the PVP is completely dissolved, solution B is obtained. (3) Under stirring, solution B is slowly added dropwise to solution A. After the addition is complete, stir for 5 min and then place it in a 200 mL polytetrafluoroethylene hydrothermal reactor. The hydrothermal reaction is carried out at 200 °C for 20 h. After cooling to room temperature, the sample is obtained. (4) Centrifuge the sample, dry it at 80 °C and grind it. Then heat it in a hydrogen-argon mixture, where the hydrogen concentration is 3%, the heat treatment temperature is 700 °C, the time is 1 h, the heating rate is 2 °C, and after cooling to room temperature, TiO2-SnO2 composite nanomaterials are obtained.
5. A titanium dioxide-tin dioxide composite nanomaterial for ammonia detection, characterized in that... Prepared by the method according to any one of claims 1 to 4; A MEMS device with Pt interdigitated electrodes was ultrasonically cleaned with deionized water and ethanol, and dried with a nitrogen gun. The resulting titanium dioxide-tin dioxide composite nanomaterial sample was then made into a slurry, uniformly coated onto the surface of the MEMS device, and dried before being placed in a muffle furnace for heat treatment at 400 ℃ for 1 h at a heating rate of 2 ℃ / min. After the chamber cooled to room temperature, the device was removed to obtain a MEMS gas sensor based on TiO2-SnO2 nanomaterials.
Citation Information
Patent Citations
Preparation method of tin-doped titanium dioxide
CN103523826A
Sn-doped TiO2 nanopowder prepared through high-water-content direct solution oxidation method and application thereof
CN110314676A
TiO2 / SnO2 gas sensor based on ultraviolet band and preparation method
CN110687170A